Multi-layered polyimide film and its manufacturing method
A multilayer polyimide film with optimized composition and layer structure addresses dimensional stability and adhesive strength issues, ensuring high thermal and moisture stability with strong copper foil bonding for flexible metal foil laminates and electronic components.
Patent Information
- Application Number
- JP2024531726
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-29
- Filing Date
- 2022-11-28
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-11-28
AI Technical Summary
Existing polyimide films face challenges with low thermal and moisture dimensional stability and decreased adhesive strength with sputtered metal plating, particularly in flexible metal foil laminates.
A multilayer polyimide film structure with specific composition ratios and layers, including a core layer and skin layers, enhances thermal and moisture dimensional stability while maintaining excellent adhesive strength with copper foil.
The multilayer polyimide film achieves high thermal dimensional stability, moisture resistance, and strong adhesion to copper foil, suitable for flexible metal foil laminates and electronic components.
Smart Images

Figure 2024543562000001 
Figure 2024543562000002 
Figure 2024543562000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer polyimide film having excellent dimensional stability and excellent adhesive strength, and more particularly to a multilayer polyimide film having high dimensional stability against heat and moisture and excellent adhesive strength, and a method for producing the same. [Background technology]
[0002] Polyimide (PI) is a polymeric material based on imide rings, which have excellent chemical stability along with a rigid aromatic main chain, and has the highest levels of heat resistance, chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials. Polyimide films have been attracting attention as a material for a variety of electronic devices that require the above-mentioned properties. An example of a microelectronic component to which polyimide films are applied is a flexible thin circuit board having a high degree of circuit integration so as to accommodate the trend toward lighter and smaller electronic products. Polyimide films are particularly widely used as insulating films for thin circuit boards. The thin circuit board generally has a structure in which a circuit including a metal foil is formed on an insulating film, and such a thin circuit board is broadly called a flexible metal foil clad laminate (Flexible Metal Foil Clad Laminate), and when a thin copper plate is used as the metal foil, it is more narrowly called a flexible copper clad laminate (FCCL).
[0003] Examples of methods for producing flexible metal foil laminates include (i) a casting method in which polyamic acid, a precursor of polyimide, is cast or coated onto a metal foil and then imidized, (ii) a metallizing method in which a metal layer is directly formed on a polyimide film by sputtering, and (iii) a lamination method in which a polyimide film and a metal foil are bonded together by heat and pressure via a thermoplastic polyimide. In particular, the metallizing method is a method for producing flexible metal foil laminates by sputtering a metal such as copper on a polyimide film having a thickness of, for example, 20 to 38 μm, and sequentially depositing a tie layer and a seed layer. This method is advantageous in forming ultra-fine circuits with a circuit pattern pitch of 35 μm or less, and is widely used to manufacture flexible metal foil laminates for COF (chip on film). Polyimide films used in flexible metal foil laminates using the metallizing method must have high dimensional stability. Usually, dimensional stability is measured by thermal dimensional stability represented by the thermal expansion coefficient, but dimensional stability against moisture represented by the hygroscopic expansion coefficient, which is no less important than thermal dimensional stability, is becoming increasingly important. That is, there is an increasing demand for polyimide films that are excellent in both thermal dimensional stability and moisture dimensional stability. However, when a polyimide film is actually designed to have a structure with a low thermal expansion coefficient and high thermal dimensional stability, a problem of low moisture dimensional stability has arisen. Furthermore, polyimide films, which have a high degree of dimensional restriction, usually have the problem of reduced adhesive strength with sputtered metal plating. Therefore, there is a strong demand for polyimide films that not only have high thermal dimensional stability and high dimensional stability against moisture, but also have excellent adhesive strength. The matters described in the above background art are intended to aid in understanding the background of the invention, and may include matters that are not prior art already known to those having ordinary skill in the art to which this technology pertains. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Republic of Korea Patent Publication No. 10-2012-0133807 Summary of the Invention [Problem to be solved by the invention]
[0005] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a polyimide multilayer film which has high dimensional stability against heat and moisture as well as excellent adhesive strength. However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0006] In order to achieve the above object, one aspect of the present invention includes a first skin layer and a second skin layer formed on one outer surface of a core layer and an opposite surface of the outer surface, respectively, The adhesive strength with copper foil is 0.8kgf / cm or more. A multi-layer polyimide film is provided.
