Method for processing fiber-reinforced composite materials
By using bio-based solvents to treat fiber-reinforced epoxy resin composites, efficient decomposition of epoxy resin and fiber recycling are achieved, solving the dependence problem of petroleum-based solvents in traditional methods, and improving treatment efficiency and sustainability.
Patent Information
- Application Number
- JP2024532822
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art lacks effective methods for treating and recycling fiber-reinforced epoxy resin composites, especially carbon fiber-reinforced epoxy resin composites, resulting in the inability to efficiently recycle their wastes, and traditional solvent pretreatment methods rely on petroleum-based solvents, affecting sustainability.
Using bio-based solvents such as levoglucosenone and its derivatives as solvents, the swelling and layering of the fiber-reinforced epoxy resin composite material is achieved by controlling the Hansen dissolution parameters and treatment temperature of the solvent, and then subjecting to enzymatic and chemical treatment to decompose the epoxy resin and recover the fiber material.
It realizes efficient decomposition of epoxy resin composite materials and fiber recycling, avoids the use of petroleum-based solvents, improves treatment efficiency and enhances sustainability, and is suitable for highly crosslinked composite materials.
Smart Images

Figure 2024543580000001 
Figure 2024543580000002 
Figure 2024543580000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for treating fiber reinforced epoxy composites with certain organic solvents capable of swelling and exfoliating the fiber reinforced epoxy composites, related composite-solvent system compositions, and processes involving said treatment method for causing degradation of fiber reinforced epoxy composites, recovering the fibers therefrom, and recycling the fibers. [Background technology]
[0002] The global demand for fiber reinforced epoxy composites, especially carbon fiber reinforced epoxy composites (CFRP embedded in epoxy resin), has increased exponentially in the last few years due to the increased demand for lightweight materials. Due to the absence of effective recycling methods, most composite waste is not treated / recycled and is sent to landfills. There is still a need for robust and effective methods to treat such composites and complete their life cycle.
[0003] Recycling of epoxy composites presents a difficult challenge since epoxies are usually highly crosslinked three-dimensional structures that are insoluble under mild conditions. Most efforts to recycle epoxy composites have focused primarily on recovering the more valuable components, namely the reinforcing fibers. Therefore, chemical treatments have been preferentially developed, as they can cause the degradation of the epoxy components without substantially damaging the reinforcing fibers (which mechanical and thermal treatments do not).
[0004] Many such chemical treatments have been reported in Y.Ma and S.Nutt in Polymer Degradation and Stability,2018,153,307-317, especially the introduction on page 2. In this paper, Ma and Nutt's work focused on the acid digestion of carbon fiber reinforced amine / epoxy composites on the one hand, and on the depolymerization of the same composites using a supersaturated solution of benzyl alcohol and tripotassium phosphate on the other hand. In both cases, they confirmed that the degradation of the epoxy matrix resulting from the chemical treatments was very slow, which was due to the very low diffusion rate inside the highly crosslinked epoxy matrix.
[0005] To increase the diffusion rate inside the epoxy matrix and accelerate their degradation, Ma and Nutt developed two strategies. One was based on fracturing the end-of-life composites with the intention of thermally decomposing them, and therefore obviously did not retain our attention. The other consisted of a pretreatment in which the composites were immersed in an organic solvent before starting the chemical treatment itself, in order to physically "permeable" (swell) the composites without destroying the fiber weave in the polymer matrix. As Ma and Nutt explain amply, "the solvent penetrates the crosslinked network, allowing the reactant molecules to reach more easily cleavable bonds <during the chemical treatment itself>, thus reducing / eliminating the rate-limiting effect of diffusion. Various solvents were evaluated, including benzyl alcohol, xylene, diethylene glycol, dimethyl ether (DGDME), and diethylene glycol methyl ether (DGME). Testing revealed that the most promising pretreatment solvent was the matrix T. g The most effective decomposition time was determined to be 1.5 hours per millimeter of laminate thickness at 40°C above 100°C, with benzyl alcohol (the solvent). Solvent pretreatment could be applied repeatedly since no chemical reaction occurred during this step. In a second step, the pretreated composite was subjected to a chemical reaction (acid digestion) to dissolve the epoxy matrix and separate the clean fibers from the matrix. The pretreatment was proven to reduce or eliminate the rate-limiting effect of diffusion and substantially increase the degradation rate of the epoxy composite by subsequent acid digestion.
[0006] Despite its demonstrated efficiency and usefulness, Ma and Nutt's solvent pretreatment still has a major drawback, namely, that it requires the use of solvents that are industrially produced from petroleum feedstocks; as well as benzyl alcohol, and the lower performance solvents preliminarily tested by these authors (xylene, diethylene glycol, DGDME and DGME). More specifically, benzyl alcohol is industrially produced from toluene via benzyl chloride, which is hydrolyzed; an alternative route involves the hydrogenation of benzaldehyde, a by-product of the oxidation of toluene to benzoic acid. Sustainability is becoming an increasingly sensitive criterion, especially when operating chemical processes. There is a strong need to provide a pretreatment method as efficient as Ma and Nutt's solvent pretreatment method that does not require the use of solvents provided by the petroleum industry. There is a strong need to provide a solvent pretreatment method as efficient as Ma and Nutt's solvent pretreatment method based on bio-based solvents, i.e., one that can be produced from renewable biological feedstocks, ideally cheap and widely available. There is a need to identify bio-based solvents that are at least as efficient overall as benzyl alcohol in their ability to promote the subsequent chemical degradation of the epoxy contained in the epoxy composite laminate, including swelling (as described by Ma and Nutt) and delamination (which is not mentioned by Ma and Nutt).
[0007] Another area for improvement of the solvent pretreatment of Ma and Nutt concerns the swelling capability of benzyl alcohol. Increasing the swelling of fiber-reinforced composites may be desirable to make the composites more permeable and further reduce the rate-limiting effects of diffusion, especially for the strongest "cured" composites, which often contain highly crosslinked epoxy components. There is a need to identify solvents, preferably bio-based solvents, that can swell fiber-reinforced epoxy composites to a greater extent than benzyl alcohol can.
[0008] All these needs remain unmet, despite the attention given to green solvents in general during the last few years. Among many other solvents, the RHODIASOLV® family of environmentally friendly solvents (commercially available from SOLVAY) and bio-derived levoglucosenone and its derivatives can be mentioned, of which the most famous is certainly silene (dihydrolevoglucosenone) marketed by CIRCA. Levoglucosenone is made in a single step from cellulose and can be easily converted to silene in one step, as taught in particular by Sherwood et al. in Chem. Commun., 2014, 50, 9650-9652. As far as levoglucosenone and its derivatives are concerned, Pacheco et al. published a very impressive study entitled "Intelligent Approach to Solvent Substitution: The Identification of a New Class of Levoglucosenone derivatives" in ChemSusChem, 2016, 9, 3503-3512. By extensively reviewing the scientific literature, Pacheco et al. were able to identify over 164 levoglucosenone derivatives in addition to silene as biosolvent candidate molecules. All of them are listed in the “Supporting Information” accompanying Pacheco’s paper. Relying on theoretical approaches using different models, especially the Hansen solubility parameters, Pacheco selected several levoglucosenone derivatives that are the best candidates to replace several major conventional solvents such as DCM, nitrobenzene, NMP, DCM, CHCl3, THF, 1,2-DCEa, ethanol, acetone, DMF, DMSO, and acetonitrile. Among the 164 candidate molecules, Pacheco did not disclose or suggest any solvent that would be a good replacement for benzyl alcohol in Ma and Nutt’s pretreatment. Moreover, Pacheco does not point to levoglucosenone or levoglucosenone derivatives as solvents that could swell fiber-reinforced epoxy composites substantially more than benzyl alcohol could.Furthermore, Applicant notes that the Hansen Solubility Parameters used by Pacheco appear to be a mixture of experimentally obtained values with values calculated from molecular SMILES using a particular version of the HSPiP software, which makes these values inconsistent with each other and makes any conclusions derived or derivable therefrom, at the very least, strongly challengeable. Applicant also notes that Pacheco used a significantly older version of the software (v4.1.xx, 2013), which is a priori less well-known than the latest one on the market (v5.3.xx).
[0009] Now, as a result of an intensive study combining experiments and reliable software calculations, the Applicant has been able to identify a small set of levoglucosenone derivatives (corresponding to only 28% of Pacheco's candidates as biosolvents) capable of fulfilling the above needs, which serves as the basis for the present invention. Summary of the Invention
[0010] The present invention relates to a process for treating a fiber-reinforced epoxy composite at a processing temperature T tr A method M for treating a fiber reinforced epoxy composite comprising contacting the fiber reinforced epoxy composite with a solvent S at Solvent S is levoglucosenone and / or levoglucosenone derivatives, for which the Hansen Solubility Parameters calculated from the SMILES of solvent S using the Yamamoto Molecular Breaking Method with HSPiP software version 5.3.06 meet the following requirements: 16≦δD≦20 16≦δP+δH≦22 2 / 5≦δH / δP≦9 / 5 where δD is the energy from dispersion forces between molecules, δP is the energy from dipole-dipole intermolecular forces between molecules, and δH is the energy from hydrogen bonds between molecules, and all three are in MPa 0.5 It is expressed as Processing temperature T tris the glass transition temperature T of fiber-reinforced epoxy composites determined by DSC according to ASTM E1356-08(2014). g At least 10°C above however, Glass transition temperature T measured by DSC according to ASTM E1356-08(2014) g If it is not possible to detect the processing temperature T tr satisfies at least one condition selected from conditions (c1) to (c3), Condition (c1) is the glass transition temperature T g2 can be determined by DMA according to ASTM D7028-07(2015), and the treatment temperature T tr is the glass transition temperature T g2 at least 10°C above the Condition (c2) is a processing temperature T tr However, the treatment is performed by subjecting the fiber-reinforced epoxy composite to a treatment temperature T tr A swelling ratio r of at least 8% as determined after complete immersion in solvent S for 5 hours at sw is a processing temperature such as to cause swelling of the fiber-reinforced epoxy composite by the solvent S; The condition (c3) concerns processing method M, wherein the processing temperature is at least 300°C.
