Recovery of halogens using oxidizing agents and phase transfer catalysts in the halogenation process of unsaturated isoolefin copolymers.

Quaternary ammonium salts as phase transfer catalysts enhance halogen utilization in brominating butyl rubber by oxidizing hydrogen bromide to molecular bromine, addressing inefficiencies in existing methods and improving bromine incorporation in the presence of water.

JP2024543637APending Publication Date: 2024-11-21ARLANXEO SINGAPORE PTE LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024534350
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-13
Filing Date
2022-12-08
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for brominating butyl rubber result in low halogen utilization due to the formation of hydrogen bromide, which is not further brominated under normal conditions, and are inefficient in the presence of water, requiring costly and energy-intensive processes to manage water content.

Method used

The use of quaternary ammonium salts as phase transfer catalysts in a two-phase reaction medium to oxidize hydrogen bromide back to molecular bromine, enhancing halogen utilization and reducing sensitivity to water.

Benefits of technology

Improves halogen utilization efficiency, allowing for higher bromine incorporation into butyl rubber while maintaining the microstructure and molecular weight of the copolymer, even in the presence of significant water content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543637000001_ABST
    Figure 2024543637000001_ABST
Patent Text Reader

Abstract

The method of producing a halogenated isoolefin copolymer involves contacting an unsaturated isoolefin copolymer cement comprising an unsaturated isoolefin copolymer dissolved in an organic solvent under halogenation conditions with a halogenating agent and an aqueous solution of an oxidizing agent and a phase transfer catalyst to form a two-phase reaction medium comprising an organic phase and an aqueous phase, wherein the oxidizing agent is capable of converting hydrogen halide to free halogen and the phase transfer catalyst is a compound represented by formula (I): JPEG2024543637000019.jpg27170 (in the formula, M + is a cation of a group VA element; X - is an anion that dissociates from a cation in aqueous solution; and R1, R2, R3 and R4 are the same or different and independently C 1~30 (It is an organic part.) The process provides improved halogen recovery, is less sensitive to the presence of water, and can use a variety of different oxidizing agents.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to European Patent Application No. 21214084.2, filed December 13, 2021, the entire contents of which are incorporated herein by reference.

[0002] This application relates to a process for halogenating unsaturated isoolefin copolymers. [Background technology]

[0003] The standard process for brominating butyl rubber to form bromobutyl rubber uses molecular bromine (Br2) as the brominating agent. This process produces hydrogen bromide (HBr) as a by-product, which, under normal conditions, does not further brominate the butyl rubber polymer. Thus, the theoretical maximum percentage of bromine present in the reaction mixture that can be incorporated into the butyl rubber polymer is 50%. However, in practice, this percentage is usually less than 45%, and less than 35% in both laboratory and production plant facilities.

[0004] Known methods for increasing bromine utilization during the bromination of butyl rubber (Patent Document 1, Patent Document 2, Patent Document 3, Patent Document 4) involve utilizing at least 0.5 moles of a water-soluble oxidizing agent, such as an organic peracid or hydrogen peroxide, per mole of brominating agent. These water-soluble oxidizing agents reoxidize the hydrogen bromide back to elemental bromine. The oxidizing agent can be an aqueous solution or an aqueous emulsion in an organic solvent. Since the oxidizing agent is only soluble in water, the reaction rate depends on the rate at which the reactants can be exchanged between the organic and aqueous phases, which requires long reaction times.

[0005] Furthermore, the process utilizing hydrogen peroxide requires the presence of very low concentrations of water in the bromination medium. The observed benefits of using hydrogen peroxide in the bromination medium are dramatically reduced when the water concentration exceeds 1% by weight, and great difficulties and costs arise industrially. This is because additional equipment and energy may be required to reduce the water content in the bromination medium from 10-20% by weight to less than 1% by weight.

[0006] In addition, some processes involve post-halogenation recycling by neutralizing HBr to produce sodium bromide (NaBr), washing the NaBr from the halogenated butyl rubber into an aqueous stream, and converting the NaBr to Br2 using Cl2 gas, such as by a blow-out process. This ex-situ recycle method is limited by the efficiency of extraction of NaBr into the aqueous phase and the dilution of NaBr in the aqueous phase. Furthermore, performing such an ex-situ process is cost-ineffective and energy-intensive.

[0007] Although phase transfer catalysts such as quaternary ammonium salts are widely used in the synthesis of organic compounds in two-phase reactions (Patent Document 5), the use of phase transfer catalysts for halogen recovery during halogenation reactions of polymers remains underdeveloped. In (Patent Document 6), the use of methyltrialkylammonium chloride as a phase transfer catalyst in the chlorination of para-alkylstyrene copolymers for selective chlorination of para-alkyl groups is disclosed. However, neither the use of phase transfer catalysts for halogen recovery nor the effect of phase transfer catalysts on removing the water sensitivity of the halogenation reaction is disclosed. Furthermore, in (Patent Document 6), the oxidizing agent is a chlorinating agent for the polymer, and the oxidizing agent is not used to return hydrogen halide and / or halide ions to the halogenating agent. Therefore, in (Patent Document 6), no halogen recycling is performed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2020 / 124222 [Patent Document 2] US Patent Application Publication No. 2014 / 0309362 [Patent Document 3] U.S. Patent No. 3,018,275 [Patent Document 4] U.S. Pat. No. 5,681,901 [Patent Document 5] U.S. Pat. No. 3,992,432 [Patent Document 6] European Patent No. 0344021 Summary of the Invention [Problem to be solved by the invention]

[0009] There remains a need for a cost-effective, efficient process for improving halogen utilization during the halogenation of isoolefin copolymers, such as butyl rubber, especially in the presence of large amounts of water. [Means for solving the problem]

[0010] It has now been discovered that quaternary salts, preferably quaternary ammonium salts, used as phase transfer catalysts for the oxidant during the bromine recovery process reduce or eliminate sensitivity to water and improve bromine recovery for a given amount of oxidant.

