Method for manufacturing a cable having an insulating layer - Patents.com

By using a Si-H containing acetophenone scavenger in the crosslinkable polymer composition for HVDC cables, the method effectively reduces acetophenone levels, maintaining crosslink density and thermal resistance, addressing the challenges of conventional XLPE manufacturing.

JP2024545204AActive Publication Date: 2024-12-05DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024535260
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-12-17
Publication Date
2024-12-05
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

Conventional methods for manufacturing HVDC cables using crosslinked ethylene-based polymers (XLPE) face challenges in reducing the production of acetophenone byproducts, which increase conductivity and lower the thermal resistance of the insulation layer, necessitating longer degassing times and reduced crosslink density.

Method used

Incorporating a Si-H containing acetophenone scavenger in the crosslinkable polymer composition, along with dicumyl peroxide, to form a crosslinked insulation layer that effectively reduces acetophenone levels through a crosslinking procedure, followed by degassing to achieve lower AP/CA ratios.

Benefits of technology

The method significantly decreases acetophenone concentration, maintaining or improving crosslink density and thermal resistance, thereby enhancing the performance of HVDC cables without extending degassing times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545204000001
    Figure 2024545204000001
  • Figure 2024545204000002
    Figure 2024545204000002
  • Figure 2024545204000003
    Figure 2024545204000003
Patent Text Reader

Abstract

The present disclosure provides a method. In one embodiment, the method includes providing an initial cable core. The initial cable core includes (i) a conductor and (ii) an initial insulation layer. The initial insulation layer includes (a) a crosslinkable polymer composition comprised of an ethylene-based polymer comprised of (1) an ethylene monomer, (2) an optional α-olefin comonomer, and (3) an optional organosiloxane comonomer. The crosslinkable polymer composition further includes (b) dicumyl peroxide (DCP), (c) a Si-H containing (AP) scavenger, (d) an optional curing coagent, and (e) an optional antioxidant. The method includes subjecting the initial cable core to a crosslinking procedure sufficient to crosslink the crosslinkable polymer composition to form a cable core having a crosslinked insulation layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Peroxide crosslinked ethylene-based polymers (XLPE) are widely used as insulation materials in industrial and urban power transmission cables, including both HVAC (high voltage alternating current) and HVDC (high voltage direct current). The direct current (DC) conductivity of XLPE is an important parameter for HVDC insulation materials, where the electric field distribution and space charge accumulation across the cable depend on the conductivity. Peroxides used for crosslinking (e.g., dicumyl peroxide, "DCP") create by-products such as methane, acetophenone, alpha-methylstyrene, and cumyl alcohol. The presence of acetophenone (AP) increases the conductivity of the insulation layer, which is detrimental to HVDC cables. To reduce the amount of AP in the insulation layer to an acceptable level, conventional HVDC cable manufacturing protocols typically require (i) lowering the DCP loading at the expense of crosslink density and / or much longer degassing times. HVDC cables made from conventional XLPE typically require at least 30 days to degas and reduce acetophenone to a suitably low level. However, lowering the DCP loading during crosslinking is problematic because it reduces the thermal resistance of the insulation layer due to the lower crosslink density and also reduces the maximum operating temperature of the HVDC cable to 70°C, whereas a more efficient operating temperature for HVDC needs to be 90°C or higher.

[0002] There is a recognized need in the art for a method in power cable manufacturing that can reduce the production of peroxide by-products and increase crosslink density in power cable insulation layers. Summary of the Invention

[0003] The present disclosure provides a method. In one embodiment, the method includes providing an initial cable core. The initial cable core includes (i) a conductor and (ii) an initial insulation layer. The initial insulation layer includes (a) a crosslinkable polymer composition comprised of an ethylene-based polymer comprised of (1) an ethylene monomer, (2) an optional α-olefin comonomer, and (3) an optional organosiloxane comonomer. The crosslinkable polymer composition further includes (b) dicumyl peroxide (DCP), (c) a Si-H containing (AP) scavenger, (d) an optional curing coagent, and (e) an optional antioxidant. The method includes subjecting the initial cable core to a crosslinking procedure sufficient to crosslink the crosslinkable polymer composition to form a cable core having a crosslinked insulation layer.

[0004] The present disclosure provides a cable. In one embodiment, the cable includes a cable core. The cable core includes (i) a conductor and (ii) a crosslinked insulation layer. The crosslinked insulation layer is formed from a crosslinkable polymer composition comprised of an ethylene-based polymer comprised of (a) (1) ethylene monomer, (2) optional α-olefin comonomer, and (3) optional organosiloxane comonomer. The crosslinkable polymer composition further includes (b) dicumyl peroxide (DCP), (c) a Si-H containing (AP) scavenger, (d) an optional curing coagent, and (e) an optional antioxidant.

[0005] definition Any reference to the Periodic Table of the Elements is to the Periodic Table of the Elements published by CRC Press, Inc., 1990-1991. References to element groups in this table are to the new notation for numbering groups.

[0006] For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or the equivalent U.S. version thereof is so incorporated by reference), particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and general knowledge in the art.

[0007] Numerical ranges disclosed herein include all values ​​between the lower limit and the upper limit (inclusive). In the case of ranges containing explicit values ​​(e.g., 1 or 2, or 3-5, or 6, or 7), all subranges between any two explicit values ​​are included (e.g., the range 1-7 above includes subranges such as 1-2, 2-6, 5-7, 3-7, 5-6, etc.).

[0008] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all test methods are current as of the filing date of this disclosure.

[0009] The term "composition" refers to a mixture of materials that make up the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0010] The terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional component, step, or procedure, whether or not it is specifically disclosed. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additive, adjuvant, or compound, whether polymeric or not, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any preceding description any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not specifically delineated or listed. The term "or" refers to the listed members individually and in any combination, unless otherwise stated. The use of the singular includes the use of the plural, and vice versa.

[0011] An "ethylene-based polymer" or "ethylene polymer" is a polymer that contains a majority amount of polymerized ethylene, based on the weight of the polymer, and may optionally include at least one comonomer. Ethylene-based polymers typically contain at least 50 mole percent (mol %) units derived from ethylene (based on the total amount of polymerizable monomers).

[0012] A "hydrocarbon" (or "hydrocarbyl" or "hydrocarbyl group") is a compound that contains only hydrogen and carbon atoms.

[0013] The terms "heterohydrocarbon" ("heterohydrocarbyl" or heterohydrocarbyl group") and similar terms, as used herein, refer to each hydrocarbon in which at least one carbon atom is replaced with a heteroatom group (e.g., Si, O, N, or P).

[0014] The term "substituted hydrocarbon" (or "substituted hydrocarbyl" or "substituted hydrocarbyl group") refers to a hydrocarbon in which one or more hydrogen atoms have been independently replaced with a heteroatom group. The term "substituted heterohydrocarbon" ("substituted heterohydrocarbyl" or "substituted heterohydrocarbyl group") and similar terms, as used herein, refer to each heterohydrocarbon in which one or more hydrogen atoms have been independently replaced with a heteroatom group.

[0015] An "interpolymer" is a polymer prepared by the polymerization of at least two different types of monomers. Thus, the generic term interpolymer includes copolymers (used to refer to polymers prepared from two different types of monomers) and polymers prepared from three or more different types of monomers.

[0016] An "olefin-based polymer" or "polyolefin" is a polymer that contains a majority mole percent of polymerized olefin monomers (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Non-limiting examples of olefin-based polymers include ethylene-based polymers and propylene-based polymers. Representative polyolefins include polyethylene, polypropylene, polybutene, polyisoprene, and various interpolymers thereof.