[0011] The present invention relates to - the use of the aforementioned solvent S for swelling fiber-reinforced epoxy composites; - a composition comprising a fiber-reinforced epoxy composite and the above-mentioned solvent S; - Process P for inducing decomposition of epoxy resin contained in fiber reinforced epoxy composites 1 The process P 1 teeth, a) subjecting a fiber reinforced epoxy composite to a pretreatment, the pretreatment comprising applying method M as described above; b) subjecting the thus pretreated fiber-reinforced epoxy composite to an enzymatic and / or chemical treatment; Including, Each of a) and b) is carried out once or several times; - Use of the method M for increasing the diffusion rate of an enzyme or compound in an epoxy resin embedded in a fiber-reinforced epoxy composite - Process P for recovering reinforcing fibers from fiber-reinforced epoxy composites 2 And, The aforementioned process P 1 decomposing an epoxy resin contained in a fiber-reinforced epoxy composite material by the above-mentioned method, thereby obtaining a material containing carbon fibers and an epoxy decomposition product; Separating the carbon fibers from the material thus obtained. Process P 2 ;and - Process P for recycling reinforcing fibers 3 And, The aforementioned process P 2 recovering carbon fibers from a fiber reinforced epoxy composite by; producing a composite material comprising a polymer and the carbon fibers thus recovered, said composite material being the same or different from the fiber-reinforced epoxy composite material comprised in the method M described above; Process P 3 Also relates to. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Processing method M Method M processes a fiber-reinforced epoxy composite at temperature T tr with a solvent S at 0.
[0013] Method M can in principle be used with solvent S in any physical state, including solid, liquid, vapor or supercritical, as long as contact is established between the fiber reinforced epoxy composite and solvent S.
[0014] For ease of implementation and efficiency, the solvent S is generally in a liquid state. The process is also advantageously operated at atmospheric pressure (about 1 atm = 101.325 kPa), although it is also possible to operate under vacuum or in a pressurized vessel. Thus, the solvent S is, on the one hand, at a processing temperature T tr Lower melting point T m On the other hand, the treatment temperature T tr Higher boiling point T b has.
[0015] The melting and boiling points of the solvent S can be determined by differential scanning calorimetry (DSC). They are advantageously determined according to the OECD guidelines (1995), test numbers 102 and 103, respectively. Furthermore, reliance can be placed on DIN 51005:2021-08, to which the aforementioned guidelines refer. A DSC Q2000 calorimeter from TA Instruments can be used. The temperature program consists of a single heating at a rate of 10° C. / min.
[0016] Solvent S can be sprayed or poured onto the fiber reinforced epoxy composite. Preferably, the fiber reinforced epoxy composite is at least partially immersed in solvent S. More preferably, at least about half of the initial mass (before treatment) of the fiber reinforced epoxy composite is immersed in solvent S. Even more preferably, the fiber reinforced epoxy composite is completely immersed in solvent S. In this way, optimal contact between the fiber reinforced epoxy composite and solvent S can be achieved.
[0017] The fiber reinforced epoxy composite may be contacted with solvent S alone. Alternatively, solvent S may be used in combination with other agents, such as one or more solvents other than solvent S. Among such other solvents, green, bio-based and / or environmentally friendly solvents are preferred. As an example of an environmentally friendly solvent, methyl 4-(dimethylcarbamoyl)-2-methylbutanoate, commercially available as RHODIASOLV® Polarclean from SOLVAY, may be mentioned. A bio-based solvent other than solvent S of particular interest is a levoglucosenone derivative whose Hansen solubility parameter does not comply with the requirements established for solvent S. An example of such a levoglucosenone derivative is a derivative of the formula [ka] (Commonly known as Cygnet 0.0, Cygnet 1.0, Cygnet 2.0, Cygnet 1.1 and Cygnet 4.0 respectively, all characterized by δP+δH<16) It is worth listing some of the ketals of silene.
[0018] During processing, the fiber reinforced epoxy composite and solvent S may remain stationary or they may be moved relative to one another. For example, the fiber reinforced epoxy composite may be fixed to a stationary surface while the solvent S is stirred. It is also possible to keep both the fiber reinforced epoxy composite and the solvent S under agitation. In a preferred embodiment, the fiber reinforced epoxy composite and the solvent S are kept stationary.
[0019] The weight ratio of solvent S and fiber reinforced epoxy composite for method M can vary considerably, depending in particular on the type of contact to be established with each other. For example, a low weight ratio can be used if the treatment is intended to be superficial. On the other hand, in general, the treatment is intended to have an effect on the core of the fiber reinforced epoxy composite, and therefore a complete immersion of the fiber reinforced epoxy composite in solvent S is preferred. Solvent S for method M is then preferably used in an amount sufficient to allow partial, preferably complete, immersion of the fiber reinforced epoxy composite. With this in mind, the weight ratio of solvent S to the fiber reinforced epoxy composite is generally at least 1, and may be at least 2, at least 5, at least 10, at least 20, or at least 40. On the other hand, from an economical point of view, this ratio is generally at most 200, and may be at most 100, at most 60, or at most 30.
[0020] The length of time during which the fiber reinforced epoxy composite and the solvent S are in contact with each other, in particular the length of time during which the fiber reinforced epoxy composite can be partially or completely immersed in the solvent S, depends in particular on the processing temperature T tr The duration can vary to a considerable extent depending on the amount of swelling that is achieved. Said duration generally ranges from 10 minutes to 100 hours. It is preferably at least 30 minutes, more preferably at least 1 hour, even more preferably at least 2 hours, even more preferably at least 4 hours. For economic reasons, the duration is determined based on the desired effect, generally a sufficiently high swelling ratio r sw Thus, it may be at most 50 hours, at most 20 hours, at most 10 hours, or at most 7 hours. The desired swelling rate may be 5% or more. The desired swelling rate is advantageously at least 8%, preferably at least 12%, more preferably at least 15%, and even more preferably at least 18%.
[0021] Glass transition temperature T of fiber-reinforced epoxy composites g [Measured by DSC according to ASTM E1356-08(2014)] compared with the treatment temperature T tr As mentioned above, the swelling ratio rsw According to method M, and subject to the conditions described above, the treatment temperature T tr , in particular the temperature at which the fiber-reinforced epoxy composite can be partially or completely immersed in the solvent S, is the glass transition temperature T of the fiber-reinforced epoxy composite, determined by DSC according to ASTM E1356-08 (2014). g must exceed T by at least 10°C. tr is T g Preferably, the temperature is at least 20° C., more preferably at least 30° C., and even more preferably at least 35° C. tr is T g However, for economic reasons and for T tr In order to have as many solvents S as possible on hand that remain in a liquid state at T tr is T g Advantageously, the reaction temperature should not exceed 200° C., preferably not more than 100° C., more preferably not more than 70° C., even more preferably not more than 50° C.
[0022] Generally, the glass transition temperature T g can be detected on fiber-reinforced epoxy composites by DSC according to ASTM E1356-08(2014), such that the glass transition temperature T g is the processing temperature T tr It serves as the basis for determining gTo determine the , a DSC Q2000 calorimeter device from TA Instruments is advantageously used. The instrument is fully calibrated with a baseline (empty cell operated under standard DSC program conditions, i.e. room temperature-about 20°C-~350°C, heat release rate of 10°C / min) and an indium calibration (100°C-180°C, 10°C / min). A fiber-reinforced epoxy composite sample is prepared. A suitable sample mass may be about 3 to about 12 mg; it can be adjusted depending on the overall fiber-reinforced epoxy composite composition, in particular its epoxy content. The sample is advantageously substantially thin and substantially flat to ensure good contact with the specimen holder in which it is placed. The specimen holder is typically an Aluminum Tzero pan (available from TA Instruments) with a hole drilled in the lid; the pan is sealed for testing. The sample is heated from room temperature (about 20°C) to 350°C using a heating rate of 10°C. Importantly, no cooling program is applied, followed by a second heating program: T g is determined during the first and only heating program; thereby determining the T on the sample that would have substantially altered the degree of crosslinking or other structural features of the epoxy upon full completion of this first heating program. g The measurement is performed under nitrogen flow gas at 50 mL / min. The midpoint temperature, i.e., the heat flow difference between the extrapolated starting end and the extrapolated end, is determined. 1 The point on the thermal curve corresponding to / 2 is the glass transition temperature T g It is defined as:
[0023] In rare cases, the glass transition temperature T g cannot be detected by DSC according to ASTM E1356-08(2014). This situation may occur especially in some highly crosslinked fiber-reinforced epoxy composites. Then, as explained above, method M is performed by increasing the processing temperature T tr It remains an applicable subject matter that satisfies at least one condition selected from conditions (c1) to (c3).
[0024] The applicant has determined the glass transition temperature T by dynamic mechanical analysis (DMA) according to ASTM D7028-07(2015) for several fiber-reinforced epoxy composites. g2 However, some DSCs can detect the glass transition temperature T g It was observed that it was not possible to detect the presence of the oxidizing agent. Then, the method M can be particularly applied when the condition (c1) is satisfied. The condition (c1) is that the treatment temperature T tr is the glass transition temperature T g2 In a preferred embodiment of (c1), T tr is T g2 at least 20° C., more preferably at least 30° C., and even more preferably at least 35° C. tr is T g2 may be further exceeded by at least 40° C., or even at least 50° C. tr is T g2 Advantageously, the reaction temperature is not more than 200° C., preferably not more than 100° C., more preferably not more than 70° C., even more preferably not more than 50° C.
[0025] For the DMA test, a Q800 Dynamic Mechanical Analyzer manufactured by TA Instruments may be used. Flat, clean, dry rectangular strip specimens of the fiber reinforced epoxy composite samples are advantageously prepared according to ASTM standards and the recommendations of the instrument manufacturer's manual. The specimens are properly conditioned to ensure dryness. Two or more specimens may be tested for each sample, and the T g2 The retention value is taken as the average of each measurement, subject to possible elimination of obvious scratch results. The specimen is placed in the DMA analyzer. Dual cantilever mode may be used with a clamp size of 35 mm (L), up to 15 mm (W) and 5 mm (T); in this mode the specimen is clamped at both ends and bent in the middle. The specimen is oscillated at a nominal frequency of 1 Hz in constant strain mode. The specimen is oscillated at a rate of 5°C / min (9°F / min) starting from room temperature (approximately 20°C) until the T g2The temperature at which a significant decrease in the storage modulus (E') begins is called the glass transition temperature (T g2 or "DMA T g "); more precisely, T g2 is determined to be the intersection of the two tangents from the storage modulus.
[0026] Conditions (c2) and (c3) also result in a glass transition temperature T g Conditions (c2) and (c3) address those rare cases where the glass transition temperature T g2 However, conditions (c2) and (c3) may be realized even if the glass transition temperature T g The glass transition temperature T g2 This is particularly useful when it is not possible to detect the presence of a fluorine-containing compound in a sample. Although such cases are very rare, they can occur, especially in some very highly crosslinked fiber-reinforced epoxy composites.