[0011] In one aspect, a process for producing a halogenated isoolefin copolymer is provided, the process comprising contacting an unsaturated isoolefin copolymer cement comprising an unsaturated isoolefin copolymer dissolved in an organic solvent with a halogenating agent and an aqueous solution of an oxidizing agent and a phase transfer catalyst under halogenation conditions to form a two-phase reaction medium comprising an organic phase and an aqueous phase, wherein the oxidizing agent is capable of converting hydrogen halide to free halogen and the phase transfer catalyst is a compound represented by formula (I): [ka] (In the formula, M + is a cation of a group VA element; X - is an anion that dissociates from a cation in aqueous solution; and R1, R2, R3, and R4 are the same or different and independently represent C 1~30 (It is an organic group) It is a compound of the formula:

[0012] The halogenation process of the present invention advantageously provides enhanced halogen utilization by oxidizing hydrogen halide (HX) formed during halogenation of unsaturated isoolefin copolymer back to molecular halogen (X2). The process is less sensitive to the presence of water in cement, provides equivalent or better bromine recovery with less oxidizing agent compared to similar processes (e.g., processes using peracid alone or hydrogen peroxide alone), and can use a variety of different oxidizing agents. The process does not fundamentally affect the microstructure and molecular weight of the resulting halogenated isoolefin copolymer, and the ability to achieve equivalent or better halogenation efficiency using less oxidizing agent is further beneficial for maintaining the microstructure and molecular weight of the halogenated isoolefin copolymer.

[0013] Additional features will be described or will become apparent during the course of the following detailed description. It should be understood that each feature described herein can be utilized in any combination with any one or more of the other described features, and that, except as would be apparent to one of ordinary skill in the art, each feature does not necessarily require the presence of other features.

[0014] For a clearer understanding, preferred embodiments will now be described in detail, by way of example only, with reference to the accompanying drawings, in which: [Brief description of the drawings]

[0015] [Figure 1]FIG. 1 is a graph of functional bromine (mol%) versus reaction time (min) showing the effect of reaction time on bromine recovery using NaClO as the oxidant and tetrabutylammonium hydrogen sulfate (PTC1) as the phase transfer catalyst. [Diagram 2] FIG. 2 is a graph of functional bromine (mol%) versus reaction time (min) showing the effect of agitation speed on bromine recovery when using NaClO as the oxidant and tetrabutylammonium hydrogen sulfate (PTC1) as the phase transfer catalyst. [Diagram 3] FIG. 3 is a graph of bromine atom efficiency (BAE) (%) versus amount of phase transfer catalyst (mmol) showing the effect of amount of phase transfer catalyst on bromine recovery when using NaClO as the oxidant and tetrabutylammonium hydrogen sulfate (PTC1) as the phase transfer catalyst. [Figure 4] FIG. 4 is a graph of functional bromine (mol%) versus reaction time (min) showing the effect of reaction time on bromine recovery using NaBrO3 as the oxidant and tetrabutylammonium hydrogen sulfate (PTC1) as the phase transfer catalyst. [Diagram 5] FIG. 5 is a graph of bromine atom efficiency (BAE) (%) versus water concentration (wt%) showing the effect of water content on bromine recovery when using NaClO as the oxidant and tetrabutylammonium hydrogen sulfate (PTC1) or methyltrioctylammonium hydrogen sulfate (PTC3) as the phase transfer catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The process comprises polymerizing at least one isoolefin monomer and at least one copolymerizable unsaturated monomer in an organic diluent to produce a halogenatable isoolefin copolymer in an organic medium. The polymerization is carried out in a polymerization reactor. Suitable polymerization reactors include flow-through polymerization reactors, plug flow reactors, moving belt or drum reactors, and the like. The process preferably comprises a slurry polymerization of the monomers.

[0017] The halogenatable isoolefin copolymer preferably comprises repeat units derived from at least one isoolefin monomer, at least one copolymerizable unsaturated monomer, and optionally one or more additional copolymerizable monomers. The halogenatable isoolefin copolymer preferably comprises an unsaturated isoolefin copolymer.

[0018] Suitable isoolefin monomers include hydrocarbon monomers having 4 to 16 carbon atoms. In one embodiment, the isoolefin monomer has 4 to 7 carbon atoms. Examples of suitable isoolefins include isobutene (isobutylene), 2-methyl-1-butene, 3-methyl-1-butene, 2-methyl-2-butene, 4-methyl-1-pentene, 4-methyl-1-pentene, and mixtures thereof. A preferred isoolefin monomer is isobutene (isobutylene).

[0019] Suitable copolymerizable unsaturated monomers include multiolefins, p-methylstyrene, β-pinene, or mixtures thereof. Multiolefin monomers include hydrocarbon monomers having 4 to 14 carbon atoms. In some embodiments, the multiolefin monomer is a conjugated diene. Examples of suitable conjugated diene monomers include isoprene, butadiene, 2-methylbutadiene, 2,4-dimethylbutadiene, piperylene, 3-methyl-1,3-pentadiene, 2,4-hexadiene, 2-neopentylbutadiene, 2-methyl-1,5-hexadiene, 2,5-dimethyl-2,4-hexadiene, 2-methyl-1,4-pentadiene, 4-butyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,3-dibutyl-1,3-pentadiene, 2-ethyl-1,3-pentadiene, 2-ethyl-1,3-butadiene, 2-methyl-1,6-heptadiene, cyclopentadiene, methylcyclopentadiene, cyclohexadiene, 1-vinylcyclohexadiene, and mixtures thereof.

[0020] The halogenatable isoolefin copolymer may optionally include one or more additional copolymerizable monomers. Suitable additional copolymerizable monomers include, for example, styrene-based monomers, such as, but not limited to, alkyl-substituted vinyl aromatic comonomers, such as C1-C4 alkyl-substituted styrenes. Specific examples of additional copolymerizable monomers include, for example, α-methylstyrene, p-methylstyrene, chlorostyrene, cyclopentadiene, and methylcyclopentadiene. Indene and other styrene derivatives may also be used. In one embodiment, the halogenatable isoolefin copolymer may include a random copolymer of isobutylene, isoprene, and p-methylstyrene.