[0017] A "polymer" is a polymeric compound prepared by polymerizing monomers, whether they are the same or different types of monomers. Thus, the generic term polymer includes the term "homopolymer" (used to refer to a polymer prepared from only one type of monomer, with the understanding that trace amounts of impurities may be incorporated into the polymer structure), and the term "interpolymer" as defined herein below. Trace amounts of impurities, such as catalyst residues, may be incorporated into and / or within the polymer. It also includes copolymers in all forms, such as random, block, etc. The terms "ethylene / α-olefin polymer" and "propylene / α-olefin polymer" refer to the above-mentioned copolymers prepared from polymerizing ethylene or propylene with one or more additional polymerizable α-olefin monomers, respectively. It is noted that while polymers are often referred to as "made of" one or more specific monomers, "based on" a specific monomer or type of monomer, "containing" a specific monomer content, etc., in this context, the term "monomer" is understood to refer to the polymerized residue of a specific monomer, and not to the unpolymerized species. Generally, polymers are referred to herein in terms of "units" that are the polymerized form of the corresponding monomers.

[0018] A "propylene-based polymer" is a polymer that contains a majority amount of polymerized propylene, based on the weight of the polymer, and may optionally include at least one comonomer. A propylene-based polymer typically contains at least 50 mole percent (mol%) of propylene-derived units (based on the total amount of polymerizable monomers).

[0019] Test Method ASTM D792, Method B (g / cc or g / cm 3 ) to measure density.

[0020] Differential Scanning Calorimetry (DSC) Differential scanning calorimetry (DSC) was used to measure the T m , T c , T g , and crystallinity. Each sample (0.5 g) was compression molded into a film at 5000 psi for 2 min at 190 °C. Approximately 5-8 mg of film sample was weighed and placed into a DSC pan. A lid was crimped onto the pan to ensure a closed atmosphere. Unless otherwise stated, the sample pan was placed into a DSC cell and then heated at a rate of 10 °C / min to a temperature of 180 °C for PE (230 °C for PP). The sample was held at this temperature for 3 min. The sample was then cooled at a rate of 10 °C / min to -90 °C for PE (-60 °C for PP) and held isothermal at that temperature for 3 min. The sample was then heated at a rate of 10 °C / min until completely melted (second heat). The melting point (T m ) and glass transition temperature (T g ) was determined from the second heating curve, and the crystallization temperature (T c ) was determined from the first cooling curve. T m and T c The peak temperatures of each of the three samples were recorded. The percent crystallinity was calculated using the heat of fusion (H) determined from the second heating curve. f) by the theoretical heat of fusion of 292 J / g for PE (165 J / g for PP) and multiplying this amount by 100 (e.g., crystallinity % = (Hf / 292 J / g) x 100 for PE). m A peak is typically observed, where the T of the polymer m The highest temperature peak is recorded as the

[0021] Gel Permeation Chromatography The chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5). The autosampler oven compartment was set at 160° Celsius and the column compartment was set at 150° Celsius. The columns were four AGILENT "Mixed A" 30 cm, 20 micron linear mixed bed columns. The chromatography solvent was 1,2,4-trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was nitrogen sparged. The injection volume used was 200 microliters and the flow rate was 1.0 milliliters / min.

[0022] Calibration of the GPC column set was performed with 21 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000 prepared in six "cocktail" mixtures with at least 10-fold intervals between the individual molecular weights. The standards were purchased from Agilent Technologies. The polystyrene standards were prepared in 0.025 grams in 50 milliliters of solvent for molecular weights equal to or greater than 1,000,000 and 0.05 grams in 50 milliliters for molecular weights less than 1,000,000. The polystyrene standards were dissolved at 80 degrees Celsius with gentle stirring for 30 minutes. The peak molecular weight of the polystyrene standards was calculated according to Equation 1 (EQ1) (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)): M ポリエチレン =A×(M ポリスチレン ) B (EQ1) where M is the molecular weight, A has a value of 0.4315, and B is equal to 1.0) was used to convert to polyethylene molecular weight.

[0023] A fifth order polynomial was used to fit each polyethylene equivalent calibration point. A small adjustment (approximately 0.375 to 0.445) was made to A to correct for column resolution and band broadening effects such that a linear homopolymer polyethylene standard was obtained at 120,000 Mw. Total theoretical plate counts were performed for the GPC column set using decane (prepared in TCB "0.04 g in 50 milliliters" and dissolved for 20 minutes with gentle agitation). Theoretical plate counts (Eq. 2, EQ2) and symmetry (Eq. 3, EQ3) were calculated using the following equations for a 200 microliter injection:

[0024]

number

[0025]

number

[0026] Samples were prepared in a semi-automated fashion using the PolymerChar "Instrument Control" software, samples were weight-targeted at 2 mg / mL, and solvent (containing 200 ppm BHT) was added via the PolymerChar high temperature autosampler to a septa-capped vial that had been pre-sparged with nitrogen. Samples were dissolved at 160 degrees Celsius under "slow" shaking for 2 hours.

[0027] Mn (GPC) , Mw (GPC) , and Mz (GPC) The calculation of was based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph according to Equations 4-6 using PolymerChar GPCOne™ software, baseline subtracted IR chromatograms at each equally spaced data collection point (i), and polyethylene equivalent molecular weights obtained from a narrow standard calibration curve for point (i) of Equation 1. Equations 4-6 (EQ4-EQ6) are as follows:

[0028]

number

[0029] To monitor deviations over time, a flow rate marker (decane) was introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow rate marker (FM) was used to linearly correct the pump flow rate (flow rate (apparent)) for each sample by aligning the RV of the respective decane peak in the sample (RV(FM sample)) with the RV of the decane peak within a narrow standard calibration (RV(FM calibrated)). Any change in time of the decane marker peak was then assumed to be related to a linear shift in flow rate (flow rate (effective)) across the run. To facilitate the highest accuracy of RV measurements of the flow rate marker peaks, the peaks of the flow rate marker concentration chromatograms were fitted to a quadratic equation using a least-squares fitting routine. The first derivative of the quadratic equation was then used to solve for the true peak position. After calibrating the system based on the flow rate marker peaks, the effective flow rate (with respect to the narrow standard calibration) was calculated as Equation 7: Flow Rate (Effective) = Flow Rate (Apparent) x (RV (FM Calibrated) / RV (FM Sample)) (Equation 7). Processing of the flow rate marker peaks was performed via PolymerChar GPCOne™ software. An acceptable flow rate correction is one that brings the effective flow rate within ±0.7% of the apparent flow rate.

[0030] MDR testing was performed on an MDR2000 (Alpha Technologies) at 180°C for 20 minutes while monitoring the change in torque according to ASTM D5289-12, Standard Test Method for Rubber Property--Vulcanization Using Rotorless Cure Meters. The minimum measured torque value is designated as "ML" expressed in deciNewton-meter (dN-m). As the curing or crosslinking proceeds, the measured torque value increases and eventually reaches a maximum torque value. The maximum or highest measured torque value is designated as "MH" expressed in dN-m. All other conditions being equal, the higher the MH torque value, the greater the degree of crosslinking. The T90 crosslinking time is determined as the time (in minutes) required to achieve a torque value equal to 90% of the difference between MH minus ML (MH-ML), i.e., 90% of the distance from ML to MH. The shorter the T90 crosslinking time, i.e., the faster the torque value is 90% of the distance from ML to MH, the faster the cure rate of the test sample. Conversely, the longer the T90 crosslinking time, i.e., the more time it takes for the torque value to reach 90% of the distance from ML to MH, the slower the cure rate of the test sample.

