Biodegradable highly absorbent resin and its manufacturing method

A biodegradable superabsorbent resin is developed using modified polysaccharides with maleic acid and carboxymethyl groups, addressing the environmental issues of conventional resins by maintaining physical properties and enhancing biodegradability.

JP2024543792AActive Publication Date: 2024-11-26LG CHEM LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024523506
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-15
Filing Date
2023-06-19
Publication Date
2024-11-26
Estimated Expiration
2043-06-19

AI Technical Summary

Technical Problem

Conventional superabsorbent resins lack biodegradability, leading to environmental pollution when disposed of, and attempts to make biodegradable resins with similar physical properties have been economically unviable.

Method used

A biodegradable superabsorbent resin is produced using a crosslinked polymer containing modified polysaccharides with maleic acid and carboxymethyl groups, where at least 60% of the repeating units are derived from modified polysaccharides with a molecular weight of 190,000 g/mol or more, and these groups are partially neutralized.

Benefits of technology

The resin maintains excellent physical properties while exhibiting biodegradability, preventing environmental pollution and ensuring effective water absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543792000001_ABST
    Figure 2024543792000001_ABST
Patent Text Reader

Abstract

The present invention provides a superabsorbent resin that exhibits excellent biodegradability without reducing the physical properties of the superabsorbent resin, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0078925 filed on June 28, 2022 and Korean Patent Application No. 10-2023-0076830 filed on June 15, 2023, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a biodegradable superabsorbent resin that exhibits excellent biodegradability without reducing the physical properties of the superabsorbent resin, and a method for producing the same. [Background technology]

[0003] Super absorbent polymer (SAP) is a synthetic polymeric material that has the ability to absorb 500 to 1,000 times its own weight in water, and different developers give it different names, such as SAM (Super Absorbency Material) or AGM (Absorbent Gel Material). Such super absorbent polymers were first put to practical use as sanitary products, and are now widely used in a variety of applications, including sanitary products such as baby diapers, soil water retention agents for gardening, water stoppers for civil engineering and construction, seedling sheets, freshness preserving agents in the food distribution industry, materials for poultices, and even electrical insulation.

[0004] Such superabsorbent resins are generally produced by bulk polymerization or suspension polymerization of acrylic acid monomers together with a crosslinking agent in the presence of a polymerization initiator to obtain a hydrogel polymer. Therefore, conventional superabsorbent resins are hardly biodegradable and cause environmental problems when they are disposed of as waste. Specifically, when various products using superabsorbent resins are disposed of by landfilling, the superabsorbent resins are not decomposed by bacteria or microorganisms in the soil, which can cause environmental pollution.

[0005] Therefore, although there have been attempts to develop superabsorbent resins that exhibit excellent biodegradability using biomass-derived materials, it has not been very easy to produce economically producible biodegradable superabsorbent resins that exhibit similar levels of physical properties to conventional superabsorbent resins.

[0006] For this reason, there is a continuing demand for development of technologies related to superabsorbent polymers that can exhibit biodegradability without reducing the basic physical properties of the superabsorbent polymers. Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, the present invention provides a superabsorbent resin that exhibits excellent biodegradability without reducing the physical properties of the superabsorbent resin, and a method for producing the same. [Means for solving the problem]

[0008] According to one embodiment of the present invention, The crosslinked polymer includes a monomer containing a modified polysaccharide containing at least one of a maleic acid group (-OCOCH=CHCOOH) and a carboxymethyl group (-CH2-COOH), At least a portion of the maleic acid groups and carboxymethyl groups are neutralized; The crosslinked polymer contains 60 parts by weight or more of a repeating unit derived from a modified polysaccharide, The molecular weight of the modified polysaccharide is 190,000 g / mol or more; A biodegradable superabsorbent polymer is provided.

[0009] According to yet another embodiment of the present invention, preparing a monomer composition including a modified polysaccharide including at least one of a maleic acid group (-OCOCH=CHCOOH) and a carboxymethyl group (-CH2-COOH) in the presence of a polymerization initiator; cross-linking the monomer composition to produce a hydrogel polymer; and drying, grinding and classifying the hydrogel polymer; In the method for producing a biodegradable highly water-absorbent resin, At least a portion of the maleic acid groups and carboxymethyl groups of the modified polysaccharide are neutralized; The crosslinked polymer contains 60 parts by weight or more of a repeating unit derived from a modified polysaccharide, The molecular weight of the modified polysaccharide is 190,000 g / mol or more; A method for making a biodegradable superabsorbent resin is provided.

[0010] Furthermore, according to yet another embodiment of the present invention, there is provided a sanitary product comprising the biodegradable highly water-absorbent resin. Effect of the Invention

[0011] The biodegradable superabsorbent polymer of the present invention exhibits excellent biodegradability by using a chemically modified polysaccharide. In addition, the biodegradable superabsorbent polymer of the present invention uses a modified polysaccharide having a weight average molecular weight above a certain level, and can be polymerized and crosslinked without unreacted modified polysaccharide, so that the various physical properties of general superabsorbent polymers are not deteriorated. Therefore, even if the biodegradable superabsorbent polymer is applied to various sanitary products, it does not cause environmental pollution problems when it is disposed of. [Brief description of the drawings]

[0012] [Figure 1] 1 shows the 1H NMR spectrum of the maleated chitosan prepared in Preparation Example 1. [Diagram 2] 1 shows the 1H NMR spectrum of the maleated modified starch produced in Preparation Example 2. [Diagram 3] 1 shows the 1H NMR spectrum of the carboxymethylated modified starch produced in Preparation Example 3. [Figure 4]1 shows the 1H NMR spectrum of the carboxymethylated modified starch produced in Preparation Example 4. [Diagram 5] 1 shows the 1H NMR spectrum of the carboxymethylated modified starch produced in Preparation Example 5. [Figure 6] 1 shows the 1H NMR spectrum of the carboxymethylated modified starch produced in Preparation Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "comprise", "have" and the like are intended to specify the presence of an implemented feature, step, component, or combination thereof, and should be understood not to preclude the presence or additional possibility of one or more other features, steps, components, or combinations thereof.

[0014] In addition, in the present invention, when it is said that each layer or element is formed "on" each other, it means that each layer or element is formed directly on each layer or element, or that other layers or elements can be additionally formed between each layer, on the object, or on the substrate.

[0015] Since the present invention can be modified in various ways and has various forms, the following detailed description will be given by way of example of a specific embodiment, but it should be understood that the present invention is not limited to the specific disclosed embodiment, but includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.

[0016] Furthermore, the terminology used in this specification is for the purpose of referring to particular embodiments only and is not intended to limit the present invention. Additionally, as used herein, the singular forms "a," "an," and "the" include the plural forms unless the context clearly dictates otherwise.

[0017] On the other hand, the term "(meth)acrylate" as used herein includes both acrylate and methacrylate.

