Reinforced Polyamide
By blending polyamide with organic amines and POE-g-MAH, the reinforced nylon compositions achieve enhanced impact strength and flowability, addressing the limitations of existing technologies and enabling the production of lightweight, high-performance parts.
Patent Information
- Application Number
- JP2024527626
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-15
- Publication Date
- 2024-12-05
AI Technical Summary
Existing reinforced nylon compositions face challenges in achieving a balance between improved impact strength, particularly at low temperatures, and maintaining good flow properties, which limits their application in industries such as automotive and electronics.
Incorporating a specific organic amine with a functionality of less than 4 into a blend of polyamide and a maleic anhydride-grafted polyolefin elastomer (POE-g-MAH) to form dynamic bonds, reducing irreversible cross-linking and enhancing compatibility, thereby improving both impact strength and flowability.
The reinforced polyamide compositions exhibit a significant increase in room temperature impact strength, up to 70%, and a reduction in capillary viscosity, enhancing the flowability by up to 40%, allowing for the production of lightweight and thinner parts with superior mechanical properties.
Smart Images

Figure 2024544940000001 
Figure 2024544940000002 
Figure 2024544940000003
Abstract
Description
[Technical field]
[0001] The present invention relates to reinforced polyamide compositions, more particularly, the present invention relates to reinforced polyamide compositions comprising a blend of a polyamide, an impact modifier, and an organic amine that imparts improved room temperature impact strength and flow properties to the reinforced polyamide composition. [Background technology]
[0002] Nylon is a generic name for a family of synthetic thermoplastic polymers composed of polyamides. Polyamides (PA) are repeating units linked by amide bonds. Nylon is a well-known synthetic thermoplastic polymer based on aliphatic or semi-aromatic polyamides in which at least 85% by weight of the amide linkages (-CO-NH-) are directly bonded to two aliphatic groups.
[0003] Synthetic processed nylon (or PA) is a plastic with excellent mechanical properties, solvent resistance, abrasion resistance, etc., and nylon materials can be melt processed into various fibers, films, or shapes to form articles / products and parts for use in various applications. For example, reinforced nylon composites can be used in applications such as automotive applications, industrial machinery applications, consumer applications, and electronic applications. However, nylon has low notched impact strength, and in particular, nylon exhibits the disadvantage of low toughness in low temperature environments, which limits the further use of nylon in industry. Therefore, the industry is constantly seeking ways to make the impact strength performance of reinforced nylon better (increase or improve).
[0004] Typically, the impact strength performance (or impact resistance) of reinforced nylon is increased by adding an impact modifier or additive to the reinforced nylon. Adding impact modifier materials to reinforced nylon is one way to improve the impact resistance of reinforced nylon at both room temperature and below room temperature, especially in the automotive field.
[0005] To improve the impact resistance of nylon, impact modifiers are typically added to nylon to form reinforced nylon compositions, which are widely used by many industries for various application areas such as automobiles, industrial machinery, consumer products, and electronic products. The performance properties of reinforced nylon compositions, such as good impact strength and good flowability, are highly desired by the above industries. A good balance of these properties is particularly desirable for designing thin-walled and lightweight parts in electronic and automotive application areas. To manufacture thin parts from reinforced nylon compositions for use in the above applications, sufficient flowability of the reinforced nylon is required, and to enable lightweight design, efficient impact modifiers are required to be added to the reinforced nylon composition to improve the stiffness / toughness / flowability balance of the reinforced nylon composition. By reducing the thickness and weight of parts made from reinforced nylon, the cost of the system can also be reduced.
[0006] So far, the main impact modifier (IM) used in reinforced nylon (which is polar) has been maleic anhydride grafted polyolefin elastomer (which is non-polar). Typically, maleic anhydride (MAH) is grafted onto the backbone of polyolefin elastomer (POE) to enhance the compatibility between POE and nylon through the reaction between the anhydride groups grafted on POE and the amine end groups in nylon, as shown in the following general chemical reaction scheme (Scheme (I)):
number
[0007] Maleic anhydride grafted polyolefin (MAH grafted POE) elastomers provide the required good compatibility properties between non-polar polyolefins and highly polar nylons. However, the reaction causes irreversible imide bonds, which significantly reduces the flow properties of the resulting nylon / POE blend compositions.
[0008] To date, many efforts have been made to improve the impact strength of reinforced nylon, including, for example, optimizing the MAH graft ratio of IM, lowering the Tg of POE, and / or providing crosslinks in POE. Most of the efforts involve designing the MAH-grafted POE (also abbreviated as "POE-g-MAH") component, such as improving the MAH level grafted onto POE. However, the aforementioned industry efforts to optimize both the impact strength and flow performance of reinforced nylon compositions have met with limited success.
[0009] For example, Chinese Patent No. 110591100 refers to an ultra-low temperature resistant toughening agent (or impact modifier) used to increase the impact strength of nylon to form ultra-low temperature resistant and impact resistant nylon (or "reinforced nylon"). The impact modifier disclosed in the reference is characterized as comprising a polyolefin elastomer comprising a polyolefin elastomer backbone and a polar monomer side chain, the polar monomer side chain being bonded to an amino silicone oil. The nylon composition of the reference requires a high loading of silicone oil (25%-50% based on POE) to act as a plasticizer, and the amino group is functionalized to act as a linker to promote compatibility between the nylon and the impact modifier. Also, the reference makes no mention of the impact modifier of the reference improving the flowability of the reinforced nylon composition. Furthermore, the reference makes no specific mention of the use of diamines or triamines, and monoamines have been found not to work to provide reinforced nylon, and data indicates that tetramines do not work either.
[0010] US Patent Application Publication No. 20060205880(A1) refers to the use of organic acids to provide high flow POE (or ionomer reinforced polyamide). The acid loading is up to 10% and the toughener has a tensile modulus in the range of 5 psi to 20,000 psi. The reference discloses the use of organic acids, known to those skilled in the art, to cut the PA molecular weight and improve the flow of the PA. However, the reference does not disclose the use of organic amines with a functionality of less than 4 to improve the impact strength of nylon compositions.
[0011] China Patent Publication No. 11174796(A) refers to a nylon composite material with improved heat resistance, which comprises polyamide, mineral, glass fiber, hyperbranched polyamide and a silane coupling agent. Although the aminosilane disclosed in the above reference provides amino groups to the nylon composite material, the aminosilane is used for filler surface modification, and no benefit to the flowability or impact strength properties of the nylon composite material is disclosed, i.e., the aminosilane in the above reference does not act to improve the flowability and impact strength of the nylon composite material.
[0012] WO2005054368(A1) mentions using organic acids to improve the flowability of reinforced polyamides (nylons) and combining inorganic and organic stabilizers to maintain good heat and UV stability. The above references describe the synergy of MAH-grafted POE+organic acid+stabilizers to balance flowability and durability. However, WO2005054368(A1) does not disclose the improvement of impact strength. It disclosed the synergy of MAH-grafted POE+organic acid+stabilizers to balance flowability and durability. However, there is no improvement in impact strength.
[0013] China Patent Application Publication No. 110580971(A) and No. 110437612(A) refer to a cladding insulation material for the outer layer of winding wire, which is a nylon composite material containing hindered amine as an antioxidant. However, hindered amine has low reactivity and cannot act as a surface reversible crosslinking agent, so it cannot improve the flowability and impact strength performance of the nylon composite material.
[0014] China Patent Publication No. 109722020 refers to nylon composites and the use of amino-functionalized polyolefin elastomers as toughening agents. The above reference does not describe improving the impact strength and / or flow of nylon composites.