[0031] Melt Index The melt index (or "I2") of ethylene-based polymers is measured according to ASTM D-1238, condition 190°C / 2.16 kg (melt index (I10) is 190°C / 10.0 kg). I10 / I2 was calculated from the ratio of I10 to I2. The melt flow rate MFR of propylene-based polymers is measured according to ASTM D-1238, condition 230°C / 2.16 kg.

[0032] Nuclear Magnetic Resonance (NMR) characterization of terpolymers 13 For C NMR experiments, samples were dissolved in tetrachloroethane-d 2 (0.025M Cr(acac) 3The tubes were dissolved in 100 mL of 5% ethanol (with or without 5% CO). The concentration was approximately 300 mg / 2.8 mL. Each tube was then heated in a heating block set at 110° C. The sample tubes were repeatedly vortexed and heated to obtain a homogenous flowing fluid. 13 C NMR spectra were obtained on a BRUKER AVANCE 600 MHz spectrometer equipped with a 10 mm C / H DUAL cryoprobe. The following acquisition parameters were used: 60 s relaxation time, 12.0 μs 90 degree pulse, 256 scans. The spectral center was 100 ppm and the spectral width was 250 ppm. All measurements were performed at 110 °C without spinning the sample. 13 C NMR spectra were referenced to the solvent resonance peak at 74.5 ppm. For Cr-containing samples, data were acquired with a 7 second relaxation time and 1024 scans.

[0033] 1 For H NMR experiments, each sample was dissolved in tetrachloroethane-d 2 (0.001M Cr(acac) 3 The tubes were dissolved in 100 mL of 100% ethanol (with or without 100 mg / 1.8 mL). The concentration was approximately 100 mg / 1.8 mL. Each tube was then heated in a heating block set at 110° C. The sample tubes were repeatedly vortexed and heated to obtain a homogenous flowing fluid. 1 H NMR spectra were obtained on a BRUKER AVANCE 600 MHz spectrometer equipped with a 10 mm C / H DUAL cryoprobe. Standard single pulse 1 H NMR experiments were performed using the following acquisition parameters: 70 s relaxation time, 17.2 μs 90 degree pulse, 32 scans. The spectrum center was 1.3 ppm and the spectrum width was 20 ppm. All measurements were performed at 110 °C without sample spinning. 1 H NMR spectra were referenced to the resonance peak of the solvent (residual protonated tetrachloroethane) at 5.99 ppm. For samples containing Cr, data were acquired with a relaxation time of 16 seconds and 128 scans. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] The present disclosure provides a method. In one embodiment, the method includes providing an initial cable core. The initial cable core includes (i) a conductor and (ii) an initial insulation layer. The initial insulation layer includes (a) a crosslinkable polymer composition comprised of an ethylene-based polymer comprised of (1) an ethylene monomer, (2) an optional α-olefin comonomer, and (3) an optional organosiloxane comonomer. The crosslinked polymer composition further includes (b) dicumyl peroxide (DCP), (c) a Si-H containing acetophenone (AP) scavenger, (d) an optional curing coagent, and (e) an optional antioxidant. The method includes subjecting the initial cable core to a crosslinking procedure sufficient to crosslink the crosslinkable polymer composition to form a cable core having a crosslinked insulation layer.

[0035] 1. Initial cable core The method includes providing an initial cable core. The initial cable core includes (i) a conductor, (ii) a first polymeric semiconductive layer, and (iii) an initial insulating layer composed of a crosslinkable polymer composition. A "conductor," as used herein, is one or more wires or fibers for conducting heat, light, and / or electricity. The conductor may be a single wire / fiber or multiple wires / fibers, and may be in stranded or tubular form. Non-limiting examples of suitable conductors include metals such as silver, gold, copper, carbon, and aluminum. The conductor may also be an optical fiber made of either glass or plastic. A "cable," as used herein, means at least one wire or optical fiber within a sheath, e.g., an insulating covering or a protective outer jacket. Typically, a cable is two or more wires or two or more optical fibers bonded together, typically within a common insulating covering and / or protective jacket. The individual wires or fibers inside the sheath may be bare, covered, or insulated. A combination cable may contain both electrical wires and optical fibers. The cables can be designed for low voltage, medium voltage, and / or high voltage applications. AC cables can be prepared according to the present disclosure and can be low voltage, medium voltage, high voltage, or extra high voltage cables. Additionally, DC cables can be prepared according to the present disclosure and can include high voltage or extra high voltage cables. Insulated conductors typically include a conductive core covered with an insulating layer. The conductive core can be solid or braided (e.g., a bundle of threads). Some insulated conductors can also contain one or more additional elements, such as a semiconducting layer(s) and / or a protective cover (e.g., a winding, tape, or sheath). Examples are coated metallic wire and electric cables, including those used in low voltage ("LV", >0 to <5 kilovolt (kV) distribution / transmission applications), medium voltage ("MV", 5 to <69 kV), high voltage ("HV", 69 to 230 kV), and extra-high voltage ("EHV", >230 kV).Power cable evaluation may use AEIC / ICEA standards and / or IEC test methods.

[0036] The initial cable core comprises a first crosslinkable polymer semiconductive layer and an optional second crosslinkable polymer semiconductive layer. In one embodiment, the first crosslinkable polymer semiconductive layer is interposed between the insulating layer composed of the crosslinkable polymer composition and the conductor, and the second crosslinkable polymer semiconductive layer surrounds the insulating layer composed of the crosslinkable polymer composition. Alternatively, the initial insulating layer directly contacts the conductor. The first crosslinkable polymer semiconductive layer and the second crosslinkable polymer semiconductive layer may be composed of the same composition or different compositions. In addition, each crosslinkable polymer semiconductive layer may be crosslinked and thus may initially comprise the crosslinkable polymer composition.

[0037] Suitable polymers for use in the first crosslinkable polymeric semiconducting layer and / or the second crosslinkable polymeric semiconducting layer include, but are not limited to, ethylene-based polymers (such as those described above), ethylene ethyl acrylate copolymers ("EEA"), ethylene butyl acrylate copolymers ("EBA"), ethylene vinyl acetate copolymers ("EVA"), polyolefin elastomers, and combinations of two or more thereof.

[0038] In one embodiment, conductive fillers are present in the first crosslinkable polymeric semiconductive layer and / or the second crosslinkable polymeric semiconductive layer. The conductive fillers are present in an amount ranging from 1 to 50 wt % based on the total weight of each crosslinkable semiconductive layer and include conductive carbon black, conductive carbon (e.g., carbon fibers, carbon nanotubes, graphene, graphite, and expanded graphite platelets), and metal particles. Optional additives include antioxidants, stabilizers, and processing aids.

[0039] 2. Insulation layer The initial cable core includes an initial insulation layer comprised of a crosslinkable polymer composition comprising a) an ethylene-based polymer comprised of (1) ethylene monomer, (2) an optional α-olefin comonomer, and / or (3) an optional organosiloxane comonomer. The crosslinkable polymer composition further comprises (b) dicumyl peroxide (DCP), (c) a Si-H containing AP scavenger, (d) an optional curing coagent, and (e) an optional antioxidant.

[0040] The ethylene-based polymer in the crosslinkable polymer composition of the initial insulating layer is a polymer that is a mixture of (1) ethylene monomer, (2) an optional α-olefin comonomer (e.g., ethylene / C 4 ~C 8 α-olefin copolymers), and / or (3) optional organosiloxane comonomers.