[0027] According to condition (c2), by trial and error experiments, the fiber-reinforced epoxy composite was treated at a processing temperature T tr The swelling ratio r of the fiber-reinforced epoxy composite by solvent S after complete immersion in solvent S for 5 h at 1000 rpm was sw is the minimum value r sw,分 (Here, the treatment temperature T tr is determined;r sw,分 is preferably 12%, more preferably 15%, and even more preferably at least 18%. sw ≧r sw,分 The processing temperature T tr The determination of T is particularly easy for the skilled person. tr(typically above 300 °C, which strongly supports / guarantees high swelling), a single experiment is generally sufficient, and operating the process at such very high temperatures is not possible without the boiling point T b This is not a problem since there are many solvents suitable as the solvent S whose treatment temperature T can be much higher than 300° C. In practice, it is preferred to use a treatment temperature T of at least 300° C. (particularly at least 350° C., at least 400° C., or even at least 450° C.). tr The likelihood of success of a process operated at 300°C is quite high because, from a practical standpoint, essentially all, if not all, cured epoxies become softer and more rubbery at temperatures substantially below 300°C; therefore, in practice, it is not practical to operate fiber-reinforced epoxy composites at such high, arbitrarily selected processing temperatures, T tr It has been shown that satisfying condition (c3), which "simply" provides for treating at 300° C., is good enough to embody the method M of the present invention. Of course, according to condition (c2), temperatures substantially lower than 300° C. can be tested for treatment and still have a fairly high expectation of success. tr Optimization of and selection of solvent S can be accomplished as a matter of routine by one of skill in the art, if necessary.
[0028] As previously suggested, according to condition (c3), the treatment temperature T trshall be at least 300° C., in some cases at least 350° C., at least 400° C., or even at least 450° C. Non-limiting examples of solvents S that may be suitable for implementing condition (c3) include solvents S13, S14, S39, S42, S52, S57, S58, S59, S75, S78, S80, S88, S96, S113, S119, S143, S156, S158, S160, S161, and S164, which have boiling points as predicted using the Yamamoto Molecular Breaking Method in HSPiP software version 5.3.06, as labeled by Pacheco et al. and used in Tables 2-12 below. Of these, solvents S57, S58, S59, S75, S119, S156, S158, S160, S161 and S164 have predicted boiling points of at least 350° C., solvents S57, S58, S59, S119 and S164 have predicted boiling points of at least 400° C., S57, S58, S59 and S119 have predicted boiling points of at least 450° C., and S58 has a predicted boiling point of 507° C. The experimental boiling points of these solvents may be somewhat higher than their predicted boiling points based on comparisons with various solvents, including silanes.
[0029] Glass transition temperature T g In the rare cases where cannot be detected by DSC according to ASTM E1356-08(2014), the skilled person can apply one of the following methods: - Method 1: Glass transition temperature T g2 can be determined by DMA according to ASTM D7028-07(2015), and if so, the glass transition temperature T g2 A processing temperature T at least 10°C higher than tr and then, if and only if the glass transition temperature cannot be detected by DMA according to ASTM D7028-07(2015), a treatment temperature T satisfying conditions (c2) and / or (c3) is used. tr Use; - Method 2: Glass transition temperature T g2Whether or not a swelling ratio r of at least 8% can be determined by DMA according to ASTM D7028-07(2015) can be determined by trial and error experiments. sw Based on the above, the processing temperature T satisfies the condition (c2). tr Determine; - Method 3: Glass transition temperature T g2 can be determined by DMA according to ASTM D7028-07(2015), the treatment temperature T satisfying condition (c3) tr , i.e., a processing temperature of at least 300° C. (optionally at least 350° C., at least 400° C., or even at least 450° C.) is used as is.
[0030] The thus treated fiber reinforced epoxy composite can be recovered from solvent S by hot filtration.
[0031] The recovered fiber reinforced epoxy composite may be washed with water, an alcohol such as ethanol, and / or mixtures thereof.
[0032] Fiber Reinforced Epoxy Composites A fiber reinforced epoxy composite comprises an epoxy resin and reinforcing fibers, may consist essentially of, or may consist of, the epoxy resin and reinforcing fibers, or may further comprise one or more other components.
[0033] The reinforcing fibers are generally embedded in an epoxy resin, commonly referred to as the "matrix" of the composite, but may be the major component by weight of the composite, which is typically a laminate.
[0034] The weight of the epoxy resin is generally at least 10% by weight, and often at least 25% by weight, based on the total weight of the composite. It may be at least 35% by weight, at least 50% by weight, or at least 65% by weight. Moreover, it is generally up to 90% by weight, and often up to 75% by weight.
[0035] Similarly, the weight of the reinforcing fibers is generally at least 10% by weight, and often at least 25% by weight, based on the total weight of the composite. It may be at least 35% by weight, at least 50% by weight, or at least 65% by weight. Moreover, it is generally at most 90% by weight, and often at most 75% by weight.
[0036] The combined weight amount of the reinforcing fibers and the epoxy resin is generally greater than 50% by weight, based on the total weight of the composite, and is often at least 80% by weight, and may be at least 90% by weight, at least 95% by weight, or at least 99% by weight.
[0037] Epoxy Resin The epoxy resin (or polyepoxide) contained in fiber reinforced epoxy composites is generally a cured product. Curing is a process in which chemical reactions occur to result in the hardening and toughening of the epoxy resin. Although curing can be induced under the action of UV or heat, epoxy resins are generally cured by the use of additives, commonly called curing agents or hardeners.
[0038] From a structural point of view, epoxy resins are generally cross-linked products, and the cross-linked structure usually results from the curing process. Therefore, the glass transition temperature T g At temperatures much lower than g2 ), e.g., at temperatures 100° C. below the glass transition temperature, the epoxy resin contained in the fiber-reinforced epoxy composite is generally substantially insoluble, essentially insoluble, or completely insoluble in the solvent S of the present invention, which is typically determined after complete immersion of the fiber-reinforced epoxy composite in solvent S for 5 hours without stirring at the temperature of interest, and has a swelling ratio r of less than 1.0%, as determined after complete immersion of the fiber-reinforced epoxy composite in solvent S for 5 hours without stirring at the temperature of interest. sw For the purposes of this invention, many fiber-reinforced epoxy composites have a glass transition temperature T g (or in some cases T g2) is equal to or greater than 125°C; and then their swelling ratio r, determined after completely immersing the fiber-reinforced epoxy composites in the solvent S without stirring for 5 hours at room temperature (about 20°C), sw is typically less than 1.0%. Fiber-reinforced epoxy composites of interest for the present invention preferably have a glass transition temperature T of at least 145° C. g (or in some cases T g2 ) and furthermore, their glass transition temperatures are generally at most 275°C, often at most 250°C.
[0039] Epoxy resins included in the fiber reinforced epoxy composites of the present invention include bisphenol-based epoxy resins (which may be based on reacting epichlorohydrin with bisphenol A and / or bisphenol F), novolacs (which may be based on reacting phenol with methanol, optionally followed by reacting the resulting novolac with epichlorohydrin), aliphatic epoxy resins, halogenated epoxy resins and glycidyl amine epoxy resins (formed by reacting an aromatic amine with epichlorohydrin).
[0040] The epoxy resin contained in the fiber-reinforced epoxy composite of the present invention can be based on at least one epoxy compound having at least two epoxide groups per molecule. Such epoxy compounds can be aromatic, cycloaliphatic or aliphatic. Suitable aromatic epoxy compounds include polyglycidyl ethers of phenols and polyphenols, epoxy compounds with fluorene rings, epoxy compounds with naphthalene rings, dicyclopentadiene-modified phenol epoxy compounds, epoxidized novolac or cresol novolac compounds, polyglycidyl adducts of amines (e.g., N,N-diglycidylaniline), triglycidylaminophenol (TGAP), triglycidylaminocresol, tetraglycidylxylenediamine, aminoalcohols (e.g., triglycidylaminophenol), polyglycidyl adducts of polycarboxylic acids (e.g., diglycidyl phthalate), polyglycidyl cyanurate (e.g., triglycidyl cyanurate), and copolymers of glycidyl (meth)acrylate and copolymerizable vinyl compounds (e.g., styrene glycidyl methacrylate).Suitable alicyclic epoxy compounds include bis(2,3-epoxycyclopentyl)ether, copolymers of bis(2,3-epoxycyclopentyl)ether and ethylene glycol, dicyclopentadiene diepoxide, 4-vinylcyclohexene dioxide, 3,4-epoxycyclohexylmethyl, 3,4-epoxycyclohexanecarboxylate, 1,2,8,9-diepoxylimonene (limonene dioxide), 3,4-epoxy-6-methylcyclohexylmethyl, 3,4-epoxy-6-methylcyclohexanecarboxylate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, 2-(7-oxabicyclo[4.1.0]hept-3-yl)spiro[1,3-dioxane-5,3'-[7]oxabicyclo[4.1.0]heptane], allylcyclopentane, 1,2,8,9-diepoxycyclopentane, 1,3,8,9-diepoxycyclopentane, 1,4,8,9-diepoxycyclopentane, 1,2,8,9-diepoxycyclopentane, 1,4 ... Examples of suitable glycidyl ethers include diepoxide of thenyl ether, 1,4-cyclohexa diepoxide, 1,4-cyclohexaneethanol diglycidyl ether, bis(3,4-epoxycyclohexylmethyl)adipate, 3,4-epoxy-6-methylcyclohexanecarboxylate, diglycidyl 1,2-cyclohexanecarboxylate, 3,4-epoxymethylcyclohexylmethyl methacrylate, 3-(oxiran-2-yl)-7-oxabicyclo[4.1.0]heptane, bis(2,3-epoxypropyl)cyclohex-4-ene-1,2-dicarboxylate, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, and poly[oxy(oxiranyl-1,2-cyclohexanediyl)]α-hydro-ω-hydroxy-ether, bi-7-oxabicyclo[4.1.0]heptane. Suitable aliphatic epoxy compounds include butanediol diglycidyl ether, epoxidized polybutadiene, dipentene dioxide, trimethylolpropane triglycidyl ether, bis[2-(2-butoxyethyloxy)ethyl]adipate, hexanediol diglycidyl ether, and hydrogenated bisphenol A epoxy resins.
[0041] The epoxy resin is preferably at least one aromatic compound A1 which contains at least two epoxide groups per molecule and at least one aromatic ring carrying at least one glycidyloxy group, at least one hardener A2; Based on.
[0042] The aromatic compound A1 advantageously corresponds to a diglycidyl ether of a bisphenol, in particular the diglycidyl ether of bisphenol A. The hardener A2 is often an amine or imidazole derivative.
[0043] More preferably, the epoxy resin is preferably at least one aromatic compound A1 which contains at least two epoxide groups per molecule and at least one aromatic ring carrying at least one glycidyloxy group, at least one hardener A2, - optionally with at least one additional compound A3 Based on.