[0015] An article entitled "Effect of glass fiber surface chemistry on the mechanical properties of glass fiber reinforced, rubber-toughened nylon 6" in Polymer, Volume 43, Issue 17, Pages 4673-4687, mentions different types of functionalized silanes, such as aminosilanes, and the effect of aminosilanes when used as surface treatments on glass fibers used in reinforced nylon 6. Aminosilanes are used in nylon 6 as crosslinking agents, but aminosilanes do not help improve the flow or impact strength of nylon 6.
[0016] In view of the limitations of known reinforced nylon compositions with respect to impact strength and flowability, it would be desirable to further improve the impact strength of reinforced nylon, especially at low temperatures such as below -30°C, without adversely affecting other properties of the reinforced nylon, such as the flowability of the reinforced nylon, and without significantly increasing the production cost of the reinforced nylon.
[0017] It would also be desirable to provide new reinforced nylon compounds, materials or compositions that have both increased toughness and flow properties, or at least find an advantageous balance of the two properties by blending the appropriate ingredients to form an improved reinforced nylon composition, such as (1) a polyamide (nylon compound, polymer, material or composition), (2) an efficient impact modifier, and (3) an organic amine. Summary of the Invention
[0018] In a broad embodiment, the present invention relates to a reinforced polyamide composition comprising a blend of (A) at least one polyamide (e.g., a nylon compound), (B) at least one impact modifier, and (C) at least one specific organic amine such that the flow and impact strength properties of the reinforced polyamide composition are improved. In a preferred embodiment, the organic amine used in the reinforced polyamide composition of the present invention has a functionality of less than 4. In another embodiment, the organic amine is used as an additive in combination with an MAH-grafted POE toughening agent, and such combination, when added to a polyamide, surprisingly forms a reinforced polyamide composition having improved flow and impact strength properties.
[0019] In another embodiment, the reinforced polyamide composition of the present invention comprises component (A), which is at least one polyamide having a concentration of 50% to 98.99% by weight, component (B), which is at least one impact modifier composition having a concentration of 1% to 50% by weight, and component (C), which is at least one organic amine having a concentration of 0.01% to 10% by weight.
[0020] In yet another embodiment, the present invention comprises a method for preparing the above reinforced polyamide composition exhibiting high flow and toughness.
[0021] In yet another embodiment, the process for preparing the reinforced polyamide composition of the present invention comprises a melt mixing step carried out in at least a twin screw extruder.
[0022] In yet another embodiment, the present invention includes articles made using the reinforced polyamide composition described above.
[0023] In one or more embodiments, the above-described reinforced polyamide compositions and methods for making articles of the present invention include extrusion and / or injection molding processes.
[0024] Additional features and advantages of embodiments of the invention are set forth in the detailed description that follows, and in part will be readily apparent to those skilled in the art from the description, or may be learned by practicing the embodiments described herein, including the detailed description and claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Temperatures used herein are in degrees Celsius (°C).
[0026] "Room temperature (RT)" and / or "ambient temperature" herein means a temperature between 20°C and 26°C, unless otherwise specified.
[0027] An "elastomer" is a polymer that has viscoelastic properties (i.e., both viscous and elastic), weak intermolecular forces, generally a low Young's modulus, and a high strain at break compared to other materials. The IUPAC (International Union of Pure and Applied Chemistry) defines the term "elastomer" as "a polymer exhibiting rubber-like elasticity."
[0028] A "polymer" is a polymeric compound prepared by polymerizing monomers of the same or different types. Thus, the generic term polymer encompasses the terms "homopolymer" (used to refer to a polymer prepared from only one type of monomer, with the understanding that trace amounts of impurities may be incorporated into the polymer structure), and "interpolymer", which includes copolymers (used to refer to a polymer prepared from two different types of monomers), terpolymers (used to refer to a polymer prepared from three different types of monomers), and polymers prepared from more than three different types of monomers. Trace amounts of impurities, such as catalyst residues, may be incorporated in and / or within the polymer. It also encompasses all forms of copolymers, such as random, block, etc. Although polymers are often referred to as "made with" one or more specific monomers, "based on" a specific monomer or type of monomer, "containing" a specific monomer content, etc., it should be noted that in this context, the term "monomer" is understood to refer to the polymerized residue of a specific monomer, and not to the non-polymerized species. Generally, polymers are referred to herein in terms of "units" which are the polymerized form of the corresponding monomers.
[0029] The term "composition" refers to a mixture of materials that make up the composition, as well as reaction products and decomposition products formed from the materials of the composition.
[0030] By "nylon polymer composition" herein is meant a combination, mixture, or blend of at least one pure nylon polymer with at least one other distinct component, such as an elastomer, glass fiber, small molecule additive, or the like.
[0031] "Impact modifiers" herein are additives that are added to various plastic resins to increase the flexibility, toughness, and impact strength of the plastic resins to meet the physical property requirements of rigid parts made from such plastic resins.
[0032] As used herein, the terms "impact toughness," "impact strength," and "impact resistance" with respect to nylon compositions refer to the performance property of impact strength of a nylon composition as evaluated by the impact method set forth in CHARPY, ISO 179. The above terms may be used interchangeably.
[0033] "Room temperature impact strength" in reference to a nylon composition herein means the impact strength value of the nylon composition tested under room temperature conditions.
[0034] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether or not they are specifically disclosed herein. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or not, unless specifically stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any succeeding description any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not expressly delineated or listed. The term "or" refers to the listed members individually and in any combination, unless otherwise specified. The use of the singular includes the use of the plural, and vice versa.
[0035] Numerical ranges disclosed herein include all values between the lower limit and the upper limit (inclusive). Ranges containing explicit values (e.g., ranges 1, or 2, or 3-5, or 6, or 7) include any subranges between any two explicit values (e.g., the range 1-7 above includes the subranges 1-2, 2-6, 5-7, 3-7, 5-6, etc.).
[0036] As used throughout this specification, the following abbreviations have the following meanings, unless the context clearly dictates otherwise: "=" means "equal to" or "equal to", "<" means "less than", ">" means "greater than", "≦" means "less than or equal to", "≧" means "greater than or equal to", "@" means "at", μm = microns, g = gram, mg = milligram, mW / m K = meter, milliwatts per degree Kelvin, kJ / m 2 = kilojoules per square metre, L = liter, mL = milliliter, g / mL = grams per milliliter, g / L = grams per liter, g / 10min = grams per 10 minutes, kg / m 3 = kilograms per cubic meter, ppm = parts per million by weight, pbw = parts by weight, rpm = revolutions per minute, m = meters, mm = millimeters, cm = centimeters, μm = micrometers, min = minutes, s = seconds, ms = milliseconds, hr = hours, Pa = pascals, MPa = megapascals, Pa·s = pascal seconds, mPa·s = millipascal seconds, g / mol = grams per mole, g / eq = grams per equivalent, mg KOH / g = milligrams of potassium hydroxide per gram, Mn = number average molecular weight, Mw = weight average molecular weight, pts = parts by weight, 1 / s or second -1 = reciprocal of seconds [s -1 ], °C = degrees Celsius, mmHg = millimeters of mercury, psig = pounds per square inch, kPa = kilopascals, % = percent, vol% = volume percent, mol% = mole percent, and wt% = weight percent.
[0037] Unless otherwise specified, all percentages, parts, ratios, and other amounts are defined by weight. For example, all percentages set forth herein are weight percentages (wt %) unless otherwise indicated.
[0038] Specific embodiments of the present invention are described herein below. These embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the inventive subject matter to those skilled in the art.
[0039] In general, the present invention comprises reinforced polyamide (e.g., nylon) blends or compositions useful for producing nylon articles / products or parts for a variety of applications, particularly those applications requiring the nylon composition to have increased impact strength and flow properties.