[0041] In one embodiment, the ethylene-based polymer is (i) a density between 0.90 g / cc and 0.93 g / cc, or between 0.91 g / cc and 0.92 g / cc; and / or (ii) An ethylene homopolymer having a MI of 0.1 g / 10 min to 10.0 g / 10 min, or 0.5 g / 10 min to 5.0 g / 10 min, or 1.0 g / 10 min to 3.0 g / 10 min.

[0042] Non-limiting examples of suitable ethylene homopolymers include LDPE DXM-446 and LDPE 505i available from Dow, Inc.

[0043] In one embodiment, the ethylene-based polymer is a telechelic ethylene-based polymer or a monochelic ethylene-based polymer. A "telechelic ethylene-based polymer" is defined as having the formula I:A 1 L 1 L 2 A 2 (In the formula, L 1 is an ethylene / α-olefin copolymer (e.g., ethylene / C 4 ~C 8α-olefin copolymer) and (L 1 (Bivalent) is A 1 and L 2 (note that it is bound to A 1 is the following: a) a vinyl group, b) Formula CH 2 =C(Y 1 )-vinylidene group, c) Formula Y 1 a vinylene group of CH=CH-; d) a vinyl group and a compound of formula Y 1 Mixtures of CH=CH- with vinylene groups, e) a vinyl group and a compound of the formula CH 2 =C(Y 1 )- with vinylidene groups, f) Formula CH 2 =C(Y 1 )- and a vinylidene group of the formula Y 1 Mixtures of CH=CH- with vinylene groups, and g) a vinyl group and a compound of the formula CH 2 =C(Y 1 )- and a vinylidene group of the formula Y 1 and a mixture of CH=CH- and vinylene groups; Y 1 independently for each occurrence, C 1 ~C 30 is a hydrocarbyl group, L 2 is C 1 ~C 32 is a hydrocarbylene group, A 2 is a hydrocarbyl group containing a hindered double bond) with an ethylene and an α-olefin comonomer (e.g., ethylene / C 4 ~C 8 α-olefin copolymer).

[0044] A "monochelic ethylene polymer" is a polymer having the formula II:A 1 L 1 (In the formula, L 1 , L 1is an ethylene / α-olefin copolymer, e.g., ethylene / C 4 ~C 8 α-olefin copolymer (L 1 (Single-valued) is A 1 (note that it is bound to A 1 is the following: a) a vinyl group, b) Formula CH 2 =C(Y 1 )-vinylidene group, c) Formula Y 1 a vinylene group of CH=CH-; d) a vinyl group and a compound of formula Y 1 Mixtures of CH=CH- with vinylene groups, e) a vinyl group and a compound of the formula CH 2 =C(Y 1 )- with vinylidene groups, f) Formula CH 2 =C(Y 1 )- and a vinylidene group of the formula Y 1 Mixtures of CH=CH- with vinylene groups, and g) a vinyl group and a compound of the formula CH 2 =C(Y 1 )- and a vinylidene group of the formula Y 1 and a mixture of CH=CH- and vinylene groups; Y1 is independently selected from the group consisting of C 1 ~C 30 Copolymers of ethylene and α-olefin comonomers (e.g., ethylene / C 4 ~C 8 α-olefin copolymer).

[0045] Telechelic and monochelic polymers are disclosed in WO 2020 / 140058 and WO 2020 / 140067, each of which is incorporated herein by reference. Telechelic and monochelic polymers are interchangeably referred to as "unsaturated POE" or "UPOE".

[0046] In one embodiment, the ethylene-based polymer in the crosslinkable polymer composition of the initial insulating layer is an ethylene / organosiloxane copolymer comprising (i) units derived from ethylene, (ii) 0.01% to 0.5% by weight of units derived from a comonomer, and (iii) optionally, units derived from a termonomer. The comonomer is represented by the formula (3): [R 1 ,R 2 SiO 2 / 2 ] n (In the formula, n is an integer of 3 or more, Each R 1 are independently 2 ~C 4 ) alkenyl or H 2 C=C(R 1a )-C(=O)-O-(CH 2 ) m - and R 1a is H or methyl, m is an integer from 1 to 4; Each R 2 are independently H, (C 1 ~C 4 ) alkyl, phenyl, or R 1 Ethylene-based polymers having monocyclic organosiloxanes (MOCOS) of formula (3) are interchangeably referred to as "ethylene / MOCOS copolymers."

[0047] In one embodiment, the MOCOS of formula (3) is 2,4,6-trimethyl-2,4,6-trivinyl-cyclotrisiloxane, having the following structure (B): Vi ) 3 " (CAS number 3901-77-7):

[0048] [ka]

[0049] In one embodiment, the MOCOS of formula (3) is 2,4,6,8-tetramethyl-2,4,6,8-tetravinyl-cyclotetrasiloxane, having the following structure (C): Vi ) 4 " (CAS number 2554-06-5):

[0050] [ka]

[0051] In one embodiment, the MOCOS of formula (3) is 2,4,6,8,10-pentamethyl-2,4,6,8,10-pentavinyl-cyclopentasiloxane, (D Vi ) 5 It is.

[0052] The MOCOS comonomer of formula (3) is present in the ethylene-based polymer in an amount from 0.01 weight percent to 2 weight percent, or from 0.01 weight percent to 0.5 weight percent, or from 0.05 weight percent to 0.45 weight percent, or from 0.1 weight percent to 0.40 weight percent, or from 0.3 weight percent to 0.5 weight percent, or from 0.15 weight percent to 0.30 weight percent, or from 0.05 weight percent to 0.15 weight percent. The weight percentages are based on the total weight of the ethylene-based polymer composition, i.e., the ethylene / MOCOS copolymer.

[0053] The crosslinkable polymer composition in the initial insulating layer comprises 0.1% to 2.4%, or 0.1% to 2.0%, or 0.7% to 1.5%, or 0.7% to 1.2% by weight of dicumyl peroxide (DCP), where the weight percentages are based on the total weight of the crosslinkable polymer composition.

[0054] The crosslinkable polymer composition in the initial insulating layer comprises a Si-H containing AP scavenger. "Si-H containing AP scavenger," as used herein, is a compound represented by Formula 4:

[0055] [ka] (In the formula, R 1 , R2 and R 3 are the same or different, and each R 1 , R 2 and R 3 are individually selected from H, substituted hydrocarbyl, unsubstituted hydrocarbyl, substituted heterohydrocarbyl, unsubstituted heterohydrocarbyl, or siloxane. The Si-H containing (AP) scavenger is a separate and distinct component from the ethylene-based polymer. In the crosslinkable polymer composition, the Si-H containing (AP) scavenger is not a comonomer to the ethylene-based polymer. Non-limiting examples of suitable Si-H containing (AP) scavengers of formula 4 include the following s1) to s20):

[0056] [ka] and combinations thereof.

[0057] In one embodiment, the Si-H containing (AP) scavengers include polyhedral oligomeric silsesquioxanes containing SiH groups, and / or inorganic silicas containing SiH groups, such as dimethylhydrogensiloxy modified silica.