[0021] In one embodiment, the halogenatable isoolefin copolymer can be formed by copolymerization of a monomer mixture. Preferably, the monomer mixture comprises about 80-99.9 mol % of at least one isoolefin monomer and about 0.1-20 mol % of at least one copolymerizable unsaturated monomer, based on the monomers in the monomer mixture. More preferably, the monomer mixture comprises about 90-99.9 mol % of at least one isoolefin monomer and about 0.1-10 mol % of at least one copolymerizable unsaturated monomer. In one embodiment, the monomer mixture comprises about 92.5-97.5 mol % of at least one isoolefin monomer and about 2.5-7.5 mol % of at least one copolymerizable unsaturated monomer. In another embodiment, the monomer mixture comprises about 97.4-95 mol % of at least one isoolefin monomer and about 2.6-5 mol % of at least one copolymerizable unsaturated monomer.

[0022] When the monomer mixture includes an additional monomer copolymerizable with the isoolefin and / or the copolymerizable unsaturated monomer, the additional copolymerizable monomer preferably replaces a portion of the copolymerizable unsaturated monomer. When a multiolefin monomer is used, the monomer mixture can also include 0.01% to 1% by weight of at least one multiolefin crosslinking agent, and when the multiolefin crosslinking agent is present, the amount of multiolefin monomer is reduced accordingly.

[0023] The unsaturated isoolefin copolymers can be prepared by any suitable method, some of which are known in the art. For example, polymerization of the monomers can be carried out in a diluent in the presence of an initiator system (e.g., Lewis acid catalyst and a proton source) capable of starting the polymerization process. Proton sources suitable for the present invention include any compound that generates protons when added to a Lewis acid or a composition containing a Lewis acid. Protons can be generated by reaction of a Lewis acid with a proton source to generate protons and corresponding by-products. Such reactions may be preferred when the proton source reacts with the protonated additive faster than it reacts with the monomer. Reactants that generate protons include, for example, water, alcohols, phenols, thiols, carboxylic acids, and the like, or any mixture thereof. Water, alcohols, phenols, or any mixture thereof are preferred. The most preferred proton source is water. The preferred ratio of Lewis acid to proton source is 5:1 to 100:1 by weight or 5:1 to 50:1 by weight. The initiator system, including a catalyst and a proton source, is preferably present in the reaction mixture in an amount of 0.02 to 0.1 weight percent, based on the total weight of the reaction mixture.

[0024] Alkyl aluminum halide catalysts are a particularly preferred class of Lewis acids for catalyzing the solution polymerization reaction according to the present invention. Examples of alkyl aluminum halide catalysts include methyl aluminum dibromide, methyl aluminum dichloride, ethyl aluminum dibromide, ethyl aluminum dichloride, butyl aluminum dibromide, butyl aluminum dichloride, dimethyl aluminum bromide, dimethyl aluminum chloride, diethyl aluminum bromide, diethyl aluminum chloride, dibutyl aluminum bromide, dibutyl aluminum chloride, methyl aluminum sesquibromide, methyl aluminum sesquichloride, ethyl aluminum sesquibromide, ethyl aluminum sesquichloride and any mixtures thereof. Diethyl aluminum chloride (EtAlCl or DEAC), ethyl aluminum sesquibromide (Et 1.5 AlCl 1.5or EASC), ethylaluminum dichloride (EtAlCl2 or EADC), diethylaluminum bromide (Et2AlBr or DEAB), ethylaluminum sesquibromide (Et 1.5 AlBR 1.5 Preferred are ethylaluminum dibromide (EtAlBr2 or EASB) and ethylaluminum dibromide (EtAlBr2 or EADB) and any mixtures thereof. In a particularly preferred initiator system, the catalyst comprises ethylaluminum sesquichloride, preferably produced by mixing equimolar amounts of diethylaluminum chloride and ethylaluminum dichloride, preferably in a diluent. The diluent is preferably the same as that used to carry out the copolymerization reaction.

[0025] The diluent may include an organic diluent. Suitable organic diluents may include, for example, alkanes, chloroalkanes, cycloalkanes, aromatics, hydrofluorocarbons (HFCs), or any mixture thereof. Chloroalkanes may include, for example, methyl chloride, dichloromethane, or any mixture thereof. Methyl chloride is particularly preferred. Alkanes and cycloalkanes may include, for example, isopentane, cyclopentane, 2,2-dimethylbutane, 2,3-dimethylbutane, 2-methylpentane, 3-methylpentane, n-hexane, methylcyclopentane, 2,2-dimethylpentane, or any mixture thereof. The alkanes and cycloalkanes are preferably C6 solvents, including n-hexane or hexane isomers, such as 2-methylpentane or 3-methylpentane, or mixtures of n-hexane and such isomers, and cyclohexane. The monomers are typically cationic polymerized in the diluent at temperatures ranging from −120° C. to +20° C., preferably from −100° C. to −50° C., more preferably from −95° C. to −65° C. The temperature is preferably about −80° C. or less.

[0026] In the slurry polymerization process, when the diluent comprises a chloroalkane (e.g., methyl chloride), the diluent and residual monomers can be removed from the unsaturated isoolefin copolymer by flash separation with steam. Removal of the diluent and residual monomers in such a "wet" process leaves a polymer with a large amount of water. Dissolving the polymer in an organic solvent results in a polymer cement with a significant water content, for example, 1% or more or 1.5% or more by weight based on the total weight of the cement. In some embodiments, the water content of the cement can be 0-30%, or 0-25%, or 1-30%, or 1.5-15%, or 2-30%, or 2-20%, or 2-15%, or 5-20%, or 5-15%, or 5-10%, or 10-15% by weight based on the total weight of the cement.