[0007] Another aspect of the present invention is a multilayer polyimide film comprising the multilayer polyimide film and an electrically conductive metal foil, A flexible metal foil laminate is provided.
[0008] Yet another aspect of the present invention includes the flexible metal foil laminate, Provide electronic components. Effect of the Invention
[0009] The present invention provides a polyimide film in which the composition ratio, reaction ratio, etc. of dianhydride and diamine components are adjusted, thereby providing a polyimide film that is excellent in thermal dimensional stability, dimensional stability against moisture, and adhesive strength. Such polyimide films are applicable to various fields requiring polyimide films with excellent dimensional stability and adhesive strength, for example, flexible metal foil laminates produced by a metallizing method or electronic parts including such flexible metal foil laminates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that corresponds to the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to explain his / her invention in the best possible way. Therefore, it should be understood that the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention and does not fully represent the technical ideas of the present invention, and that there may be various equivalents and modifications that can replace them at the time of this application.
[0011] In this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that in this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0012] As used herein, "dianhydride acid" is intended to include precursors or derivatives thereof, which may not technically be dianhydrides, but which are nevertheless diamines. It should react with the amine to form a polyamic acid, which is then converted back to a polyimide.
[0013] As used herein, "diamine" is intended to include precursors or derivatives thereof, which may not technically be diamines, but which nevertheless must react with a dianhydride to form a polyamic acid, which is then converted back to a polyimide.
[0014] Whenever an amount, concentration, or other value or parameter is given herein as a range, a preferred range or a list of an upper preferred value and a lower preferred value, it should be understood to specifically disclose all ranges formed by any pair of any upper range limit or preferred value, and any lower range limit or preferred value, regardless of whether a range is otherwise disclosed.
[0015] Where a range of numerical values is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values recited when defining a range.
[0016] The multilayer polyimide film according to one embodiment of the present invention may include a first skin layer and a second skin layer formed on one outer surface of a core layer and an opposite surface of the outer surface, respectively, and may have an adhesive strength to a copper foil of 0.8 kgf / cm or more.
[0017] That is, the multilayer polyimide film may be a three-layered multilayer polyimide film having a core layer and a first skin layer and a second skin layer formed on one outer surface of the core layer and on the opposite surface of the core layer, respectively.
[0018] On the other hand, the components and composition ratios of the first and second skin layers may be the same or different. In addition, the first and second skin layers may have the same or different thicknesses.The copper foil is formed on at least one surface of the multi-layered polyimide film of the present invention by a sputter-electroplating method.
[0019] In one embodiment, the multilayer polyimide film may have a thermal expansion coefficient in a transverse direction (TD) of 2.0 ppm / °C or more and 6.0 ppm / °C or less, and a moisture expansion coefficient in a transverse direction (TD) of 3.0 ppm / RH% or more and 6.0 ppm / RH% or less.
[0020] The thermal expansion coefficient in the transverse direction (TD) may be, for example, 2.5 ppm / °C or more and 6.0 ppm / °C or less.
[0021] The moisture expansion coefficient in the transverse direction (TD) may be, for example, 4.5 ppm / RH% or more and 6.0 ppm / RH% or less.
[0022] In one embodiment, the core layer of the multilayer polyimide film is obtained by imidizing a polyamic acid solution containing a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA) and a diamine component including paraphenylenediamine (PPD) and m-tolidine.
[0023] On the other hand, at least one of the first skin layer and the second skin layer is made of biphenyl tetraacetate. The polyamic acid solution is obtained by imidization reaction of a polyamic acid solution containing a dianhydride component including two or more selected from the group consisting of dicarboxylic dianhydride, pyromeristic dianhydride, oxydiphthalic anhydride (ODPA), and benzophenonetetracarboxylic dianhydride (BTDA), and a diamine component including one or more selected from the group consisting of oxydianiline (ODA) and 1,3-bisaminophenoxybenzene (TPE-R).
[0024] For example, any one or more of the first skin layer and the second skin layer may use, as the dianhydride acid component, biphenyltetracarboxylic dianhydride and pyromelitic dianhydride together, or biphenyltetracarboxylic dianhydride, pyromelitic dianhydride and oxydiphthalic anhydride together, or biphenyltetracarboxylic dianhydride, pyromelitic dianhydride and benzophenonetetracarboxylic dianhydride together. Also, for example, at least one of the first skin layer and the second skin layer may use only oxydianiline as the diamine component, or may use oxydianiline and 1,3-bisaminophenoxybenzene together.