[0058] The crosslinkable polymer composition may optionally include a curing coagent. Non-limiting examples of suitable curing coagents include triallyl isocyanurate ("TAIC"), triallyl cyanurate ("TAC"), triallyl trimellitate ("TATM"), N2,N2,N4,N4,N6,N6-hexaallyl-1,3,5-triazine-2,4,6-triamine ("HATATA"), triallyl orthoformate, pentaerythritol triallyl ether, triallyl citrate, and triallyl aconitate, α-methyl styrene dimer ("AMSD"), acrylate coagents such as trimethylolpropane triacrylate, triacrylate, "TMPTA"), trimethylolpropane trimethylacrylate, "TMPTMA", ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, and propoxylated glyceryl triacrylate, vinyl coagents such as 1,2-high vinyl content polybutadiene, trivinyl cyclohexane, "TVCH", 4,6-trimethyl-2,4,6-trivinyl-cyclotrisiloxane (VD3), 2,4,6,8-tetramethyl-2,4,6,8-tetravinyl-cyclotetrasiloxane (VD4). 2,4,6,8,10-pentamethyl-2,4,6,8,10-pentavinyl-cyclopentasiloxane, VD5.When present, the curing coagent is present in an amount of from greater than 0 to 5 wt%, or from 0.1 to 2.5 wt%, or from 0.2 to 2 wt%, or from 0.3 to 1.5 wt%, or from 0.4 to 1.0 wt%, based on the total weight of the crosslinkable polymer composition.

[0059] The crosslinkable polymer composition includes an optional antioxidant. When present in the crosslinkable polymer composition, the antioxidant is a collection of organic or oxygen molecules that inhibit oxidation. The antioxidant serves to impart antioxidant properties to the polyolefin composition and / or the crosslinked polyolefin product. Non-limiting examples of suitable antioxidants include 2,6-di-tert-butyl-4-methylphenol; 2-(tert-butyl)-4,6-dimethylphenol; 2-(tert-butyl)-4-ethyl-6-methyl-phenol; 2-(tert-butyl)-4-isopropyl-6-methylphenol; 2,4-di-tert-butyl-6-methylphenol; 2,4,6-tri-tert-butylphenol; 2,6-di-tert-butyl-4-isopropylphenol; 2,6-Di-tert-butyl-4-ethylphenol;2,6-di-tert-butylphenol;2-(tert-butyl)-6-methylphenol;2,6-diisopropyl-4-methylphenol;2-isopropyl-4,6-dimethylphenol;4-ethyl-2-isopropyl-6-methylphenol;2,4-diisopropyl-6-methylphenol;4-(tert-butyl)-2-isopropyl-6-methylphenol;2-(tert-butyl)-6-isopropyl 4-Methyl-2,6-di-tert-pentylphenol;2,4-Dimethyl-6-(tert-pentyl)phenol;2-ethyl-4-methyl-6-(tert-pentyl)phenol;2-ethyl-4-methyl-6-(tert-pentyl)phenol;2-tert-butyl-4,6-diisopropylphenol;2,4-Di-tert-butyl-6-isopropylphenol;2-tert-butyl-4-methyl-6-(tert-pentyl)phenol;4-methyl-2,6-di-tert-pentylphenol;2,4-dimethyl-6-(tert-pentyl)phenol;2-ethyl-4-methyl-6-( tert-Pentyl)phenol;2-(tert-butyl)-6-ethyl-4-methylphenol;2-Ethyl-6-isopropyl-4-methylphenol;2,6-Diethyl-4-methylphenol;Octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (IRGANOX1076);Pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate (IRGANOX1010);1,3,5-Tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (IRGANOX3114);(1,3,5-trimethyl-2,4,5-tris(3',5'-di-tert-butyl)-4'-hydroxybenzyl)-benzene (IRGANOX1330);Hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (IRGANOX259);Benzenepropanoic acid, 3,5-bis(1,1 -Dimethyl-ethyl)-4-hydroxy-C7-C9 branched alkyl ester (IRGANOX1135);3,5-bis(1,1-dimethylethyl)-4-hydroxybenzenepropanoic acid thiodi-2,1-ethanediyl ester (IRGANOX1035);N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide] (IRGANOX1098);1,2-bis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamoyl)hydrazine (I RGANOX1024;2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol (IRGANOX565);Ethylene bis(oxyethylene) bis-(3-(5-tert-butyl-4-hydroxy-m-tolyl)-propionate) (IRGANOX245);4,6-bis(octylthiomethyl)-o-cresol (IRGANOX1520);4,6-bis(dodecylthiomethyl)-o-cresol (IRGANOX1726);3,5-Tris (4-(tert-butyl)-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazinane-2,4,6-trione (CYANOX1790); Phenol, 2-(5-chloro-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)-4-methyl (TINUVIN326); Phenol, 2-(2H-benzotriazol-2-yl)-4-methyl (TINUVINP); 2-(2H-benzotriazol-2-yl)-4,6-ditertpentylphenol (TINUVIN328);2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (TINUVIN329);Phenol, 2-(2H-benzotriazol-2-yl)-4-methyl-6-dodecyl (TINUVIN571);2,2'-methylenebis(6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol) (TINUVIN360);2-(4,6-diphenyl-1,3,5-triazine- 2-(2H-benzotriazol-2-yl)-5-[(hexyl)oxy]-phenol (TINUVIN 1577); 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (TINUVIN 234); 4,4''-thiobis(2-tert-butyl-5-methylphenol (TBM-6); 3,4-dihydro-2,5,7,8-tetramethyl-2-(4,8,12-trimethyltridecyl)-2H-1-benzopyran-6-ol (IRGANOX E201), and combinations thereof. When present, antioxidants are present in an amount of greater than 0% to 5% by weight, or 0.01% to 2% by weight, or 0.05% to 1% by weight, or 0.1% to 0.5% by weight, or 0.15% to 0.3% by weight, based on the total weight of the crosslinkable polymer composition;

[0060] The crosslinkable polymer composition may also contain other additives, including, but not limited to, processing aids, fillers, carbon black, nanoparticles, coupling agents, UV absorbers or stabilizers, antistatic agents, nucleating agents, slip agents, plasticizers, lubricants, viscosity modifiers, tackifiers, antiblocking agents, surfactants, extender oils, acid scavengers, flame retardants, and metal deactivators. When present, additives other than fillers are typically used in amounts ranging from 0.001% to 10% by weight, or from 0.01% to 7% by weight, or from 0.05% to 5% by weight, or from 0.1% to 3% by weight, based on the total weight of the crosslinkable polymer composition. When fillers are present, they are present in amounts ranging from 1% to 50% by weight, or from 2% to 40% by weight, or from 5% to 30% by weight, or from 10% to 20% by weight, based on the total weight of the crosslinkable polymer composition. Non-exemplary examples of suitable fillers include clays, precipitated silicas and silicates, fumed silica, calcium carbonate, ground minerals, aluminum trihydroxide, magnesium hydroxide, and carbon black having a typical arithmetic mean particle size greater than 15 nanometers.

[0061] 3. Crosslinking Procedure The method includes subjecting the initial cable core to a crosslinking procedure sufficient to crosslink the crosslinkable polymer composition to form a cable core having a crosslinked insulation layer. The initial cable core containing the inner and outer semiconductive layers and the insulation layer can be prepared in various types of extruders, for example single screw or twin screw type. A description of a conventional extruder can be found in U.S. Pat. No. 4,857,600, which is incorporated herein by reference. A non-limiting example of coextrusion and extruders can be found in U.S. Pat. No. 5,575,965, which is incorporated herein by reference. A typical extruder has a hopper at its upstream end and a die at its downstream end. The hopper feeds into a barrel containing a screw. At the downstream end, there is a screen pack and a breaker plate between the end of the screw and the die. The screw section of the extruder can be considered to be divided into three sections, a feed section, a compression section, and a metering section, and two zones, a back heating zone and a front heating zone, which sections and zones run from upstream to downstream. In the alternative, there may be multiple (three or more) heating zones along the axis from upstream to downstream. When the extruder has two or more barrels, the barrels are connected in series. The length to diameter ratio of each barrel ranges from 15:1 to 30:1.