[0018] The term "polymer" or "polymeric polymer" used in the present specification means a state in which a water-soluble ethylenically unsaturated monomer is polymerized, and can include all water content ranges or particle size ranges. Among the above polymers, a polymer having a water content (water content) of about 40% by weight or more in a state after polymerization and before drying can be called a hydrogel polymer, and particles obtained by crushing and drying such a hydrogel polymer can be called a crosslinked polymer.

[0019] The term "superabsorbent resin particles" refers to a particulate material that includes a crosslinked polymer obtained by polymerizing a modified polysaccharide that contains acidic groups and in which at least a portion of the acidic groups have been neutralized.

[0020] In addition, depending on the context, the term "super absorbent polymer" refers to a crosslinked polymer obtained by polymerizing a modified polysaccharide having acidic groups and at least a portion of the acidic groups being neutralized, or a base resin in the form of a powder consisting of super absorbent resin particles obtained by pulverizing the crosslinked polymer, or is used to encompass all of the crosslinked polymers or base resins that have been subjected to additional processes, such as surface crosslinking, fine powder regranulation, drying, pulverization, classification, etc., to be made into a state suitable for commercialization.

[0021] Conventionally used superabsorbent resins are produced by polymerizing an acrylic acid monomer together with a crosslinking agent in the presence of a polymerization initiator, and the superabsorbent resins produced in this manner are not biodegradable, causing environmental problems.

[0022] Therefore, development of superabsorbent resins that can exhibit biodegradability has been underway. Materials such as polysaccharide, polyaspartic acid, and polyglutamic acid have been cited as biodegradable materials from which such biodegradable resins can be manufactured. However, it has been difficult to replace superabsorbent resins manufactured from acrylic acid monomers by reducing the water absorption capacity, which is an important physical property of superabsorbent resins.

[0023] Therefore, the inventors have confirmed that when a superabsorbent resin is produced using a modified polysaccharide containing at least one of a maleic acid group (-OCOCH=CHCOOH) and a carboxymethyl group (-CH2-COOH) as a monomer, not only is the resin excellent in biodegradability but also all of its physical properties are superior to those of previously known biodegradable materials, and thus completed the present invention.

[0024] Hereinafter, the biodegradable highly water-absorbent resin and the method for producing the same will be described in more detail with reference to specific embodiments of the invention.

[0025] Biodegradable super absorbent resin Specifically, the biodegradable superabsorbent polymer according to one embodiment of the invention comprises a cross-linked polymer of monomers including modified polysaccharides containing one or more of maleic acid groups (-OCOCH=CHCOOH) and carboxymethyl groups (-CH2-COOH).

[0026] Here, the crosslinked polymer has a structure formed by polymerizing a monomer including a modified polysaccharide having at least a partially neutralized maleic acid group (-OCOCH=CHCOOH) and a carboxymethyl group (-CH2-COOH). At this time, the modified polysaccharide is polymerized to grow into a main chain, and at the same time, the functional group in the structure is polymerized to form a crosslinked polymerized structure, and the overall physical properties of the superabsorbent resin can be significantly improved by having such a crosslinked polymerized structure.

[0027] In addition, the crosslinked polymer contains 60 parts by weight or more of the repeating unit derived from the modified polysaccharide. That is, the crosslinked polymer contains a high content of the modified polysaccharide compared to other unsaturated monomers, and further, the main chain composed of the modified polysaccharide is crosslinked and polymerized, and is more biodegradable than other superabsorbent resins having a high content of unsaturated monomers. Preferably, the crosslinked polymer may contain 80 parts by weight or more, 85 parts by weight or more, 90 parts by weight or more, or 95 parts by weight or more of the repeating unit derived from the modified polysaccharide.

[0028] Furthermore, the modified polysaccharide of the present invention has a molecular weight of 190,000 g / mol or more, and it has been confirmed that a superabsorbent resin cross-linked from a modified polysaccharide in this range is advantageous in forming a cross-linked structure and has excellent overall water absorption properties compared to a superabsorbent resin polymerized from a modified polysaccharide in a lower range.

[0029] Meanwhile, polysaccharides, i.e., polysaccharides, refer to polymeric carbohydrate molecules composed of glucose repeating units, including polymeric molecules composed of glucosamine repeating units in which an amino group has been introduced to the hydroxyl group bonded to the second carbon atom of the glucose repeating units and / or N-acetylglucosamine repeating units in which an N-acetylamino group has been introduced to the hydroxyl group bonded to the second carbon atom of the glucose repeating units. Therefore, the polysaccharides can be any compound generally known as polysaccharides. For example, starch composed of glucose repeating units, chitosan composed of glucosamine repeating units and N-acetylglucosamine repeating units, etc., can be used, but are not limited thereto.

[0030] In addition, the modified polysaccharide used in the biodegradable superabsorbent resin is a concept distinct from unmodified polysaccharides that are generally obtained naturally or synthetically, and refers to polysaccharides in which the hydroxyl groups (-OH) in the glucose repeating units constituting the polysaccharide are replaced with other functional groups by chemical and / or heat treatment. Such modified polysaccharides can exhibit physical properties different from unmodified polysaccharides due to the functional groups introduced in place of the hydroxyl groups (-OH).

[0031] For example, the modified polysaccharide is a modified starch, a modified cellulose or a modified chitosan.

[0032] On the other hand, the modified polysaccharide is substituted with one or more of a maleic acid group (-OCOCH=CHCOOH) and a carboxymethyl group (-CH2-COOH), and at least a portion of the maleic acid group (-OCOCH=CHCOOH) and the carboxymethyl group (-CH2-COOH) are neutralized.

[0033] The maleic acid group (-OCOCH=CHCOOH) in the polysaccharide may be introduced by maleic acid or maleic anhydride. For example, the hydroxyl group (-OH) in the unmodified polysaccharide molecule can be replaced by a maleic acid group (-OCOCH=CHCOOH) by maleic anhydride.

[0034] In addition, the carboxymethyl group (-CH2-COOH) in the polysaccharide may be introduced by any one of glycolic acid, monochloroacetic acid and salts thereof, and specific examples thereof include glycolic acid, monochloroacetic acid, sodium monochloroacetate, sodium glycolate, potassium monochloroacetate, and potassium glycolate. For example, the hydroxyl group (-OH) present in the unmodified polysaccharide molecule can be replaced by a carboxymethyl group (-CH2-COOH) by glycolic acid.

[0035] On the other hand, the degree of substitution (DS) of the maleic acid group (-OCOCH=CHCOOH) of the modified polysaccharide is defined as "DS" below. M " and is 0.15 to 1.5. When the substitution degree of the maleic acid group is less than 0.15, a large amount of modified polysaccharide that does not participate in cross-linking polymerization may remain, and when the substitution degree of the maleic acid group is more than 1.5, a large amount of maleic anhydride used for introducing the maleic acid group may not be completely removed, which may affect the physical properties of the final superabsorbent resin. Preferably, the degree of substitution of maleic acid groups is 0.20 or more, 0.25 or more, 0.30 or more, 0.35 or more, 0.40 or more, 0.45 or more, 0.50 or more, 0.55 or more, 0.60 or more, 0.65 or more, 0.70 or more, 0.75 or more, 0.80 or more, or 0.85 or more; or 1.45 or less, 1.40 or less, 1.35 or less, 1.30 or less, 1.25 or less, 1.20 or less, 1.15 or less, 1.10 or less, 1.05 or less, 1.00 or less, or 0.95 or less.