[0044] In some preferred embodiments, the epoxy resin is at least one aromatic compound A1 which contains at least two epoxide groups per molecule and at least one aromatic ring carrying at least one glycidyloxy group, at least one hardener A2; Based solely on.
[0045] The expression "epoxy resin based on" should of course be understood to mean an epoxy resin comprising a mixture and / or reaction product of the various basic components used in this composition, some of which are intended or capable of reacting at least partially with each other or with their direct chemical surroundings during the various stages of the manufacture of the fiber-reinforced epoxy composite or the finished product comprising such a composite, in particular during the commonly applied curing processes. In other words, the epoxy resin is prepared from at least one aromatic compound A1 and at least one curing agent A2, as described below.
[0046] The term "aromatic" as used herein with respect to organic compounds A1 or A2 means that an organic compound containing one or more aryl moieties may each be optionally interrupted by one or more heteroatoms, typically selected from oxygen, nitrogen and sulfur heteroatoms, and one or more carbon atoms of the one or more aryl moieties may be optionally substituted with one or more organic groups, typically selected from alkyl, alkoxyl, hydroxyalkyl, cycloalkyl, alkoxyalkyl, haloalkyl, aryl, alkaryl, aralkyl.
[0047] The term "aryl," as used herein with respect to organic compounds A1 or A2, means a cyclic, coplanar, 5-14 membered organic group having a delocalized conjugated π system and a plurality of π electrons equal to 4n+2, where n is 0 or a positive integer, and includes compounds such as benzene, in which each of the ring members is a carbon atom, compounds such as furan, pyridine, imidazole and thiophene, in which one or more of the ring members is a heteroatom, typically a heteroatom selected from oxygen, nitrogen and sulfur atoms, and fused ring systems such as naphthalene, anthracene and fluorene, in which one or more of the ring carbons may be substituted with one or more organic groups, typically selected from alkyl, alkoxyl, hydroxyalkyl, cycloalkyl, alkoxyalkyl, haloalkyl, aryl, alkaryl, halo groups, such as phenyl, methylphenyl, trimethylphenyl, nonylphenyl, chlorophenyl or trichloromethylphenyl.
[0048] As used herein, "epoxide groups" refer to vicinal epoxy groups, i.e., 1,2-epoxy groups.
[0049] Aromatic compound A1 The aromatic compound A1 has at least two epoxide groups per molecule and at least one aromatic ring having at least one glycidyloxy group. The aromatic compound A1 according to the present invention has at least two epoxide groups per molecule, and one of the at least two epoxide groups can be an epoxide group derived from the glycidyloxy group of the aromatic ring having at least one glycidyloxy group.
[0050] Suitable aromatic compounds A1 include polyglycidyl ethers of phenols and polyphenols, such as diglycidyl resorcinol, 1,2,2-tetrakis(glycidyloxyphenyl)ethane or 1,1,1-tris(glycidyloxyphenyl)methane; diglycidyl ethers of bisphenols, such as the diglycidyl ether of bisphenol A (bis(4-hydroxyphenyl)-2,2-propane), the diglycidyl ether of bisphenol F (bis(4-hydroxyphenyl)methane), the diglycidyl ether of bisphenol C (bis(4-hydroxyphenyl)-2,2-dichloroethylene) and the diglycidyl ether of bisphenol S (4,4'-sulfonyldiphenol) and their oligomers; polyglycidyl ethers of aromatic alcohols; epoxidized novolac compounds; epoxidized cresol novolac compounds; polyglycidyl ethers of aminophenols, such as triglycidyl aminophenol (TGAP); triglycidyl aminocresol.
[0051] Some commercially available aromatic compounds A1 of interest are the triglycidyl ethers of p-aminophenol (available from Huntsman as MY 0510), the triglycidyl ethers of m-aminophenol (available from Huntsman as MY 0610), the diglycidyl ethers of bisphenol A based materials such as 2,2-bis(4,4'-dihydroxyphenyl)propane (available from Dow as DER 661 or from Momentive as EPON 828), the glycidyl ethers of phenol novolac resins (available from Dow as DEN 431 or DEN 438), and the diglycidyl derivatives of dihydroxydiphenylmethane (available from Huntsman as PY 306).
[0052] The aromatic compound A1 is preferably selected from the diglycidyl ethers of bisphenols, such as the diglycidyl ethers of bisphenol A (bis(4-hydroxyphenyl)-2,2-propane), bisphenol F (bis(4-hydroxyphenyl)methane), bisphenol C (bis(4-hydroxyphenyl)-2,2-dichloroethylene) and bisphenol S (4,4′-sulfonyldiphenol), in particular bisphenol A diglycidyl ethers.
[0053] Hardener A2 The hardeners for epoxy resins are well known to those skilled in the art. The hardener A2 can be an amine, such as a primary amine, a secondary amine or a tertiary amine, a ketimine, a polyamide resin, an imidazole derivative, a polymercaptan, an anhydride, a boron trifluoride amine complex, a dicyandiamide, an organic acid hydrazide, a photohardener or an ultraviolet hardener.
[0054] Suitable anhydrides as hardener A2 include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tricarboxylic anhydride, ethylene glycol bistrimellitate, glycerol tristrimellitate, maleic anhydride, tetrahydrophthalic anhydride, enomethylene tetrahydrophthalic anhydride, methyl endo methyl dene tetrahydrophthalic anhydride, dodecenyl succinic anhydride, hexahydrophthalic anhydride, hexahydro-4-methylphthalic anhydride, succinic anhydride, methylcyclohexene dicarboxylic anhydride, alkylstyrene-maleic anhydride copolymers, chlorendic anhydride, polyazelaic anhydride.
[0055] Exemplary polyamines suitable as curing agent A2 include diethylenetriamine (DTA), triethylenetetramine (TTA), tetraethylenepentamine (TEPA), dipropenediamine (DPDA), diethylaminopropylamine (DEAPA), bis(hexamethylene)triamine, mixtures containing bis(hexamethylene)triamine and non-volatile amines (such as the mixture known as "Amine 248"), N-aminoethylpiperazine (N-AEP), menthanediamine (MDA), isophoronediamine (IPDA), 1,3-bis(aminomethyl)cyclohexane, m-xylylenediamine (MXDA), xylylenediamine trimer, metaphenylenediamine (MPDA), diaminodiphenylmethane (DDM), diaminodiphenylsulfone (DDS), and 4,4'-methylenebis(2,6-diethylaniline).
[0056] Exemplary imidazole derivatives suitable as curing agent A2 include 2-methylimidazole, 2-phenyl-imidazole, 3-benzyl-2-methylimidazole, 5-methyl-2-phenylimidazole, 2-ethyl-4-methylimidazole, 5-ethyl-2-methylimidazole and 1-cyanoethyl-2-undecylimidazolium trimellitate.
[0057] The curing agent A2 is preferably a polyamine, optionally an imidazole compound; the polyamine may be aliphatic or aromatic. More preferably, the curing agent A2 contains several primary amine groups and / or is an imidazole compound.
[0058] Optional further compound A3 As possible further compounds A3, mention may be made of compounds other than the aromatic compounds A1 which have at least two epoxide groups per molecule, in particular cycloaliphatic or aliphatic compounds which have at least two epoxide groups per molecule.
[0059] Other possible additional compounds A3 may include monoepoxide compounds having only one epoxide group per molecule, including aromatic monoepoxide compounds, monoalicyclic monoepoxide compounds and aliphatic monoepoxide compounds. Exemplary monoepoxide compounds are isobutylene oxide, styrene oxide, 3,3'-bis(chloromethyl)oxacyclobutane and olefinic monoepoxides such as cyclododecadiene monoepoxide, 3,4-epoxy-1-butene.
[0060] Reinforced Fiber Fiber-reinforced epoxy composites contain reinforcing fibers. They can be mineral or organic. They can be derived from biological sources; as can wood fibers. According to the invention, the reinforcing fibers are advantageously chosen from glass fibers, basalt fibers, aramid fibers, polyester fibers and carbon fibers. Glass fibers exist in many categories, among which the M (for high tensile modulus) and S (for high tensile strength) categories are especially worth mentioning. Basalt fibers are materials made up of ultrafine fibers of basalt, composed of the minerals plagioclase, pyroxene and olivine; they are somewhat similar to glass fibers. Aramid (i.e. aromatic polyamide) fibers include (i) para-aramid fibers, in particular polyparaphenylene terephthalamide fibers (available from DuPont as KEVLAR® fibers) and fibers consisting of wholly aromatic polyamides obtained by polycondensation of terephthaloyl chloride with a mixture of p-phenylenediamine and 3,4'-diaminodiphenyl ether (available from Teijin as TECHNORA® fibers), and (ii) meta-aramid fibers, such as NOMEX® fibers (available from DuPont). In polyester fibers, the polyester is preferably a liquid crystal polymer, for example one obtained by polycondensation of 4-hydroxybenzoic acid and 6-hydroxynaphthalene-2-carboxylic acid; as are VECTRAN® fibers marketed by Kuraray.
[0061] The reinforcing fibers are preferably carbon fibers. Carbon fibers (or CF, graphite fibers or graphite fibers) generally have a diameter of about 5-10 μm. They have several advantages, including high stiffness, high tensile strength, low strength-to-weight ratio, high chemical resistance, high temperature resistance and low thermal expansion. These properties make carbon fibers very popular in aerospace, civil engineering, military and competitive sports. Depending on the precursors for making the fibers, carbon fibers may be turbostratic or graphitic, or may have a hybrid structure in which both graphitic and turbostratic parts are present.
[0062] The carbon fibres may in particular be PAN-based carbon fibres or pitch-based carbon fibres.
[0063] In fiber reinforced epoxy composites, the fibers, especially carbon fibers, may be non-woven or patterned with woven fabrics such as plain weave, twill, harness satin, or fish weave. Each fabric contains unique properties that make it excellent for use in some designs and not others.
[0064] Optional components of fiber-reinforced epoxy composites In addition to the epoxy resin and reinforcing fibers, the fiber reinforced epoxy composite can include a thermoplastic resin, such as bisphenol A polysulfone (PSU), polyethersulfone (PESU), polyphenylsulfone (PPSU), polyamide (PA), polyamideimide (PAI), polyimide (PI), polyetherimide (PEI), polyester (PE), polyphenylene sulfide (PPS), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyolefin (PO), or a combination thereof. In some embodiments, the thermoplastic resin is in particulate form. It can act as a toughening agent.
[0065] Other possible components of fiber reinforced epoxy composites include accelerators that enhance or accelerate the cure of the epoxy resin, as well as performance modifiers such as core-shell rubbers, flame retardants, wetting agents, pigments, dyes, UV absorbers, fillers, conductive particles, and viscosity modifiers.
[0066] Solvent S Solvent S is levoglucosenone and / or a levoglucosenone derivative.
