Additive removal device and additive removal method using the same
The continuous additive removal device and method efficiently extract plasticizers from polymers using a swelling and shrinking solvent process, addressing inefficiencies in conventional methods by minimizing solvent use and maintaining polymer quality.
Patent Information
- Application Number
- JP2024521871
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-27
- Filing Date
- 2023-05-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-18
AI Technical Summary
Conventional methods for removing plasticizers from recycled polymers are inefficient, requiring large amounts of solvents and resulting in poor physical properties of the recycled polymer, high equipment costs, and environmental hazards due to the use of phthalate plasticizers.
A continuous additive removal device and method using a barrel with a screw mechanism, where polymers are impregnated with a swelling solvent to diffuse and extract additives, followed by shrinking with a shrinking solvent, minimizing solvent use and maintaining polymer structure.
The device enables efficient removal of additives with reduced solvent usage, improving economic efficiency and maintaining polymer quality, while allowing for continuous processing and reducing environmental impact.
Smart Images

Figure 2024544471000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0140595 filed on October 27, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to an additive removal device for removing additives contained in a polymer for recycling the polymer, and a method for removing additives using the same. [Background technology]
[0003] Recently, the use of polymeric materials such as resins or plastics has increased as resin materials with properties required for various uses and purposes have been developed. In general, resins or plastics require a lot of energy from the extraction of crude oil to their manufacture, and a large amount of carbon is emitted in the process. Furthermore, when the resin or plastic contained in the final product is discarded, environmental pollution and social costs for its disposal are incurred. Therefore, recycling of discarded resins is essential from the viewpoint of reducing energy consumption, reducing carbon emissions, and preventing environmental pollution. In this way, plastics made by recycling resins discarded after use by final consumers are called PCR (Post-Consumer Recycled) resins, and attempts and efforts are being made to obtain PCR resins with the desired purity and properties.
[0004] Meanwhile, polyvinyl chloride (PVC) has hard or soft properties, excellent moldability, and is cost-competitive, making it versatile and applicable in a variety of fields. However, PVC cannot be used alone, and is mixed with plasticizers to give PVC flexibility and improve its workability and other physical properties to achieve various physical properties.
[0005] However, phthalate-based plasticizers, which have been used as plasticizers in the past, are harmful to the environment and human body and are subject to strict regulations in Korea and abroad, and in order to recycle polymers such as existing polyvinyl chloride resins in which such phthalate-based plasticizers are used, it is difficult to commercialize them unless the phthalate-based plasticizers are removed. Therefore, in order to recycle polymers in which phthalate-based plasticizers are used, attempts have recently been made to effectively remove the phthalate-based plasticizers remaining in the recovered polymers.
[0006] As part of this, in order to remove additives such as plasticizers from the recovered polymer, a method of dissolving the recovered polymer using a solvent and then recrystallizing it using an antisolvent, the so-called dissolution recrystallization method, has been mainly used. However, in this case, the amount of solvent and antisolvent used for dissolution and recrystallization is excessively large, and the physical properties of the recycled polymer thus regenerated are poor. Furthermore, since the amount of solvent used is large, excessive costs for facilities and equipment are incurred in proportion to the amount of solvent used.
[0007] Therefore, there is a need to develop an apparatus that can efficiently remove additives such as plasticizers contained in the recovered polymer while minimizing the amount of solvent used, and a method for removing additives from the polymer using the same. Summary of the Invention [Problem to be solved by the invention]
[0008] The problem to be solved by the present invention is to provide a continuous processing method capable of removing plasticizers contained in polymers with high efficiency for recycling the polymers, in order to solve the problems mentioned in the Background of the Invention, and to provide an apparatus for removing additives contained in polymers optimized for the same. [Means for solving the problem]
[0009] According to one embodiment of the present invention for solving the above problems, there is provided an additive removal device including: a barrel having an internal space and a polymer inlet on one side and a polymer outlet on the other side; a screw provided in the internal space of the barrel and rotatable around an axis; and a solvent outlet provided at the one end of the barrel, wherein the barrel is located between the polymer inlet and the polymer outlet, and includes a swelling solvent inlet adjacent to the polymer inlet and a shrinking solvent inlet adjacent to the polymer outlet.
[0010] The present invention provides a method for removing an additive, comprising the steps of preparing an additive removal device, supplying a polymer containing an additive to the polymer inlet, supplying a swelling solvent and a shrinking solvent to the swelling solvent inlet and the shrinking solvent inlet, respectively, transporting the supplied polymer to a polymer outlet by axial rotation of the screw, swelling the polymer in a swelling zone from the polymer inlet to the swelling solvent inlet, and shrinking the polymer in a shrinking zone from the swelling solvent inlet to the shrinking solvent inlet. Effect of the Invention
[0011] The additive removal device of the present invention is capable of continuously extracting additives from polymers even with a small device size and a small amount of solvent used, and can also improve the efficiency of removing the additives.