[0036] The degree of substitution (DS) of the carboxymethyl group (-CH2-COOH) of the modified polysaccharide is defined as "DS C " and is 0.20 to 1.2. When the degree of substitution of the carboxymethyl group is less than 0.20, a large amount of modified polysaccharide that does not participate in cross-linking polymerization may remain, and when the degree of substitution of the carboxymethyl group is more than 1.2, glycolic acid, etc., used in large amounts for the introduction of the carboxymethyl group may not be completely removed, which may affect the physical properties of the final superabsorbent resin. Preferably, the degree of substitution of the carboxymethyl group is 0.21 or more, 0.22 or more, 0.23 or more, 0.24 or more, or 0.25 or more; 1.15 or less, 1.1 or less, 1.05 or less, or 1.0 or less.

[0037] Here, the degree of substitution of maleic acid or carboxymethyl group means the average number of hydroxyl groups (-OH) substituted with maleic acid or carboxymethyl group per glucose repeating unit. That is, since there are three hydroxyl groups per glucose repeating unit, the theoretical maximum degree of substitution is 3, and a degree of substitution of 0.1 means that one hydroxyl group is substituted per 10 glucose repeating units. The degree of substitution of maleic acid and carboxymethyl group is determined by the average number of hydroxyl groups (-OH) substituted with maleic acid or carboxymethyl group per glucose repeating unit. 1 The formula can be calculated through H NMR analysis, and more specific details are given in the Preparation Examples described below.

[0038] Meanwhile, at least a part of the maleic acid group and carboxymethyl group of the modified polysaccharide is neutralized, and the degree of neutralization can be adjusted according to the type of modified polysaccharide and the final superabsorbent resin properties to be realized. For example, modified starch has a high molecular weight and is insoluble in water, but the degree of neutralization can be increased to neutralize the carboxyl group (COOH) into a carboxylate (COO-) form to increase the solubility in water. Specifically, the degree of neutralization of the modified polysaccharide may be 40 to 95 mol%, or 40 to 80 mol%, or 45 to 75 mol%.

[0039] In one embodiment, the modified polysaccharide may include at least one of repeating units represented by the following formulas 1 to 4.

[0040] [ka]

[0041] In the above chemical formulas 1 to 4, Each M is independently hydrogen or an alkali metal.

[0042] Specifically, in the above chemical formulas 1 to 4, M + are each independently H + , Na + , or K + It is.

[0043] For example, when the modified polysaccharide is a modified starch or modified dextrin, it may contain repeating units represented by Chemical Formula 1 and Chemical Formula 3, and when the modified polysaccharide is a modified chitosan, it may contain repeating units represented by Chemical Formula 2 and Chemical Formula 4.

[0044] In addition, the modified polysaccharide has a weight-average molecular weight of 190,000 g / mol or more, but if the weight-average molecular weight of the modified starch is too low, there is a problem that a large amount of unreacted modified starch remains because crosslinking is not performed sufficiently, and if it is too high, there is a problem that the acid treatment and introduction of functional groups themselves are difficult due to the entanglement phenomenon of the polymer chains of the high molecular weight modified polysaccharide, making it difficult to prepare the modified polysaccharide itself. Preferably, the weight-average molecular weight of the modified polysaccharide is 200,000 g / mol or more, 250,000 g / mol or more, or 300,000 g / mol or more, and 1,000,000,000 g / mol or less, 500,000,000 g / mol or less, 100,000,000 g / mol or less, or 50,000,000 g / mol or less.

[0045] The molecular weight of the modified polysaccharide may vary depending on the type of the substance. Specifically, the molecular weight of the modified starch is 400,000 g / mol to 1,000,000,000 g / mol, and preferably, the molecular weight of the modified starch is 1,000,000 g / mol or more, 5,000,000 g / mol or more, 10,000,000 g / mol or more, or 20,000,000 g / mol or more, but may be 500,000,000 g / mol or less, 100,000,000 g / mol or less, or 50,000,000 g / mol or less.

[0046] Specifically, the molecular weight of the modified cellulose or modified chitosan is 190,000 g / mol to 10,000,000 g / mol, preferably 200,000 g / mol or more, 250,000 g / mol or more, or 300,000 g / mol or more, but may be 5,000,000 g / mol or less, 2,000,000 g / mol or less, 1,000,000 g / mol or less, or 700,000 g / mol or less.

[0047] Here, the weight average molecular weight (Mw) can be measured using gel permeation chromatography (GPC / MALLS). A specific method for measuring the weight average molecular weight will be described in the examples below.

[0048] Meanwhile, the modified polysaccharide may be modified starch. The modified starch may contain amylose and amylopectin in a weight ratio of 1:99 to 50:50 based on the total weight. The modification in which the hydroxyl group bonded to the 6th carbon of the glucose repeating unit is replaced with another substituent may occur in both amylose and amylopectin, but it is advantageous in terms of processability and solubility that the content of amylopectin is equal to or higher than the content of amylose.

[0049] The modified starch may have a gelatinization temperature of 50 to 90° C. and a peak viscosity (BU) of 50 to 1,000.

[0050] The modified starch may be one or more starches modified from potato starch, corn starch, rice starch, wheat starch, tapioca starch, and sweet potato starch. In particular, potato starch, which has a high amylopectin content, is preferred in terms of processability and solubility.

[0051] Meanwhile, the monomer may further include an acrylic acid-based compound having an acid group that is at least partially neutralized.

[0052] The acrylic acid monomer is a compound represented by the following formula 3:

[0053] [Chemical formula 3] R-COOM'

[0054] In the above chemical formula 2, R is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M' is a hydrogen atom, a monovalent or divalent metal, an ammonium group or an organic amine salt.

[0055] Preferably, the monomer may be one or more selected from the group consisting of (meth)acrylic acid, and monovalent (alkali) metal salts, divalent metal salts, ammonium salts and organic amine salts of these acids.

[0056] In this way, when (meth)acrylic acid and / or a salt thereof is used as the acrylic acid monomer, a highly water-absorbent resin having improved water absorption properties can be obtained.

[0057] Here, the acrylic acid monomer may have an acidic group, and at least a part of the acidic group may be neutralized. Preferably, the monomer may be partially neutralized with an alkaline substance such as sodium hydroxide, potassium hydroxide, or ammonium hydroxide. In this case, the neutralization degree of the acrylic acid monomer may be 40 to 95 mol%, 40 to 80 mol%, or 45 to 75 mol%. The range of the neutralization degree may be adjusted according to the final physical properties. However, if the neutralization degree is too high, the neutralized monomer may precipitate, making it difficult to smoothly carry out polymerization, and conversely, if the neutralization degree is too low, the water absorption of the polymer may be greatly reduced and the polymer may exhibit properties similar to elastic rubber, which is difficult to handle.