[0027] In a slurry or solution polymerization process, when the diluent comprises a chloroalkane (e.g., methyl chloride) or an alkane (e.g., hexane), the diluent and residual monomers can be removed from the unsaturated isoolefin copolymer by flash separation or simple distillation using a heated organic solvent in which the unsaturated isoolefin copolymer is soluble. If simple distillation is used, a portion of the organic diluent may remain in the cement as an organic solvent. Removal of the diluent and residual monomers in such a "dry" process results in a polymer cement containing low water, for example, less than 1% by weight, or even less than 0% by weight, of water based on the total weight of the cement.

[0028] To form halogenated isoolefin copolymer, unsaturated isoolefin copolymer can be subjected to halogenation process using halogenating agent under halogenation conditions.Halogenation can be carried out by applying the process known to those skilled in the art (e.g. Rubber Technology, 3rd Ed., Edited by Maurice Morton, Kluwer Academic Publishers, pp.297-300 or U.S. Patent No. 5,886,106 issued on March 23, 1999, both of which are incorporated herein by reference) and modifying the process as described herein.

[0029] To improve the efficiency of the halogenation, the halogenation process is modified by contacting the unsaturated isoolefin copolymer cement, in which the unsaturated isoolefin copolymer is dissolved in an organic solvent, with a halogenating agent and an aqueous solution of an oxidizing agent and a phase transfer catalyst. A two-phase reaction medium is formed, which includes an organic phase and an aqueous phase. The oxidizing agent in-situ oxidizes the halides produced in the halogenation process back to the free form (i.e., molecular halogen), improving the halogen atom efficiency of the halogenation process.

[0030] Halogenating agents useful for halogenating the unsaturated isoolefin copolymer may include molecular chlorine (Cl2) or molecular bromine (Br2) and / or organic or inorganic halide precursors thereto, such as dibromodimethylhydantoin, trichloroisocyanuric acid (TClA), n-bromosuccinimide, sodium bromide, hydrogen bromide, and the like. Preferably, the halogenating agent comprises chlorine (Cl2) or bromine (Br2), more preferably bromine. Preferably, the halogenation comprises bromination. The amount of halogenating agent added is controlled so that the final halogen content in the halogenated isoolefin copolymer is at least 0.05 mol%, preferably 0.05-2.5 mol%. The amount of halogenating agent used has a linear relationship with the final halogen content (i.e., functional halogen content) of the halogenated isoolefin copolymer. The higher the amount of halogenating agent, the higher the functional halogen content in the halogenated isoolefin copolymer.

[0031] The halogenation is carried out in a reaction medium comprising an organic solvent, which is preferably an aliphatic solvent, and which preferably comprises an alkane, more preferably hexane or pentane.

[0032] The halogenation can be carried out for a period of time to achieve the desired halogenation level. The period of time is preferably 60 minutes or less. Significant halogenation of the unsaturated isoolefin copolymer can be achieved in 20 minutes or less, or 10 minutes or less, or even 5 minutes or less. Preferably, the halogenation is carried out for at least 1 minute. Preferably, the halogenation time is from 1 to 60 minutes, or from 1 to 20 minutes, or from 1 to 10 minutes, or from 1 to 5 minutes.

[0033] The halogenation can be carried out at any suitable temperature, preferably up to about 90°C. In some embodiments, the temperature can be up to about 80°C. In other embodiments, the temperature can be up to about 65°C. The increase in halogenation efficiency at low temperatures is more pronounced with higher concentrations of unsaturated isoolefin copolymer in the reaction medium. Temperatures in the range of 0-70°C, or 0-50°C, or 0-45°C, or 15-45°C, or 20-45°C, or 40-45°C, or 30-70°C, or 20-60°C, or 23-54°C, or 23-45°C, or 10-35°C, or 20-30°C are preferred. In one embodiment, the unsaturated isoolefin copolymer is cooled before contacting the solution of the unsaturated isoolefin copolymer cement with the aqueous solution of the halogenating agent and the oxidizing agent.

[0034] The halogenation can be carried out with or without mixing the reaction medium. Preferably, the reaction medium is mixed during the halogenation. Mixing can be carried out by any suitable method, such as stirring, mixing, etc. More preferably, the reaction medium is stirred, preferably at a speed of 600 rpm or greater. Stirring is more preferably carried out using a mechanical stirrer.

[0035] The unsaturated isoolefin copolymer is preferably present in the reaction medium in an amount of 1 to 60% by weight based on the total weight of the reaction medium, more preferably in an amount of 5 to 50% by weight, preferably 5 to 40% by weight, more preferably 10 to 33% by weight, even more preferably 10 to 30% by weight, for example 25% by weight, based on the total weight of the reaction medium.

[0036] The aqueous phase is formed from the aqueous solution of the oxidizing agent and the phase transfer catalyst, the water produced by the halogenation reaction, and additional water contained in the unsaturated isoolefin polymer cement. The aqueous solution of the oxidizing agent and the phase transfer catalyst, together with the water produced by the halogenation reaction, typically comprises less than 4% by weight of the reaction medium, for example 0.16 to 3.6% by weight, based on the total weight of the reaction medium.

[0037] The reaction medium may contain 0 to 20% by weight of additional water, based on the total weight of the reaction medium, resulting from the water contained in the unsaturated isoolefin polymer cement, depending on the process used to prepare the polymer cement. The additional water is water from the unsaturated isoolefin polymer cement and does not include water used to prepare the aqueous solution of the oxidizing agent or water generated by the halogenation reaction. It is an advantage of the process of the present invention that the reaction medium may contain a significant amount of additional water, for example, 1 to 20% by weight of additional water, based on the total weight of the reaction medium. In some embodiments, the additional water may account for 1.5 to 15% by weight of the reaction medium, or 2 to 20% by weight, or 2 to 15% by weight, or 5 to 20% by weight, or 5 to 15% by weight, or 5 to 10% by weight of the reaction medium, based on the total weight of the reaction medium. Nevertheless, in some embodiments, the reaction medium may contain only trace amounts of additional water, for example, less than 1% by weight of additional water, or even 0% by weight of additional water, based on the total weight of the reaction medium.

