Zn-Al-Mg alloy-plated steel material containing V, Ce, La, and Mn and its manufacturing method

A Zn-Al-Mg alloy plated steel with optimized Al, Mg, V, Ce, and Mn compositions and controlled manufacturing processes addresses the formability and corrosion resistance issues, achieving high corrosion resistance and formability suitable for home appliances and automobiles.

JP2024544668APending Publication Date: 2024-12-03PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024532884
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2022-08-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing Zn-Al-Mg alloy plated steel sheets face challenges in achieving high formability and corrosion resistance, particularly in applications requiring good stamping forming performance and bonding with high-strength steel substrates.

Method used

A Zn-Al-Mg alloy plated steel material with specific compositions of Al, Mg, V, Ce, and Mn, along with controlled manufacturing processes, including degreasing, continuous annealing, hot-dip plating, and rapid cooling, to optimize the plating layer's composition and bonding with the steel base material.

Benefits of technology

The resulting steel material exhibits high corrosion resistance, excellent formability, and good bonding with the steel base material, meeting requirements for applications in home appliances and automobiles, with improved resistance to red rust and excellent paint adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544668000001
    Figure 2024544668000001
  • Figure 2024544668000002
    Figure 2024544668000002
  • Figure 2024544668000003
    Figure 2024544668000003
Patent Text Reader

Abstract

The present invention relates to a Zn-Al-Mg alloy-plated steel material containing V, Ce, La, and Mn and a manufacturing method thereof, which belongs to the technical field of steel metallurgy production. The Zn-Al-Mg alloy-plated steel material containing V, Ce, La, and Mn of the present invention has a plating layer with chemical compositions, in mass%, of Al: 0.5-5%, Mg: 0.5-3.0%, V: 0.05-1%, Ce: 0.01-0.50%, La: 0.01%-0.30%, Mn: 0.025%-1.0%, and the balance: Zn and unavoidable impurities, in which Al / Mg is 1.0-1.5, and the total amount of V+Ce+La is 0.03-1.0%. The Zn-Al-Mg alloy-plated steel material of the present invention not only meets the user's requirements for high corrosion resistance of steel materials, but also meets the requirements for excellent stamping forming performance or high strength steel, and is particularly applicable to the fields of home appliances and automobiles, and is expected to be well applied and popularized.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Zn-Al-Mg alloy-plated steel material containing V, Ce, La and Mn and a manufacturing method thereof, which belongs to the technical field of steel metallurgy production. [Background technology]

[0002] Zn-Al-Mg alloy plating attracted wide attention overseas in the 1980s and became an important research subject in the specialized field of hot-dip galvanizing and zinc alloy plating. Research results by domestic and foreign peers have shown that when the Zn and Al contents in the plating layer are the same, hot-dip Zn-Al-Mg alloy-plated steel sheets with added Mg have better corrosion resistance and better material processing and application performance (formability, weldability and paintability), which may replace the conventional hot-dip galvanized steel sheets or zinc alloy-plated steel sheets, and a wide range of market demand is expected.

[0003] Hot-dip Zn-Al-Mg alloy-plated steel sheets were industrialized and applied by steel companies such as Nippon Steel Corporation, Nisshin Steel Corporation, and ThyssenKrupp Corporation in the 2000s, and are now mainly used in the construction industry, and are gradually entering home appliances, automobile manufacturing, and other industries. In China, research into Zn-Al-Mg alloy plating is relatively slow, and currently only manufacturers such as Baosteel, Shougang, Jiuquan iron and steel, and Pangang are selling hot-dip Zn-Al-Mg alloy-plated steel sheets.

[0004] Conventional hot-dip Zn-Al-Mg alloy-coated steel sheets can be divided into three types: "low aluminum" (WAl<5%), "medium aluminum" (5%≦WAl<13%), and "high aluminum" (47%≦WAl≦57%). Different types of Zn-Al-Mg alloy-coated steel sheets have different Al and Mg contents in the coating layer, so there are differences in the structure and quality performance of the coating layer, and their application fields are also different.