[0012] Furthermore, according to the method for removing additives of the present invention, unlike the conventional dissolution and recrystallization method, the polymer recovered from the waste resin is not dissolved in a solvent, but is impregnated with a swelling solvent to selectively diffuse and extract the additives inside the polymer, thereby making it possible to remove the additives from the polymer. This reduces the amount of solvent used and simplifies the required equipment, improving economy.
[0013] Next, when removing the swelling solvent from the polymer swollen by impregnation with the swelling solvent, the swollen polymer can be shrunk by applying a shrinking solvent to the swollen polymer, thereby efficiently reducing the amount of the solvent in the polymer and the amount of the additive present in the solvent. [Brief description of the drawings]
[0014] [Figure 1] 1 is a vertical cross-sectional view showing an additive removal device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The terms and words used in the description and claims of the present invention should not be interpreted limitedly to their ordinary or dictionary meanings, but should be interpreted in a way that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0016] In order to facilitate understanding of the present invention, the present invention will now be described in more detail with reference to FIG.
[0017] The additive removal device 1 according to one embodiment of the present invention includes a barrel 10 providing an internal space and having a polymer inlet 20 on one side and a polymer outlet 30 on the other side, a screw 70 provided in the internal space of the barrel 10 and rotating on its axis, and a solvent outlet 60 provided at the one end of the barrel 10, and the barrel 10 is located between the polymer inlet 20 and the polymer outlet 30 and may include a swelling solvent inlet 40 adjacent to the polymer inlet and a shrinking solvent inlet 50 adjacent to the polymer outlet.
[0018] First, the polymer may be a polymer recovered from waste resin, obtained by pretreating the waste resin, and may be in the form of particles. Meanwhile, the waste resin may be recovered from various products or applications molded using resin or a composition thereof, regardless of whether the waste resin is hard or soft. In addition, the recovered polymer may be a single type of polymer, or may be a resin composition blended with other resins.
[0019] The pretreatment means a series of processes for treating the waste resin into a polymer suitable for application to the additive removal device of the present invention. For example, the pretreatment may be a process of first washing the waste resin with a solvent such as water to remove relatively large foreign matter such as dust, drying, and then pulverizing the waste resin into particles.
[0020] Specifically, the average particle size (D50) of the polymer may be 0.1 mm or more and 2 mm or less. As the average particle size of the recovered polymer is smaller, the impregnation speed of the impregnation solvent increases and the removal speed of the additive increases, but there is a drawback in that the processing time increases in order to produce a recovered polymer with a small average particle size.
[0021] The type of polymer suitable for application to the additive removal device according to one embodiment of the present invention is not particularly limited, but when the additive to be removed by the additive removal device is a plasticizer, the polymer may be polyvinyl chloride (PVC).
[0022] Meanwhile, additives such as plasticizers, fillers, flame retardants, stabilizers, bulking agents, viscosity reducers, colorants, and heat stabilizers may be used to impart desired physical properties to the resin during or after the polymerization of the polymer, during molding, and other manufacturing processes of the product, and the additives used remain in the resin manufactured by the additives. Therefore, the additives may also be contained in waste resin recovered from products in order to recycle the resin.
[0023] When producing a recycled polymer from a polymer recovered from the waste resin, the additives must be appropriately removed for the following reasons.
[0024] First, if an excessive amount of additives remain, it may be difficult to produce a recycled polymer with good physical properties, etc. The additives may cause the recycled polymer to deform or have poor physical properties such as poor surface properties, or to have poor color properties such as discoloration.
[0025] Secondly, some additives have recently been restricted in use due to their environmental and human toxicity, i.e., due to regulations that did not exist at the time of the manufacture of the product, it is becoming increasingly possible to produce recycled polymers by removing regulated additives from recovered polymers to a desired level or lower.
[0026] For the above reasons, the additive that needs to be removed from the recovered polymer containing the additive may be mainly a plasticizer. Specifically, the plasticizer may be a phthalate-based plasticizer. More specifically, the phthalate-based plasticizer may be one or more of dioctyl phthalate (DOP), dibutyl phthalate (DBP), dioctyl terephthalate (DOTP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), di-(2-ethylhexyl) terephthalate (DEHTP), and butyl benzyl phthalate (BBP).