[0038] The oxidizing agent can be any suitable oxidizing agent for converting hydrogen halide to free halogen. Some examples include hydrogen peroxide, metal salts of hydrogen peroxide, organic peracids, metal salts of organic peracids, inorganic oxyacids, metal salts of inorganic oxyacids, and the like, and mixtures thereof. The metal salts preferably contain an alkali metal cation (e.g., Li + , Na + , K + In some embodiments, the oxidizing agent comprises H2O2, NaHSO5, Na2S2O8, NaClO, NaBrO, NaBrO3, NaIO3, NaClO, NaClO3, NaClO4, NaIO4, NaOO(CO)R5, where R5 is C 1~8 alkyl moiety), KHSO5, K2S2O8, KClO, KBrO, KBrO3, KIO3, KClO3, KClO4, KIO4, KOO(CO)R5 (wherein R5 is C 1~8 alkyl moiety), compounds which produce the oxidizing agents described above, or mixtures thereof.

[0039] The phase transfer catalyst (PTC) forms ionic associations and / or hydrogen bonds with the oxidant molecule or its oxidant anion, facilitating the transfer of the oxidant to the organic phase. The phase transfer catalyst extracts the oxidant molecule or its oxidant anion from the aqueous phase to the organic phase. The counter anion of the phase transfer catalyst and the metal cation associated with the oxidant anion (if any) remain in the aqueous phase. When the phase transfer catalyst is used together with the oxidant, the bromine recovery efficiency is increased over that reported in prior art processes.

[0040] The phase transfer catalyst is a compound of formula (I) as described above. Preferably, the VA group element is N or P, more preferably N. Preferably, the phase transfer catalyst is a quaternary ammonium salt. Preferably, the anion is a halide (e.g., F, Cl, Br, I), OH, - , HSO4 - , BF4 - , NO3 - , CF3SO3 - , CH3C6H4SO3 - , CH3COO - , ICl2 - , ClO4 - , SO4 2- , SCN - , PF6 - , HF2 - More preferably, the anion is Cl, Br, OH - , or HSO4 - Preferably, R1, R2, R3, and R4 are the same or different and are independently an aliphatic hydrocarbyl moiety, an aromatic hydrocarbyl moiety, or both an aliphatic hydrocarbyl moiety and an aromatic hydrocarbyl moiety. More preferably, R1, R2, R3, and R4 are the same or different and are independently an alkyl, aryl, alkaryl, aralkyl, or cycloalkyl moiety. Even more preferably, R1, R2, R3, and R4 are the same or different and are independently a C1-C 30 Straight chain alkyl moiety or C6-C 16 Particularly preferably, R1, R2, R3, and R4 are the same or different and independently represent C1 to C 10 Straight chain alkyl moiety or C6-C11 It is an aralkyl moiety.

[0041] In a particularly preferred embodiment, R1, R2, R3, and R4 together comprise a total of 25 or more carbon atoms. When the total number of carbon atoms is 25 or more, halogen recovery can be performed without sensitivity to water. The total number of carbon atoms is preferably 120 or less, more preferably 40 or less.

[0042] Some particularly preferred examples of compounds of formula (I) are tetramethylammonium hydroxide, ethyltrimethylammonium iodide, triethylmethylammonium chloride, tetraethylammonium hydrogen sulfate, tetraethylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate, n-octyltrimethylammonium chloride, methyltrioctylammonium hydrogen sulfate, tetrahexylammonium hydrogen sulfate, tetra-n-octylammonium iodide, diauryidimethylammonium bromide, benzyltrimethylammonium bromide, or mixtures thereof.

[0043] The phase transfer catalyst is preferably used in an amount such that the phase transfer catalyst and the oxidant are present in the aqueous solution at a molar ratio of phase transfer catalyst to oxidant of 0.005 or more. More preferably, the molar ratio of phase transfer catalyst to oxidant is 0.006 or more, or 0.01 or more, or 0.013 or more. The molar amount of phase transfer catalyst compared to the oxidant can be small while effectively increasing the halogen recovery rate, but large amounts of phase transfer catalyst can also be utilized. For example, the molar ratio of phase transfer catalyst to oxidant can be as high as 10 or more. However, in many embodiments, the molar ratio of phase transfer catalyst to oxidant is preferably 10 or less, more preferably 1 or less. Preferably, the amount of phase transfer catalyst is at least 0.13 mmol, more preferably at least 0.2 mmol, or at least 0.25 mmol.

[0044] The oxidizing agent and phase transfer catalyst are preferably premixed in an aqueous solution prior to introducing the aqueous solution into the reaction medium containing the cement, although in some circumstances it is possible to introduce the oxidizing agent and phase transfer catalyst separately into the reaction medium containing the cement, preferably with the phase transfer catalyst added first and then the oxidizing agent. The oxidizing agent and phase transfer catalyst are preferably added to the reaction medium before the halogenating agent is introduced.

[0045] The concentration of the oxidizing agent present in the reaction medium is preferably at least 0.06 moles of oxidizing agent per mole of halogenating agent or at least 0.1 moles of oxidizing agent per mole of halogenating agent. The concentration of the oxidizing agent present in the reaction medium is preferably 0.2 to 5 moles, more preferably 0.25 to 4 moles, even more preferably 0.5 to 3 moles of oxidizing agent per mole of halogenating agent. The desired concentration of the oxidizing agent is a function of the desired halogenation time. For a halogenation time of 5 minutes, 0.5 to 2 moles, for example 2 moles of oxidizing agent per mole of halogenating agent is preferred. A low concentration of the oxidizing agent may be offset by a longer halogenation time. The efficiency of the halogenation can be improved by adjusting the stirring speed of the reaction medium.