[0067] As used herein, the term "levoglucosenone derivatives" is intended to denote chemical compounds that can be synthesized from levoglucosenone feedstock. The synthesis may require one and only one reaction, or a reaction scheme with several successive reactions (steps) is required. The number of successive reactions (steps) required to synthesize the desired levoglucosenone derivatives may vary widely; in particular it may be 2, 3, 4, 5, 6 or 7; it is generally up to 10. Many reaction schemes suitable for synthesizing solvent S according to the present invention are described on pages 28-38 of the "Supplementary Information" attached to the Pacheco paper and / or in the references referenced in Table 14 of the title of this patent. The synthesis of levoglucosenone derivatives advantageously requires no more than seven successive reactions, preferably no more than five, and even more preferably no more than three successive reactions. Most preferably, the levoglucosenone derivatives can be synthesized from levoglucosenone or silene by only one reaction.
[0068] Melting point and boiling point of solvent S The melting point of solvent S is advantageously below 100° C., preferably at most 50° C.; more preferably, solvent S is liquid at room temperature (about 20° C.) and atmospheric pressure (about 1 atm = 101.325 kPa).
[0069] The boiling point of solvent S is generally at least 100° C. Advantageously at least 150° C., preferably at least 175° C., more preferably at least 200° C. The boiling point of silane, as determined experimentally using OECD Guideline (1995) Test No. 103 and reported specifically in the Sigma-Aldrich safety data sheet, is 227° C.
[0070] Hansen solubility parameter for solvent S The Hansen Solubility Parameters of solvent S calculated from the Simplified Molecular-Input Line-Entry System (SMILES) of solvent S using the Yamamoto Molecular Breaking Method with HSPiP software version 5.3.06 meet all of the following requirements: 16≦δD≦20 16≦δP+δH≦22 2 / 5≦δH / δP≦9 / 5 where δD, δP and δH are as defined above.
[0071] δD is preferably at least 17, more preferably at least 18, and even more preferably at least 18.5.
[0072] It is δP+δH that is important. Preferably, δP+δH is at least 17, more preferably at least 18, even more preferably at least 19. On the other hand, it is preferred that δP+δH is at most 21, and more preferably at most 20.
[0073] The ratio δH / δP is also very important. In general, the lower the δH / δP, the higher the swelling effect of the solvent S. On the other hand, the higher the δH / δP, the higher the exfoliation effect of the solvent S. Whatever the ratio δH / δP of the solvent S, good results can be achieved, taking into account the overall balance between the swelling effect and the level of exfoliation effect that can be achieved. Thus, if the skilled person wishes to do so, he can easily adjust δH / δP to a value that he considers optimal for a possible subsequent method, process or use of the fiber reinforced epoxy composite treated by the above-mentioned method M, possibly step b) of process P1. In particular, δH / δP may be at least 1 / 2, at least 2 / 3, at least 4 / 5, at least 1, at least 5 / 4, at least 3 / 2, or at least 7 / 4. Furthermore, δH / δP may be at most 7 / 4, at most 3 / 2, at most 5 / 4, at most 1, at most 4 / 5, at most 2 / 3, at most 4 / 7, or at most 1 / 2.
[0074] Group G1 of solvent S Solvents S belonging to the first group G1, characterized by δH / δP<1, are generally capable of causing very high swelling of fiber-reinforced epoxy composites in combination with a moderately high degree of exfoliation.
[0075] In some embodiments, the solvents S of group G1 preferably have a δH / δP of at most 4 / 5, more preferably at most 2 / 3, whereas their δH / δP is preferably at least 1 / 2.
[0076] Excellent results were obtained when silane was used as solvent S.
[0077] Solvent S group G2 Solvents S belonging to another group G2, characterized by δH / δP≧1, are generally capable of causing delamination of fiber-reinforced epoxy composites to a very high degree in combination with a moderately high swelling ratio.
[0078] In some embodiments, the solvents S of group G2 preferably have a δH / δP of at least 5 / 4, more preferably at least 3 / 2, whereas their δH / δP is preferably at most 7 / 4.
[0079] Good results are obtained when levoglucosanol and / or levoglucosenol are used as solvent S. Levoglucosanol can be available as threo-levoglucosanol (1,6-anhydro-3,4-dideoxy-β-D-threo-hexopyranose, CAS Registry Number: 39682-49-039682-48-9), erythro-levoglucosanol (1,6-anhydro-3,4-dideoxy-β-D-erythro-hexopyranose, CAS Registry Number: 39682-48-9) or a mixture thereof. Similarly, levoglucosenol can be available as threo-levoglucosenol (1,6-anhydro-3,4-dideoxy-β-D-threo-hex-3-enopyranose, CAS Registry Number: 50705-28-7), erythro-levoglucosenol (1,6-anhydro-3,4-dideoxy-β-D-erythro-hex-3-enopyranose, CAS Registry Number: 58394-28-8), or a mixture thereof.
[0080] Formula of solvent S The solvent S may be of a general formula selected from the group consisting of formulas (I) to (X), as shown below: [ka] During the ceremony, (-) indicates any carbon-carbon bond that, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; R 1 , R 2 and R 3 are each independently: (i) a hydrogen atom; (ii) a halogen atom, (iii) a C1-C4 alkyl, a C1-C4 alkenyl, a C1-C4 alkynyl or a C1-C4 alkoxy, (iv) a C1-C4 alkyl, a C1-C4 alkoxy and a carboalkoxy group -COOR, where R is a C1-C6 alkyl, or (v) [ka] Or -R' a-S(=O)-R a or -R' a -S(=O)2-R a wherein R a is C1-C4 alkyl or phenyl, R' a is C1-C6 alkanediyl or C2-C6 alkenediyl, -R' a -S(=O)-R a or -R' a -S(=O)2-R a and; R 4 is hydrogen, C1-C4 alkyl or -R' d -OH or R' d is C1-C4 alkanediyl; R 5 is hydrogen or C1-C4 alkyl; R 6 and R 7 are, independently of one another, phenyl optionally substituted once or twice by a monovalent radical selected from: (i) hydrogen, (ii) a halogen atom, (iii) a C1-C4 alkyl, or (iv) a carboalkoxy radical -COOR, where R is a C1-C6 alkyl, a C1-C4 alkoxy and a carboalkoxy radical -COOR, or two of whose carbon atoms are substituted adjacent to one another, [ka] a ring having an oxymethyleneoxy group -O-CH2-O-, where the asterisks indicate the two adjacent carbon atoms of the phenyl ring; R 8 is hydrogen or C1-C4 alkoxy; R' is a C1-C6 alkanediyl; however, R 1 and R 2 is (i) a C1-C6 alkanediyl group, (ii) a C2-C6 alkenediyl group, (iii) -R' b ~N=N- group, where R' bis a C1-C4 alkanediyl group, the carbon atoms of which are optionally further substituted two times, as defined herein [ka] (In the formula, R' c is nil or C1-C4 alkanediyl), forming a spiro linkage shown as b ~N=N- group, or (iv) -CH2-C(=O)-CH(-COOR b )-group, in which R b is C1-C4 alkyl, -CH2-C(=O)-CH(-COOR b )-group, resulting in R 1 and R 2 form a ring with the two carbon atoms to which they are attached, and R 1 and R 2 When and are combined in such a way that there are no carbon-carbon bonds, R 2 The carbon atom to which is bonded is a group R 2ビス wherein R 2ビス is a C1-C4 alkyl or halogen atom; 2ビス may be further substituted by R 6 and 7 is a C1-C6 alkanediyl group, a C2-C6 alkenediyl group or a group of the formula [ka] can be combined into a cycloalkenediyl group of the formula:
[0081] In some embodiments, the solvent S is a moiety M 1 、 Part M 2 、 Part M 3 Or part M 4 Includes.
[0082] Part M 1 An embodiment based on In some embodiments, the solvent S is a moiety M of formula (FI)1 Including, [ka] wherein (-) represents any carbon-carbon bond that, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; The carbon atom bearing the asterisk is substituted with a monovalent or divalent group and has at least one oxygen atom R O Includes: R O is advantageously selected from the group consisting of (i) oxo (=O), (ii) hydroxyl (-OH), (iii) alkoxy (-OR) where R is C1-C6 alkyl (preferably methyl), (iv) an optionally substituted oxyethyleneoxy group (-O-R' e -O-), wherein R' e is a C1-C4 alkyl group (preferably methyl) or a C1-C4 hydroxyalkyl group -R' d -OH, where R' d is a C1-C4 alkanediyl (preferably, -CH2-), d an optionally substituted oxyethyleneoxy group (-O-R') which is ethanediyl optionally substituted with -OH; e (v) a group of formula -O-CH2-C(=O)-CH2-, (vi) a carboxyalkyl group -R'-COOH, where R' is a C1-C6 alkanediyl (preferably -CH2- or -CH2-CH2-), and (vii) a carboalkoxyalkyl group -R'-COOR, where R' is a C1-C6 alkanediyl and R is a C1-C6 alkyl. 1 ~E 5 The same is true.
[0083] Embodiment E 1 First embodiment E 1 wherein the solvent S is of formula (I) [ka] where (-) represents any carbon-carbon bond that, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; R 1 and R 2 is as described above, and formula (I) is subject to the above-mentioned conditions.
[0084] The solvent S may contain an optional carbon-carbon bond (-), as shown in formula (Ia): [ka] In the formula, R 1 and R 2 is as described above and formula (Ia) is subject to the above-mentioned conditions. Alternatively and preferably, any carbon-carbon bond (-) is not present in formula (I); then the solvent S can be represented by formula (Ib): [ka] In the formula, R 1 and R 2 is as described above, and formula (Ib) complies with the above-mentioned conditions.
[0085] Embodiment E 1 So, R 1 and R 2 are, independently of one another, advantageously H, a halogen atom, a C1-C4 alkyl, a C1-C4 alkenyl, a C1-C4 alkoxy, a phenyl, -R' a -S(=O)-R a or -R' a -S(=O)2-R a wherein R a is C1-C4 alkyl or phenyl, R' a is C1-C6 alkanediyl or C2-C6 alkenediyl, -R' a -S(=O)-R a or -R' a -S(=O)2-R a and however, R 1 and R 2is (i) a C1-C6 alkanediyl group, (ii) a C2-C6 alkenediyl group, (iii) -R' b ~N=N- group, where R' b is a C1-C4 alkanediyl group, the carbon atoms of which are optionally further substituted two times, as defined herein [ka] (In the formula, R' c is nil or C1-C4 alkanediyl) forming a spiro linkage as shown in b ~N=N-group, or (iv) -CH2-C(=O)-CH(-COOR b )-group, in which R b is C1-C4 alkyl, -CH2-C(=O)-CH(-COOR b )-group, so that R 1 and R 2 form a ring with the two carbon atoms to which they are attached, and R 1 and R 2 When and are combined in such a way that there are no carbon-carbon bonds, R 2 The carbon atom to which is bonded is a group R 2ビス wherein R 2ビス is a C1-C4 alkyl or halogen atom; 2ビス It may be further substituted by:
[0086] First partial embodiment E 11 So, R 1 and R 2 is H. Solvent S is then (1S,5R)-6,8-dioxabicyclo[3.2.1]oct-2-en-4-one (commonly and herein referred to as levoglucosenone) or (1S,5R)-6,8-dioxabicyclo[3.2.1]octan-4-one (commonly and herein referred to as silene). Their chemical structures, SMILES and Hansen parameters are given in Table 1.