[0040] In a broad embodiment, the reinforced polyamide composition comprises a combination, mixture, or blend of (A) at least one polyamide, such as nylon, (B) at least one impact modifier, and (C) at least one organic amine compound. To increase or improve the flow and impact strength properties of the reinforced polyamide composition, the reinforced polyamide composition is prepared, for example, by mixing (A) at least one polyamide, (B) at least one impact modifier, and (C) at least one organic amine compound in predetermined concentrations under predetermined conditions, such as melt blending temperatures using extrusion techniques.
[0041] For example, in one preferred embodiment, the reinforced polyamide composition may comprise a blend of 50% to 98.99% by weight of at least one polyamide, component (A), 1% to 50% by weight of at least one impact modifier composition, component (B), and 0.01% to 10% by weight of at least one organic amine, component (C). The nylon composition of the present invention may further comprise (D) one or more other optional compounds, if desired.
[0042] In the present invention, it has been discovered that the impact strength of reinforced nylon composites can be significantly improved by blending predetermined amounts of specific organic amines, impact modifier products (e.g., POE-g-MAH), and reinforced nylon.
[0043] It is hypothesized that the presence of certain organic amines in the above blend composition increases the dynamic bond between POE and nylon. For example, when certain organic amines combine with impact modifier products such as POE-g-MAH, the MAH in the POE is replaced with amide and / or acid chemicals, and due to this replacement, the dynamic bond between POE and nylon is increased. In addition, the dynamic bond formed can significantly improve the flowability of the reinforced nylon compound while maintaining good compatibility between nylon and POE. It is theorized that by adding organic amines to the nylon blend composition, the additive reacts with the anhydride groups in the POE-g-MAH to form amide, acid, or salt chemicals. Some embodiments of the general chemical reaction scheme of the additive reacting with MAH to form dynamic bonds with nylon are shown in the following general chemical reaction schemes, schemes (II), (III), and (IV).
number
number
number
[0044] After any of the above reaction schemes (II), (III) and (IV), the MAH groups in the POE are consumed, thus preventing irreversible crosslinking between the MAH and the amine groups in the nylon. However, the amide, acid or salt can still form dynamic or hydrogen bonds with the amine groups in the nylon during compounding or injection molding processes, which are processes carried out at temperatures above 200°C. The bonds formed between the amide, acid or salt and the amine groups in the nylon provide good compatibility between the nylon and POE, while maintaining or improving the impact strength of the resulting reinforced nylon.
[0045] The polyamide compound of the nylon composition, component (A), is a polymer containing repeating amide groups (R-CO-NH-R') as an integral part of the polymer backbone. The polyamide compound useful in the present invention may include one or more polyamide compounds. Suitable polyamide resins that can be used in the present invention include any polyamide known in the art. Polyamides useful in the present invention include, but are not limited to, aliphatic, semi-crystalline, aromatic or semi-aromatic nylon resins. Nylon resins are essentially those prepared from lactam or diamine and aliphatic, semi-aromatic or aromatic dicarboxylic acid starting materials. Suitable lactams useful in the present invention include, for example, caprolactam and laurolactam. Suitable amines useful in the present invention include, for example, tetramethylenediamine, hexamethylenediamine (HMD), 2-methylpentamethylenediamine, undecaethylenediamine, dodecamethylenediamine, 2.2.4-(2,4,4-trimethylhexamethylenediamine, 5-methylnonamethylenediamine, metaxylylenediamine (MXD), paraxylylenediamine, and 2-methyl-1,5-pentamethylenediamine (MPMD). Suitable diamines useful in the present invention include, for example, tetramethylenediamine, hexamethylenediamine (HMD), 2-methylpentamethylenediamine, undecaethylenediamine, dodecamethylenediamine, 2.2.4-(2,4,4-trimethylhexamethylenediamine, 5-methylnonamethylenediamine, metaxylylenediamine (MXD), paraxylylenediamine, and 2-methyl-1,5-pentamethylenediamine (MPMD). Examples of the carboxylic acids include adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid (DDDA), terephthalic acid (TPA), isophthalic acid (IPA), 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium-sulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid. In the present invention, nylon homopolymers or copolymers derived from these starting materials are used either alone or as a mixture.Specific examples of polyamide resins that are desirable for the compositions of the present invention include the following: (nylon 6); polyundecaneamide (nylon 11); polylauramide (nylon 12); polyhexamethylene adipamide (nylon 66); polytetramethylene adipamide (nylon 46); polyhexamethylene sebacamide (nylon 610); polyhexamethylene dodecamide (nylon 612); polyhexamethylene terephthalamide (6T); polyhexamethylene isoterephthalamide (61); 2-methylpentamethylene Polyhexamethylene terephthalamide (DT); 2-methylpentamethylene isophthalamide (DI); Polyhexamethylene terephthalamide / polycapramide copolymer (nylon 6T / 6); Polyhexamethylene terephthalamide / polydodecanamide copolymer (nylon 6T / 12); Polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (nylon 66 / 6T); Polyhexamethylene adipamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 61); Polyhexamethylene adipamide Polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 61 / 6); Polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 61); Polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 6T / 61); Polyhexamethylene terephthalamide / poly(2-methylpentamethylene) terephthalamide copolymer (nylon 6T / M5T); Polyhexa methylene terephthalamide f-polyhexamethylene sebacamide / polycapramide copolymer (nylon 6T / 610 / 6); polyhexamethylene terephthalamide / polydodecanamide / polyhexamethylene adipamide copolymer (nylon 6T / 12 / 66); polyhexamethylene terephthalamide / polydodecanamide / -polyhexamethylene isophthalamide copolymer (nylon 6T / 12 / 61); poly m-xylylene adipamide (nylon MXD6); and mixtures and copolymers of any of the above compounds.
[0046] In some preferred embodiments, the polyamide component, component (A), can be any polyamide for which impact strength is desired. For example, a reinforced polyamide composition component useful in the present invention can be component (A) which is essentially at least one polyamide selected from the group consisting of: (A1) nylon-4,6; (Aii) nylon-6,6; (Aiii) nylon-6,10; (Aiv) nylon-6,9; (Av) nylon-6,12; (Avi) nylon-11; (Avii) nylon-12; (Aviii) 6T-12T; (Aix) 6I-12I; (Ax) at least one polyamide formed from 2-methylpentamethylenediamine and / or hexamethylenediamine and one or more acids selected from the group consisting essentially of (Axa) adipic acid, (Axb) isophthalic acid, (Axc) terephthalic acid, and (Axd) mixtures thereof; and (Axi) blends and / or copolymers of said nylons and polyamides.
[0047] In other preferred embodiments, the polyamide may be selected from the group consisting of nylon 6 (a polycaprolactam made from self-polymerizing caprolactam), nylon 6,6 (a hexamethylenediamine-adipic acid condensation product, a long chain synthetic polyamide with repeating amide groups in the polymer backbone), nylon 4, nylon 11, nylon 6,10, or combinations thereof.
[0048] In yet another preferred embodiment, the polyamide compound useful in the present invention is nylon 6, nylon 6,6 or mixtures thereof.
[0049] In some embodiments, the polyamide component, component (A), can be selected from commercially available compounds. For example, in some embodiments, some of the commercially available polyamide compounds useful in the present invention can include Ultramid B3S nylon 6 (available from BASF), Ultramid A3W nylon 66 (available from BASF), and mixtures thereof.
[0050] The concentration of the polyamide component, component (A), can be, for example, 50% to 98.99% by weight in one embodiment, 60% to 92% by weight in another embodiment, and 70% to 90% by weight in yet another embodiment, based on the weight of the components in the reinforced polyamide composition.