[0005] Patent Document 1 discloses a highly corrosion-resistant single-bath Zn-Al-Mg rare earth protective plating layer and its manufacturing method, which uses a single-bath hot-dip plating method to form a Zn-Al-Mg alloy plating layer on a metal surface. The plating layer and the metal substrate each maintain their original properties, and have a metallurgical bonding interface of 99.9% or more. The plating layer has a dense structure, stable composition, zero leakage plating, and excellent corrosion resistance, and can resist salt spray corrosion for up to 2060 hours. The corrosion resistance of the alloy plating layer is better than that of ordinary hot-dip pure zinc plating layers, and the service life is improved. This single-bath plating method is recyclable and industrializable, and overcomes the shortcomings of the difficulty of plating between metal and Zn-Al-Mg alloy plating solution, the difficulty of forming a good bonding interface between the two, and the tendency of leakage plating, so it can be widely used to produce a co-penetrating layer on metal surface with Zn-Al-Mg alloy plating solution containing 5%-12% Al and 1%-6% Mg, which forms a ternary eutectic of Zn / Al / MgZn2 and various binary eutectics, which are the main reasons for its high corrosion resistance. The above-mentioned high corrosion-resistant single-bath Zn-Al-Mg rare earth protective plating layer adopts a composition system of medium aluminum.

[0006] Patent Document 2 discloses a hot-dip plated steel sheet having high corrosion resistance and a manufacturing method thereof. The hot-dip plated steel sheet includes a substrate and an Al-Zn-Si-Mg plating layer formed on the substrate, and the chemical components of the plating layer are, in mass%, Al: 45% to 65%, Si: 0.1% to 3%, Mg: 0.2% to 5%, Mn: 0.001% to 0.15%, Cr: 0.001% to 0.5%, and the balance: Zn and unavoidable impurities. The manufacturing method thereof includes (1) pre-treating the steel sheet, (2) immersing the steel sheet in a plating solution tank at 560 to 595°C to perform hot-dip plating, and (3) removing the steel sheet from the plating solution and cooling it stepwise. The hot-dip plated steel sheet has excellent corrosion resistance and significantly suppresses the generation of white rust and the development of red rust, as well as the dispersion of coating layer destruction originating from cut portions. The hot-dip galvanized steel sheet having high corrosion resistance employs a high aluminum composition.

[0007] High corrosion resistance Zn-Al-Mg steel sheets are mainly composed of medium and high aluminum composition systems. As the Al and Mg content increases, the corrosion resistance of the coating layer improves, but the forming and welding performance decreases. In the fields of home appliances and automobiles, Zn-Al-Mg alloy-coated steel sheets must have good formability to meet the stamping forming performance requirements of users, but the current Zn-Al-Mg alloy-coated steel sheets with medium and high aluminum composition systems still cannot meet the requirements of users. In automotive steel materials, the higher the strength of high-strength steel, the more alloy elements in the steel substrate, which leads to poor infiltration of the coating solution and the steel substrate, which seriously affects the application of Zn, Al, and Mg in high-strength steel. Therefore, it is necessary to develop Zn-Al-Mg alloy-coated steel sheets with high formability and high corrosion resistance. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] China Patent Application Publication No. 105063532 [Patent Document 2] China Patent Publication No. 109402547 Summary of the Invention [Problem to be solved by the invention]

[0009] The technical problem to be solved by the present invention is to provide a Zn-Al-Mg alloy-plated steel material containing V, Ce, La and Mn, which has high formability and high corrosion resistance, and a method for producing the same. [Means for solving the problem]

[0010] In order to solve the above technical problems, the present invention employs the following technical means. A Zn-Al-Mg alloy plated steel material containing V, Ce, La, and Mn according to one embodiment of the present invention has a plating layer having chemical compositions, in mass%, of Al: 0.5-5%, Mg: 0.5-3.0%, V: 0.05-1%, Ce: 0.01-0.50%, La: 0.01%-0.30%, Mn: 0.025%-1.0%, other trace alloy elements: ≦0.3%, and the balance: Zn and unavoidable impurities, in which the Al / Mg ratio is 1.0-1.5 and the total amount of V+Ce+La is 0.3-1.0%.