[0062] In one embodiment, the cable core is prepared from a continuous vulcanization line consisting of a single extruder, vulcanization tube, and cooling tube.

[0063] After extrusion, the resulting initial cable core is subjected to or otherwise subjected to a crosslinking procedure to crosslink the crosslinkable polymer composition in the initial insulation layer. The initial cable core may enter a heat curing zone downstream of the extrusion die. The heat curing zone is maintained at a temperature in the range of 150°C to 400°C, or 160°C to 350°C, or 170°C to 300°C. The heat curing zone is heated by pressurized steam or inductively heated with pressurized nitrogen gas. The crosslinking procedure provides a crosslinked insulation layer from the crosslinkable polymer composition.

[0064] In one embodiment, one or both of the first (inner) polymeric semiconducting layer and / or the second (outer) polymeric semiconducting layer are crosslinked during a crosslinking procedure.

[0065] In one embodiment, after the crosslinking step, the method includes cooling the cable core with the crosslinked insulation layer to ambient temperature to form a cooled cable core with the crosslinked insulation layer. The term "ambient temperature" as used herein refers to a temperature between 20°C and 24°C, or between 21°C and 23°C.

[0066] The crosslinking procedure forms or otherwise creates dicumyl peroxide decomposition by-products (or "DCP decomposition by-products") in the crosslinked insulating layer. The term "dicumyl peroxide decomposition by-products" refers to decomposition products formed during the crosslinking step and / or the curing step and / or the cooling step by the decomposition and reaction of dicumyl peroxide. DCP decomposition by-products include cumyl alcohol (CA), acetophenone (AP), methane, alpha methyl styrene, and combinations thereof. The Si-H containing (AP) scavengers react with, inhibit, or otherwise quench acetophenone that is generated during the crosslinking procedure and / or any subsequent curing and / or cooling.

[0067] After the crosslinking step, the method includes cooling the cable core with the crosslinked insulation layer to ambient temperature to obtain an R of less than 0.57. AP / CAThe method includes forming a cooled cable core having a cross-linked insulation layer having a cross-linked insulation layer having a value of 0.01 to 0.01. The respective amounts of acetophenone and cumyl alcohol are determined by headspace gas chromatography / flame ionization detection as described in the Examples section below. The term "cooled cable core having a cross-linked insulation layer" as used herein refers to a cable core having a cross-linked insulation layer immediately after the cross-linking procedure, specifically 1 to 60 minutes after the cable core has been cooled to or otherwise reached ambient temperature, and "cooled cable core having a cross-linked insulation layer" refers to a post-cross-linked cable core 1 to 60 minutes after reaching ambient temperature and prior to the degassing procedure. "Cold crosslinked XLPE plaque" (and / or "cold crosslinked POE plaque"), as used herein, refers to the crosslinked ethylene-based polymer plaque used to replicate the cooled cable core with crosslinked insulation layer in the Examples section (below), i.e., the cold crosslinked XLPE plaque (and / or cold crosslinked POE plaque) immediately after the crosslinking procedure, specifically, 1 to 60 minutes after the plaque has been cooled to or otherwise reached ambient temperature, and "cold crosslinked XLPE (and / or "cold crosslinked POE plaque")" refers to the post-crosslinked plaque 1 to 60 minutes after reaching ambient temperature and prior to the degassing procedure. AP / CA The values ​​indicate the reduction in AP in this method. With the same DCP loading, the ratio of AP to CA is reduced (i.e., R AP / CA value decreases), the AP concentration decreases.

[0068] In one embodiment, the cooling cable core having a crosslinked insulation layer is "composition (C)" and "similar composition (SC)" is defined as "a composition identical to composition (C) except that it does not contain component (c), i.e., the Si-H containing (AP) scavenger." Composition (C) is R AP / CA Value "R AP / CA (C)" and composition (SC) has R AP / CA Value (SC) "R AP / CA Composition (C) has the following formula 5: formula 5 R AP / CA % decrease in = [(RAP / CA (C)-R AP / CA (SC)) / R AP / CA (SC)] × 100% Determined by, R AP / CA R at least 2.0% greater than (SC) AP / CA Decline in the RiR AP / CA "

[0069] In one embodiment, the cooling cable core having a crosslinked insulation layer, i.e., composition (C), has an R of 2.0% or more to 35% or less, or 5% or more to 30% or less, or 10% or more to 25% or less, or 10% or more to 20% or less. AP / CA There is a decrease in

[0070] In one embodiment, the method includes degassing a cooled cable core having a crosslinked insulation layer at a temperature between 50° C. and 80° C. to reduce the amount of acetophenone in the crosslinked insulation layer to less than 1000 ppm, wherein the degassing time is reduced by more than 2%, or more than 5%, or more than 10%, or more than 15%, or more than 20%, or more than 30%, or more than 35%, or more than 40%, or more than 45%.

[0071] 4. Cable The present disclosure provides a cable. In one embodiment, the cable includes a cable core. The cable core is comprised of (i) a conductor and (ii) a crosslinked insulation layer. The crosslinked insulation layer is formed from a crosslinkable polymer composition comprised of an ethylene-based polymer comprised of (1) ethylene monomer, (2) an optional organosiloxane comonomer, and / or (3) an optional organosiloxane comonomer. The crosslinkable polymer composition further comprises b) dicumyl peroxide (DCP) and a Si-H containing (AP) scavenger, (c) a Si-H containing (AP) scavenger, (d) an optional curing coagent, and (e) an optional antioxidant.

[0072] It is understood that DCP is consumed during crosslinking to form a crosslinked insulation layer of the cable. In the crosslinked insulation layer of the cable, the Si-H-containing (AP) scavenger is composed of the following (s1) to (s20):

[0073] [ka] and combinations thereof.

[0074] In one embodiment, the cable includes a cable core having a cross-linked insulation layer comprised of 95% to 99.9% by weight of ethylene homopolymer and 0.1% to 2.0%, or 0.2% to 1.5%, or 0.3% to 1.0%, or 0.4% to 0.8% by weight of a Si-H containing (AP) scavenger. The weight percentages are based on the total weight of the cross-linked insulation layer. In further embodiments, the cross-linked insulation layer comprises 0.1% to 2%, or 0.2% to 1.5%, or 0.3% to 1%, or 0.4% to 0.8% of a curing coagent. It is understood that the ethylene homopolymer, the Si-H containing (AP) scavenger, and the optional curing agent total 100% by weight of the cross-linked insulation layer.

[0075] In one embodiment, the cable is made of 95% to 99.9% by weight telechelic ethylene / C 4 ~C 8 The cable core includes a crosslinked insulation layer comprised of an α-olefin copolymer and 0.1 wt% to 2.0 wt%, or 0.2 wt% to 1.5 wt%, or 0.3 wt% to 1.0 wt%, or 0.4 wt% to 0.8 wt% of a Si-H containing (AP) scavenger. The weight percentages are based on the total weight of the crosslinked insulation layer. In further embodiments, the crosslinked insulation layer comprises 0.1 wt% to 2.0 wt%, or 0.2 wt% to 1.5 wt%, or 0.3 wt% to 1 wt%, or 0.4 wt% to 0.8 wt% of a curing coagent. The telechelic ethylene / C 4 ~C 8 It is understood that the α-olefin copolymer, the Si—H containing (AP) scavenger, and the optional curing agent together make up 100% by weight of the crosslinked insulating layer.