[0027] Meanwhile, the method for removing additives according to an embodiment of the present invention selectively dissolves only the additive while maintaining the shape of the polymer, which is different from the conventional method of dissolving the polymer itself using a dissolving solvent and then recrystallizing it. In the case of additives such as plasticizers that have good compatibility with resins, such a dissolution recrystallization method is difficult to remove, and in particular, in this case, an excessive amount of solvent (antisolvent) is required, which not only increases the cost of the solvent but also increases the cost of purifying it, resulting in poor purification efficiency relative to the cost.
[0028] Therefore, the method for removing an additive of the present invention first contacts a polymer containing an additive with a swelling solvent to impregnate the polymer with the swelling solvent to swell the polymer, and then diffuses the additive in the polymer with the swelling solvent, thereby removing the additive from the polymer. Next, the polymer impregnated with the swelling solvent is contacted with a shrinking solvent to shrink the polymer, thereby minimizing the content of the solvent present in the polymer. That is, the polymer in a swollen state is shrunk by the shrinking solvent, so that the swelling solvent containing the additive inside is discharged to the outside of the polymer as much as possible, and finally the content of the additive in the polymer can be reduced.
[0029] Here, the term "immersion" refers not only to washing the additive (plasticizer) present on the surface of the recovered polymer with the impregnation solvent, but also to the impregnation solvent penetrating into the interior of the recovered polymer by diffusion, thereby dissolving the additive (plasticizer) therein.
[0030] Furthermore, the present invention provides an optimal additive removal device 1 that can perform the additive removal method continuously, can reduce the amount of swelling solvent and shrinking solvent used, thereby improving economy, and can improve the efficiency of removing additives, specifically plasticizers.
[0031] In view of this, the barrel 10 according to an embodiment of the present invention is an element constituting the main body of the additive removal device 1, and may be tubular extending in the length direction and having an internal space. The barrel 10 may be made of a material that is not deformed by the solvent described below, and more specifically, may be made of a metal material or a glass material.
[0032] The internal space is a space where the polymer supplied to the polymer inlet 20 is transported to the polymer outlet 30 by the screw 70, and where the solvents supplied to the swelling solvent inlet 40 and the shrinking solvent inlet 50 are transported by gravity, and may refer to a space where additives contained in the polymer are removed by swelling and shrinking of the polymer.
[0033] Specifically, the barrel 10 may have a polymer inlet 20 on one side and a polymer outlet 30 on the other side. The polymer may be a polymer containing an additive, and the polymer may be supplied to the polymer inlet 20 and sequentially contacted with a swelling solvent and a shrinking solvent, which will be described later, to remove the additive therefrom, and the polymer from which the additive has been removed may be discharged through the polymer outlet 30.
[0034] Meanwhile, the additive remover 1 may include a screw 70 that is installed in the internal space of the barrel 10 and rotates around its axis, and may include a torque supplying device 80 at the other end of the barrel 10 to apply a torque to the screw 70. Here, the other end may be an end of the barrel 10 adjacent to the polymer outlet 30.
[0035] The torque supplying device 80 supplies a driving force for axial rotation to the screw 70, and specifically may be a motor.
[0036] Specifically, the screw 70 may include a shaft 71 that is connected to a torque supplying device 80 and rotates around its axis, and a plate 72 that is fixed to the outer circumferential surface of the shaft 71 and extends in a spiral shape along the length of the shaft 71. The plate 72 may rotate around the shaft 71 as a rotation axis by the torque provided by the torque supplying device 80. Thus, the polymer supplied to the polymer inlet 20 may be loaded onto the plate 72 and continuously transported to the polymer outlet 30 by the axial rotation of the screw 70.
[0037] On the other hand, the supply flow rate (g / min) of the polymer supplied to the polymer inlet 20 is determined by the volume (cm) of one pitch p of the screw. 3 ), bulk density of the supplied polymer (g / cm 3 ) and screw rotation speed (RPM, min -1) and specifically, the following general formula 1 can be satisfied.
[0038] [General formula 1] Volume of one pitch p of the screw (cm 3 )*bulk density of supplied polymer (g / cm 3 )*Screw rotation speed (min -1 )*0.1≦polymer supply flow rate (g / min) ≦volume of one screw pitch p (cm 3 )*bulk density of supplied polymer (g / cm 3 )*Screw rotation speed (min -1 )*0.5
[0039] Meanwhile, according to one embodiment of the present invention, in the additive removal device 1, an extension line of the rotation axis of the screw 70, specifically, an extension line of the shaft 71, may be disposed so as to be inclined with respect to the ground. That is, the surface height of the polymer outlet 30 may be disposed higher than the surface height of the polymer inlet 20. By making the length of the support stand supporting the polymer outlet 30 side longer than the length of the support stand supporting the polymer inlet 20 side as a support stand for supporting the additive removal device 1, an inclination angle z between the extension line of the rotation axis of the screw 70 and the ground may be realized.