[0087] [Table 1]
[0088] (1S,5R)-6,8-dioxabicyclo[3.2.1]oct-2-en-4-one (IUPAC name calculated by Lexichem TK 2.7.0 - Pubchem Release 2021.05.07), commonly and herein referred to as levoglucosenone, can be represented interchangeably by any one of the following three formulas: [ka] Its CAS Registry Number is 37112-31-5.
[0089] (1S,5R)-6,8-dioxabicyclo[3.2.1]oct-2-en-4-one (IUPAC name calculated by Lexichem TK 2.7.0 - Pubchem Release 2021.05.07), commonly and herein referred to as silene or levoglucosenone, can be represented interchangeably by any one of the following three formulas: [ka] Its CAS Registry Number is 53716-82-8.
[0090] Partial embodiment E 11 The preferred solvent S is silane.
[0091] Second Partial Embodiment E 12 So, R 1 is H and R 2 is different from H. This subembodiment E 12 So, R 2 may in particular be a C1-C4 alkyl or halogen atom, in particular a halogen atom, more particularly a bromine atom. 12 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds are given in Table 2.
[0092] [Table 2]
[0093] Third Partial Embodiment E 13 So, R 1 Unlike H, R 2 is H. This subembodiment E 13 So, R 1 is particularly C1-C4 alkyl, -R' a -S(=O)-R a or -R' a -S(=O)2-R a where R' may be a is C1-C6 alkanediyl or C2-C6 alkenediyl, R a is C1-C4 alkyl or phenyl. In particular, R 1 -R' a -S(=O)-R a or -R' a -S(=O)2-R a, where R' may be a is as mentioned above, and R a is phenyl. 13 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds are given in Table 3.
[0094] [Table 3]
[0095] Fourth Partial Embodiment E 14 So, R 1 and R 2 and are both different from H. 14 So, R 1 and R 2 may in particular be C1-C4 alkyl, or R 1 and R 2 is (i) a C1-C6 alkanediyl group (particularly, -CH2-) or (ii) -R' b -N=N- group, where R' bis a C1-C4 alkanediyl group (particularly CH2-), the carbon atoms of which are optionally further substituted twice, as defined herein [ka] (In the formula, R' c is nil or C1-C4 alkanediyl (preferably nil), forming a spiro bond as shown in b -N=N- group, resulting in R 1 and R 2 form a ring having the two carbon atoms to which they are attached. 14 So, R 1 and R 2 When and are combined in this way, R 2 The carbon atom to which is attached generally is a group R, including when any carbon-carbon bond is not present in formula (I), such as in formula (Ib). 2ビス Not further substituted by E 14 Chemical structures, SMILES, Hansen parameters and access codes to one or more source references of exemplary compounds are provided in Table 4.
[0096] [Table 4]
[0097] Embodiment E 2 Second embodiment E 2 In the formula (II) [ka] where (-) represents any carbon-carbon bond that, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; R 1 , R 2 and R 3 is as described above, and formula (II) complies with the above-mentioned conditions.
[0098] Solvent S may contain any carbon-carbon bond (-) of formula (II), such as formula (IIa): [ka] In the formula, R 1 , R 2 and R 3 is as described above, and formula (IIa) is subject to the above-mentioned conditions. Alternatively and preferably, any carbon-carbon bond (-) is not present in formula (II); then the solvent S can be represented by formula (IIb): [ka] In the formula, R 1 , R 2 and R 3 is as described above, and formula (IIb) complies with the above-mentioned conditions. The solvent S of formula (IIb) that complies with this condition can be represented by formula (IIc) or (IId), [ka] This is R 2 is bonded to a carbon atom that is a group R 2ビス where R 12 is R as described above. 1 and R 2 is a divalent radical resulting from the combination of 2ビス is a C1-C4 alkyl or halogen atom.
[0099] Embodiment E 2 So, R 1 , R 2 and R 3 are, independently of one another, advantageously H, C1-C4 alkyl, C1-C4 alkenyl, C1-C4 alkynyl, C1-C4 alkoxy, halogen atoms, [ka] -R' a -S(=O)-R a or -R' a -S(=O)2-Ra wherein R a is C1-C4 alkyl or phenyl, R' a is C1-C6 alkanediyl or C2-C6 alkenediyl, -R' a -S(=O)-R a or -R' a -S(=O)2-R a and however, R 1 and R 2 is (i) a C1-C6 alkanediyl group, (ii) a C2-C6 alkenediyl group, (iii) -R' b ~N=N- group, where R' b is a C1-C4 alkanediyl group, the carbon atoms of which are optionally further substituted two times, as defined herein [ka] (In the formula, R' c is nil or C1-C4 alkanediyl) forming a spiro linkage as shown in b ~N=N-group, or (iv) -CH2-C(=O)-CH(-COOR b )-group, in which R b is C1-C4 alkyl, -CH2-C(=O)-CH(-COOR b )-group, resulting in R 1 and R 2 form a ring with the two carbon atoms to which they are attached, and R 1 and R 2 When and are combined in such a way that there are no carbon-carbon bonds, R 2 The carbon atom to which is bonded is a group R 2ビス wherein R 2ビス is a C1-C4 alkyl or halogen atom; 2ビス It may be further substituted by:
[0100] First partial embodiment E 21 So, R 1 , R2 and 3 is H. E 21 The chemical structure, SMILES, Hansen parameters and access code to one or more source references of solvent S according to are given in Table 5.
[0101] [Table 5]
[0102] Second Partial Embodiment E 22 So, R 1 and R 2 is H and R 3 is different from H. This subembodiment E 22 So, R 3 is particularly C1-C4 alkyl, C1-C4 alkenyl, C1-C4 alkynyl, [ka] or -R' a -S(=O)-R a wherein R a is C1-C4 alkyl or phenyl, R' a R is C1-C6 alkanediyl or C2-C6 alkenediyl. 3 but [ka] If R a is preferably phenyl. 3 -R' a -S(=O)-R a If R a is preferably C1-C4 alkyl, in particular methyl. 22 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds are given in Table 6.
[0103] [Table 6]
[0104] Third Partial Embodiment E 23 So, R 1 or R 2 is H, but not both of them, R 3 is H. This subembodiment E 23 In some cases, a group other than H, R 1 or R 2 may in particular be C1-C4 alkyl or C1-C4 alkoxy. 23 So, R 2 is advantageously H and R 1 means different from H; in particular, R 1 can be C1-C4 alkoxy. 23 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds are given in Table 7.
[0105] [Table 7]
[0106] Fourth Partial Embodiment E 24 So, R 1 and R 2 Unlike H, R 3 is H. This subembodiment E 24 So, R 1 and R 2 may, independently of one another, in particular be C1-C4 alkyl. 24 Now, R1 and R 2 can also be combined into a C1-C6 alkanediyl group (especially methylene) or a C2-6 alkenediyl group (especially methylene), so that R 1 and R 2 form a ring with the two carbon atoms to which they are attached, with the proviso that R 1 and R 2 and so combined that any carbon-carbon bond is absent in formula (II), R 2 The carbon atom to which is bonded is R 2ビスis a C1-C4 alkyl or halogen atom; 2 can be further substituted with bis, 12 is R 1 and R 2 It is a divalent radical resulting from the combination of E 24 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds according to the present invention are given in Table 8.
[0107] [Table 8]
[0108] Embodiment E 3 , E 4 and E 5 Embodiment E 3 , E 4 and E 5 In the above, the solvent S is represented by the formula (III). [ka] [Preferably, the compound represented by formula (IIIb) [ka] ], formula (IV) [ka] [Preferably, the compound represented by formula (IVb) [ka] or formula (V) [ka] [Preferably, the formula (Vb) [ka] ] where (-) represents any carbon-carbon bond that, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; R 1 , R2 , R 4 is as described above, and the above formula complies with the above conditions.
[0109] Embodiment E 3 , E 4 and E 5 So, R 1 and R 2 may, independently of one another, in particular be H, C1-C4 alkyl, C1-C4 alkenyl, C1-C4 alkoxy or a halogen atom, with the proviso that R 1 and R 2 is (i) a C1-C6 alkanediyl group, (ii) a C2-C6 alkenediyl group, or (iii) -CH2-C(=O)-CH(-COOR b )-group (wherein, R b is C1-C4 alkyl; preferably, R 1 and R 2 are hydrogen or are combined with a methylene group. 3 So, R 4 is advantageously hydrogen or -CH2OH.
[0110] Embodiment E 3 , E 4 and E 5 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds according to the present invention are given in Table 9.
[0111] [Table 9]
[0112] Part M 1 Some solvents S based on embodiment E 1 ~E 5 Correspondingly, it does not conform to any of the above formulas (I) to (V). As an example, mention may be made of a solvent of formula (XI). [ka] S119, as labeled by Pacheco et al., has AX-II as the access code to the source reference, its SMILES is O=C1CC(C)(C)CC2=C1C3CC(O)(O2)C4OCC3O4, and Hansen parameters δD=18.6, δP=10.9, and δH=8.6.
[0113] Part M 2 An embodiment based on In some other embodiments, the solvent S is a moiety M 1 The moiety M of formula (F-II) is isomeric with 2 Including, [ka] wherein (-) represents any carbon-carbon bond that, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; The carbon atom with an asterisk is a carbon atom that is bound to at least one oxygen atom R O R is substituted with a monovalent or divalent group containing O is advantageously a moiety M 1 As specified for R O can be oxo (=O); 6 The same is true for.
[0114] Embodiment E 6 Embodiment E 6 So, the solvent S is represented by the formula (VI) [ka] [Preferably, the compound represented by formula (VIb) [ka] where (-) represents any carbon-carbon bond that, if present, combines with another carbon-carbon bond to form a carbon-carbon double bond; R 1 and R 2 is as described above, and formulas (VI) and (VIb) comply with the above-mentioned conditions. 1and R 2 is advantageously R of formula (I) 1 and R 2 Preferably, R 1 and R 2 are both hydrogen.