[0025] In one embodiment, the core layer may have a biphenyltetracarboxylic dianhydride content of 40 mol% or more and 60 mol% or less, and a pyromellitic dianhydride content of 40 mol% or more and 60 mol% or less, based on a total content of the dianhydride acid components of 100 mol%, and a paraphenylenediamine content of 50 mol% or more and 70 mol% or less, and a m-tolidine content of 30 mol% or more and 50 mol% or less, based on a total content of the diamine components of 100 mol%.
[0026] In one embodiment, at least one of the first skin layer and the second skin layer may have a biphenyltetracarboxylic dianhydride content of 15 mol% or more and 85 mol% or less, a pyromellitic dianhydride content of 15 mol% or more and 60 mol% or less, an oxydiphthalic anhydride content of 35 mol% or less, and a benzophenonetetracarboxylic dianhydride content of 35 mol% or less, based on a total content of 100 mol% of the dianhydride acid components, a content of oxydianiline of 20 mol% or more and 100 mol% or less, and a content of 1,3-bisaminophenoxybenzene of 80 mol% or less, based on a total content of 100 mol% of the diamine components.
[0027] The paraphenylenediamine of the present invention is a rigid monomer, and by increasing the content of paraphenylenediamine, the synthesized polyimide has a more linear structure, which contributes to improving the mechanical properties of the polyimide.
[0028] Furthermore, m-tolidine has a methyl group that exhibits hydrophobicity, and contributes to the low moisture absorption characteristic related to the dimensional stability of the polyimide film against moisture.
[0029] The polyimide chain derived from the biphenyltetracarboxylic dianhydride of the present invention has a structure called a charge transfer complex (CTC), i.e., a regular linear structure in which an electron donor and an electron acceptor are located close to each other, and intermolecular interactions are strengthened.
[0030] This structure has the effect of preventing hydrogen bonding with moisture, which reduces the moisture absorption rate. This maximizes the effect of reducing the moisture absorption of the polyimide film, which affects the dimensional stability against moisture.
[0031] In addition, pyromellitic dianhydrides are preferred in that they are dianhydride acid components having a relatively rigid structure and can impart suitable elasticity to the polyimide film.
[0032] In order for the polyimide film to have excellent dimensional stability, the content ratio of the dianhydride acid is important. For example, as the content ratio of biphenyltetracarboxylic dianhydride decreases, it becomes difficult to expect a low moisture absorption rate due to the CTC structure, and the dimensional stability against moisture also decreases.
[0033] In addition, biphenyltetracarboxylic dianhydride contains two benzene rings corresponding to the aromatic moiety, whereas pyromelitic dianhydride contains one benzene ring corresponding to the aromatic moiety.
[0034] An increase in the content of pyromellitic dianhydride in the dianhydride acid component can be understood as an increase in the imide groups in the molecule based on the same molecular weight, which can be understood as a relative increase in the ratio of imide groups derived from the pyromellitic dianhydride in the polyimide polymer chain compared to the imide groups derived from biphenyltetracarboxylic dianhydride.
[0035] In other words, an increase in the content of pyromellitic dianhydride is seen as a relative increase in imide groups with respect to the entire polyimide film, and this makes it difficult to expect high dimensional stability against moisture due to a low moisture absorption rate.
[0036] Conversely, if the content ratio of the pyromellitic dianhydride is decreased, the components having a relatively rigid structure are decreased, and the elasticity of the polyimide film may be decreased below a desired level.
[0037] For this reason, if the content of the biphenyltetracarboxylic dianhydride exceeds the above range or the content of the pyromellitic dianhydride falls below the above range, the dimensional stability of the polyimide film may be reduced.
[0038] Conversely, if the content of the biphenyltetracarboxylic dianhydride is below the above range or the content of the pyromellitic dianhydride is above the above range, this may also adversely affect the dimensional stability of the polyimide film.