[0051] In a broad embodiment, the toughening agent component or impact modifier of the present invention, component (B), comprises at least one toughening agent component and can comprise two or more toughening agent components. The impact modifier used in combination with the polyamide component (A) and the organic amine component (C) can be one or more impact modifier compounds having the following predetermined properties: MAH graft rate, density, and melt index prior to being mixed with the other components of the reinforced nylon composition.
[0052] For example, the impact modifier has an MAH graft level of from 0.1% to 5% in one embodiment, from 0.2% to 2.0% in another embodiment, and from 0.3% to 1.0% in yet another embodiment.
[0053] For example, the impact modifier has a density from 0.80 g / cc to 0.95 g / cc in one embodiment, from 0.83 g / cc to 0.93 g / cc in another embodiment, and from 0.85 g / cc to 0.92 g / cc in yet another embodiment.
[0054] For example, the impact modifier has a melt index (MI; according to ASTM D1238 at 190° C. and 2.16 kg) of from 0.1 g / 10 min to 100 g / 10 min in one embodiment, from 0.3 g / 10 min to 50 g / 10 min in another embodiment, and from 0.5 g / 10 min to 20 g / 10 min in yet another embodiment.
[0055] In some embodiments, the toughener component, component (B), may be, for example, (Bi) (Bia) at least one polymerized ethylene; (Bib) at least one polymerized α-olefin having from 3 carbon atoms to 12 carbon atoms; (Bic) at least one polymerized unsaturated monomer having from 4 carbon atoms to 14 carbon atoms and selected from the group consisting essentially of: (Bic1) branched compounds; (Bic2) linear compounds; (Bic3) cyclic compounds; and (Bic4) mixtures thereof; and (Bid) at least one polymer selected from the group consisting essentially of mixtures thereof; (Bii) at least one unsaturated monomer selected from the group consisting essentially of: (Biia) at least one α,β ethylenically unsaturated dicarboxylic acid having from 3 carbon atoms to 8 carbon atoms; (Biib) at least one α,β ethylenically unsaturated dicarboxylic acid having from 3 carbon atoms to 8 carbon atoms; at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid: (Biib1) at least one monoester of an alcohol having 1 carbon atom to 29 carbon atoms; (Biib2) at least one anhydride of at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid; (Biib3) at least one metal salt of at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid, (Biib4) at least one monoester of at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid; (0 percent to 100 percent of the at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid have 0 percent to 100 percent of the carboxylic acid groups ionized by neutralization with a metal ion); (Biii) selected from the group consisting essentially of a mixture of components (Bi) and (Bii).
[0056] In some embodiments, the toughening agent component (impact modifier; component (B)) comprises maleic anhydride functionalized elastomeric ethylene copolymers, maleic anhydride functionalized ethylene, alpha-olefin copolymers, terpolymers of ethylene, acrylic esters and maleic anhydride, maleic anhydride grafted (MAH) polyolefin elastomers (e.g., POE-g-MAH); and combinations thereof. In one preferred embodiment, the toughening agent component, component (B), is POE-g-MAH.
[0057] In some embodiments, the toughening agent component can be selected from commercially available compounds including, for example, Exxelor series products (available from ExxonMobil); and Tafmer series products (available from Mitsui Chemicals, Inc.), and mixtures thereof.
[0058] The concentration of the impact modifier, component (B), used to prepare the nylon composition of the present invention includes, for example, in one embodiment, from 1 wt. % to 50 wt. %, in another embodiment, from 8 wt. % to 35 wt. %, and in yet another embodiment, from 10 wt. % to 25 wt. %, based on the weight of the components in the reinforced nylon composition.
[0059] In a broad embodiment, the organic amines useful in the present invention, component (C), include at least one organic amine component and can include two or more organic amine components. The organic amines used in combination with the polyamide component (A) and toughener component (B) can include one or more organic amine compounds having the following predetermined properties: a functionality of less than 4 and a Mw of less than 10,000 prior to being mixed with the other components of the reinforced nylon composition.
[0060] For example, the organic amine can have a functionality of less than 4 in one typical embodiment, and less than 3 in another embodiment. In other embodiments, the organic amine can have a functionality of from 1 to less than 4 in one embodiment; from 1 to 3 in another embodiment, and from 1 to 2 in yet another embodiment.
[0061] In general, the organic amine compound useful in the present invention can comprise one or more organic amine compounds known in the amine technical field.For example, the suitable organic amine component (C) that can be used in the present invention can include, but is not limited to, the organic amine selected from the group consisting essentially of: (Ci) at least one primary amine group; (Cii) at least one secondary amine group; and (Ciii) a mixture of at least one primary amine group of component (Ci) and at least one secondary amine group of component (Cii) in one molecule, provided that the functionality of the molecule is less than 4.
[0062] In some embodiments, the organic amine, component (C), can be selected from the group consisting essentially of R-NH, R-NH-R', NH-R-NH, R-NH-R'-NH, R-NH-R'-NH-R'', and mixtures thereof, where R, R', and R'' are each independently an alkyl, aryl, or alkoxy group having 2 to 30 carbon atoms.
[0063] In some embodiments, the organic amine, component (C), used in the present invention may comprise one or more amines including, for example, hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, laurylamine, stearamine, benhenamine, aminoethylethanolamine (AEEA), ethylamino(ethyl)amine (EAEA), polyetheramines (e.g., Jeffamine), and mixtures thereof.
[0064] In another embodiment, the organic amine component (C) can be at least one polydimethylsiloxane (PDMS) having at least one primary amine group, at least one secondary amine group, or a mixture thereof. The at least one primary amine group, at least one secondary amine group, or a mixture of the organic amine component (C) can be present at the end or side of the polydimethylsiloxane.
[0065] In yet other embodiments, the organic amine component can be selected from commercially available compounds including, for example, Jeffamine (a polyetheramine available from Huntsman Corporation), AEEA and EAEA (both available from The Dow Chemical Company); KF-8010 and X-22-161A (both available from SHIN-ETSU Chemical Company); and mixtures thereof.
[0066] The concentration of the organic amine compound, component (C), used to prepare the reinforced nylon composition of the present invention includes, for example, in one embodiment, 0.01% to 10% by weight, in another embodiment, 0.02% to 8% by weight, in yet another embodiment, 0.04% to 6% by weight, in yet another embodiment, 0.05% to 4% by weight, and in yet another embodiment, 0.06% to 3% by weight, based on the weight of the components in the reinforced nylon composition.
[0067] In some embodiments of the present invention, various amines can be either (1) used to soak the POE-g-MAH or (2) blended with the POE-g-MAH prior to adding the components to the reinforced nylon composition. As a result of using the soaking or blending method, the capillary viscosity of the reinforced nylon composition is significantly reduced (meaning that the flowability is improved) using the soaking or blending method.
[0068] By way of illustration of the present invention, but not by way of limitation thereto, for example, reinforced nylon exhibits a 25% capillary viscosity reduction (e.g., 770 s) by immersion of 0.45 wt % (based on the weight of POE-g-MAH) EAEA (2:1 molar ratio of amine to anhydride) in POE-g-MAH grafted with 0.50 wt % MAH and having a melt index of 1.6 g / 10 min measured at 190° C. under a load of 2.16 kg. -1 from 356 Pa s to 264 Pa s) and an increase in room temperature impact strength of 70% (e.g., 43.6 kJ / m 2 from 73.9 kJ / m 2Surprisingly, the impact strength of several other POE-g-MAH grades with different MAH grafting ratios, e.g., 0.90 wt. % MAH and 0.35 wt. % MAH, and with different melt index values of 1.3 g / 10 min and 1.4 g / 10 min, respectively (melt index values are measured at 190° C. and 2.16 kg load) was also significantly improved.