[0058] In addition, the crosslinked polymer of the monomer containing the modified polysaccharide can be crosslinked and polymerized through the mediation of an internal crosslinking agent. The term "internal crosslinking agent" used in this specification is used to distinguish it from a surface crosslinking agent that is usually used to crosslink the surface of the superabsorbent resin particles, and plays a role in crosslinking and polymerizing the modified polysaccharide. The crosslinking in the above step is performed regardless of the surface or the inside, but when the surface crosslinking process of the superabsorbent resin particles is performed, the particle surface of the finally produced superabsorbent resin has a structure crosslinked by the surface crosslinking agent, and the inside has a structure crosslinked by the internal crosslinking agent.

[0059] When a monomer containing a modified polysaccharide is crosslinked in the presence of an internal crosslinking agent, the main chain formed by the polymerization of the polysaccharide is crosslinked by the internal crosslinking agent to form a three-dimensional network structure. In this way, when the three-dimensional network structure is crosslinked by the internal crosslinking agent, the water retention capacity and pressurized water absorption capacity, which are various physical properties of the superabsorbent resin, can be significantly improved compared to when the superabsorbent resin is not crosslinked by the internal crosslinking agent.

[0060] The internal crosslinking agent may be any compound that allows the introduction of crosslinking bonds during polymerization of the modified polysaccharide. Non-limiting examples of the internal crosslinking agent include N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, propylene glycol ... Polyfunctional crosslinking agents such as (meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, ethylene glycol diglycidyl ether, propylene glycol, glycerin, or ethylene carbonate can be used alone or in combination of two or more, but are not limited thereto. Of these, N,N'-methylenebisacrylamide or polyethylene glycol diacrylate can be preferably used.

[0061] The cross-linking polymerization of the modified starch in the presence of such an internal cross-linking agent can be carried out by thermal polymerization, photopolymerization or hybrid polymerization in the presence of a polymerization initiator and, if necessary, a thickener, a plasticizer, a storage stabilizer, an antioxidant, etc., the details of which will be described later.

[0062] The superabsorbent polymer may be in the form of particles having an average particle size of 150 to 850 μm. In this case, such particle size can be measured according to the EDANA WSP 220.3 method of the European Disposables and Nonwovens Association (EDANA). More specifically, the superabsorbent polymer composition may be about 90% by weight, preferably 95% by weight or more, based on the total weight, of superabsorbent polymer particles having a particle size of about 150 to 850 μm, and less than about 10% by weight, more specifically less than about 5% by weight, of fine powder having a particle size of less than about 150 μm. If the superabsorbent polymer contains a large amount of fine powder having a particle size of less than 150 μm, it is not preferable because it may deteriorate various physical properties of the superabsorbent polymer.

[0063] The biodegradable highly water-absorbent resin may have a water retention capacity (CRC) of 20 to 50 g / g as measured by EDANA method WSP241.3.

[0064] Manufacturing method of biodegradable superabsorbent resin Meanwhile, the biodegradable highly water-absorbent resin can be produced by the following production method: preparing a monomer composition including a modified polysaccharide including at least one of a maleic acid group (-OCOCH=CHCOOH) and a carboxymethyl group (-CH2-COOH) in the presence of a polymerization initiator; cross-linking the monomer composition to produce a hydrogel polymer; and drying, grinding and classifying the hydrogel polymer; In the method for producing a biodegradable highly water-absorbent resin, At least a portion of the maleic acid groups and carboxymethyl groups of the modified polysaccharide are neutralized; The crosslinked polymer contains 60 parts by weight or more of a repeating unit derived from a modified polysaccharide, The molecular weight of the modified polysaccharide is 190,000 g / mol or more; A method for producing a biodegradable highly water-absorbent resin.

[0065] Meanwhile, the modified polysaccharide can be prepared by reacting a polysaccharide with at least one of maleic acid, maleic acid anhydride, glycolic acid, monochloroacetic acid, and salts thereof.

[0066] Specifically, the modified polysaccharide can be prepared by reacting a polysaccharide with at least one of maleic acid, maleic anhydride, glycolic acid, monochloroacetic acid, and salts thereof to prepare a polysaccharide having at least one of a maleic acid group and a carboxymethyl group introduced therein. The reaction of the polysaccharide with at least one of maleic acid, maleic anhydride, glycolic acid, monochloroacetic acid, and salts thereof can be carried out at a temperature of 50 to 100° C. for 4 to 12 hours.

[0067] As an example, the acid-treated polysaccharide can be maleated using maleic anhydride, thereby producing a maleic acid substituted polysaccharide.

[0068] In addition, before producing the modified polysaccharide, the non-modified polysaccharide can be treated with an acid. Such an acid treatment is carried out in order to break the rigid structure of starch due to hydrogen bonds and increase the production efficiency for the above-mentioned modification of polysaccharides such as maleation and carboxylmethylation. Specifically, the acid treatment can be carried out using an acidic solution such as hydrochloric acid at a temperature of 25 to 50°C for 6 to 48 hours.

[0069] Next, the modified starch thus prepared may be cross-linked in the presence of a polymerization initiator to form a hydrogel polymer.

[0070] The steps may include mixing the modified starch and a polymerization initiator to prepare a monomer composition, and thermally or photopolymerizing the monomer composition to form a hydrogel polymer.

[0071] Additionally, the monomer composition may further include an acrylic acid-based compound having at least a partially neutralized acid group. The modified polysaccharide and the acrylic acid-based compound may be included in the monomer composition in a weight ratio of 99:1 to 60:40. When the above range is satisfied, the biodegradable superabsorbent resin can exhibit excellent biodegradability while at the same time improving water absorption and water retention.

[0072] Also, the monomer composition may further include an internal crosslinking agent. In this case, the description of the internal crosslinking agent is referred to above. In the monomer composition, the internal crosslinking agent may be used in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the modified polysaccharide. For example, the internal crosslinking agent may be used in an amount of 0.1 parts by weight or more, or 0.2 parts by weight or more, and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less based on 100 parts by weight of the modified polysaccharide. If the content of the upper internal crosslinking agent is too low, crosslinking may not occur sufficiently, making it difficult to achieve strength above an appropriate level, and if the content of the upper internal crosslinking agent is too high, the internal crosslinking density may increase, making it difficult to achieve the desired water retention ability.