[0115] Embodiment E 6 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds according to the present invention are given in Table 10.
[0116] [Table 10]
[0117] Part M 3 An embodiment based on In some other embodiments, the solvent S is a moiety M of formula (F-III) 3 Including, [ka] wherein (-) represents any carbon-carbon bond that, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; The carbon atom with an asterisk is connected to at least one oxygen atom R O,2 R is substituted with a monovalent group containing O,2 is advantageously (i) a hydroxymethyl group, -CHOH; (ii) an alkoxymethyl group, -CHOR c (In the formula, R c is C1-C6 alkyl), (iii) a formyloxymethyl group -CH2-OC(=O)-H and (iv) a group of the formula --CH2-OC(=O)-R c (In the formula, R c is C1-C6 alkyl. 7 and E 8 The same is true.
[0118] Embodiment E 7 and E 8 Embodiment E 7 and E 8 In the above, the solvent S is represented by the formula (VII) [ka] [Preferably, the compound represented by formula (VIIb) [ka] ], or formula (VIII) [ka] [Preferably, the compound represented by formula (VIIIb) [ka] wherein (-) represents any carbon-carbon bond which, if present, may combine with another carbon-carbon bond to form a carbon-carbon double bond; 5 , R 6 and R 7 is as described above, and the above formulas (VII), (VIIb), (VIII) and (VIIIb) comply with the above conditions.
[0119] Embodiment E 7 and E 8 So, R 5 is preferably hydrogen or methyl, more preferably hydrogen.
[0120] Embodiment E 7 and E 8 In this case, preferably, (i) R 6 and R 7 and (ii) R 6 Or R 7one of which is a hydrogen atom and the other is a phenyl group optionally substituted by one monovalent radical selected from 1-C4 alkyl (preferably methyl), C1-C4 alkoxy (preferably methoxy) and a carboalkoxy group -COOR, where R is a C1-C6 alkyl (preferably methyl), or a carboalkoxy group -COOR, where R is a C1-C6 alkyl (preferably methyl), or the two carbon atoms are adjacent to each other and [ka] a ring having an oxymethyleneoxy group -O-CH-O-, where the asterisks indicate two adjacent carbon atoms of the phenyl ring, substituted to form a ring; or (iii) R 6 and R 7 is combined with a C1-C6 alkanediyl group or a C2-C6 alkenediyl group.
[0121] Embodiment E 7 and E 8 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds according to the present invention are given in Tables 11 and 12, respectively.
[0122] [Table 11]
[0123] [Table 12]
[0124] Part M 4 An embodiment based on In some other embodiments, the solvent S is a moiety M of formula (F-IV) 4 Including, [ka] where the carbon atom bearing the asterisk represents at least one oxygen atom R O,2 The moiety M is substituted with a monovalent group containing3 As in the case of part M 4 R O,2 is advantageously (i) a hydroxymethyl group -CHOH; (ii) an alkoxymethyl group -CHOR c (In the formula, R c is C1-C6 alkyl), (iii) a formyloxymethyl group -CH2-OC(=O)-H and (iv) a group of the formula -CH2-OC(=O)-R c (In the formula, R c is C1-C6 alkyl. 9 and E 10 The same is true.
[0125] Embodiment E 9 and E 10 Embodiment E 9 and E 10 Then, the solvent S is represented by the formula (IX): [ka] or formula (X), [ka] In the formula, R 5 , R 6 , R 7 and R 8 is as described above, and the above formulas (IX) and (X) are subject to the above conditions.
[0126] Embodiment E 9 and E 10 So, R 5 is preferably hydrogen or methyl, in particular methyl.
[0127] E 9 and E 10 In the above, preferably, (i) R 6 and R 7 and both represent hydrogen atoms, or (ii) R 6 or R 7is a hydrogen atom and the other is a C1-C4 alkyl group (preferably methyl), or (iii) R 6 and R 7 But, the formula [ka] is combined with a C1-C6 alkanediyl group, a C2-C6 alkenediyl group, or a cycloalkenediyl group.
[0128] E 9 and E 10 In R 8 is often C1-C4 alkoxy, especially methoxy.
[0129] Embodiment E 9 and E 10 Chemical structures, SMILES, Hansen parameters and access codes to source references for exemplary compounds according to the present invention are given in Table 13.
[0130] [Table 13]
[0131] Some special solvents S are 1 , M 2 , M 3 Or M 4 By way of example, mention may be made of the solvent of formula (XII): [ka] S69, as labeled by Pacheco et al., has AM-9a as the access code to the source reference, its SMILES is N#CCCC(CCl)OC=O, and the Hansen parameters are δD=17.3, δP=12.8, and δH=8.1.
[0132] In the left column of Tables 2-12 above, the solvent S is identified by the label S<number>, which is identical to the label used by Pacheco et al., followed in brackets and italics by the code that allows access to it based on the source reference, also used by Pacheco et al. When the code is in the form <alphabet>-<number>, the alphabet before the dash constitutes the label that refers to the source reference / citation as specified in Table 14. The number after the dash point refers to the compound label used in the original reference. For this reason, abbreviations, alphabets, numbers and Roman numerals are possible; no common format is used to aid in finding the compounds in the respective references. When a compound label is followed by (m), this is an original modification to the referenced structure, (m2) denotes a second structural modification, (m3) a third structural modification, etc. Some compounds have more than one label because they appear in multiple references, and therefore each compound is also labeled individually.
[0133] [Table 14]
[0134] Use of Solvent S The present invention also relates to the use of a solvent S for swelling a fiber reinforced epoxy composite, wherein the solvent S and the fiber reinforced epoxy composite are as described above.
[0135] Preferably, when the fiber reinforced epoxy composite is a laminate, it is further used to delaminate the fiber reinforced epoxy composite laminate.
[0136] The fiber-reinforced epoxy composite is treated at temperature T without stirring in solvent S. tr The swelling rate after complete immersion in water for 5 hours may be 5% or more, advantageously at least 8%, preferably at least 12%, more preferably at least 15%, even more preferably at least 18%.
[0137] Other Aspects of the Invention composition The present invention also relates to a composition comprising a fibre reinforced epoxy composite as defined above and a solvent S as defined above, such as the composition described above in relation to method M.
[0138] Process P 1 The present invention also provides a process P for inducing the decomposition of an epoxy resin contained in a fiber-reinforced epoxy composite. 1 Regarding the process P 1 teeth, a) subjecting a fibre reinforced epoxy composite to a pretreatment, the pretreatment comprising applying method M as previously defined; b) subjecting the thus pretreated fiber-reinforced epoxy composite to an enzymatic and / or chemical treatment; Including, Each of a) and b) is carried out once or several times.
[0139] In some preferred embodiments, this includes b) subjecting the thus pretreated fiber reinforced epoxy composite to an enzymatic treatment but not to a chemical treatment, or b) subjecting the thus pretreated fiber reinforced epoxy composite to an enzymatic treatment and then to one or more chemical treatments.
[0140] The advantage of enzymatic degradation is that it generally means milder and safer conditions with less impact on the environment. As taught by Eliaz et al. in Materials (Basel), 2018, 11, 2123, some bacteria that may degrade epoxy resins are Rhodococcus rhodochrous and Ochrobactrum anthropi.
[0141] As far as the chemical treatment is concerned, this treatment advantageously comprises: - contacting the fiber reinforced epoxy composite with an aqueous solution of phosphoric acid and / or its salts; - contacting the fiber reinforced epoxy composite with an organic solution of phosphoric acid and / or its salts; - contacting the fiber reinforced epoxy composite with an aqueous solution of a strong Bronsted base; - subjecting the fibre reinforced epoxy composite to an acid digestion treatment Includes at least one of the following:
[0142] More preferably, process P 1 Step b) of b1) contacting a fiber reinforced epoxy composite with an enzyme; b2) contacting the fiber reinforced epoxy composite with an aqueous solution of phosphoric acid and / or its salts; b3) contacting the fiber reinforced epoxy composite with an aqueous solution of a strong Bronsted base; Each of b1), b2) and b3) is carried out once or several times.
[0143] Using Method M The present invention also relates to the use of the above-mentioned method M for increasing the diffusion rate of an enzyme or chemical compound in an epoxy resin embedded in a fiber-reinforced epoxy composite.
[0144] Advantageously, the enzyme or chemical compound, as the case may be, is selected from enzymes and chemicals capable of reacting with epoxy resins, in particular with hardened and / or crosslinked epoxy resins.
[0145] Preferably, the enzyme or compound is selected from enzymes and chemicals capable of reacting with epoxy resins according to reactions or reaction schemes that can cause degradation of the fibre reinforced epoxy composite, in particular the aforementioned epoxy resins and fibre reinforced epoxy composites.
[0146] Process P 2 and P 3 The present invention also relates to a process P for recovering reinforcing fibers from fiber-reinforced epoxy composites. 2 With regard to this, - The aforementioned process 1decomposing an epoxy resin contained in a fiber-reinforced epoxy composite material by the above-mentioned method, thereby obtaining a material containing carbon fibers and an epoxy decomposition product; - separating the carbon fibers from the material thus obtained; Includes.
[0147] This is the process P for recycling reinforcing fibers. 3 This includes: - Process P mentioned above 2 recovering carbon fibers from a fiber reinforced epoxy composite by; - producing a composite material comprising a polymer and the carbon fibers thus recovered, said composite material being identical or different from the fiber-reinforced epoxy composite material comprised in method M above; Includes.
[0148] Advantages of the Invention The present invention has several advantages.
[0149] The present invention provides a method as efficient as the solvent pretreatment method of Ma and Nutt that does not require the use of solvents provided by the petroleum industry. It provides a treatment method M that is as efficient as the solvent pretreatment method of Ma and Nutt that is based on a bio-based solvent S, i.e., one that can be produced from renewable biological feedstocks. Silene, which is or can become a potentially cheap and widely available solvent, is a suitable and preferred solvent S.
[0150] Bio-based solvents S of either Group 1 or 2 as described above are also generally at least as efficient as benzyl alcohol in their ability to promote the subsequent chemical degradation of the epoxy contained in the epoxy composite laminate, including swelling (as described by Ma and Nutt) and delamination (which is not mentioned by Ma and Nutt).