[0039] In the present invention, the polyamic acid can be produced, for example, by (1) A method in which the entire amount of the diamine component is placed in a solvent, and then the dianhydride component is added in an amount substantially equimolar to the diamine component to polymerize it; (2) A method in which the entire amount of the dianhydride component is placed in a solvent, and then a diamine component is added in an amount substantially equimolar to the dianhydride component to polymerize it; (3) A method in which a part of the diamine component is placed in a solvent, a part of the dianhydride component is mixed with the reaction components in a ratio of about 95 to 105 mol %, the remaining diamine component is added, and the remaining dianhydride component is added successively thereto, so that the diamine component and the dianhydride component are polymerized in substantially equimolar amounts; (4) A method in which a dianhydride component is placed in a solvent, a part of the components in the diamine compound is mixed in a ratio of 95 to 105 mol % relative to the reactive components, and then another dianhydride component is added, followed by the remaining diamine component, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (5) A mixture of a part of the diamine component and a part of the dianhydride component in a solvent is and a method of forming a first composition by reacting a part of the diamine component and a part of the dianhydride acid component in another solvent so that one of them is in excess to form a second composition, and then mixing the first and second compositions to complete the polymerization, in which if the diamine component is in excess when the first composition is formed, the dianhydride acid component is in excess in the second composition, and if the dianhydride acid component is in excess in the first composition, the diamine component is in excess in the second composition, and the first and second compositions are mixed to polymerize so that the total diamine components and dianhydride acid components used in these reactions are substantially equimolar.
[0040] In the present invention, the polymerization method of the polyamic acid as described above can be defined as a random polymerization method, and the polyimide film prepared from the polyamic acid of the present invention prepared by the above process can be preferably applied in terms of maximizing the effects of the present invention, which are to improve dimensional stability and chemical resistance.
[0041] However, in the above polymerization method, the length of the repeating unit in the polymer chain is relatively short as described above, so that there may be a limit to the excellent properties of the polyimide chain derived from the dianhydride acid component. Therefore, the polymerization method of polyamic acid that can be particularly preferably used in the present invention is the block polymerization method.
[0042] On the other hand, the solvent for synthesizing the polyamic acid is not particularly limited, and any solvent that dissolves the polyamic acid can be used, but an amide-based solvent is preferable. Specifically, the organic solvent may be an organic polar solvent, more specifically, an aprotic polar solvent, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more kinds as needed.
[0043] In one example, the organic solvent that can be particularly preferably used is N,N-dimethylformamide or N,N-dimethylacetamide.
[0044] In addition, in the process for producing the polyamic acid, a filler may be added for the purpose of improving various properties of the film such as sliding properties, thermal conductivity, corona resistance, loop hardness, etc. The filler to be added is not particularly limited, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0045] The particle size of the filler is not particularly limited and may be determined depending on the film properties to be modified and the type of filler to be added. In general, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm.
[0046] If the particle size is below this range, the modifying effect is unlikely to be achieved, whereas if it exceeds this range, the surface properties may be significantly damaged or the mechanical properties may be significantly reduced.
[0047] The amount of the filler to be added is not particularly limited, and may be determined depending on the film properties to be modified, the particle size of the filler, etc. In general, the amount of the filler to be added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight, relative to 100 parts by weight of polyimide.
[0048] If the amount of the filler added is less than this range, the modifying effect of the filler is unlikely to be exhibited, and if the amount exceeds this range, the mechanical properties of the film may be significantly damaged. The method of adding the filler is not particularly limited, and any known method may be used.
[0049] In the production method of the present invention, the polyimide film is produced by a thermal imidization method and a chemical imidization method.
[0050] Alternatively, the imidation layer may be produced by a hybrid imidation method in which a thermal imidization method and a chemical imidization method are performed in parallel.
[0051] The thermal imidization method is a method in which a chemical catalyst is excluded and the imidization reaction is induced by a heat source such as hot air or an infrared dryer. The thermal imidization method can imidize the amic acid groups present in the gel film by heat-treating the gel film at a variable temperature in the range of 100 to 600°C, specifically, by heat-treating the gel film at 200 to 500°C, more specifically, by heat-treating the gel film at 300 to 500°C, to imidize the amic acid groups present in the gel film. However, even during the process of forming the gel film, a portion of the amic acid (approximately 0.1 mol % to 10 mol %) is imidized, and therefore the polyamic acid composition can be dried at a variable temperature in the range of 50°C to 200°C, which also falls within the category of the thermal imidization method.
[0052] In the case of the chemical imidization method, a polyimide film can be produced using a dehydrating agent and an imidization agent by methods known in the art.