[0040] Meanwhile, the swelling solvent and shrinking solvent introduced into the internal space of the barrel 10 can be transported to the solvent discharge section 60 by gravity due to the inclination angle z between the extension line of the rotation axis of the screw 70 and the ground, and the introduced swelling solvent and shrinking solvent can be prevented from flowing back to the polymer discharge port 30 and being lost.
[0041] Furthermore, by controlling the inclination angle z between the extension line of the rotation axis of the screw 70 and the ground, the time the swelling solvent and the shrinking solvent remain in the device and the time the solvent contacts the polymer can be determined, thereby making it possible to more efficiently remove additives from the polymer.
[0042] Specifically, the inclination angle z between the extension line of the rotation center axis of the screw 70 and the ground may be 5 degrees to 30 degrees. The inclination angle z is also related to the flow rate of the swelling solvent and shrinking solvent supplied. If the inclination angle is more than 30 degrees, the solvent supplied to the barrel 10 through the swelling solvent inlet 40 or shrinking solvent inlet 50 is discharged without being sufficiently retained in the internal space of the barrel, that is, even though it has the ability to swell or shrink the polymer, it is discharged in an excessively short time, so that an excessive amount of solvent is required and further, the amount of energy required in the purification process for reusing the solvent increases. On the other hand, if the inclination angle is less than 5 degrees, the solvent supplied to the barrel is likely to be discharged from the polymer outlet 30 and disappear, and the solvent that has reached the vicinity of the solvent outlet, i.e., the solvent in which the additives are concentrated, cannot be smoothly discharged from the solvent outlet, so that the efficiency of removing the additives in the polymer may decrease.
[0043] According to an embodiment of the present invention, a swelling solvent may be supplied to the swelling solvent inlet 40 and a shrinking solvent may be supplied to the shrinking solvent inlet 50 .
[0044] Furthermore, the internal space of the barrel 10 may be functionally divided into a swelling zone 100 from the polymer inlet 20 to the swelling solvent inlet 40 and a shrinkage zone from the swelling solvent inlet 40 to the shrinkage solvent inlet 50. Specifically, the swelling zone 100 refers to a region from a cross section including the center of the polymer inlet 20 to a cross section including the center of the swelling solvent inlet 40 as a cross section of the barrel 10, and the shrinkage zone 200 refers to a region from a cross section including the center of the swelling solvent inlet 40 to a cross section including the center of the shrinkage solvent inlet 50.
[0045] First, the polymer containing additives supplied through the polymer inlet 20 passes through the swelling zone 100 and the shrinkage zone 200 in the process of being transported to the polymer outlet 30 by the axial rotation of the screw 70 .
[0046] The distance x from the polymer inlet 20 to the swelling solvent inlet 40 may be the length of the swelling zone 100, and the distance y from the swelling solvent inlet 40 to the shrinking solvent inlet 50 may be the length of the shrinking zone 200. The ratio x / y of the distance x from the polymer inlet 20 to the swelling solvent inlet 40 and the distance y from the swelling solvent inlet 40 to the shrinking solvent inlet 50 may be 0.1 to 60, specifically 1 to 30. If the ratio x / y is less than 0.1, the residence time of the polymer in the shrinking zone may be longer than necessary, which may reduce the economic efficiency of the process, and if the ratio x / y is more than 60, the residence time of the polymer in the shrinking zone may be shorter than necessary, which may cause a problem that the swollen polymer is difficult to sufficiently shrink.
[0047] Meanwhile, in the swelling zone 100, the polymer containing the additive comes into contact with the swelling solvent, so that the swelling solvent impregnates the polymer, and the polymer swells while maintaining its inherent molecular structure. The additive contained in the polymer diffuses through the impregnating solvent and is dissolved out of the recovered polymer, so that the additive in the polymer can be removed.
[0048] For efficient removal of additives from polymers, it is important to select a swelling solvent used to swell the polymer. First, the swelling solvent must be rapidly and uniformly impregnated into the polymer particles, and the maximum amount of additive contained in the polymer must be dissolved by the swelling solvent impregnated in the polymer. Therefore, the swelling solvent must be selected taking into consideration the type of polymer and the type of additive to be removed.