[0069] In some embodiments, the reinforced polyamide compositions of the present invention may further comprise one or more optional components, additives or other medicinal compounds, if desired. Optional compounds, component (D), useful in the reinforced polyamide compositions of the present invention may include, for example, fillers, lubricants, plasticizers, pigments, dyes, antioxidants, stabilizers, nucleating agents, flame retardants, and blowing agents, and mixtures thereof.
[0070] Generally, the concentration of the optional compounds when used in the reinforced polyamide includes, for example, from 0% to 50% by weight in one embodiment, from 0.01% to 40% by weight in another embodiment, and from 0.1% to 30% by weight in yet another embodiment.
[0071] In one typical embodiment, a reinforced nylon composition can be produced by combining, blending, or mixing (A) at least one polyamide (e.g., nylon compound), (B) at least one impact modifier component, (C) at least one organic amine, and (D) optional additives as needed. The resulting reinforced polyamide composition comprising said mixture exhibits at least a 10 percent reduction in capillary viscosity compared to a conventional polyamide composition not containing any one or more of components (A)-(C) in said mixture, particularly component (C), which is at least one organic amine.
[0072] As an illustration of one embodiment of the present invention, but without limitation, a general method for producing the reinforced nylon composition of the present invention includes mixing, combining or blending (A) at least one polyamide at a concentration of 50% to 98.99% by weight based on the weight of the reinforced nylon composition; (B) at least one toughening agent at a concentration of 1% to 50% by weight based on the weight of the reinforced nylon composition; (C) at least one organic amine at a concentration of 0.01% to 10% by weight based on the weight of the reinforced nylon composition; and (D) any optional components, optionally at a concentration of less than 50% by weight based on the weight of the reinforced nylon composition.
[0073] In some embodiments, the method of the present invention for preparing a reinforced polyamide composition exhibiting improved toughness comprises melt mixing, in a single step, component (A) a polyamide, component (B) a toughening agent, and component (C) an organic amine at a predetermined temperature and for a predetermined time. The single-step melt mixing step can be carried out at a temperature of 200° C. or higher in one embodiment, at a melt temperature of 200° C. to 360° C. in another embodiment, at 220° C. to 350° C. in another embodiment, at 230° C. to 340° C. in yet another embodiment, and at 250° C. to 300° C. in yet another embodiment. The duration of the single-step melt mixing step can be greater than 1 second in one embodiment, 5 seconds to 10 minutes in another embodiment, 20 seconds to 10 minutes in yet another embodiment, and 30 seconds to 5 minutes in yet another embodiment. In one embodiment, the above melt mixing single-step method can be carried out in at least one extruder, such as a conventional twin-screw (at least two screws) extruder.
[0074] In another embodiment, the method of the present invention for preparing a reinforced polyamide composition exhibiting high flow and toughness can include at least two steps: (I) a first step of mixing at least two components at a predetermined temperature for a predetermined time to form a blend composition component: (α) component (B) which is at least one impact modifier, such as the maleic anhydride grafted polyolefin elastomer (POE-g-MAH) described above; and (β) component (C) which is at least one organic amine compound, such as the organic amine described above; and (II) a second step of mixing at a predetermined temperature for a predetermined time to form a reinforced polyamide composition: (γ) component (A) which is at least one polyamide, such as the polyamide (or nylon) described above; and (δ) the blend component (i.e., composition mixture) from step (I).
[0075] The first mixing step (I) can be carried out, for example, by immersing components (B) and (C) together and then mixing the components, for example, using at least one twin-screw extruder. The temperature of the first mixing step (I) can be less than 90°C in one embodiment, 0°C to 60°C in another embodiment, and 10°C to 55°C in yet another embodiment. The time of the first mixing step (I) can be more than 1 hour in one embodiment, 1 hour to 48 hours in another embodiment, and 2 hours to 24 hours in yet another embodiment.
[0076] The temperature of the second melt-mixing step (II) may be greater than 200°C in one embodiment, 200°C to 360°C in another embodiment, 220°C to 350°C in yet another embodiment, 230°C to 340°C in yet another embodiment, and 250°C to 300°C in yet another embodiment. The time of the second melt-mixing step (II) may be 1 second or more in one embodiment, 5 seconds to 10 minutes in another embodiment, 20 seconds to 10 minutes in yet another embodiment, and 30 seconds to 5 minutes in yet another embodiment. In one embodiment, the second melt-mixing step (II) may be carried out in at least one extruder having at least two screws, for example, a conventional twin-screw extruder known in the art.
[0077] In another embodiment, a method for preparing a reinforced polyamide composition exhibiting high flow and toughness can include at least three steps: (i) a first step of melt mixing at least two components: (α) at least one impact modifier, such as component (B) of the impact modifier described above, such as POE-g-MAH; and (β) at least one organic amine component, such as the organic amine component (C) described above, to form an impact modifier and organic amine mixture; (ii) a second step of pelletizing the impact modifier / organic amine mixture from step (i) to form a plurality of composite pellets; and (iii) a third step of melt mixing at least two components: (γ) at least one polyamide; and (ε) a plurality of composite pellets from step (ii) to form a reinforced polyamide composition. In one embodiment, the third step (ii) of melt mixing can be carried out in at least one extruder, such as a conventional twin screw extruder.
[0078] The temperature of the first melt mixing step (i) may be greater than 100° C. in one embodiment, from 100° C. to 200° C. in another embodiment, and from 120° C. to 180° C. in yet another embodiment. The time for the first mixing step (i) may be greater than 20 seconds / hr in one embodiment, from 20 seconds / hr to 10 minutes in another embodiment, and from 30 seconds to 5 minutes in yet another embodiment.
[0079] The pelletizing step (B) is carried out using conventional equipment such as a strand cutter to cut the resin exiting the extruder into pellets of a desired size.
[0080] The temperature of the third melt-mixing step (iii) may be more than 200° C. in one embodiment, 200° C. to 360° C. in another embodiment, 220° C. to 350° C. in yet another embodiment, 230° C. to 340° C. in yet another embodiment, and 250° C. to 300° C. in still another embodiment. The time of the third melt-mixing step (iii) may be 5 seconds or more in one embodiment, 5 seconds to 10 minutes in another embodiment, 20 seconds to 10 minutes in yet another embodiment, and 30 seconds to 5 minutes in yet another embodiment.
[0081] The embodiments of the inventive process for preparing a reinforced polyamide composition and its steps as described above can be carried out by conventional equipment known to those skilled in the art, for example, mixing of the components to form a uniform or homogeneous mixture can be carried out by known blenders or mixers such as twin screw extruders, melt kneaders, batch mixers, and the like.
[0082] Generally, a small (e.g., less than 500 nm) POE phase size in the reinforced nylon is required to affect the impact strength of the reinforced nylon. Also, a strong interaction between nylon (polar) and elastomer (non-polar) is required to increase the strength of the reinforced nylon composition, and the strong interaction between nylon (polar) and elastomer (non-polar) achieves the desired small particle size POE phase in the nylon phase. Based on the total weight of the nylon reinforcement, the content of component (A), which is a nylon component, the content of component (B), which is a polar impact modifier, and the content of organic amine component (C) should be within a predetermined concentration range.
[0083] As an example of one embodiment of the present invention, but not limited thereto, a general method for producing the nylon composition of the present invention described above includes mixing, combining or blending in a twin-screw extruder 50% to 98.99% by weight of at least one polyamide, component (A), 1% to 50% by weight of at least one impact modifier composition, component (B), and 0.01% to 10% by weight of at least one organic amine. The reinforced nylon composition of the present invention may further include (D) one or more other optional compounds, if desired.