[0053] As an example of the composite imidization method, a polyimide film can be produced by adding a dehydrating agent and an imidization agent to a polyamic acid solution, heating the solution at 80 to 200°C, preferably 100 to 180°C, partially curing and drying the solution, and then heating the solution at 200 to 400°C for 5 to 400 seconds.
[0054] Meanwhile, the multi-layer polyimide film of the present invention described above is manufactured by using at least one of coextrusion and coating.
[0055] In the co-extrusion method, a polyamic acid solution or a polyimide resin produced by imidizing the polyamic acid solution is filled in a storage tank, and then the solution is extruded in multiple layers onto a casting belt using a co-extrusion die, and then cured to produce a multi-layered polyimide film. This method has high productivity and ensures high interfacial adhesion reliability by mixing different types of polyimide resins at the interfaces. For example, a method for producing a multilayer polyimide film of the present invention includes a first filling step of filling a first storage tank with a first solution, which is a first polyamic acid solution or a first polyimide resin produced by imidizing the first polyamic acid solution; a second filling step of filling a second storage tank with a second solution, which is a second polyamic acid solution or a second polyimide resin produced by imidizing the second polyamic acid solution; a co-extrusion step of co-extruding the first and second solutions through a co-extrusion die having a first flow path connected to the first storage tank, a second flow path connected to the second storage tank, and a third flow path connected to the second storage tank, respectively; and a curing step of curing the first and second solutions extruded by the co-extrusion.
[0056] The first polyamic acid solution is for forming the core layer, and is preferably produced by polymerizing a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA) with a diamine component including paraphenylenediamine (PPD) and m-tolidine.
[0057] The second polyamic acid solution is for forming the first skin layer and the second skin layer, and is preferably produced by polymerizing a dianhydride acid component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride, pyromeristic dianhydride, oxydiphthalic anhydride (ODPA), and benzophenonetetracarboxylic dianhydride (BTDA), and a diamine component including one or more selected from the group consisting of oxydianiline (ODA) and 1,3-bisaminophenoxybenzene (TPE-R).
[0058] Meanwhile, when the first polyamic acid solution is used as the first solution and the second polyamic acid solution is used as the second solution, it is preferable to further include an imidization step of imidizing the first and second solutions co-extruded before the curing step.
[0059] The present invention provides a flexible metal foil laminate comprising the above-mentioned multilayer polyimide film and an electrically conductive metal foil.
[0060] The metal foil used is not particularly limited, but when the flexible metal foil laminate of the present invention is used for electronic or electrical equipment, the metal foil may be, for example, copper or a copper alloy, stainless steel or an alloy thereof, nickel or a nickel alloy (including alloy 42), aluminum or an aluminum alloy.
[0061] In general flexible metal foil laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, and are also preferably usable in the present invention. In addition, the surface of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer.
[0062] In the present invention, the thickness of the metal foil is not particularly limited, and may be any thickness that can exhibit sufficient functionality depending on the application.
[0063] The flexible metal foil laminate according to the present invention may have a structure in which a metal foil is laminated on at least one surface of the multilayer polyimide film. EXAMPLES
[0064] The functions and effects of the present invention will be described in more detail below through specific manufacturing examples and examples of the present invention, however, these manufacturing examples and examples are presented only as examples of the present invention and do not limit the scope of the invention.
[0065] Manufacturing example: Manufacturing of multi-layer polyimide film A first polyamic acid solution to be used for manufacturing the core layer was prepared by polymerizing dianhydride and diamine components selected from biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), oxydiphthalic anhydride (ODPA), benzophenonetetracarboxylic dianhydride (BTDA), paraphenylenediamine (PPD), m-tolidine (MTD), 1,3-bisaminophenoxybenzene (TPE-R), and oxydianiline (ODA). A dianhydride acid and a diamine component were selected from biphenyltetracarboxylic dianhydride, pyromeritic dianhydride, oxydiphthalic anhydride, benzophenonetetracarboxylic dianhydride, paraphenylenediamine, m-tolidine, 1,3-bisaminophenoxybenzene, and oxydianiline, and were polymerized to produce a second polyamic acid solution used in the production of the first and second skin layers. The first polyamic acid solution and the second polyamic acid solution prepared above are co-extruded. The resulting polyimide film was co-extruded, imidized, and cured to produce a multi-layer polyimide film having a core layer and a first skin layer and a second skin layer formed therearound. Here, however, the core layer was produced by co-extruding a first polyamic acid solution, and the first and second skin layers were produced by co-extruding a second polyamic acid solution. In preparing the polyamic acid, the solvent may be an aprotic solvent, typically an amide-based solvent, such as N,N'-dimethylformamide, N,N'-dimethylacetamide, N-methyl-pyrrolidone, or a combination thereof. The dianhydride and diamine components may be added in the form of powder, lump, or solution. It is preferable to add them in the form of powder at the beginning of the reaction to proceed with the reaction, and then add them in the form of a solution to adjust the polymerization viscosity. The resulting polyamic acid solution is mixed with an imidization catalyst and a dehydrating agent and applied to a support. Examples of catalysts that may be used include tertiary amines (eg, isoquinoline, β-picoline, pyridine, etc.), and examples of dehydrating agents include, but are not limited to, acid anhydrides.