[0011] Furthermore, the chemical composition of the plating layer satisfies at least one of the following conditions (1) to (3): (1) the plating layer contains 0.8-3.2% Al, 0.8-2.5% Mg, 0.05-0.40% V, 0.03-0.30% Ce, 0.02%-0.20% La, and 0.10%-1.0% Mn, (2) the Al / Mg ratio is 1.0-1.2, and (3) the total amount of V+Ce+La is 0.10-0.35%.

[0012] Furthermore, the total amount of the unavoidable impurities is 0.010% or less, of which Pb≦0.002%, Sb≦0.002%, Sn≦0.002%, As≦0.002%, Te≦0.002%, and Cd≦0.002%.

[0013] Furthermore, the weight of the plating layer on both sides is 30 to 400 g / m 2 and preferably, the weight of the plating layer is 150 to 320 g / m on both sides. 2 It is.

[0014] Furthermore, the steel substrate of the steel material is at least one selected from IF steel, low carbon aluminum quenching steel, bake hardening steel, QP steel, DP steel, TRIP steel, and TWIP steel.

[0015] The method for producing the Zn-Al-Mg alloy plated steel material includes a degreasing and cleaning step for the steel substrate, a continuous annealing step, a hot dip plating step, and an air knife purging step.

[0016] Furthermore, the H2 content in the furnace during the continuous annealing process is controlled to 3.5% or more by volume, and preferably, the H2 content in the furnace during the continuous annealing process is controlled to 4.0 to 8.0% by volume.

[0017] Furthermore, the temperature of the steel substrate when it enters the molten zinc pot is controlled to 420 to 520°C, the temperature of the plating solution during the hot-dip plating process is 410 to 520°C, and the temperature difference between the temperature of the steel substrate when it enters the molten zinc pot and the temperature of the plating solution is controlled to ±10°C.

[0018] Furthermore, after plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 260°C or less until it reaches the top turning roll, and preferably, after plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 200 to 260°C until it reaches the top turning roll. Effect of the Invention

[0019] The beneficial effects of the present invention are as follows: The Zn-Al-Mg alloy-plated steel of the present invention adopts a low aluminum composition system and controls the composition of the plating layer, thereby obtaining a Zn-Al-Mg alloy-plated steel sheet with high corrosion resistance and high formability. According to tests, the Zn-Al-Mg alloy-plated steel of the present invention has a time until red rust appears under neutral salt spray test conditions of 600 hours, even 3200 hours or more, no cracks are visible to the naked eye after 0T bending, and has a time until red rust appears on the bent part under neutral salt spray test conditions of 500 hours or more, even 3000 hours or more, and has excellent adhesion of the paint layer after painting. The Zn-Al-Mg alloy-plated steel is particularly applicable to the fields of home appliances and automobiles, and is expected to be well applied and popularized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention provides a Zn-Al-Mg alloy plated steel material containing V, Ce, La and Mn, the steel material having a plating layer having chemical compositions, in mass%, of Al: 0-5%, Mg: 0.5-3.0%, V: 0.05-1%, Ce: 0.01-0.50%, La: 0.01%-0.30%, Mn: 0.025%-1.0%, other trace alloy elements: ≦0.3%, and the balance: Zn and unavoidable impurities, in which Al / Mg is 1.0-1.5, the total amount of V+Ce+La is 0.3-1.0%, and the other trace alloy elements are at least one selected from B, Si, Ti, Ca, Mn, Mo, Cr, Nb, Yt and Bi.