[0049] From this viewpoint, when the additive is a phthalate-based plasticizer, the swelling solvent may be one or more of cyclohexanone, cyclopentanone, N,N-dimethylacetamide, tetrahydrofuran, pyridine, 3-pentanone, 2-pentanone, dimethylformamide, methyl ethyl ketone, dichloromethane, 4-methylpentan-2-one, nitrobenzene, 1,4-dioxane, 1,1,2,2-tetrachloroethane, acetone, ethyl acetate, chloroform, and dimethyl sulfoxide, and more specifically, methyl ethyl ketone. The solvent can be easily impregnated into the polymer, and is also excellent in the ability to dissolve the additive, for example, the phthalate-based plasticizer, in the polymer, and therefore can be preferably used.
[0050] In this way, in order to sufficiently impregnate the swelling solvent into the polymer in the swelling zone 100 and smoothly dissolve the internal additive due to the swelling of the polymer, the supply flow rate (cm 3 / min) can be determined by the supply flow rate of the polymer and the bulk density of the supplied polymer. Specifically, the following general formula 2 can be satisfied.
[0051] [General formula 2] Feed flow rate of the polymer (g / min) / bulk density of the polymer (g / cm 3 )*0.5≦Flow rate of swelling solvent (cm 3 / min) ≦ Supply flow rate of supplied polymer (g / min) / Bulk density of supplied polymer (g / cm 3 )*10
[0052] That is, the supply volume flow rate of the swelling solvent (cm 3 / min) / Volumetric flow rate of polymer (cm 3 When the supply volume flow rate (cm / min) of the swelling solvent is 0.5 or more, the polymer can be sufficiently swollen and the residual additives in the polymer can be smoothly removed. 3 / min) / Volumetric flow rate of polymer (cm 3When the reaction rate (R / min) is 10 or less, unnecessary solvent usage can be reduced, and purification costs due to excessive solvent usage can be reduced, thereby improving the economic efficiency of the process.
[0053] Meanwhile, the residence time of the polymer in the swelling zone 100 can satisfy the following general formula 3 in relation to a value represented by the average particle diameter (D50, mm) of the polymer.
[0054] [General formula 3] Average particle size of polymer (mm)*5≦Residence time in swelling zone (min)≦Average particle size of polymer (mm)*240
[0055] That is, when the polymer is retained in the swelling zone 100 for a time longer than [a value represented by the average particle diameter of the polymer*5], the swelling solvent can penetrate into the polymer and the additives can be sufficiently dissolved. On the other hand, when the polymer is retained for a time longer than [a value represented by the average particle diameter of the polymer*240], the economic efficiency of the process may decrease. Specifically, when the screw rotation speed (RPM) is excessively reduced in order to increase the retention time, the yield of the polymer from which the additives have been removed per unit time decreases, or when the length of the swelling zone 100 is increased in order to increase the retention time, the size of the apparatus may increase.
[0056] Meanwhile, a mixture of the swelling solvent and the shrinking solvent may exist in the swelling zone 100. That is, the shrinking solvent supplied to the shrinking solvent inlet 50 passes through the shrinking zone 200 and the swelling zone 100 and is discharged to the solvent outlet 60, so that the swelling solvent and the shrinking solvent exist together in the swelling zone 100.
[0057] If the amount of shrinking solvent is excessively large compared to the swelling solvent in the swelling zone 100, the swelling of the polymer by the swelling solvent and the solvent impregnation may be reduced, so the flow rates of the swelling solvent and the shrinking solvent in the swelling zone 100 must be controlled at an appropriate ratio. Meanwhile, since the flow rates of the swelling solvent and the shrinking solvent in the swelling zone 100 are ultimately determined by the flow rate of the swelling solvent supplied to the swelling solvent inlet 40 and the flow rate of the shrinking solvent supplied to the shrinking solvent inlet 50, it is important to appropriately control the flow rate ratio for smooth impregnation of the swelling solvent and swelling of the polymer.
[0058] In view of this, the flow rate ratio of the volumetric flow rate of the shrinking solvent supplied to the shrinking solvent inlet to the volumetric flow rate of the swelling solvent supplied to the swelling solvent inlet may be 30 volume % to 300 volume %. If the volumetric flow rate of the shrinking solvent is supplied at 300 volume % or less of the volumetric flow rate of the swelling solvent, i.e., if the swelling solvent is present in the swelling zone 100 in an amount three times or more than the shrinking solvent, the additive dissolution function of the swelling solvent due to the polymer swelling may be reduced. Meanwhile, in consideration of the function of the shrinking solvent in the shrinking zone 200 and the efficiency of removing additives from the polymer thereby, the volumetric flow rate of the shrinking solvent needs to be maintained at a predetermined level or more. Therefore, if the flow rate ratio of the volumetric flow rate of the shrinking solvent to the volumetric flow rate of the swelling solvent is less than 30 volume %, the polymer shrinking function in the shrinking zone may not be smoothly realized due to insufficient supply of the shrinking solvent.