[0066] Examples and Comparative Examples As shown in Table 1 (components and composition ratios of the core layer) and Table 2 (components and composition ratios of the skin layer) below, the contents of the dianhydride acid component and the diamine component in the core layer and skin layer in Examples 1 to 6 and Comparative Examples 1 to 9 were adjusted to produce multilayer polyimide films according to the production examples. The first and second skin layers of Examples 1 to 6 and Comparative Example 9 were manufactured to have the same composition and component ratio, and also to the same thickness. However, Comparative Examples 1 to 8 correspond to single-layer polyimide films, and only the core layer was produced.
[0067] [Table 1]
[0068] [Table 2]
[0069] The coefficient of thermal expansion (CTE), coefficient of hydroscopic expansion (CHE) and adhesive strength of the prepared polyimide film were measured and are shown in Table 3 below.
[0070] [Table 3]
[0071] (1) Measurement of thermal expansion coefficient The coefficient of thermal expansion (CTE) was measured using a TA thermomechanical analyzer, model Q400. The manufactured multilayer polyimide film was cut into a width of 4 mm and a length of 20 mm, and then heated from 30°C to 400°C at a rate of 10°C / min while applying a tension of 0.05 N under a nitrogen atmosphere, and then cooled again at a rate of 10°C / min to measure the slope in the range from 50°C to 200°C.
[0072] (2) Measurement of hygroscopic expansion coefficient The coefficient of moisture expansion (CHE) was measured by adjusting the humidity to 3% RH at 25°C under a minimum load (approximately 1 g for a 25 mm × 150 mm sample) to prevent the manufactured multilayer polyimide film from becoming loose, allowing the film to absorb moisture until it was completely saturated, and then measuring the dimensions. Thereafter, the humidity was adjusted to 90% RH, and the film was allowed to absorb moisture to saturation in the same manner, after which the dimensions were measured, and the dimensional change rate was calculated from both results.
[0073] (3) Measurement of adhesive strength A copper thin film layer having a thickness of about 80-300 nm was deposited on the manufactured multi-layer polyimide film by sputtering as a copper seed layer for electroplating electrodes, and a copper conductive layer having a thickness of about 8-9 μm was formed by electroplating to manufacture a flexible metal foil laminate for COF. The flexible metal foil laminate was etched into a rod shape of 2 mm width by a wet etching method, and then a 90° peel test was carried out using a Universal Testing Machine, and the adhesive strength was measured by pulling at a speed of 20 mm / min.
[0074] As a result of the measurements, the multilayer polyimide films of Examples 1 to 6 exhibited the following properties: a thermal expansion coefficient in the width direction of 2.0 ppm / °C or more and 6.0 ppm / °C or less, a moisture expansion coefficient in the width direction of 3.0 ppm / RH% or more and 6.0 ppm / RH% or less, and an adhesive strength to copper foil of 0.8 kgf / cm or more. In contrast, the polyimide films of Comparative Examples 1 to 8 and the multilayer polyimide film of Comparative Example 9, which were composed of only one layer and had different components and / or composition ratios from those of the Examples, were unable to satisfy the properties required of the multilayer polyimide film of the present application in at least one of the properties of thermal expansion coefficient, hygroscopic expansion coefficient, and adhesion to copper foil. Therefore, the multilayer polyimide films of Examples 1 to 6 produced within the appropriate range of the present application were all excellent in thermal dimensional stability, dimensional stability against moisture, and adhesion to copper foil. However, it was confirmed that when the appropriate range of the present application is exceeded, it is difficult to satisfy all of the thermal dimensional stability, dimensional stability against moisture, and adhesion to copper foil of the multilayer polyimide films of the present application. In other words, it was confirmed that the multilayer polyimide film that has excellent dimensional stability and adhesion to copper foil and satisfies all of the various conditions applicable to various fields of application is the multilayer polyimide film manufactured within the appropriate range of the present application.