[0021] Currently, in this field, medium to high aluminum composition systems are mainly adopted to ensure the corrosion resistance of Zn-Al-Mg alloy plated steel, but as the Al and Mg contents increase, the forming and welding performance of the steel material is significantly reduced, making it difficult to meet the requirements for stamping forming performance in home appliances, automobiles and other fields. In view of the above problems, the present invention optimizes the Mg and Al contents (contents) in the plating layer and adds other alloying elements to achieve various effects as follows: V causes heterogeneous nucleation during the formation of the plating layer to refine the grain size of the plating layer, thereby improving the ductility of the plating layer and improving the corrosion resistance of the plating layer. Ce and La increase the fluidity of the plating solution, reduce the surface tension of the plating solution, increase the infiltration of the plating solution into the steel substrate, and improve the bonding effect between the plating layer and the steel substrate. Mn strengthens the bonding effect between the plating layer and the steel base material (especially high-strength steel containing Mn) and can form Mn-rich intermetallic compounds, which allows the plating layer to have excellent plasticity and toughness and facilitate subsequent processing, thereby meeting the users' requirements for high corrosion resistance and high formability. However, if the content of V, Ce, La, and Mn is too high, an oxide film is formed on the surface of the alloy plating solution, which increases zinc slag and affects the surface quality of the plating layer.

[0022] In the manufacturing process of the coating layer, the process needs to be limited to ensure that the coating layer has good surface quality and performance. The thickness of the coating layer needs to be controlled within a certain range, taking into account the strength of the air knife jet and the fluidity of the coating solution. If the weight of the coating layer is too large and the pressure of the jet is small, the surface quality and thickness of the coating layer cannot be controlled, and if the flow rate of the jet is finite and the fluidity of the coating solution is constant, the thickness of the coating layer will be too thin. The wettability of the coating solution to the surface of different steel sheets is different, and only steel sheets with good wettability can form a coating layer with good adhesion. The annealing atmosphere is to improve the good reducibility of the steel substrate surface, and generally the higher the H2 content, the more appropriate it is, but the higher the H2 content, the higher the risk of explosion. The temperature of the coating solution needs to be such that the coating solution is in a molten state and has appropriate fluidity. The addition of V and Mn widens the temperature range of the coating solution, but if the temperature is too high, the amount of zinc oxide slag will increase. In order to ensure complete solidification of the coating layer, the temperature of the steel sheet needs to be reduced to below its freezing point before it reaches the first turning roll. Furthermore, zinc, aluminum and magnesium are easily oxidized, so rapid cooling can improve the surface quality.

[0023] The technical means of the present invention will be described below with reference to examples. Those skilled in the art will understand that the following examples are for illustrating the present invention and do not limit the scope of the present invention. If no specific techniques or conditions are shown in the examples, they will be in accordance with the techniques or conditions described in the literature in the field or the product specifications. If no manufacturer is shown, the reagents or equipment used are commercially available and common.

[0024] Example 1: Production of Zn-Al-Mg alloy-plated steel material according to the present invention The plating layer has a weight of 50g / m 2(Both sides) and the main components are, in mass%, Al: 0.8%, Mg: 0.6%, V: 0.10%, La: 0.05%, Ce: 0.15%, Mn: 0.20%, Pb: 0.002%, Sb: 0.001%, Cr: 0.001%, Cd: 0.001%, Sn: 0.001%, and the balance is Zn. The steel substrate is DP steel.

[0025] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip galvanizing process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel is rinsed and cleaned after the degreasing process. During the continuous annealing process, the H2 content in the furnace is controlled to 5.0% by volume. The temperature of the steel strip when it enters the molten zinc pot is 450°C, and during the hot dip galvanizing process, the temperature of the plating solution is maintained at 440°C. After plating, the steel strip is rapidly cooled so that the temperature of the strip is 260°C when it reaches the top turning roll.

[0026] (Test Method) Corrosion resistance: Neutral salt spray test is used to accelerate corrosion. The test conditions and methods are carried out in accordance with GB / T10125-2012 "Salt spray test of artificial atmosphere corrosion test". The test equipment is a salt spray corrosion test box, the corrosive medium is a deionized NaCl solution with a concentration of 50g / L and a pH value of 6.5, the test temperature is set at 35±2℃, the size of the test piece is 75mm×150mm×0.8mm, and the edges are sealed with 5mm of transparent tape to prevent edge corrosion from affecting the results. The test piece is placed at an angle of 15°~25° to the vertical. The time until red rust appears on the surface of the test piece is observed.