[0073] In addition, the polymerization initiator can be appropriately selected depending on the polymerization method, and when a thermal polymerization method is used, a thermal polymerization initiator can be used, when a photopolymerization method is used, a photopolymerization initiator can be used, and when a hybrid polymerization method (a method using both heat and light) is used, both a thermal polymerization initiator and a photopolymerization initiator can be used. However, even in the photopolymerization method, a certain amount of heat is generated by light irradiation such as ultraviolet irradiation, and a certain amount of heat is generated by the progress of the polymerization reaction, which is an exothermic reaction, so a thermal polymerization initiator can also be used in addition.

[0074] The photopolymerization initiator can be any compound capable of forming radicals by exposure to light such as ultraviolet light, without any limitations on its composition.

[0075] The photopolymerization initiator may be one or more selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Specific examples of acylphosphine include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate. More detailed information on various photoinitiators is provided in Reinhold Schwalm's book "UV Coatings: Basics, Recent Developments and New Application" (Elsevier, 2007), p. 115, and is not limited to the above examples.

[0076] The thermal polymerization initiator may be at least one selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid. Specifically, examples of persulfate initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8), and examples of azo initiators include 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, and 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride. dihydrochloride, 2-(carbamoylazo)isobutylonitrile, 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), etc. A wide variety of thermal polymerization initiators are described in detail in Odian's book 'Principle of Polymerization' (Wiley, 1981), p. 203, and are not limited to the above examples.

[0077] The polymerization initiator can be used in an amount of 2 parts by weight or less per 100 parts by weight of the modified polysaccharide. That is, if the concentration of the polymerization initiator is too low, the polymerization rate may be slowed down and a large amount of residual monomer may be extracted in the final product, which is not preferable. On the other hand, if the concentration of the polymerization initiator is higher than the above range, the polymer chain forming the network may be shortened, the content of water-soluble components may increase, and the water absorption capacity under pressure may be reduced, which is not preferable, and the physical properties of the resin may be reduced.

[0078] The monomer composition may further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.

[0079] The monomer composition containing the monomer may be in the form of a suspension if it is insoluble, such as starch, which has a high molecular weight, or in the form of a solution dissolved in a solvent such as water, such as dextrin, which has a low molecular weight. The solid content in the monomer composition, i.e., the concentrations of the monomer, the internal crosslinking agent, and the polymerization initiator, may be appropriately adjusted in consideration of the polymerization time and reaction conditions. For example, the solid content in the monomer composition may be 10 to 80% by weight, or 15 to 60% by weight, or 30 to 50% by weight.

[0080] When the monomer composition has a solid content in the above range, it is possible to eliminate the need to remove unreacted monomers after polymerization by using the gel effect phenomenon that occurs in the polymerization reaction of a high-concentration aqueous solution, and it may be advantageous to adjust the grinding efficiency when grinding the polymer described below.

[0081] The solvent that can be used at this time may be any solvent capable of dissolving the above-mentioned components, and may be any combination of at least one selected from the group consisting of water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, and N,N-dimethylacetamide.

[0082] On the other hand, the cross-linking polymerization of the modified polysaccharide can be carried out without any particular limitation as long as it can form a hydrogel polymer by thermal polymerization, photopolymerization or hybrid polymerization.

[0083] Specifically, polymerization methods are broadly divided into thermal polymerization and photopolymerization depending on the polymerization energy source. Thermal polymerization can usually be carried out in a reactor having a stirring shaft such as a kneader, and photopolymerization can be carried out in a reactor equipped with a movable conveyor belt or in a flat-bottomed vessel, but the above-mentioned polymerization methods are merely examples, and the present invention is not limited to the above-mentioned polymerization methods.

[0084] For example, the hydrogel polymer obtained by thermal polymerization by supplying hot air to a reactor such as a kneader equipped with an agitator shaft or by heating the reactor as described above may have a shape of several centimeters to several millimeters when discharged from the reactor outlet, depending on the shape of the agitator shaft equipped in the reactor. Specifically, the size of the obtained hydrogel polymer varies depending on the concentration of the monomer composition injected and the injection speed, and a hydrogel polymer having a weight average particle size of 2 to 50 mm can be obtained.

[0085] In addition, when photopolymerization is performed in a reactor equipped with a movable conveyor belt or a flat-bottomed vessel as described above, the form of the hydrogel polymer obtained may be a sheet-like hydrogel polymer having the width of the belt. In this case, the thickness of the polymer sheet varies depending on the concentration of the monomer composition to be injected and the injection speed or injection amount, but it is preferable to supply the monomer composition so that a sheet-like polymer having a thickness of about 0.5 to about 5 cm is obtained. If the monomer composition is supplied so that the thickness of the sheet-like polymer is too thin, the production efficiency is low, which is undesirable, and if the thickness of the sheet-like polymer exceeds 5 cm, the polymerization reaction may not be uniform over the entire thickness due to the excessively thick thickness.

[0086] At this time, the water-containing gel polymer obtained by this method may have a water content of 40 to 70% by weight. For example, the water content of the water-containing gel polymer may be 40% by weight or more, 45% by weight or more, or 50% by weight or more, and 70% by weight or less, 65% by weight or less, or 60% by weight or less. If the water content of the water-containing gel polymer is too low, it may be difficult to secure an appropriate surface area in the subsequent pulverization step, and the efficiency of drying may decrease. If the water content of the water-containing gel polymer is too high, the pressure applied in the subsequent pulverization step may increase, and the water absorption capacity under pressure may decrease, and a lot of energy and a long time may be required in the drying step after pulverization.

[0087] Meanwhile, throughout this specification, the term "moisture content" refers to the amount of moisture in the total weight of the hydrogel polymer, and is calculated by subtracting the weight of the polymer in a dry state from the weight of the hydrogel polymer. Specifically, it is defined as a value calculated by measuring the weight loss due to the evaporation of moisture in the polymer during the process of drying by increasing the temperature of the crumb-state polymer through infrared heating. Here, the drying for measuring the moisture content is performed by increasing the temperature to about 50°C at room temperature and then vacuum drying at 50°C for about 6 hours.

[0088] Meanwhile, after preparing the hydrogel polymer, a coarse grinding process may be optionally carried out to grind the prepared hydrogel polymer prior to the subsequent drying and grinding processes.

[0089] The coarse pulverization process is a process for increasing the drying efficiency in the subsequent drying process and controlling the particle size of the final superabsorbent resin powder. The pulverizer used here is not limited in terms of configuration, and specifically may include any one selected from the group of pulverizing devices consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a meat chopper, and a disc cutter, but is not limited to the above examples.

[0090] The coarse pulverization step can be carried out so that the hydrogel polymer has a particle size of about 2 to about 10 mm, for example. It is technically difficult to pulverize the hydrogel polymer to a particle size of less than 2 mm due to the high water content of the hydrogel polymer, and the pulverized particles may aggregate with each other. On the other hand, when the hydrogel polymer is pulverized to a particle size of more than 10 mm, the efficiency of the subsequent drying step is not increased significantly.

[0091] Next, the hydrogel polymer prepared in the previous step is dried, crushed and classified to prepare a base resin.