[0075] The examples of the multilayer polyimide film and the method for manufacturing the multilayer polyimide film of the present invention are merely preferred examples that enable a person having ordinary skill in the art to easily carry out the present invention, and the present invention is not limited to the above-mentioned examples, and the scope of the present invention is not limited by these examples. Therefore, the true technical scope of the present invention must be determined by the technical ideas of the appended claims. In addition, it is obvious to a person skilled in the art that various substitutions, modifications and changes are possible within the scope of the present invention, and it is obvious that the parts that can be easily modified by a person skilled in the art are also included in the scope of the present invention. [Industrial Applicability]
[0076] The present invention provides a polyimide film in which the composition ratio, reaction ratio, etc. of dianhydride and diamine components are adjusted, thereby providing a polyimide film that is excellent in thermal dimensional stability, dimensional stability against moisture, and adhesive strength. Such polyimide films are applicable to various fields requiring polyimide films with excellent dimensional stability and adhesive strength, for example, flexible metal foil laminates produced by a metallizing method or electronic parts including such flexible metal foil laminates.
Claims
1. a first skin layer and a second skin layer formed on one outer surface of a core layer and on an opposite surface of the outer surface, respectively; The adhesive strength with copper foil is 0.8 kgf / cm or more. Multi-layer polyimide film.
2. The thermal expansion coefficient in the transverse direction (TD) is 2.0 ppm / °C or more and 6.0 ppm / °C or less; The moisture expansion coefficient in the transverse direction (TD) is 3.0 ppm / RH% or more and 6.0 ppm / RH% or less. The multilayer polyimide film according to claim 1 .
3. The core layer comprises a dianhydride acid component including biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA); A polyamic acid solution containing a diamine component including paraphenylenediamine (PPD) and m-tolidine is subjected to an imidization reaction. The multilayer polyimide film according to claim 1 .
4. At least one selected from the group consisting of the first skin layer and the second skin layer includes a dianhydride acid component including at least two selected from the group consisting of biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, oxydiphthalic anhydride (ODPA) and benzophenonetetracarboxylic dianhydride (BTDA); and a diamine component including at least one selected from the group consisting of oxydianiline (ODA) and 1,3-bisaminophenoxybenzene (TPE-R), The multilayer polyimide film according to claim 1 .
5. The content of the biphenyltetracarboxylic dianhydride is 40 mol% or more and 60 mol% or less, and the content of the pyromellitic dianhydride is 40 mol% or more and 60 mol% or less, based on 100 mol% of the total content of the dianhydride acid components; the content of the paraphenylenediamine is 50 mol % or more and 70 mol % or less, and the content of the m-tolidine is 30 mol % or more and 50 mol % or less, based on 100 mol % of the total content of the diamine components; The multilayer polyimide film according to claim 3 .
6. With respect to 100 mol% of the total content of the dianhydride acid components, the content of the biphenyltetracarboxylic dianhydride is 15 mol% or more and 85 mol% or less, the content of the pyromellitic dianhydride is 15 mol% or more and 60 mol% or less, the content of the oxydiphthalic anhydride is 35 mol% or less, and the content of the benzophenonetetracarboxylic dianhydride is 35 mol% or less, the content of the oxydianiline is 20 mol % or more and 100 mol % or less, and the content of the 1,3-bisaminophenoxybenzene is 80 mol % or less, based on 100 mol % of the total content of the diamine components; The multilayer polyimide film according to claim 4.
7. The multilayer polyimide film is produced by one or more methods selected from the group consisting of coextrusion and coating. The multilayer polyimide film according to any one of claims 1 to 6.
8. A multilayer polyimide film according to any one of claims 1 to 6, comprising an electrically conductive metal foil. Flexible metal foil laminate.
9. The flexible metal foil laminate of claim 8, Electronic components.
Citation Information
Patent Citations
Laminate for wiring board
JP2006270029A
Method and apparatus for providing home cooking contents in multiple languages
KR1020220126597A
Method for Preparing Multilayered Polyimide Film and Multilayered Polyimide Film by the Method
KR1020120133807A