[0059] Meanwhile, the polymer swollen by the swelling solvent may be transferred to the shrink zone 200 in the barrel 10. The swollen polymer in the shrink zone 200 may come into contact with the shrink solvent. Specifically, the polymer transferred from the swelling zone 100 to the shrink zone 200 is impregnated with the swelling solvent in which the additive is dissolved, and if the swollen polymer is dried without removing the swelling solvent from the swollen polymer, the dissolved plasticizer remains in the regenerated polymer, and the efficiency of removing the plasticizer may decrease. Therefore, it is important to remove the swelling solvent from the swollen polymer. According to the present invention, the swollen polymer is shrunk by a chemical means using a shrink solvent, thereby minimizing the content of the solvent and the content of the plasticizer present in the swollen polymer.
[0060] The shrinking solvent is preferably a solvent that swells the polymer to a low degree, unlike the swelling solvent, and when the additive is a phthalate-based plasticizer, it is preferably a solvent that dissolves the phthalate-based plasticizer to a high degree. From this perspective, when the additive is a phthalate-based plasticizer, the shrinking solvent may be one or more of ethyl alcohol, toluene, cyclohexanol, isopropyl alcohol, benzene, cyclohexane, 1-pentanol, 1-butanol, 1-propanol, hexane, and diethyl ether, and may be isopropyl alcohol. Such a shrinking solvent can efficiently shrink the swollen polymer, and also has an excellent degree of dissolving the phthalate-based plasticizer, and can easily remove the plasticizer present inside the polymer to the outside of the polymer when the swollen polymer shrinks.
[0061] In order to facilitate the shrinkage of the polymer swollen by the shrinking solvent in the shrinking zone 200 and the smooth removal of the swelling solvent (and additives contained therein) from the swollen polymer, the supply flow rate of the shrinking solvent supplied through the shrinking solvent inlet 50 may be determined based on the supply flow rate of the polymer and the bulk density of the supplied polymer. Specifically, the following general formula 4 may be satisfied.
[0062] [General formula 4] Feed flow rate of the polymer (g / min) / bulk density of the polymer (g / cm 3 )*0.25≦Flow rate of shrink solvent (cm 3 / min) ≦ Supply flow rate of supplied polymer (g / min) / Bulk density of supplied polymer (g / cm 3 )*5
[0063] The residence time of the polymer in the shrinkage zone 200 may be 0.5 to 10 minutes. If the residence time of the polymer in the shrinkage zone 200 is short, such as less than 0.5 minutes, the shrinking solvent cannot penetrate deep enough into the polymer, so that the shrinkage of the swollen polymer becomes difficult and the efficiency of removing additives may decrease. If the residence time of the polymer in the shrinkage zone 200 is 10 minutes or more, the residence time becomes longer than necessary, which is not economical in terms of the amount of solvent used and the size of the apparatus.
[0064] According to an embodiment of the present invention, the shrinkable polymer that has passed through the shrink zone 200 may be discharged to the outside of the additive removal apparatus 1 through the polymer outlet 30. The discharged polymer may be subjected to a drying process to remove the swelling solvent and shrinkable solvent remaining in the polymer. The dryer in which the drying process is performed may be, for example, a paddle dryer, a floating bed dryer, a vacuum dryer, or a devolatilizing extruder.
[0065] Meanwhile, according to an embodiment of the present invention, the swelling solvent and the shrinking solvent may be discharged through a solvent discharge unit 60 .
[0066] The solvent discharge unit 60 may be coupled to the barrel 10 at one end of the barrel 10, and may include a solvent outlet. The solvent discharge unit 60 may be detachable from the one end of the barrel 10 for cleaning the inside of the barrel 10, etc.
[0067] The solvent discharged through the solvent discharge unit 60 may include a swelling solvent, a shrinking solvent, and additives dissolved therein. Therefore, a purification process for separating the swelling solvent, the shrinking solvent, and the additives from the discharged solvent may be performed, and the solvent and the additives may be reused.
[0068] The present invention will be described in more detail with reference to the following examples. However, the following examples are merely for the purpose of illustrating the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of the present invention, and the scope of the present invention is not limited to these examples.
[0069] Examples and Example 1 First, an additive removal apparatus 1 as shown in Fig. 1 was prepared. Specifically, the additive removal apparatus included a barrel 10 having an inner diameter of 6 cm with a polymer inlet 20 on one side and a polymer outlet 30 on the other side, a motor 80 was installed at the other end of the barrel, and a screw 70 connected to the motor was installed inside the barrel. The additive removal apparatus included a swelling solvent inlet 40 and a shrinking solvent inlet 50 between the polymer inlet and the polymer outlet. Here, the ratio x / y of the distance x from the polymer inlet to the swelling solvent inlet and the distance y from the swelling solvent inlet to the shrinking solvent inlet was 4.