[0092] The drying method can be selected and used without any limitation in its structure as long as it is a method commonly used in the drying process of hydrogel polymers. Specifically, the drying step can be performed by hot air supply, infrared radiation, microwave radiation, ultraviolet radiation, etc.

[0093] Specifically, the drying can be carried out under vacuum conditions at a temperature of less than 100° C., specifically, at a temperature of about 30° C. to about 80° C. If the drying temperature is 100° C. or higher, it is not suitable because the modified polysaccharide may be decomposed, and if the drying temperature is less than 30° C., the drying time may be excessively long.

[0094] Meanwhile, the drying time can be about 20 to about 90 minutes in consideration of process efficiency, but is not limited thereto.

[0095] The water content of the polymer after such a drying step may be about 5 to about 10% by weight.

[0096] After the drying step, a grinding step is carried out.

[0097] The pulverization process can be carried out so that the particle size of the polymer powder, i.e., the base resin, is about 150 to about 850 μm. Specific examples of the pulverizer used to pulverize to such a particle size include a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, and a jog mill, but the present invention is not limited to the above examples.

[0098] In addition, after the above-mentioned pulverization step, a process of classifying the pulverized polymer powder according to particle size may be further carried out in order to control the physical properties of the superabsorbent resin to be manufactured as a final product.

[0099] Preferably, polymers having a particle size of about 150 to about 850 μm are classified, and only the polymers having such a particle size are used as the base resin, and can be made into a product through a surface crosslinking reaction stage.

[0100] The base resin obtained as a result of the above process may have a powder form including a crosslinked polymer crosslinked by an acrylic acid monomer and an internal crosslinking agent. Specifically, the base resin may have a powder form having a particle size of 150 to 850 μm.

[0101] On the other hand, there is also provided a sanitary product containing the above-mentioned biodegradable highly water-absorbent resin.

[0102] In the following, preferred embodiments are presented to aid in understanding the invention, but the following embodiments are merely for the purpose of illustrating the invention and are not intended to limit the invention thereto. EXAMPLES

[0103] Production Example 1: Production of modified chitosan (M / S) 20g of chitosan (200-600mPa.s, 0.5% in 0.5% acetic acid at 20℃, manufactured by TCI) and 100g of maleic anhydride were added to a 500ml three-neck flask containing 200ml of water and stirred at 70℃ for 6 hours. After the reaction, the mixture was precipitated in acetone solvent and filtered to remove excess maleic anhydride, and then dried at 50℃ for more than 24 hours to obtain maleated chitosan.

[0104] The weight average molecular weight of the produced chitosan is 3.3×10 5 g / mol, and the degree of substitution (DS M ) was 0.94. At this time, the degree of substitution of the substituent 1 It was calculated based on the integral ratio of the peaks corresponding to the vinyl of the maleic acid group (CH=CH, 6.3 ppm, 5.8 ppm) in H NMR, and the specific calculation method is as follows.

[0105] First, the maleated chitosan was 1The H NMR spectrum was obtained and is shown in Figure 1. Referring to Figure 1, it was confirmed that maleic acid groups were introduced into chitosan because peaks appeared at 6.3 ppm and 5.8 ppm, which correspond to the vinyl groups of the maleic acid groups, and the degree of substitution of maleic acid groups (-OCOCH=CHCOOH) in the maleated chitosan was determined based on the integral ratio of these peaks.

[0106] Production Example 2: Production of Modified Starch 1 (M / S-1) 20g of starch (Starch from potato, manufactured by Aldrich) and 100g of maleic anhydride were added to a three-neck flask containing 200ml of water (250ml) and stirred at 70°C for 6 hours. After the reaction, the mixture was precipitated in acetone solvent and filtered to remove excess maleic anhydride, and then dried at 50°C for more than 24 hours to obtain maleated modified starch.

[0107] The modified starch produced has a weight average molecular weight of 3.4×10 7 g / mol, and the degree of substitution (DS M ) was 0.88.

[0108] At this time, the degree of substitution of the substituent is determined based on the maleated modified starch produced. 1 After obtaining the H NMR spectrum, the integral ratio of the peaks corresponding to the vinyl of the maleic acid group (CH=CH, 6.45 ppm, 6.28 ppm) in the spectrum was calculated, and the maleated modified starch 1 The 1 H NMR spectrum is shown in Figure 2. The specific calculation method was the same as that of the modified chitosan (M / S) in Preparation Example 1, and the remaining Preparation Examples were calculated in the same manner.

[0109] Production Example 3: Production of Modified Starch 2 (M / S-2) Starch (Starch from poatato, manufactured by Aldrich), isopropyl alcohol (IPA) and NaOH aqueous solution (concentration: about 40%) were mixed in a 500mL RBF (Round Bottom Flask) and stirred at room temperature for about 20 minutes. The weight ratio of the mixture was 1:4:0.8 (starch:IPA:NaOH aqueous solution). Next, about 80 parts by weight of sodium monochloroacetate was added to 100 parts by weight of the starch, and the mixture was heated to 60°C and stirred for about 1 hour, and then cooled to room temperature. After cooling to room temperature, the solvent was removed, the reactant was dissolved in water, and precipitated in methanol to remove water-soluble impurities, filtered to recover the starch, and dried in a vacuum drying oven at 40°C for about 12 hours to obtain a solid target product.

[0110] 50 mg of the obtained solid target substance was mixed with 200 mg of a 30% DSO in D0 solution, and the mixture was stirred at 50° C. for about 1 hour to induce a hydrolysis reaction. 1 H NMR analysis was performed on the carboxymethylated modified starch produced. 1 The 1 H NMR spectrum is shown in Figure 3.

[0111] The modified starch produced has a weight average molecular weight of 1.2×10 7 g / mol, and the degree of substitution of the carboxymethyl group (DSc) was 0.6.

[0112] Production Example 4: Production of Modified Starch 3 (M / S-3) Starch (Starch from corn, manufactured by Samyang), isopropyl alcohol (IPA) and NaOH aqueous solution (concentration: about 40%) were mixed in a 500mL RBF (Round Bottom Flask) and stirred at room temperature for about 20 minutes. The weight ratio of the mixture was 1:4:0.8 (starch:IPA:NaOH aqueous solution). Next, about 80 parts by weight of sodium monochloroacetate was added to 100 parts by weight of the starch, and the mixture was heated to 60°C and stirred for about 1 hour, and then cooled to room temperature. After cooling to room temperature, the solvent was removed, the reactants were dissolved in water, and precipitated in methanol to remove water-soluble impurities, filtered to recover the starch, and dried in a vacuum drying oven at 40°C for about 12 hours to obtain a solid target product.

[0113] 50 mg of the obtained solid target substance was mixed with 200 mg of a 30% DSO in D0 solution, and the mixture was stirred at 50° C. for about 1 hour to induce a hydrolysis reaction. 1 H NMR analysis was performed on the carboxymethylated modified starch produced. 1 The 1 H NMR spectrum is shown in Figure 4.