[0084] As mentioned above, the reinforced polyamide composition of the present invention exhibits several advantageous benefits, including, for example, (1) increased RT impact strength; and (2) reduced capillary viscosity of the reinforced nylon composition, which means that the flowability of the reinforced nylon composition is improved. For example, the combination of an organic amine and an impact modifier (e.g., POE-g-MAH) with the reinforced nylon component can advantageously function to effectively further reinforce the nylon composition, i.e., boost or enhance the room temperature impact strength of the reinforced polyamide composition. The reinforced polyamide composition exhibits increased impact strength balanced with good flowability properties, while other mechanical performances of the reinforced nylon composition, such as flexural modulus, tensile strength, elongation, heat distortion temperature (HDT), etc., are maintained at optimized levels when the polyamide is blended with POE-g-MAH and an organic amine to form the reinforced nylon composition.
[0085] For example, in one general embodiment, the nylon compositions of the invention containing a particular organic amine and an impact modifier along with the nylon component advantageously exhibit at least a 10% increase in room temperature (RT) impact strength as compared to nylon compositions containing different conventional impact modifiers. In another embodiment, the reinforced polyamide compositions of the invention exhibit at least a 15% increase in RT impact strength, and in yet another embodiment, the reinforced polyamide compositions of the invention exhibit at least a 20% increase in RT impact strength. In yet another embodiment, the reinforced polyamide compositions of the invention containing a particular organic amine and an impact modifier along with the nylon component exhibit a 10% to 50% increase in RT impact strength as compared to polyamide compositions containing other conventional impact modifiers.
[0086] In addition, the reinforced polyamide compositions of the present invention exhibit reduced capillary viscosity, which in turn provides improved flow properties for the composition. For example, in one embodiment, the capillary viscosity of the reinforced polyamide composition exhibits a 5% to 40% reduction compared to polyamide compositions containing other conventional impact modifiers, in another embodiment, a 7% to 35% reduction compared to polyamide compositions containing other conventional impact modifiers, and in yet another embodiment, an 8% to 30% reduction compared to polyamide compositions containing other conventional impact modifiers.
[0087] Another advantage of the nylon composition of the present invention is that the nylon composition can be used to manufacture lighter weight articles / products or parts that have thinner walls and use less composition due to the above-mentioned improved properties of RT impact strength of the composition.
[0088] Articles / products or parts made from the reinforced nylon compositions of the present invention can include, for example, electronic devices, automotive parts, gear, toys, and the like.
[0089] Once components (A), (B) and (C) are thoroughly and uniformly mixed together in molten form, the resulting molten mixture can be used to form an article / product or molded part using conventional methods and equipment. For example, an article / product or molded part can be formed from the composition using injection molding, extrusion, or blow molding methods.
[0090] In one preferred embodiment, the article / product or molded part is produced and processed using, for example, injection molding methods and extrusion equipment such as twin screw extruders. In general, a method for producing the article of the invention from the reinforced polyamide composition of the invention can be, for example: (X) providing a reinforced polyamide composition by mixing (A) at least one polyamide, (B) an impact modifier, and (C) an organic amine; (Y) processing the composition of step (X) into an article using an extrusion process to form the article.
[0091] To make thinner and therefore lighter parts, it is necessary for the nylon composition to have high impact strength so that the nylon composition can flow through thinner walls. The use of the nylon composition of the present invention provides both improved flow properties and toughness. Such high performance properties allow for the gauge reduction of interior and exterior parts and articles that require superior impact resistance properties.
[0092] The impact modifier additive, the reinforced nylon composition, and the articles, products, or parts made from the reinforced nylon composition can be used in a wide range of polymer compositions and structures. In general, the reinforced nylon composition containing the impact modifier of the present invention is used in applications that require parts with higher impact strength (i.e., increased toughness and durability) than parts made from conventional copolymers. For example, but not limited to, the reinforced nylon composition can be used in a variety of applications and can be formed into molded articles that are useful in areas requiring impact resistance and strength. In one embodiment, for example, the reinforced nylon composition can be used in automotive applications to make rigid parts and components for automobiles. The automotive products can be manufactured by conventional polymer processing. EXAMPLES
[0093] The following inventive examples (Inv. Ex.) and comparative examples (Comp. Ex.) (collectively "Examples") are presented herein to more fully illustrate the features of the present invention, but are not intended to be construed, either explicitly or implicitly, as limiting the scope of the claims. Inventive examples are identified by Arabic numerals, and comparative examples are represented by alphabetical letters. The following experiments analyzed the performance of embodiments of the compositions described herein. Unless otherwise indicated, all parts and percentages are by weight based on total weight.
[0094] raw materials Some of the raw materials (ingredients) used in the examples are listed in Table I. The three different grades of POE-g-MAH used in the examples are designated POE-g-MAH1 (having a MAH graft level of 0.50 wt% and a melt index (MI) of 1.6 g / 10 min), POE-g-MAH2 (having a MAH graft level of 0.90 wt% and a MI of 1.3 g / 10 min), and POE-g-MAH3 (having a MAH graft level of 0.35 wt% and a MI of 1.4 g / 10 min).
[0095] Some of the amines used in the examples include ethylamino(ethyl)amine (EAEA), a diamine with a functionality of 2; aminoethylethanolamine (AEEA), a diamine with a functionality of 3; and triethylenetetramine (TETA), a tetramine with a functionality of 4. [Table 1]
[0096] compound The reinforced nylon composite formulations used in the examples were made based on the formulations set forth in Table II for the Series 1 experiments and Table III for the Series 2 experiments. [Table 2] [Table 3]
[0097] The general procedures used to prepare the reinforced nylon composite compound samples listed in Tables II and III, and the methods used to test the samples, are described in the Test Procedures set forth herein below.
[0098] Dipping Method for Blending Amine with POE The amines used in the examples were blended with POE using POE pellets and a soaking method. The soaking method involves first mixing the amine with the POE pellets at room temperature, and then allowing the low molecular weight amine to penetrate the POE pellets. For example, the soaking method was performed as follows: 400 g of POE pellets were first placed in a 2 L plastic container, and then the amine was added to the container according to the weight percentage of the amine present in the container to form the formulations described in Tables II and III. The container was shaken in different directions for 5 minutes (e.g., the container was shaken up and down and side to side at the same frequency). After shaking the container for 5 minutes, the container was allowed to stand for 5 minutes. After allowing the container to stand for 5 minutes, the container was picked up and the steps of shaking the container and standing for 5 minutes were repeated. The combined steps of shaking and standing the container were repeated 6 times. After repeating 6 times, the container was kept at room temperature for another 3 hours.
[0099] Compounding POE soaked in nylon A number of nylon samples were first dried in a dehumidifier at 120°C for at least 4 hours. A twin screw extruder (ZSK18 twin screw extruder available from Coperion Company) was used to compound the soaked POE into the dried nylon samples. The following extruder parameters were used: power = 19.2KW, D = 18mm, L / D = 48. The extruder conditions / parameters for compounding the amine / POE pellets and nylon samples were as follows: the extruder barrel temperatures were set as follows: Zone 1 = 150°C, Zone 2 = 195°C, Zone 3 = 260°C, Zone 4 = 260°C, Zone 5 = 260°C, Zone 6 = 260°C, and Zone 7 = 250°C, ranging from RT to about 350°C. The extruder screw speed was 300 rpm, and the feed rate of the blended material to the extruder was 10 kg / hr. After the compounding process, the resulting compound was cut into pellets having a diameter of 0.5 mm to 1 mm and a length of 2 mm to 5 mm.
[0100] Test Method The following test methods and measurement procedures were used to test samples prepared according to the above general procedure for preparing reinforced nylon composition samples for testing.