[0027] Formability: The test piece is bent at 0T (180° bend, the radius of the bend is 0), and the appearance of cracks is observed with the naked eye. In addition, the time until red rust appears on the bent part is observed under the neutral salt spray test conditions, and the neutral salt spray test conditions and methods are carried out in accordance with GB / T10125-2012 "Salt spray test for artificial atmosphere corrosion test".

[0028] Paintability: After oiling the plated steel sheet, it is degreased, washed, ceramic coated or phosphate treated, spray painted and dried. Then, the adhesion between the paint layer and the steel sheet is checked by a cross-cut test. If the paint layer does not fall off, it indicates good adhesion.

[0029] Test results: The Zn-Al-Mg alloy plated steel produced in this embodiment has good surface quality, excellent corrosion resistance, formability and paintability. The plated steel shows red rust appearance time of more than 70 hours under neutral salt spray test conditions, no obvious cracks are visible to the naked eye after 0T bending, and shows red rust appearance time of more than 600 hours under neutral salt spray test conditions. The coating layer has excellent adhesion after painting, which meets the requirements of users.

[0030] Example 2: Production of Zn-Al-Mg alloy plated steel material according to the present invention The plating layer weighs 150g / m 2 (Both sides) and the main components are, in mass%, Al: 1.5%, Mg: 1.5%, V: 0.15%, Ce: 0.10%, La: 0.10%, Mn: 0.15%, Pb: 0.001%, Sb: 0.002%, Cr: 0.001%, Cd: 0.001%, Sn: 0.001%, and the balance is Zn. The steel substrate is TWIP steel.

[0031] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip coating process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel is rinsed and cleaned after the degreasing process. During the continuous annealing process, the H2 content in the furnace is kept at 6.0% by volume. The temperature of the steel strip when it enters the molten zinc pot is 470°C, and during the hot dip coating process, the temperature of the coating solution is kept at 460°C. After coating, the steel strip is rapidly cooled so that the temperature of the strip reaches 200°C when it reaches the top turning roll.

[0032] The test method was the same as in Example 1. Test results: The Zn-Al-Mg alloy plated steel produced in this embodiment has good surface quality, excellent corrosion resistance, formability and paintability. The plated steel shows red rust after more than 1800 hours under neutral salt spray test conditions, no obvious cracks are visible to the naked eye after 0T bending, and shows red rust after more than 1700 hours under neutral salt spray test conditions. The coating layer has excellent adhesion after painting, which meets the requirements of users.

[0033] Example 3: Production of Zn-Al-Mg alloy plated steel material according to the present invention The plating layer weighs 320g / m 2 (Both sides) and the main components are, in mass%, Al: 3.2%, Mg: 2.5%, V: 0.10%, La: 0.15%, Ce: 0.20%, Mn: 0.05%, Pb: 0.002%, Sb: 0.001%, Cr: 0.001%, Cd: 0.002%, Sn: 0.002%, and the balance is Zn. The steel substrate is QP steel.

[0034] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip coating process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel is rinsed and cleaned after the degreasing process. During the continuous annealing process, the H2 content in the furnace is kept at 4.5% by volume. The temperature of the steel strip when it enters the molten zinc pot is 510°C, and during the hot dip coating process, the temperature of the coating solution is kept at 500°C. After coating, the steel strip is rapidly cooled so that the temperature of the strip is 200°C when it reaches the top turning roll.

[0035] The test method was the same as in Example 1. Test results: The Zn-Al-Mg alloy plated steel produced in this embodiment has good surface quality, excellent corrosion resistance, formability and paintability. The plated steel shows red rust after 3200 hours or more under neutral salt spray test conditions, no obvious cracks are visible to the naked eye after 0T bending, and shows red rust after 3000 hours or more under neutral salt spray test conditions. The coating layer has excellent adhesion after painting, which meets the requirements of users.

[0036] Comparative Example The plating layer weighs 180g / m 2 (Both sides) and the main components are, in mass%, Al: 1.6%, Mg: 1.6%, Pb: 0.001%, Sb: 0.001%, Cr: 0.001%, Cd: 0.001%, Sn: 0.001%, and the balance is Zn. The steel substrate is QP steel.