[0046] In the process of the present invention, all or part of the halogenating agent may comprise hydrogen halide (HX) added to the aqueous phase. The added HX can function as a source of halogenating agent since HX is converted to molecular halogen (X2) by an oxidizing agent in the aqueous phase. EXAMPLES

[0047] Scheme 1 shows an example of a process for producing halogenated isoolefin copolymer. As shown in Scheme 1, with Br2 as the halogenating agent, a suitable oxidizing agent and a phase transfer catalyst, the phase transfer catalyst ionically associates and / or hydrogen bonds with the oxidizing agent anion. In this way, the phase transfer catalyst can extract the oxidizing agent anion from the aqueous phase and oxidize the HBr generated in the organic phase back to Br2. Furthermore, the bromide ion that migrates to the aqueous phase is oxidized by the oxidizing agent anion to reform Br2 and preferentially return to the organic phase. In this way, the utilization efficiency of bromine in the bromination reaction can be increased. In some cases, for example, when the oxidizing agent is hydrogen peroxide, the phase transfer catalyst extracts the oxidizing agent molecule into the organic phase. [ka]

[0048] Materials and Methods: Isobutylene-isoprene polymer (IIR) and epoxidized soybean oil (ESBO) were obtained from ARLANXEO (Sarnia, Ontario, Canada site). The remaining materials were used as received: sodium hypochlorite (10-15% available chlorine, Sigma-Aldrich), sodium bromate (Sigma-Aldrich), potassium peroxymonosulfate (Sigma Aldrich's Oxone™ with >4% active oxygen by weight), hexane (VWR), sodium hydroxide (VWR), 99.99% bromine (Sigma Aldrich), 35% by weight peracetic acid solution (Evonik), 30% by weight hydrogen peroxide (Sigma-Aldrich), glacial acetic acid (Sigma-Aldrich), 95-98% sulfuric acid (Sigma-Aldrich), calcium stearate (Alfa Aesar), Irganox™ 1010 (BASF), tetramethylammonium hydroxide (Sigma-Aldrich), tetrabutylammonium hydrogen sulfate (Sigma-Aldrich), tetrabutylammonium bromide (Sigma-Aldrich), methyltrioctylammonium hydrogen sulfate (Sigma-Aldrich), benzyltrimethylammonium bromide (Sigma-Aldrich).

[0049] Scheme 2 shows the structures of the phase transfer catalysts (PTCs) used in the examples. PTC0 is tetramethylammonium hydroxide. PTC1 is tetrabutylammonium hydrogen sulfate. PTC2 is tetrabutylammonium bromide. PTC3 is methyltrioctylammonium hydrogen sulfate. PTC4 is benzyltrimethylammonium bromide. [ka]

[0050] Bromination Reaction 250 g of isobutylene-isoprene copolymer (butyl rubber, IIR) was chopped into small pieces and placed in a 5 L jacketed reactor equipped with an overhead stirrer and pre-filled with 1053 mL of hexane. The stirring speed was set at 150 rpm while the aforementioned base material pieces were added to the reactor. The solution was stirred for 24 hours to completely dissolve the butyl rubber. After the isobutylene-isoprene copolymer was completely dissolved, 60 mL of water was added to the reactor by pipette to obtain a butyl rubber cement. In examples where an oxidant other than Oxone was used to recover bromine, the oxidant and phase transfer catalyst were first dispersed in a 4 mL water / 4 mL hexane mixture, and then the resulting solution was added to the reactor before adding bromine. In examples where Oxone was used to recover bromine, Oxone and phase transfer catalyst were first dissolved in 25 mL water / 4 mL hexane. The amounts of oxidant and phase transfer catalyst are indicated in the examples.

[0051] The reactor was heated using a circulating bath connected to the jacketed reactor set at 45° C. and the butyl rubber cement was stirred at 350 rpm for 30 minutes. Bromine (Br2) (1.76 mL, 5.49 g, 0.0343 mol) was then added via syringe and the reaction was stirred for 5 minutes, or in some examples, 1 hour.

[0052] For 1 h of bromination, 10 mL samples of the reaction medium were pipetted at 5, 20, 40, and 60 min into vials containing 10 mL of 2.5 M NaOH, which were then vigorously shaken to quench (deactivate) residual bromine, HBr, and oxidant. The halogenated polymer samples in the vials were then recovered by precipitating the polymer solution in ethanol and drying the precipitate under vacuum at 60° C. for 48 h.

[0053] After 5 minutes or 1 hour, a predetermined amount of 2.5M aqueous NaOH was added to the remaining reaction medium to quench the reaction. An additional 250 mL of water was added to aid mixing. The mixture was continued to be stirred at 350 rpm for 5 minutes. An additional 1 L of water was added and stirred at 350 rpm for an additional 5 minutes. Agitation was reduced to 150 rpm and stirred for an additional 5 minutes. The reactor agitation was stopped and the aqueous phase was withdrawn through the bottom drain valve. The brominated isobutylene-isoprene copolymer cement was washed with additional water until the pH was 7 to remove residual inorganic salts. A solution of polymer stabilizers (4.52 g calcium stearate, 0.125 g Irganox™ 1010 and 3.25 g ESBO) in hexane was added to the reactor and the cement was stirred for 5 minutes. The cement was withdrawn and steam-set using low pressure steam for approximately 1 hour. Small pieces of brominated polymer samples were cut from the final product and dried overnight in a vacuum oven at 60°C.

[0054] The microstructure and bromine content of the dried samples were 1 H-NMR spectroscopy was used to analyze.

[0055] Bromine Utilization Calculation Bromine utilization in a bromination process can be measured using the bromine atom efficiency (BAE) as given by the following equation:

number

[0056] In some conventional methods (e.g., U.S. Pat. Nos. 3,018,275 and 5,681,901), the bromine utilization is measured using the number of molecules of molecular bromine added to the reaction, resulting in a numerical value that is twice the BAE since there are two bromine atoms per molecule of molecular bromine. Furthermore, these conventional methods use X-ray diffraction to estimate the amount of Br bound to the polymer. However, this method also measures the NaBr that is generated during the neutralization process and trapped within the polymer matrix. The trapped NaBr does not necessarily measure the amount of Br that is chemically bound to the polymer, which usually results in a bromine utilization numerical value that is higher than the actual efficiency.

[0057] Example 1: Control without using phase transfer catalyst (PTC) A control experiment was performed using NaClO (sodium hypochlorite) as the oxidant. It is clear from Table 1 that increasing the amount of oxidant increases the bromine recovery.