[0114] The modified starch produced has a weight average molecular weight of 3×10 7 g / mol, and the degree of substitution of the carboxymethyl group (DSc) was 0.6.

[0115] Production Example 5: Production of Modified Starch 4 (M / S-4) Starch (Starch from poatato, manufactured by Daesang), isopropyl alcohol (IPA) and NaOH aqueous solution (concentration: about 40%) were mixed in a 500mL RBF (Round Bottom Flask) and stirred at room temperature for about 20 minutes. The weight ratio of the mixture was 1:4:0.8 (starch:IPA:NaOH aqueous solution). Next, about 80 parts by weight of sodium monochloroacetate was added to 100 parts by weight of the starch, and the mixture was heated to 60°C and stirred for about 1 hour, and then cooled to room temperature. After cooling to room temperature, the solvent was removed, the reactants were dissolved in water, and precipitated in methanol to remove water-soluble impurities, filtered to recover the starch, and dried in a vacuum drying oven at 40°C for about 12 hours to obtain a solid target product.

[0116] 50 mg of the obtained solid target substance was mixed with 200 mg of a 30% DSO in D0 solution, and the mixture was stirred at 50° C. for about 1 hour to induce a hydrolysis reaction. 1 H NMR analysis was performed on the carboxymethylated modified starch produced. 1 The 1 H NMR spectrum is shown in Figure 5.

[0117] The modified starch produced has a weight average molecular weight of 1.9×10 7 g / mol, and the degree of substitution of the carboxymethyl group (DSc) was 0.6.

[0118] Production Example 6: Production of Modified Starch 5 (M / S-5) Starch (Starch from corn, manufactured by Daesang), isopropyl alcohol (IPA) and NaOH aqueous solution (concentration: about 40%) were mixed in a 500mL RBF (Round Bottom Flask) and stirred at room temperature for about 20 minutes. The weight ratio of the mixture was 1:4:0.8 (starch:IPA:NaOH aqueous solution). Next, about 80 parts by weight of sodium monochloroacetate was added to 100 parts by weight of the starch, and the mixture was heated to 60°C and stirred for about 1 hour, and then cooled to room temperature. After cooling to room temperature, the solvent was removed, the reactant was dissolved in water, and precipitated in methanol to remove water-soluble impurities, filtered to recover the starch, and dried in a vacuum drying oven at 40°C for about 12 hours to obtain a solid target product.

[0119] 50 mg of the obtained solid target substance was mixed with 200 mg of a 30% DSO in D0 solution, and the mixture was stirred at 50° C. for about 1 hour to induce a hydrolysis reaction. 1 H NMR analysis was performed on the carboxymethylated modified starch produced. 1 The 1 H NMR spectrum is shown in Figure 6.

[0120] The modified starch produced has a weight average molecular weight of 2.4×10 7 g / mol, and the degree of substitution of the carboxymethyl group (DSc) was 0.8.

[0121] Comparative Production Example 1: Production of modified starch (M) 20g of starch (soluble, manufactured by Mita Chemicals) and 60g of maleic anhydride were added to a 500ml three-neck flask containing 200ml of water and stirred at 70°C for 6 hours. After the reaction, the mixture was precipitated in acetone solvent and filtered to remove excess maleic anhydride, and then dried at 50°C for more than 24 hours to obtain maleated modified starch (M).

[0122] The final modified starch (M) had a weight average molecular weight of 1.5×10 5 g / mol, and the degree of substitution (DS M ) was 0.81.

[0123] Comparative Example 2: Preparation of modified chitosan (M-1) 20g of chitosan (5-20mPa.s, 0.5% in 0.5% acetic acid at 20℃, manufactured by TCI) and 100g of maleic anhydride were added to a 500ml three-neck flask containing 200ml of water and stirred at 70℃ for 6 hours. After the reaction, the mixture was precipitated in acetone solvent and filtered to remove excess maleic anhydride, and then dried at 50℃ for more than 24 hours to obtain maleated modified starch (M).

[0124] The final modified chitosan (M-1) had a weight average molecular weight of 5×10 4 g / mol, and the degree of substitution (DS M ) was 1.11.

[0125] Comparative Production Example 3: Production of modified starch (M-2) Starch (soluble, manufactured by Tokuyama Pharmaceutical Co., Ltd.), isopropyl alcohol (IPA) and NaOH aqueous solution (concentration: about 40%) were mixed in a 500mL RBF (Round Bottom Flask) and stirred at room temperature for about 20 minutes. The weight ratio of the mixture was 1:4:0.8 (starch:IPA:NaOH aqueous solution). Next, about 80 parts by weight of sodium monochloroacetate was added to 100 parts by weight of the starch, and the mixture was heated to 60°C and stirred for about 1 hour, and then cooled to room temperature. After cooling to room temperature, the solvent was removed, the reactants were dissolved in water, and precipitated in methanol to remove water-soluble impurities, filtered to recover the starch, and dried in a vacuum drying oven at 40°C for about 12 hours to obtain a solid target product.

[0126] The final modified starch (M-2) had a weight average molecular weight of 9.2×10 4 g / mol, and the degree of substitution of carboxymethyl (DS M(c?) ) was 0.68.

[0127] Example 1 50 mL of distilled water and 3 g of modified chitosan (M / S) of Preparation Example 1 were added to a 250 mL RBF (Round Bottom Flask), and the mixture was stirred in an oil bath at 35°C for 30 minutes or more to fully dissolve the modified chitosan in the distilled water. Then, an initiator was added. As the initiator, about 0.03 g of ammonium persulfate was added. After the initiator was added, the mixture was further stirred at a temperature of about 70°C for about 4 hours to perform crosslinking. After crosslinking, ethanol was added to precipitate a polymer material containing a crosslinked polymer, and the polymer material was filtered and dried overnight in a vacuum drying oven at 40°C to obtain the target polymer material. The dried polymer thus obtained was pulverized using a pulverizer and classified using a standard mesh sieve of the ASTM standard to obtain a base resin having a particle size of 300 to 600 μm, which was used as a superabsorbent resin.

[0128] Example 2 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified starch (M / S-1) of Preparation Example 2 was used instead of the modified chitosan (M / S) of Example 1.

[0129] Example 3 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified starch (M / S-2) of Preparation Example 3 was used instead of the modified chitosan (M / S) in Example 1.

[0130] Example 4 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified starch (M / S-3) of Preparation Example 4 was used instead of the modified chitosan (M / S) in Example 1.

[0131] Example 5 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified starch (M / S-4) of Preparation Example 5 was used instead of the modified chitosan (M / S) in Example 1.

[0132] Example 6 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified starch (M / S-5) of Preparation Example 6 was used instead of the modified chitosan (M / S) in Example 1.

[0133] Comparative Example 1 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified starch (M) of Comparative Preparation Example 1 was used instead of the modified chitosan (M / S) in Example 1.