[0037] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip coating process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel is rinsed and cleaned after the degreasing process. During the continuous annealing process, the H2 content in the furnace is controlled to 3.5% by volume. The temperature of the steel strip when it enters the molten zinc pot is 470°C, and the temperature of the coating solution is maintained at 470°C during the hot dip coating process. After coating, the steel strip is rapidly cooled so that the temperature of the strip reaches 300°C when it reaches the top turning roll.

[0038] The test method was the same as in Example 1. Test results: The surface quality of the Zn-Al-Mg alloy plated steel produced in this comparative example is inferior to that of the present invention, with bright spot defects, and the corrosion resistance, formability and paintability are also somewhat poor. The plated steel takes more than 1400 hours to develop red rust under neutral salt spray testing conditions, has slight cracks visible to the naked eye after 0T bending, and takes more than 1100 hours to develop red rust on the bent part under neutral salt spray testing conditions.

[0039] It is to be understood that the particular features, structures, materials, or configurations described herein may be combined in any suitable manner in any one or more embodiments, and that the various features of the different embodiments and embodiments described herein may be combined with each other, unless mutually inconsistent, as would be understood by one of ordinary skill in the art.

[0040] (Additional Note) (Appendix 1) A plating layer having chemical compositions in mass % of Al: 0.5-5%, Mg: 0.5-3.0%, V: 0.05-1%, Ce: 0.01-0.50%, La: 0.01%-0.30%, Mn: 0.025%-1.0%, other trace alloy elements: ≦0.3%, and the balance: Zn and unavoidable impurities, in which Al / Mg is 1.0-1.5 and the total amount of V+Ce+La is 0.3-1.0%. Zn-Al-Mg alloy plated steel material containing V, Ce, La, and Mn.

[0041] (Appendix 2) The chemical composition of the plating layer is The plating layer contains Al: 0.8-3.2%, Mg: 0.8-2.5%, V: 0.05-0.40%, Ce: 0.03-0.30%, La: 0.02%-0.20%, and Mn: 0.10%-1.0%. Al / Mg is 1.0 to 1.2, and The total amount of V+Ce+La is 0.10% to 0.35%. 2. The Zn-Al-Mg alloy plated steel material according to claim 1,

[0042] (Appendix 3) The total content of the unavoidable impurities is 0.010% or less, of which Pb≦0.002%, Sb≦0.002%, Sn≦0.002%, As≦0.002%, Te≦0.002%, Cd≦0.002%; 2. The Zn-Al-Mg alloy plated steel material according to claim 1,

[0043] (Appendix 4) The weight of the plating layer on both sides is 30 to 400 g / m 2 and preferably, the weight of the plating layer is 150 to 320 g / m on both sides. 2 That is, 2. The Zn-Al-Mg alloy plated steel material according to claim 1,

[0044] (Appendix 5) The steel substrate of the steel material is at least one selected from IF steel, low carbon aluminum quenching steel, bake hardening steel, QP steel, DP steel, TRIP steel and TWIP steel; 2. The Zn-Al-Mg alloy plated steel material according to claim 1,

[0045] (Appendix 6) The process includes degreasing and cleaning of steel substrates, continuous annealing, hot-dip plating, and air knife purging. 6. A method for producing a Zn-Al-Mg alloy-plated steel material containing V, Ce, La and Mn according to any one of claims 1 to 5.

[0046] (Appendix 7) During the continuous annealing process, the H content in the furnace is controlled to 3.5% by volume or more, and preferably, during the continuous annealing process, the H content in the furnace is controlled to 4.0 to 8.0% by volume. The manufacturing method according to claim 6,

[0047] (Appendix 8) The temperature of the steel substrate when entering the molten zinc pot is controlled to 420 to 520°C, the temperature of the plating solution during the hot-dip coating process is 410 to 520°C, and the temperature difference between the temperature of the steel substrate when entering the molten zinc pot and the temperature of the plating solution is controlled to ±10°C. The manufacturing method according to claim 6,

[0048] (Appendix 9) After plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 260°C or less until it reaches the top turning roll, and preferably, after plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 200-260°C until it reaches the top turning roll. The manufacturing method according to claim 6,

[0049] (Appendix 10) A Zn-Al-Mg alloy-plated steel material obtained by the manufacturing method according to any one of claims 6 to 9.