[0101] Capillary Viscosity Test The compounded nylon / POE samples were first dried in a dehumidifier at 120°C for at least 4 hours, and after drying the compounded samples, the compounded samples were sealed in aluminum bags under vacuum. The moisture content in the compounded nylon / POE samples was tested by the so-called Karl Fischer method using an 874 Oven Sample Processor (available from Thermo-Fisher Co.Ltd.). It is recommended that the moisture in the compounded nylon / POE samples be less than 1,000 ppm before testing the samples using the capillary viscosity test. The capillary rheometer instrument used for the capillary viscosity test was a Gottfert rheograph 26 (available from Gottfert Inc.). The test temperature used for the capillary viscosity test was 260°C. The length of the capillary used was 30 mm, and the diameter of the capillary was 1 mm. The shear rates used for the tests ranged from 90 1 / s to 7,000 1 / s. Tabulated data on viscosity are reported at a shear rate of 770 1 / s.
[0102] Injection molding method The compounded nylon / POE pellets were first dried in a dehumidifier at 120°C for at least 4 hours, and then the samples were injection molded. An injection molding machine, Fanuc Roboshot S-2000i100BH (available from Fanuc), was used for the injection molding process. The compounded samples were injection molded to produce test specimens, which were impact tested using the impact strength test described herein below. The parameters of the injection molding machine and process were as follows: the barrel temperature of the injection screw was set at 250°C-260°C, the cooling temperature was 190°C, the cooling time was 15 seconds, the injection speed was 30 mm / sec, and the injection pressure was 200 MPa.
[0103] Impact Strength Test The impact strength test method used to test the impact performance of the specimens prepared in the examples is described in CHARPY, ISO 179 ("ISO" stands for "International Organization for Standardization"). CHARPY, ISO 179 specifies a method for determining the Charpy impact strength of plastics under defined conditions. The specimens used in this test are flat test specimens made from the formulations in Tables II and III and have the following dimensions: 80 mm length x 10 mm width x 4 mm thickness. CHARPY, ISO 179 defines a method used to determine the resistance of plastics to fracture when impacted in a three-point bending configuration using a pendulum system with an appropriately sized hammer arm. The test is uninstrumented and is used to determine the energy required to break the specimen. The different test parameters are specified according to the type of material from which the specimen is made as well as the type of notch cut in the specimen.
[0104] In the examples described herein, the following general procedure was followed: All specimens were notched with a radius of 2 mm. Before testing, all specimens were first dried in a dehumidifier at 120° C. for 4 hours. The specimens were then equilibrated in the humidifier at room temperature for 2 days.
[0105] Each specimen to be tested was mounted horizontally in a pendulum impact tester and supported free at both ends. The hammer of the tester was released and allowed to penetrate the specimen. If no breakage occurred with the first hammer arm used, successively heavier hammers were used until breakage occurred. At breakage, the energy obtained and the type of breakage were then recorded.
[0106] The shock test conditions used were as follows: 4 Joules pendulum volume and specimen conditioning at room temperature for ≥ 6 hours or at -40°C in a freezer for ≥ 6 hours. Samples in the freezer were removed from the freezer and shocked within 5 seconds. Test conditions were room temperature (i.e., temperature of 23°C ± 2°C) and 50% RH ± 10% RH.
[0107] Test results The viscosity results for the reinforced nylon formulations listed in Tables II and III were obtained by performing the Capillary Viscosity Test described above; the viscosity results for the formulations in Table II for Series 1 experiments are listed in Table IV; and the viscosity results for the formulations in Table II for Series 2 experiments are listed in Table V. [Table 4] [Table 5]
[0108] Injection molded test specimens were prepared from the reinforced nylon formulations set forth in Tables II and III, and the impact strengths of some of the injection molded test specimens made from some of the reinforced nylon formulations set forth in Tables II and III were obtained by conducting the above-described impact strength tests on injection molded test specimens prepared according to the above-described injection molding method. The impact strength results for the test specimens made from the formulations in Table II for Series 1 of the experiments are set forth in Table VI; the impact strength results for the test specimens made from the formulations in Table III for Series 2 of the experiments are set forth in Table VII. [Table 6] Notes about Table VI: (1) NT means that the sample was not tested. [Table 7] Notes for Table VII: (1) NT means that the sample was not tested.
[0109] Discussion of results Series 1 Test Results In series 1, listed in Table IV, different types and loadings of organic amines were soaked into MAH-grafted POE (POE-g-MAH1) of series 1. The soaked POE was then blended with B3s (medium viscosity nylon 6 available from BASF). The capillary viscosity and impact strength are listed in Tables IV and VI, respectively. The capillary viscosity was tested at different shear rates, from low to high shear rates. However, Table IV shows that the capillary viscosity was 770 s -1 6 shows the capillary viscosity of the samples tested at a shear rate of 1000 s. This shear rate was chosen to simplify the data obtained from the test, since the capillary viscosity results at different shear rates showed similar trends. As noted in Table VI, the reinforced nylon sample with POE-g-MAH1 (Example J) shows higher impact strength compared to the non-reinforced nylon sample (Comparative Example A, no amine is used in Comparative Example A), but the viscosity for Comparative Example B increased significantly with POE-g-MAH1 as part of the composition. It is common to observe a viscosity increase due to crosslinking between the grafted MAH and the amine groups at the nylon chain ends. By immersing the organic amine in POE-g-MAH1, the samples containing POE-g-MAH1 soaked with amine (e.g., Inventive Example 1 to Inventive Example 7, Comparative Example C and Comparative Example D) showed lower viscosity than the comparative sample (Comparative Example B). Using the same organic amine, the viscosity of the examples decreased with increasing organic amine loading. For example, Inventive Example 2 has a lower viscosity than Inventive Example 1, and Inventive Example 5 has a lower viscosity than Inventive Example 3 and Inventive Example 4. This surprising phenomenon clearly indicates that the organic amine helps to reduce the viscosity of the reinforced nylon, thereby improving the flowability of the reinforced nylon composition.
[0110] Furthermore, the room temperature impact strength of the test pieces made from the reinforced nylon composition samples of Inventive Example 12 to Inventive Example 18 is significantly improved compared to the nylon composition sample of Comparative Example J, especially when the functionality of the organic amine used in the examples is less than 3. When the functionality of the amine used in the examples is greater than 3, such as the tetraamine triethylenetetramine (TETA), overcrosslinking of the POE occurs, and such overcrosslinking significantly reduces the impact strength of the reinforced nylon. For example, Comparative Example L showed a significantly lower RT impact strength than Comparative Example J. Therefore, it is beneficial to control the functionality of the amine to 3 or less. In Comparative Example M, an aminosilane was tested, but it resulted in a nylon with an undesirably low impact strength. The poor impact strength of the sample of Comparative Example M can be attributed to overcrosslinking of the POE, since the amine Z-6020 is a trimethoxylsilane that provides a high crosslink density.
[0111] Series 2 Test Results In series 2, as described in Tables V and VII, various POE samples with different graft levels of MAH were used as impact modifiers (e.g., POE-g-MAH1 had a graft level of 0.50%, POE-g-MAH2 had a graft level of 0.90%, and POE-g-MAH3 had a graft level of 0.35%). The impact modifiers were added to a nylon 6 matrix (BASF B3s) and tested. As shown in Table V, the viscosity of the reinforced nylon 6, which is made by impregnating nylon 6 with amines, is significantly lower than the viscosity of the comparative nylon composition without amines. For example, the nylon sample of inventive Example 8 was compared with the nylon sample of Comparative Example B; the nylon samples of inventive Example 9 and inventive Example 10 were compared with the nylon sample of Comparative Example F; and the nylon sample of inventive Example 11 was compared with the nylon sample of Comparative Example G. The above results show that the organic amines of the present invention have a surprisingly beneficial effect on the capillary viscosity in different types of POE.