[0058] [Table 1]

[0059] Example 2: Effect of phase transfer catalyst on bromine recovery The effect of phase transfer catalyst on bromine recovery was investigated using NaClO as oxidant and PTC1 as phase transfer catalyst. From Table 2 comparing C2 and P1, it is clear that the use of a small amount of quaternary salt phase transfer catalyst increases functional bromine compared to bromination without phase transfer catalyst using the same oxidant and amount of oxidant. Similarly, comparing C3 and P1, the use of phase transfer catalyst reduces the amount of oxidant required to obtain the same functional bromine. Reducing the amount of oxidant is beneficial to maintaining the microstructure of the brominated butyl rubber.

[0060] [Table 2]

[0061] Example 3: Effect of reaction time on bromine recovery The effect of reaction time on bromine recovery was investigated using NaClO as the oxidant and PTC1 as the phase transfer catalyst. From Table 3 and Figure 1, it is clear that long reaction times are not necessary to obtain maximum bromine recovery. Maximum bromination of butyl rubber is achieved within 5 minutes.

[0062] [Table 3]

[0063] Example 4: Effect of stirring speed on bromine recovery The effect of stirring speed on bromine recovery was investigated using NaClO as the oxidant and PTC1 as the phase transfer catalyst. From Table 4 and Figure 2, it is clear that the faster the stirring speed, the better the bromine recovery.

[0064] [Table 4]

[0065] Example 5: Effect of different amounts of phase transfer catalyst on bromine recovery Using NaClO as oxidant and PTC1 as phase transfer catalyst, the effect of different amounts of phase transfer catalyst on bromine recovery was investigated. From Table 5 and Figure 3, it is clear that efficient bromine recovery can be achieved with an amount of phase transfer catalyst as low as 0.13 mmol (PTC:oxidant ratio 0.0032). Better results are obtained with an amount of phase transfer catalyst of 0.27 mmol (PTC:oxidant ratio 0.0067) or more. Bromine recovery does not improve further when the amount of phase transfer catalyst exceeds 0.53 mmol (PTC:oxidant ratio 0.013).

[0066] [Table 5]

[0067] Example 6: Effect of NaBrO3 oxidant on bromine recovery with and without phase transfer catalyst Using NaBrO3 as the oxidant and PTC1 as the phase transfer catalyst, the effect of different oxidants on the bromine recovery at four different reaction times with and without phase transfer catalyst was investigated. From Table 6 and Figure 4, it can be seen that the quaternary salt phase transfer catalyst is more effective than other Na + It appears to work for oxidizing agents containing NaBrO3. Furthermore, the use of a phase transfer catalyst shortens the time to achieve maximum bromine recovery when NaBrO3 is used as the oxidizing agent.

[0068] [Table 6]

[0069] Example 7: Effect of different phase transfer catalysts on bromine recovery The effect of different quaternary salt phase transfer catalysts on bromine recovery was investigated using NaClO as the oxidant and PTC0, PTC1, PTC2, PTC3, and PTC4 as the phase transfer catalysts. From Table 7, it is clear that all the quaternary salt phase transfer catalysts perform similarly to increase bromine recovery. Furthermore, lesser amounts of PTC3 were required to achieve essentially the same bromine recovery, suggesting that the longer the alkyl chain on the phase transfer catalyst, the lesser the amount of phase transfer catalyst required.

[0070] [Table 7]

[0071] Example 8: Effect of moisture content on bromine recovery The effect of the water content of the reaction medium on the bromine recovery was investigated using NaClO as the oxidant and PTC1 and PTC3 as the phase transfer catalysts. From Table 8 and Figure 5, it is clear that when PTC3 is used as the phase transfer catalyst, the bromine recovery is almost independent of the water content of the reaction medium, suggesting that the longer alkyl chain quaternary salts virtually eliminate the water content sensitivity of the bromine recovery.

[0072] [Table 8]

[0073] Example 9: Effect of different oxidants on bromine recovery Potassium peroxymonosulfate (Oxone™), peracetic acid (PAA), in-situ generated PAA, and hydrogen peroxide (HO) were used as oxidants, and PTC1, PTC2, and PTC3 were used as phase transfer catalysts to study the effect of different oxidants on bromine recovery with different phase transfer catalysts.

[0074] Potassium peroxymonosulfate: Table 9 shows the results obtained using potassium peroxymonosulfate as the oxidant. It is clear from Table 9 that the quaternary salt phase transfer catalyst works well with potassium peroxymonosulfate as the oxidant to improve bromine recovery.

[0075] [Table 9]

[0076] 35%PAA(Evonik(TM)): Table 10 shows the results obtained using 35% PAA (Evonik™) as the oxidant. It is clear from Table 10 that the quaternary salt phase transfer catalyst works in conjunction with the peracetic acid oxidant to improve bromine recovery.

[0077] [Table 10]

[0078] In-situ generated PAA: Table 11 shows the results obtained using in situ generated PAA as the oxidant. The in situ generated PAA was prepared from 5.5 mL of 30% H2O2, 10.5 mL of acetic acid, and 0.5 mL of H2SO4. From Table 11, it is clear that the quaternary salt phase transfer catalyst works with the in situ generated peracetic acid oxidant to improve the bromine recovery.

[0079] [Table 11]

[0080] hydrogen peroxide: Table 12 shows the results obtained using hydrogen peroxide as the oxidant. It is clear from Table 12 that the quaternary salt phase transfer catalyst works with the hydrogen peroxide oxidant to improve bromine recovery.

[0081] [Table 12]

[0082] The novel features will be apparent to those skilled in the art upon reading the description herein. However, it should be understood that the scope of the claims should not be limited by the embodiments, but should be given the broadest interpretation consistent with the language of the claims and the entire specification.