[0076] In one embodiment, the cable is made of 95% to 99.9% by weight of monoethylene / carbonyl 4 ~C8 The cable core includes a crosslinked insulation layer comprised of an α-olefin copolymer and 0.1 wt% to 2.0 wt%, or 0.2 wt% to 1.5 wt%, or 0.3 wt% to 1.0 wt%, or 0.4 wt% to 0.8 wt% of a Si-H containing (AP) scavenger. The weight percentages are based on the total weight of the crosslinked insulation layer. In further embodiments, the crosslinked insulation layer comprises 0.1 wt% to 2.0 wt%, or 0.2 wt% to 1.5 wt%, or 0.3 wt% to 1.0 wt%, or 0.4 wt% to 0.8 wt% of a curing coagent. Monochelic ethylene / C 4 ~C 8 It is understood that the α-olefin copolymer, the Si—H containing (AP) scavenger, and the optional curing agent together make up 100% by weight of the crosslinked insulating layer.

[0077] In one embodiment, the cable includes a cable core having a crosslinked insulation layer comprised of 95% to 99.9% by weight of an ethylene / organosiloxane copolymer and 0.1% to 2.0% by weight, or 0.2% by weight, or 1.5% by weight, or 0.3% to 1.0% by weight, or 0.4% to 0.8% by weight of a Si-H containing (AP) scavenger. The ethylene / organosiloxane copolymer may be any ethylene / MOCOS copolymer previously disclosed herein. The weight percentages are based on the total weight of the crosslinked insulation layer. In further embodiments, the crosslinked insulation layer includes 0.1% to 2.0% by weight, or 0.2% to 1.5% by weight, or 0.3% to 1.0% by weight, or 0.4% to 0.8% by weight of a curing coagent. It is understood that the ethylene / organosiloxene copolymer, the Si-H containing (AP) scavenger and the optional curing agent total 100% by weight of the crosslinked insulating layer.

[0078] In one embodiment, the cross-linked insulating layer is in direct contact with the conductor. The term "direct contact" refers to a layer configuration in which the cross-linked insulating layer is located directly adjacent to the conductor, with no intervening layer or structure between the conductor and the cross-linked insulating layer.

[0079] In one embodiment, the cable includes a cable core with a first cross-linked polymeric semiconductive layer disposed or otherwise interposed between a cross-linked insulating layer and a conductor. The first cross-linked polymeric semiconductive layer surrounds the conductor and the cross-linked insulating layer surrounds the first cross-linked semiconductive layer. In a further embodiment, a second cross-linked polymeric semiconductive layer surrounds the cross-linked insulating layer. The first cross-linked polymeric semiconductive layer and the second cross-linked polymeric semiconductive layer may be composed of the same composition or different compositions, as previously disclosed herein.

[0080] In one embodiment, the cable includes a cooled cable core, i.e., a cable core immediately after crosslinking. The cooled cable core includes a crosslinked insulation layer having decomposition by-products selected from the group consisting of cumyl alcohol (CA), acetophenone (AP), methane, alpha methyl styrene, and combinations thereof. The crosslinked insulation layer of the cooled cable core has an AP / CA ratio of less than 0.57 at a time from 1 minute after the crosslinking procedure and cooling to ambient temperature to 60 minutes after the crosslinking procedure and cooling to ambient temperature and before the degassing procedure.

[0081] In one embodiment, the cable includes a cooling cable core having a crosslinked insulation layer identified as composition (C). A similar composition "(SC)" (as defined herein above) is the same composition as (C) except that it does not contain component (c), i.e., the Si-H containing (AP) scavenger. Composition (C) is a composition comprising R AP / CA (C), and composition (SC) has R AP / CA (SC). Composition (C) has the following formula 5: formula 5 R AP / CA % decrease in = [(R AP / CA (C)-R AP / CA (SC)) / R AP / CA (SC)] × 100% Determined by, R AP / CA R at least 2.0% greater than (SC) AP / CA Decline in the RiR AP / CA "

[0082] In one embodiment, the cooling cable core having a crosslinked insulation layer, i.e., composition (C), has an R of 2.0% or more to 50% or less, or 5% or more to 40% or less, or 10% or more to 30% or less, or 10% or more to 20% or less. AP / CA There is a decrease in

[0083] By way of example and not by way of limitation, several embodiments of the present disclosure will now be detailed in the following examples.

[0084] 1.Material The materials used in the comparative samples (CS) and inventive examples (IE) are provided in Tables 1A-1C below.

[0085] [Table 1]

[0086] [Table 2]

[0087] [Table 3]

[0088] 2. Calibration Curve Setup for AP and CA Measurements 2.1: Preparation of crosslinked blank sheet containing no AP or CA (Luperox101 does not produce AP or CA) a. 1 wt% of Luperox 101 was immersed in a POE blank sheet for 6 hours (hr) at 50°C. 1 wt% of Luperox 101 was immersed in an LDPE blank sheet for 6 hours at 70°C. b. A POE blank sheet and an LDPE blank sheet are compression molded at 180°C to prepare two respective crosslinked plaques, each having a thickness of 1 mm. c. Degas each plaque in a vacuum oven at 70° C. for 1 day.

[0089] 2.2: Preparation of cross-linked POE and XLPE calibration samples a. Cut a 1 gram (g) sample from the crosslinked POE blank or XLPE blank sheet and place into a 20 milliliter (mL) headspace vial. b. Calibration standards were prepared by injecting 0.005 g of AP standard chemical into a headspace vial containing 1 g of POE or XLPE sample. The headspace vial was then sealed with a crimp cap and is hereafter referred to as the "calibration sample." c. Calibration standards were prepared by injecting 0.005 g of CA standard chemical into a headspace vial containing 1 g of POE / XLPE sample. The headspace vial was then sealed with a crimp cap and is hereafter referred to as the "calibration sample."

[0090] 2.3: Add the calibration samples to the HSGC under the conditions in Table 1 for analysis to obtain the correlation between the peak area from the HSGC and the AP or CA concentration in the calibration samples.

[0091] [Table 4]

[0092] 3. Sample Preparation for AP and CA Measurements 3.1 Compression Molding to Prepare Crosslinked Plaques from Example Compounds Approximately 30 g of sample compound in pellet form is placed between two pieces of PET film in a 1 mm thick mold. The filled mold is then placed in a hot press machine (LabTech). b.Preheat at 120℃ for 10 minutes. c. Ventilate 8 times and for 0.2 seconds each. d. The platens are closed and a pressure of 15 MPa is applied to the mold for 20 minutes while the temperature is increased to 182°C within 6.5 minutes. e. The mold is continued to be maintained at 15 MPa and cooled to 24°C. f. Remove the mold from the machine.

[0093] 3.2 Headspace Gas Chromatography (GC) Sample Preparation a. The cured plaque with two PET films on either side is removed from the mold. b. Quickly peel off the PET film. c. Cut out two sheets (approximately 1 g) of the center of the plaque and place them into two headspace GC vials and immediately seal the vials. d. The sealed GC headspace vial is weighed and the sample weight can be calculated by the difference between the empty vial and the vial containing the sample.