[0112] The above results from Table VII also show that: (1) the room temperature impact strength values of the amine-impregnated polyamide samples are much better than the non-impregnated polyamide samples, as evidenced, for example, by comparing Inventive Example 19 through Inventive Example 22 with Comparative Example N; and (2) the flexural modulus performance of the amine-impregnated polyamide samples is essentially maintained at a comparable level as the non-amine-impregnated polyamide samples, as evidenced, for example, by Inventive Examples 13, 14, 15, 16, 21, and 22.
[0113] Based on the above results, it can be concluded that organic amine-impregnated POE can significantly improve the fluidity and room temperature impact strength of reinforced nylon (or polyamide).
[0114] Other embodiments Embodiment 1: The reinforced polyamide composition of the present invention, wherein the at least one polyamide component (A) is selected from the group consisting essentially of: (ai) nylon-4,6; (Aii) nylon-6,6; (Aiii) nylon-6,10; (Aiv) nylon-6,9; (Av) nylon-6,12; (Avi) nylon-11; (Avii) nylon-12; (Aviii) 6T-12T; (Aix) 6I-12I; (Ax) at least one polyamide formed from 2-methylpentamethylenediamine and / or from hexamethylenediamine and one or more acids; and (Axi) blends or copolymers of said nylons and polyamides.
[0115] Embodiment 2: A composition of the invention, wherein the at least one polyamide, component (Ax), is selected from the group consisting essentially of (Axa) adipic acid, (Axb) isophthalic acid, (Axc) terephthalic acid, and (Axd) mixtures thereof.
[0116] Embodiment 3: The composition of the present invention, wherein the at least one impact modifier, component (B), is selected from the group consisting essentially of: (Bi) at least one polymer selected from the group consisting of: (Bia) at least one polymerized ethylene; (Bib) at least one polymerized α-olefin having from 3 carbon atoms to 12 carbon atoms; (Bic) at least one polymerized unsaturated monomer having from 4 carbon atoms to 14 carbon atoms; and (Bid) mixtures thereof; and (Bii) at least one unsaturated monomer selected from the group consisting essentially of: (Biia) at least one α,β ethylenically unsaturated dicarboxylic acid having from 3 carbon atoms to 8 carbon atoms; and (Biib) at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid; and (Biii) a mixture of components (Bi) and (Bii).
[0117] Embodiment 4: A composition of the invention, wherein component (Bic), which is at least one polymerized unsaturated monomer having from 4 carbon atoms to 14 carbon atoms, is selected from the group consisting essentially of: (Bic1) branched compounds; (Bic2) linear compounds; (Bic3) cyclic compounds; and (Bic4) mixtures thereof.
[0118] Embodiment 5: A composition of the invention, wherein the at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid, component (Biib), is selected from the group consisting essentially of: (Biib1) at least one monoester of an alcohol having from 1 carbon atom to 29 carbon atoms; (Biib2) at least one anhydride of at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid; (Biib3) at least one metal salt of at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid; (Biib4) at least one monoester of at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid; (0 percent to 100 percent of the at least one derivative of at least one α,β ethylenically unsaturated dicarboxylic acid have 0 percent to 100 percent of the carboxylic acid groups ionized by neutralization with a metal ion); and (Biib5) mixtures thereof.
[0119] Embodiment 6: A reinforced polyamide composition of the present invention, wherein the at least one organic amine, component (C), comprises amine groups selected from the group consisting essentially of: (ci) at least one primary amine group; (Cii) at least one secondary amine group; and (Ciii) a mixture of at least one primary amine group of component (Ci) and at least one secondary amine group of component (Cii) in one molecule, provided that the functionality of the molecule is less than 4.
[0120] Embodiment 7: A reinforced polyamide composition of the present invention, wherein the reinforced polyamide composition containing at least one organic amine exhibits at least a 10 percent increase in room temperature impact strength, or a 10% decrease in capillary viscosity, or both a 10% increase in room temperature impact and a 10% decrease in capillary viscosity, compared to a conventional polyamide composition not containing at least one organic amine.
Claims
1. (A) at least one polyamide; (B) at least one impact modifier; and and (C) at least one organic amine, wherein the concentration of said at least one organic amine, component (C), is from 0.01% to 10% by weight.
2. 2. The reinforced polyamide composition of claim 1, wherein the at least one organic amine, component (C), contains an amine per molecule, with the proviso that the functionality of the molecule is less than four.
3. 2. The reinforced polyamide composition of claim 1, wherein the at least one polyamide, component (A), has a concentration of 50% to 98.99% by weight, the at least one impact modifier composition, component (B), has a concentration of 1% to 50% by weight, and the at least one organic amine, component (C), has a concentration of 0.01% to 10% by weight.
4. 2. The reinforced polyamide composition of claim 1, wherein the at least one impact modifier, component (B), is a maleic anhydride grafted polyolefin elastomer.
5. The at least one organic amine, component (C), is R-NH 2 , R-NH-R', NH 2 -R-NH 2 , R-NH-R'-NH 2 10. The reinforced polyamide composition of claim 1, wherein R, R', and R'' are each independently an alkyl group, an aryl group, an aryl group, or an alkoxy group having from 2 to 30 carbon atoms.
6. 2. The reinforced polyamide composition of claim 1, wherein the at least one organic amine, component (C), is at least one polyetheramine.
7. 2. The reinforced polyamide composition of claim 1, wherein the at least one organic amine, component (C), is at least one polydimethylsiloxane having at least one primary amine group, or at least one secondary amine group, or a mixture thereof, wherein the at least one primary amine group, the at least one secondary amine group, or a mixture thereof is present at the end or side of the at least one polydimethylsiloxane.
8. 1. A method for preparing a reinforced polyamide composition exhibiting high flow and toughness, comprising the steps of: (A) at least one polyamide; (B) at least one impact modifier; and (C) melt mixing the blend in one step with at least one organic amine, wherein the concentration of the organic amine is 0.01% to 10% by weight; The process wherein said melt mixing step is carried out at a melt mixing temperature above 200°C.
9. 1. A method for preparing a reinforced polyamide composition exhibiting high flow and toughness, comprising the steps of: (I) mixing at least two of the following components at a temperature of less than 90° C. for a period of time: (α) at least one impact modifier (B); (β) immersing at least one organic amine (C) to form a blended composite component; (II) mixing at least two of the following components at a temperature above 200° C. for a period of time: (γ) at least one polyamide; (δ) melt mixing said blend composite components from step (I) to form a reinforced polyamide composition.
10. 1. A method for preparing a reinforced polyamide composition exhibiting high flow and toughness, comprising the steps of: (i) At least two of the following components at a temperature above 90° C.: (α) at least one toughening agent component; (β) melt mixing at least one siloxane-based component to form a blend composite component; (ii) pelletizing the blended composite components from step (i) to form a plurality of composite pellets; (iii) At a temperature above 200° C., at least two of the following components: (γ) at least one polyamide; (ε) melt mixing the plurality of composite pellets from step (ii) to form a reinforced polyamide composition.
11. 10. An article made from the reinforced polyamide composition of claim 1.
Citation Information
Patent Citations
Thermoplastic resin composition
JP1988146928A
Thermoplastic resin composition
JP1988199755A
Stabilizer-containing, highly fluid, reinforced, and weather-resistant polyamide composition
JP2007512427A
Thermoplastic polyamides with polyetheramines
JP2011506725A
Polyamide resin composition
JP2014141630A