Claims

1. A method for producing a halogenated isoolefin copolymer, comprising contacting an unsaturated isoolefin copolymer cement comprising an unsaturated isoolefin copolymer dissolved in an organic solvent with a halogenating agent and an aqueous solution of an oxidizing agent and a phase transfer catalyst under halogenation conditions to form a two-phase reaction medium comprising an organic phase and an aqueous phase, wherein the oxidizing agent is capable of converting hydrogen halide to free halogen and the phase transfer catalyst is a compound represented by the formula (I): 【Chemistry 1】 (In the formula, M + is a cation of a Group VA element; X - is an anion that dissociates from the cation in aqueous solution; and R 1 , R 2 , R 3 , and R 4 are the same or different and independently C 1~30 (It is an organic group) The method for producing the compound of formula (1).

2. The method of claim 1 , wherein the Group VA element is N or P.

3. The method of claim 1 , wherein the Group VA element is N.

4. The anion is a halide, OH - , H.S.O. 4 - , B.F. 4 - , NO 3 - , C.F. 3 SO 3 - , C.H. 3 C 6 H 4 SO 3 - , C.H. 3 COO - , I.C.I. 2 - , ClO 4 - , S.O. 4 2- , S.C.N. - , P.F. 6 - , or HF 2 - The method according to any one of claims 1 to 3, wherein

5. The anion is a halide, OH - , or HSO 4 - The method according to any one of claims 1 to 3, wherein

6. Said C 1~30 The method of any one of claims 1 to 5, wherein the organic group contains aliphatic hydrocarbyl moieties, aromatic hydrocarbyl moieties, or both aliphatic and aromatic hydrocarbyl moieties.

7. Said C 1~30 The organic group is C 1~30 The method of any one of claims 1 to 5, comprising a straight chain alkyl group.

8. R 1 , R 2 , R 3 , and R 4 The method of any one of claims 1 to 7, wherein together contain a total of 25 or more carbon atoms.

9. 6. The method of any one of claims 1 to 5, wherein the compound of formula (I) is tetramethylammonium hydroxide, ethyltrimethylammonium iodide, triethylmethylammonium chloride, tetraethylammonium hydrogen sulfate, tetraethylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate, n-octyltrimethylammonium chloride, methyltrioctylammonium hydrogen sulfate, tetrahexylammonium hydrogen sulfate, tetra-n-octylammonium iodide, diauryldimethylammonium bromide, or a mixture thereof.

10. 10. The method of any one of claims 1 to 9, wherein the oxidizing agent comprises hydrogen peroxide, a metal salt of hydrogen peroxide, an organic peracid, a metal salt of an organic peracid, an inorganic oxyacid, a metal salt of an inorganic oxyacid, or a mixture thereof.

11. The oxidizing agent is H 2 O 2 , NaHSO 5 , Na 2 S 2 O 8 , NaClO, NaBrO, NaBrO 3 , NaIO 3 , NaClO, NaClO 3 , NaClO 4 , NaIO 4 , NaOO(CO)R 5 (In the formula, R 5 is C 1~8 alkyl group), KHSO 5 , K 2 S 2 O 8 , KClO, KBrO, KBrO 3 , K.I.O. 3 , KClO 3 , KClO 4 , K.I.O. 4 , KOO(CO)R 5 10. The method of claim 1, further comprising the step of:

12. The halogenating agent is molecular chlorine (Cl 2 ), molecular bromine (Br 2 ), organic halides, Cl 2 Or Br 2 or any mixture thereof.

13. The halogenating agent is Br 2 The method according to any one of claims 1 to 11, wherein

14. 14. The method of any one of claims 1 to 13, wherein the phase transfer catalyst and the oxidant are present in the aqueous solution in a molar ratio of phase transfer catalyst to oxidant of 0.005 or greater.

15. The process according to any one of claims 1 to 14, wherein the phase transfer catalyst is present in the aqueous solution in an amount of at least 0.13 mmol.

16. The process according to any one of claims 1 to 15, wherein the reaction medium is stirred at 600 rpm or more using a mechanical stirrer.

17. 17. The method according to any one of claims 1 to 16, wherein the cement has a water content of 1% by weight or more, based on the total weight of the cement.

18. 18. The method of claim 17, wherein the water content of the cement is 1.5% by weight or more.

19. 18. The method of claim 17, wherein the water content of the cement is 1 to 30% by weight.

20. 18. The method of claim 17, wherein the water content of the cement is 2 to 20% by weight.

21. The method according to any one of claims 1 to 20, wherein the unsaturated isoolefin copolymer cement is prepared by polymerizing at least one isoolefin monomer and at least one copolymerizable unsaturated monomer in an organic diluent, and removing the organic diluent and residual monomers by steam flash separation.

22. 22. The method of claim 21, wherein the at least one isoolefin monomer is isobutene and the at least one copolymerizable unsaturated monomer is isoprene, p-methylstyrene, or β-pinene.

23. 22. The method of claim 21, wherein the at least one isoolefin monomer is isobutene, and the at least one copolymerizable unsaturated monomer is isoprene, and the unsaturated isoolefin copolymer further comprises one or more additional copolymerizable monomers selected from the group consisting of alpha-methylstyrene, p-methylstyrene, chlorostyrene, cyclopentadiene, methylcyclopentadiene, and indene.

24. The method of any one of claims 21 to 23, wherein the organic diluent comprises methyl chloride.

25. The process of any one of claims 1 to 24, wherein the unsaturated isoolefin copolymer is present in the reaction medium in an amount of from 10 to 33 weight percent, based on the total weight of the reaction medium.

26. 26. The method of any one of claims 1 to 25, wherein the step of contacting the unsaturated isoolefin copolymer cement with the halogenating agent is carried out at a temperature in the range of 20 to 45°C for a period of 1 to 60 minutes.

27. 27. The method of any one of claims 1 to 26, wherein the oxidizing agent converts the halide to a free halogen in-situ.

Citation Information

Patent Citations

  • Para-alkylstyrene / isoolefin copolymers

    EP0344021A2

  • Process for producing brominated butyl rubber

    US20140309362A1

  • Halogenation of low unsaturation rubbery polymers in the presence of oxidizing agen

    US3018275A

  • Phase transfer catalysis of heterogeneous reactions by quaternary salts

    US3992432A

  • Process for halogenating isomonoolefin copolymers

    US5681901A