[0070] The additive removal device was placed on a support table, and the inclination between the extension of the rotation axis of the screw and the ground was adjusted to 15 degrees.
[0071] Next, a polymer powder sample containing PVC recycled polymer (D50: 200 μm) containing 14.3 wt % of phthalate plasticizer was prepared, and methyl ethyl ketone (MEK) was prepared as a swelling solvent and isopropyl alcohol (IPA) was prepared as a shrinking solvent. Next, MEK was poured into the swelling solvent inlet 40 at a depth of 15.5 cm. 3 10.6 cm of IPA was injected into the shrink solvent inlet 50 at a volumetric flow rate of 10.6 cm / min (mass flow rate of 0.75 kg / hr).3 After confirming that the normal state had been reached by supplying the polymer powder sample at a volumetric flow rate of 4.2 g / min (=0.25 kg / hr) to the polymer inlet 20, the polymer powder sample was supplied to the polymer inlet 20 at a mass flow rate of 4.2 g / min (=0.25 kg / hr). Meanwhile, the screw rotation speed was set to 1 rpm so that the polymer powder sample passed through the swelling zone 100 and the shrinkage zone 200 in that order, and was discharged to the polymer outlet 30. Here, the residence time of the polymer in the swelling zone was 24 minutes, and the residence time in the shrinkage zone was 6 minutes.
[0072] 0.5g of the discharged PVC polymer was sampled from the polymer outlet 30 and subjected to gas chromatography-flame ionization detection analysis (GC-FID) to calculate the content of residual phthalate-based plasticizer in the sample. Here, the gas chromatography-flame ionization detection analysis (GC-FID) device used was an Agilent 7890A GC system. As a result, the content of residual plasticizer was 100ppm.
[0073] Example 2 In comparison with Example 1, 7.5 cm of MEK was added to the swelling solvent inlet 40. 3 2.7 cm of IPA was injected into the shrink solvent inlet 50 at a volumetric flow rate of 1.0 kg / min (mass flow rate of 0.375 kg / hr). 3 The plasticizer in the PVC polymer was removed using the same device and method as in Example 1, except that the plasticizer was supplied at a volumetric flow rate of 100 ml / min (0.125 kg / hr in terms of mass flow rate).
[0074] The residual plasticizer concentration of the discharged PVC polymer was measured in the same manner as in Example 1, and was found to be 250 ppm.
[0075] Comparative Example 1 In comparison with Example 1, no solvent was supplied to the swelling solvent inlet 40, and 25.9 cm of MEK, the swelling solvent, was supplied only to the shrinking solvent inlet 50. 3 The plasticizer in the PVC polymer was removed using the same apparatus and method as in Example 1, except that the polymer was supplied at a rate of 1.25 kg / hr / min (mass flow rate of 1.25 kg / hr) and the residence time of the polymer in the apparatus was set to 30 minutes.
[0076] The residual plasticizer concentration of the discharged PVC polymer was measured in the same manner as in Example 1, and was found to be 4,200 ppm.
[0077] Comparative Example 2 In comparison with Comparative Example 1, the shrinking solvent IPA was injected at 26.5 cm only into the shrinking solvent injection port 50. 3 The plasticizer in the PVC polymer was removed using the same device and method as in Comparative Example 1, except that the plasticizer was supplied at a rate of 1.25 kg / hr in mass flow rate.
[0078] The residual plasticizer concentration of the discharged PVC polymer was measured in the same manner as in Example 1, and was found to be 62,000 ppm.
[0079] Comparative Example 3 In comparison with Comparative Example 1, a mixed solvent obtained by mixing MEK as a swelling solvent and IPA as a shrinking solvent at a weight ratio of 1:1 was poured into the shrinking solvent inlet 50 at 26.0 cm 3 The plasticizer in the PVC polymer was removed using the same device and method as in Comparative Example 1, except that the plasticizer was supplied at a rate of 1.25 kg / hr in mass flow rate.
[0080] The residual plasticizer concentration of the discharged PVC polymer was measured in the same manner as in Example 1, and was found to be 1,400 ppm.