[0134] Comparative Example 2 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified chitosan (M-1) of Comparative Preparation Example 2 was used instead of the modified chitosan (M / S) in Example 1.

[0135] Comparative Example 3 A superabsorbent resin was prepared in the same manner as in Example 1, except that the modified starch (M-2) of Comparative Preparation Example 3 was used instead of the modified chitosan (M / S) in Example 1.

[0136] Experimental Example The properties of the superabsorbent resins produced in the above Examples and Comparative Examples were evaluated by the following methods, and the results are shown in Table 1 below.

[0137] Unless otherwise indicated, all of the following physical property evaluations were performed at constant temperature and humidity (23±1°C, relative humidity 50±10%), and saline or salt water refers to a 0.9 wt% sodium chloride (NaCl) aqueous solution.

[0138] (1) Weight average molecular weight The weight average molecular weight is measured by GPC / MALLS, and the detailed measurement method is as follows.

[0139] 1) Preparation of mobile phase 1000 mL of 100 mM NaNO3 aqueous solution containing 0.02% NaN3 was filtered through a solvent clarification system.

[0140] 2) Preparation of sample solution 5 mL of 100 mM NaNO3 aqueous solution containing 0.02% NaN3 was added to 25 mg of sample, heated at 110°C for 1 hour, filtered through a 0.45 micrometer nylon syringe filter, and applied to the analysis.

[0141] 3)GPC / MALLS conditions Stationary phase: Shodex OH-Pak 804 column, Shodex OH-Pak 80 column Mobile phase: 100 mM NaNO3 aqueous solution containing 0.02% NaN3 Flow rate: 0.4mL / min Stationary phase temperature: 25℃ Injection volume: 100 microliters Analysis time: 120 minutes

[0142] (2)Centrifuge Retention Capacity (CRC) The water retention capacity of each resin was measured by the no-load absorbency using EDANA WSP 241.3.

[0143] Specifically, the highly water-absorbent resin W0(g) (approximately 0.2g) was evenly placed in a nonwoven envelope, sealed, and then immersed in physiological saline (0.9% by weight) at room temperature. After 30 minutes, the envelope was centrifuged at 250G for 3 minutes to remove water, and the mass of the envelope W2(g) was measured. The same procedure was also performed without using the resin, and the mass W1(g) at that time was measured. The CRC(g / g) was calculated using the obtained masses according to the following formula.

[0144] [Formula 1] CRC(g / g)={[W2(g)-W1(g)] / W0(g)}-1

[0145] (3) Biodegradability test Measurements were performed based on the KS M ISO 14851 standard.

[0146] [Table 1]

[0147] As can be seen from Table 1 above, the biodegradable highly water-absorbent resin containing the high molecular weight modified polysaccharide according to the present invention was confirmed to have excellent water absorption properties and also excellent biodegradability.

Claims

1. Maleic acid group (-OCOCH=CHCOOH) and carboxymethyl group (-CH 2 -COOH), At least a portion of the maleic acid groups and carboxymethyl groups are neutralized; The crosslinked polymer contains 60 parts by weight or more of a repeating unit derived from a modified polysaccharide, The molecular weight of the modified polysaccharide is 190,000 g / mol or more; Biodegradable super absorbent resin.

2. 2. The biodegradable highly water-absorbent resin according to claim 1, wherein the degree of substitution of maleic acid groups in the modified polysaccharide is 0.15 to 1.

5.

3. 2. The biodegradable highly water-absorbent resin according to claim 1, wherein the degree of substitution of carboxymethyl groups in the modified polysaccharide is 0.2 to 1.

2.

4. 2. The biodegradable superabsorbent resin according to claim 1, wherein the modified polysaccharide is modified starch, modified cellulose or modified chitosan.

5. 2. The biodegradable superabsorbent resin according to claim 1, wherein the maleic acid group is introduced by maleic acid or maleic acid anhydride.

6. 2. The biodegradable highly absorbent resin according to claim 1, wherein the carboxymethyl group is introduced by any one of glycolic acid, monochloroacetic acid, and salts thereof.

7. The biodegradable highly absorbent resin according to claim 1, wherein the modified polysaccharide contains at least one of repeating units represented by the following chemical formulas 1 to 4: [Formula 1] In the above chemical formulas 1 to 4, Each M is independently hydrogen or an alkali metal.

8. 2. The biodegradable highly absorbent resin according to claim 1, wherein the crosslinked polymer contains 80 parts by weight or more of repeating units derived from a modified polysaccharide.

9. 2. The biodegradable highly absorbent resin according to claim 1, wherein the molecular weight of the modified polysaccharide is from 300,000 g / mol to 1,000,000,000 g / mol.

10. 2. The biodegradable highly absorbent resin according to claim 1, wherein the molecular weight of the modified polysaccharide is 300,000 g / mol to 50,000,000 g / mol.

11. The biodegradable highly absorbent resin according to claim 4, wherein the molecular weight of the modified starch is from 400,000 g / mol to 1,000,000,000 g / mol.

12. 5. The biodegradable highly water-absorbent resin according to claim 4, wherein the molecular weight of the modified cellulose or modified chitosan is 190,000 g / mol to 10,000,000 g / mol.

13. The biodegradable highly absorbent resin according to claim 1 , wherein the monomer further comprises an acrylic acid compound having at least a partially neutralized acid group.

14. The biodegradable highly water-absorbent resin according to claim 1 , wherein the crosslinked polymer is crosslinked by an internal crosslinking agent.

15. In the presence of a polymerization initiator, maleic acid group (-OCOCH=CHCOOH) and carboxymethyl group (-CH 2preparing a monomer composition including a modified polysaccharide having at least one of the following moieties: cross-linking the monomer composition to prepare a hydrogel polymer; and drying, grinding and classifying the hydrogel polymer; In the method for producing a biodegradable highly water-absorbent resin, At least a portion of the maleic acid groups and carboxymethyl groups of the modified polysaccharide are neutralized; The crosslinked polymer contains 60 parts by weight or more of a repeating unit derived from a modified polysaccharide, The molecular weight of the modified polysaccharide is 190,000 g / mol or more; A method for producing a biodegradable highly water-absorbent resin.

16. The method for producing the biodegradable superabsorbent resin according to claim 15, wherein the modified polysaccharide is produced by reacting the polysaccharide with at least one of maleic acid, maleic acid anhydride, glycolic acid, monochloroacetic acid, and salts thereof.

17. The method for producing a biodegradable highly absorbent resin according to claim 15, wherein the monomer composition further comprises an internal crosslinking agent.

18. A sanitary product comprising the biodegradable highly absorbent resin according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Water-absorbing resin and its production

    JP1995228640A

  • Biodegradable water-absorbing material, its production method, and composting aid comprising the material

    JP2006328346A

  • Plant-based composite water-absorbing polymer and method for manufacturing the same

    JP2012012549A

  • Biodegradable highly absorbent resin and its manufacturing method

    JP2023509980A

  • All-cellulose super absorbent hydrogels and method of producing same