Claims

1. A plating layer having chemical compositions, in mass %, of Al: 0.5-5%, Mg: 0.5-3.0%, V: 0.05-1%, Ce: 0.01-0.50%, La: 0.01%-0.30%, Mn: 0.025%-1.0%, other trace alloy elements: ≦0.3%, and the balance: Zn and unavoidable impurities, wherein Al / Mg is 1.0-1.5 and the total amount of V+Ce+La is 0.3-1.0%. The present invention relates to a Zn-Al-Mg alloy plated steel material containing V, Ce, La and Mn.

2. The chemical composition of the plating layer is The plating layer contains Al: 0.8 to 3.2%, Mg: 0.8 to 2.5%, V: 0.05 to 0.40%, Ce: 0.03 to 0.30%, La: 0.02% to 0.20%, and Mn: 0.10% to 1.0%. Al / Mg is 1.0 to 1.2; and The total amount of V+Ce+La is 0.10 to 0.35%.

2. The Zn-Al-Mg alloy plated steel material according to claim 1.

3. The total amount of the unavoidable impurities is 0.010% or less, in which Pb≦0.002%, Sb≦0.002%, Sn≦0.002%, As≦0.002%, Te≦0.002%, and Cd≦0.002%; 2. The Zn-Al-Mg alloy plated steel material according to claim 1.

4. The weight of the plating layer on both sides is 30 to 400 g / m 2 and preferably, the weight of the plating layer is 150 to 320 g / m on both sides. 2 That is, 2. The Zn-Al-Mg alloy plated steel material according to claim 1.

5. The steel substrate of the steel material is at least one selected from IF steel, low carbon aluminum quenching steel, bake hardening steel, QP steel, DP steel, TRIP steel and TWIP steel; 2. The Zn-Al-Mg alloy plated steel material according to claim 1.

6. The process includes degreasing and cleaning of steel substrates, continuous annealing, hot-dip plating, and air knife purging.

6. A method for producing a Zn-Al-Mg alloy-plated steel material containing V, Ce, La, and Mn according to claim 1.

7. During the continuous annealing process, H in the furnace 2 The content is controlled to 3.5% by volume or more, and preferably, H in the furnace during the continuous annealing process is 2 The content is controlled to 4.0 to 8.0% by volume. The method according to claim 6 .

8. The temperature of the steel substrate when entering the molten zinc pot is controlled to 420 to 520°C, the temperature of the plating solution during the hot-dip coating process is 410 to 520°C, and the temperature difference between the temperature of the steel substrate when entering the molten zinc pot and the temperature of the plating solution is controlled to ±10°C. The method according to claim 6 .

9. After plating, the strip is cooled rapidly so that the temperature of the strip is below 260°C until it reaches the top turning roll, and preferably after plating, the strip is cooled rapidly so that the temperature of the strip is between 200 and 260°C until it reaches the top turning roll. The method according to claim 6 .

10. A Zn-Al-Mg alloy plated steel material obtained by the manufacturing method according to any one of claims 6 to 9.

Citation Information

Patent Citations

  • Zinc-magnesium clad steel plate for hot stamping forming and manufacturing and hot stamping methods thereof

    CN108913950A

  • Hot-dip galvanized aluminum-magnesium alloy coated steel plate for ultra-deep drawing and preparation method thereof

    CN112575276A

  • Hot dip zn-al-mg based alloy plated steel having excellent corrosion resistance

    JP2002332555A

  • High strength hot dip galvanized steel sheet having excellent plating adhesion on high working and excellent ductility, and production method therefor

    JP2003055751A

  • Highly corrosion-resistant hot dip galvanized steel

    JP2009256703A