[0081] From the above results, it was possible to efficiently remove additives in a polymer in a continuous manner by utilizing the additive removal device of the present invention. With reference to Examples 1 and 2, it can be confirmed that a high additive removal efficiency can be achieved when a solvent for swelling a polymer and a solvent for shrinking the polymer are introduced into the swelling solvent inlet and shrinking solvent inlet of the additive removal device, respectively. On the other hand, when only one of the swelling solvent or shrinking solvent is used at the same flow rate (Comparative Examples 1 and 2) or when a mixture of the same solvents is used at the same flow rate, it is difficult to achieve a desired plasticizer removal efficiency (Comparative Example 3).
Claims
1. a barrel providing an interior space and having a polymer inlet on one side and a polymer outlet on the other side; A screw provided in the internal space of the barrel and rotating on its axis; a solvent discharge portion provided at the one end portion of the barrel, The barrel is located between the polymer inlet and the polymer outlet, and includes a swelling solvent inlet adjacent to the polymer inlet and a shrinking solvent inlet adjacent to the polymer outlet.
2. 2. The additive removing device according to claim 1, wherein the inclination between the extension of the rotation axis of the screw and the ground is 5 degrees to 30 degrees.
3. The other end of the barrel is provided with a torque supply device, 2. The additive removal device according to claim 1, wherein the screw includes a shaft that is connected to the torque supply device and rotates along its axis, and a plate that is fixed to an outer circumferential surface of the shaft and extends in a spiral shape along the length of the shaft.
4. 2. The additive removal apparatus according to claim 1, wherein the polymer introduced into the polymer inlet by the axial rotation of the screw is transported to the polymer outlet and discharged.
5. 2. The additive removal apparatus according to claim 1, wherein the internal space of the barrel is partitioned into a swelling zone from the polymer inlet to the swelling solvent inlet and a shrinking zone from the swelling solvent inlet to the shrinking solvent inlet.
6. 2. The additive removal device according to claim 1, wherein a ratio x / y of a distance x from the polymer inlet to the swelling solvent inlet and a distance y from the swelling solvent inlet to the shrinking solvent inlet is 0.1 to 60.
7. Providing an additive removal apparatus as claimed in claim 1; supplying a polymer containing an additive to the polymer inlet, and supplying a swelling solvent and a shrinking solvent to the swelling solvent inlet and the shrinking solvent inlet, respectively; transferring the supplied polymer to a polymer outlet by axial rotation of the screw; Swelling the polymer in a swelling zone from the polymer inlet to the swelling solvent inlet; and shrinking the polymer in a shrink zone from the swelling solvent inlet to the shrink solvent inlet.
8. The method for removing an additive according to claim 7, wherein the additive is one or more phthalate-based plasticizers selected from the group consisting of dioctyl phthalate (DOP), dibutyl phthalate (DBP), dioctyl terephthalate (DOTP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), di-(2-ethylhexyl) terephthalate (DEHTP), and butyl benzyl phthalate (BBP).
9. 8. The method for removing an additive according to claim 7, wherein the polymer is polyvinyl chloride (PVC).
10. The swelling solvent is one or more of cyclohexanone, cyclopentanone, N,N-dimethylacetamide, tetrahydrofuran, pyridine, 3-pentanone, 2-pentanone, dimethylformamide, methyl ethyl ketone, dichloromethane, 4-methylpentan-2-one, nitrobenzene, 1,4-dioxane, 1,1,2,2-tetrachloroethane, acetone, ethyl acetate, chloroform, and dimethyl sulfoxide. The method for removing an additive according to claim 7.
11. 8. The method for removing an additive according to claim 7, wherein the shrinking solvent is one or more of ethyl alcohol, toluene, cyclohexanol, isopropyl alcohol, benzene, cyclohexane, 1-pentanol, 1-butanol, 1-propanol, hexane, and diethyl ether.
12. The method for removing an additive according to claim 7, wherein the residence time of the polymer in the swelling zone and the average particle size (D50) of the polymer satisfy the following general formula 3. [General formula 3] Average particle size of polymer (mm) * 5 ≦ residence time in swelling zone (min) ≦ average particle size of polymer (mm) * 240
13. 8. The method for removing an additive according to claim 7, wherein a flow rate ratio of a flow rate of the shrinking solvent supplied to the shrinking solvent inlet to a flow rate of the swelling solvent supplied to the swelling solvent inlet is 30% by volume to 300% by volume.
14. 8. The method of claim 7, wherein the residence time of the polymer in the shrinkage zone is from 0.5 minutes to 10 minutes.
15. The method for removing an additive according to claim 7, wherein the supplied swelling solvent and shrinking solvent are transported to a solvent discharge section by gravity and discharged.
Citation Information
Patent Citations
Treatment for reclaiming waste polyvinyl chloride
JP1982038834A
Extractor
JP2006009033A
Treating apparatus for thermoplastic resin composition containing additive
JP2007146176A