[0151] Group 1 bio-based solvents S, as described above, allow for achieving increased swelling of fiber-reinforced composites, which may be desirable to make the composite more permeable and further reduce the rate-limiting effects of diffusion, especially for the strongest "cured" composites, which often contain highly crosslinked epoxy components. Group 1 bio-based solvents S can swell fiber-reinforced epoxy composites to a greater extent than benzyl alcohol can. EXAMPLES
[0152] Experimental procedure material A 1 cm × 1 cm × 0.334 cm composite specimen containing 16 carbon fibers (70.52 wt%) embedded by epoxy resin (29.48%) produced by the mixture and subsequent polymerization of diglycidyl ether bisphenol A (DGEBA as the epoxy source) and 4,4'-methylenebis(2,6-diethylaniline (M-DEA, as the hardener). The epoxy resin component is a crosslinked network, the simplified representation of which can be as follows: [ka] where n is an integer corresponding to the number of repeating units in the epoxy resin. The glass transition temperature was 164° C. as measured by DSC using ASTM E 1356-08(2014) for the composite.
[0153] Benzyl alcohol (boiling point 199° C., molecular weight MW 108.1 g / mol) is hereinafter referred to as “BZA.”
[0154] Methyl 4-(dimethylcarbamoyl)-2-methylbutanoate is commercially available from SOLVAY as RHODIASOLV® Polarclean solvent (boiling point 282° C., MW 187.2 g / mol), hereafter referred to as “PLC.”
[0155] Silene is commercially available from CIRCA as CYREN™ solvent (boiling point 227° C., MW 114 g / mol), hereinafter referred to as “CRN”.
[0156] Solvent Treatment The solvent bath was heated to the target temperature (100° C. or 200° C. in the following examples). The mass ratio of the composite specimen to the solvent forming the solvent bath was 1:50 (the amount of solvent was high enough to allow the complete immersion of the composite specimen in the solvent bath, thereby ensuring good reproducibility of the results). When the solvent reached the target temperature, the specimen was completely immersed in the solvent bath without stirring and maintained at such temperature for 5 hours without stirring. The immersed specimen was then hot filtered and the recovered specimen was washed alternately with Milli-Q® water (18.2 mΩ) and absolute ethanol, using 200 ml of each water and ethanol for each gram of composite specimen.
[0157] Swelling rate and peeling degree To estimate the swelling effect of the solvent treatment, we relied on the mass gain of the composite specimens. The swelling ratio r sw (expressed in %) was calculated using the formula Equ1:
number
[0158] In Equation 1, m 初期 and m 最終 are the masses of the composite specimen before and after treatment, respectively.
[0159] To estimate the delamination effect of the solvent treatment, we relied on the number of composite sheets that were peeled off from the composite specimen. The swelling ratio d exf (expressed in %) was calculated using Equ.2:
number
[0160] In Equ. 2, nc 複合材試験片is the actual number of pure composite specimens treated with a given solvent (which may be one or more), and X is the number of carbon fiber sheets stacked to form the composite specimen. In these examples, each composite specimen is prepared from 16 carbon fiber sheets stacked together; therefore, X is 16. In this formula, n 複合材シート n is the number of composite sheets that separated from one or more composite specimens for a given solvent after the specimens were subjected to solvent treatment. In practice, square or near-square structures formed from carbon fibers embedded in epoxy resin were counted as released sheets; all untreated composite specimens contained 16 carbon fibers, so n 複合材シート can vary from 1 to 15 depending on the specimen.
[0161] Since both swelling and delamination are believed to be important in promoting the degradation of fiber-reinforced epoxy composites, a solvent treatment that efficiently produces both effects is desirable. A figure of merit PI, which reflects the overall degradation of the composite specimens, was calculated. deg can be defined as follows: PI deg =1 / 100 r sw d exf . PI deg is the degradation performance index, and r sw and d exf and are the swelling ratio and degree of peeling, respectively, defined above, both expressed in %.
[0162] Solvent treatment results and considerations The results of the solvent treatment are shown in Table 15. The comparative examples with BZA are in accordance with what can be considered the closest prior art known to the applicant, i.e., the paper by Ma and Nutt on polymer degradation and stability, which is discussed in the Background section. Examples of PLC, an environmentally friendly solvent, are also provided for comparison with CRN, but to the best of the applicant's knowledge, they do not form part of the prior art; therefore, their presentation should not be construed as an admission by the applicant that they do form part of the prior art.
[0163] [Table 15]
[0164] Regardless of the nature of the solvent, all treatments CE1-CE3 were performed at 100°C, i.e. below the glass transition temperature of the epoxy resin matrix, and poor results were obtained with little swelling and delamination of the composite specimens. The applicant believes that below the glass transition temperature of the epoxy resin matrix, molecular chains from the material likely remain frozen, causing steric hindrance and acting as a physical barrier to the solvent.
[0165] On the other hand, all composite specimens (CE4, CE5 and E1) substantially decomposed when treated at temperatures above the glass transition temperature of the epoxy resin matrix, here 200° C. The Applicant believes that at such temperatures the free volume of the resin probably increased and localized polymer segment motion allowed solvent diffusion in the matrix, promoting on the one hand swelling of the resin and mass gain of the composite specimens, and on the other hand fragmentation of the resin due to covalent bond breaking and delamination of the composite specimens.
[0166] Treatment with BZA at 200°C, i.e. above the glass transition temperature of the epoxy resin matrix, made it possible to achieve the highest degree of exfoliation. On the other hand, the epoxy specimens were best swollen with CRN (Example E1 according to the invention). Nothing would have suggested to a person skilled in the art that the swelling capacity of CRN would far exceed that of BZA above the glass transition temperature of the epoxy resin matrix; on the contrary, the results obtained at 100°C would have suggested that BZA should have been a better candidate for swelling the epoxy resin. Without being bound by any theory, the applicant believes that the significantly higher swelling capacity of CRN may be due to its lower hydrogen bonding strength (δH) when compared to BZA.
[0167] Notably, by treating epoxy specimens with CRN above the glass transition temperature of the epoxy resin, as in Example E1, it was possible to achieve a moderately high level of delamination without reaching the delamination of BZA. Nevertheless, in terms of overall degradation, including swelling effect and achievable level, CRN was unexpectedly qualified as a solvent to perform at least as BZA, as revealed by the DPI index of CRN. Without being bound by any theory, the applicant believes that the high overall decomposition performance of CRN can be achieved thanks to the appropriate combination of high dispersion power (δP) and lower hydrogen bonding power (δH).
[0168] Finally, in the CRN / BZA comparison, CRN has the important advantage of being a bio-based solvent that can be synthesized from cellulose, a low-cost and widely available renewable resource, which is clearly not the case for BZA.
[0169] Finally, compared to several other green solvents such as PLC, CRN, etc., it showed both superior swelling and stripping capabilities when used as a solvent above the glass transition temperature of epoxy resins. Nothing in the prior art suggests such superior degradation performance of CRN over PLC.
Claims
1. The fiber-reinforced epoxy composite is treated at a temperature T tr a method M for treating said fiber reinforced epoxy composite comprising contacting said fiber reinforced epoxy composite with a solvent S at The solvent S is levoglucosenone and / or a levoglucosenone derivative, for which the Hansen solubility parameters calculated from the SMILES of the solvent S using the Yamamoto Molecular Breaking Method with HSPiP software version 5.3.06 meet the following requirements: 16≦δD≦20 16≦δP+δH≦22 2 / 5≦δH / δP≦9 / 5 where δD is the energy from dispersion forces between molecules, δP is the energy from dipole-dipole intermolecular forces between molecules, and δH is the energy from hydrogen bonds between molecules, and all three are in MPa 0.5 It is expressed as The processing temperature T tr is the glass transition temperature T of the fiber-reinforced epoxy composite determined by DSC according to ASTM E1356-08 (2014). g At least 10°C above however, If the glass transition temperature cannot be detected by DSC according to ASTM E1356-08 (2014), the treatment temperature T tr satisfies at least one condition selected from conditions (c1) to (c3), Condition (c1) is the glass transition temperature T g2 can be determined by DMA according to ASTM D7028-07 (2015), and the treatment temperature T tr is the glass transition temperature T g2 at least 10°C above The condition (c2) is the treatment temperature T tr However, the treatment is performed without stirring the fiber-reinforced epoxy composite at the treatment temperature T tr A swelling ratio r of at least 8% as determined after complete immersion in said solvent S for 5 hours at 100° C. sw a treatment temperature which causes swelling of the fiber reinforced epoxy composite by the solvent S; The method, wherein condition (c3) is that the treatment temperature is at least 300° C.
2. Glass transition temperature T g can be detected by DSC according to ASTM E1356-08 (2014), and the glass transition temperature T g A processing temperature T at least 30° C. higher than tr 2. The method of claim 1, comprising fully immersing the fiber reinforced epoxy composite in the solvent S at 0.5° C. for at least 1 hour.
3. The method of claim 1 or 2, wherein the fiber reinforced epoxy comprises carbon fiber.
4. 4. The method according to claim 1, wherein the solvent S is characterized in that 18≦δP+δH≦20.
5. 5. The method according to claim 1, wherein the solvent S is characterized by δH / δP<1.
6. The method of claim 5 , wherein the solvent S is silane.
7. 5. The method according to claim 1, wherein the solvent S is characterized by δH / δP≧1.
8. The method according to claim 7, wherein the solvent S is levoglucosenol and / or levoglucosanol.
9. 2. Use of the solvent S as defined in claim 1 for swelling a fibre reinforced epoxy composite, preferably use of silene for swelling a fibre reinforced epoxy composite containing carbon fibres.
10. 10. The use according to claim 9, wherein the solvent S is a laminate and further for delaminating the fiber reinforced epoxy composite.
11. A composition comprising a fiber reinforced epoxy composite and said solvent S as defined in claim 1, preferably wherein said fiber reinforced epoxy composite comprises carbon fibers and said solvent S is silane.
12. Process P for inducing decomposition of epoxy resin contained in fiber reinforced epoxy composites 1 The process P 1 but, a) subjecting the fibre reinforced epoxy composite to a pretreatment, said pretreatment comprising applying the method M according to any one of claims 1 to 8; b) subjecting the thus pretreated fiber reinforced epoxy composite to an enzymatic and / or chemical treatment; Including, A process wherein each of a) and b) is carried out once or several times.
13. Use of the method M according to any one of claims 1 to 8 for increasing the diffusion rate of an enzyme or chemical compound in the epoxy matrix of a fibre reinforced epoxy composite.
14. Process P for recovering reinforcing fibers from fiber-reinforced epoxy composites 2 And, Process P according to claim 12 1 decomposing the epoxy resin contained in the fiber-reinforced epoxy composite material by the above-mentioned method, thereby obtaining a material containing carbon fibers and epoxy decomposition products; - separating the carbon fibres from the material thus obtained; The process includes:
15. Process P for recycling reinforcing fibers 3 And, Process P according to claim 14 2 recovering carbon fibers from a fiber reinforced epoxy composite by - producing a composite material comprising a polymer and the carbon fibers thus recovered, said composite material being identical or different to the fiber reinforced epoxy composite material relating to method M of claims 1 to 3.