[0094] 4.AP and CA measurements The sealed headspace vial containing 1 g of plaque sample was transferred to a headspace autosampler and conditioned at 150 °C for 30 minutes (min). An aliquot of 1 ml of gas sample in the headspace vial was then injected and analyzed directly by GC / FID (gas chromatography / flame ionization detector). The GC oven was programmed from 50 °C (2 min) to 220 °C (8 min) at 15 °C min. The FID temperature was 250 °C, with hydrogen flow rate of 40 mL min, air flow rate of 400 mL min, and nitrogen flow rate of 25 mL min. The inlet was operated at 250 °C in split mode with a ratio of 50:1, the separation column was a 30 m × 0.32 mm i.d. × 0.50 μm DB-WAX capillary column, and the helium carrier gas flow rate was 2 mL min.

[0095] 5.Calculation The concentrations of acetophenone and cumyl alcohol were calculated according to the following formulas in Table 2B below.

[0096] [Table 5] * POE refers to cooled crosslinked POE plaque; ** XLPE refers to chill crosslinked XLPE plaque.

[0097] As an example, Table 2C provides the calculation results of (i) AP and (ii) CA for CS-2, IE-10, and IE-11. Two specimens are taken for each sample of CS-2, IE-10, and IE-1. The final AP and CA values ​​are the average of these two specimens. AP / CA Values ​​are the final AP value divided by the final CA value for each sample.

[0098] [Table 6] ** XLPE refers to cross-linked plaque.

[0099] [Table 7] ** XLPE refers to cross-linked plaque.

[0100] 5. Results and Discussion: As mentioned above, DCP decomposes during the curing step to generate cumyloxyl radicals. Some of the cumyloxyl radicals undergo beta-scission to form AP and methyl radicals. Both cumyloxyl and methyl radicals abstract hydrogen from polyethylene and initiate crosslinking of the polymer to form CA and methane. The concentration of these by-products in the freshly cured samples is determined by the amount of DCP added. The higher the amount of DCP added, the higher the by-product concentration.

[0101] As shown in Table 3, 3000 ppm AP and 5200 ppm CA were present in the freshly cured CS-1 sample (cooled crosslinked plaque) containing 1.2% DCP, and R AP / CAThe inventors have surprisingly found that in the presence of SiH-1, SiH-2, SiH-3 and SiH-4 (i.e., in IE-1, IE-2, IE-3, IE-4 and IE-5), R AP / CA The R value decreased, especially for IE-3 with 0.7% SiH-4, compared to CS-1. AP / CA It was found that a 35.7% reduction in the amount of oxidized carbon dioxide was achieved. Without being bound by any particular theory, it is believed that the Si radical initiated by the active radical in the system adds to the carbonyl group of AP and bonds to the Si-H scavenger via the Si-OC bond.

[0102] At higher DCP loadings, i.e., IE-6 and 7 in Table 3, SiH-4 effectively reduces AP. AP / CA The value (0.372-0.378) is similar to that of IE-3 (0.369).

[0103] Additional curing coagents such as TAIC and VD4 do not affect the reduction in AP, as shown in IE-8 and IE-9.

[0104] [Table 8]

[0105] As shown in Table 3, the comparison of IE-1, IE-2, IE-3, IE-4, IE-5, IE-6, IE-7, IE-8, and IE-9 with CS-1 shows that SiH-1, SiH-2, SiH-3, and SiH-4 are R AP / CA IE-1 to IE-9 are less than 0.57 or R of 0.350 to 0.559. AP / CA Value and RiR of 13% to 38% AP / CA (with respect to the cooled crosslinked plaque).

[0106] [Table 9]

[0107] As shown in Table 4, SiH-4 has an RiR of 34% to 39%. AP / CA and the corresponding R AP / CA The values ​​were between 0.340 and 0.390 (for cold crosslinked plaques composed of copolymers of ethylene and VD4).

[0108] [Table 10]

[0109] As shown in Table 5, the comparison of IE-14 and IE-15 with CS-6 shows that SiH-5 (containing a vinyl group) and R AP / CA IE-14 and IE-15 have an R of 0.400 to 0.470. AP / CA Value and RiR of 15% to 30% AP / CA (with respect to the cooled crosslinked plaque).

[0110] Comparison of IE16 and IE-17 with CS-7 shows that SiH-4 is R AP / CA IE-16 and IE-17 exhibited R values ​​of 0.470 to 0.480 in the presence of antioxidants. AP / CA Value and RiR of 10% to 12% AP / CA (with respect to the cooled crosslinked plaque).

[0111] [Table 11]

[0112] As shown in Table 6, SiH-4 achieves a reduction in AP in POE (UPOE). Comparison of IE18 and IE-19 with CS-8 and CS-9, respectively, shows that SiH-4 achieves a reduction in AP in POE (UPOE). AP / CA IE-18 and IE-19 have an R of 0.370 to 0.420. AP / CA Value and RiR of 28% to 40% AP / CA This indicates that the condition is present.

[0113] The data in Tables 3-6 show that SiH-containing (AP) scavengers are effective in reducing acetophenone in different polymer matrix platforms and in combination with different ingredients such as curing coagents and antioxidants.

[0114] The present disclosure is not limited to the embodiments and examples contained herein, but is specifically intended to include portions of the embodiments and modified forms of those embodiments, including combinations of elements of different embodiments, within the scope of the following claims.

Claims

1. 1. A method comprising: The method further comprising: (i) a conductor; (ii) providing an initial cable core comprising an initial insulation layer comprising a crosslinkable polymer composition; subjecting said initial cable core to a crosslinking procedure sufficient to crosslink said crosslinkable polymer composition to form a cable core having a crosslinked insulation layer; Including, The crosslinkable polymer composition comprises: (a) (1) ethylene monomer, (2) an optional α-olefin comonomer; (3) an ethylene-based polymer, optionally including an organosiloxane comonomer; and (b) dicumyl peroxide (DCP); (c) a Si—H containing (AP) scavenger; and (d) an optional curing coagent; and (e) an optional antioxidant; and A method comprising:

2. 10. The method of claim 1, comprising cooling the cable core with the cross-linked insulation to ambient temperature to form a cooled cable core with the cross-linked insulation.

3. said crosslinking step forms dicumyl peroxide decomposition by-products selected from the group consisting of cumyl alcohol (CA), acetophenone (AP), methane, alpha methyl styrene, and combinations thereof; The method further comprising: The cable core having the cross-linked insulation layer is cooled to ambient temperature to obtain an R of less than 0.

57. AP/CA 3. The method of claim 2, further comprising forming a cooling cable core having a cross-linked insulation layer having a value.

4. The crosslinked insulation layer of the cooled cable core has an R of less than 0.57 from 1 minute after the crosslinking procedure and cooling to ambient temperature to 60 minutes after the crosslinking procedure and cooling to ambient temperature. AP/CA The method of claim 3 having a value.

5. the cooling cable core having said crosslinked insulation layer is composition (C), and a similar composition (SC) is defined as a composition identical to (C) except that it does not contain component (c), i.e., said Si—H containing (AP) scavenger; The composition (C) is R AP/CA and the composition (SC) has R AP/CA (SC), The composition (C) is a compound represented by the formula 5 Formula 5 R AP/CA % decrease in = [(R AP/CA (C)-R AP/CA (SC)) / R AP/CA (SC)] × 100% R is determined by AP/CA R at least 2.0% greater than (SC) AP/CA The method according to any one of claims 2 to 4, having a reduction in

6. degassing the cooled cable core having the cross-linked insulation layer after the cooling; and reducing the amount of acetophenone in the crosslinked insulation layer to less than 1000 ppm.

7. The Si—H-containing (AP) scavenger is selected from the following (s1) to (s20): 【Chemistry 1】 The method of any one of claims 1 to 6, wherein the compound is selected from the group consisting of:

8. A cable including a cable core, The cable core is (i) a conductor; (ii) a cross-linked insulating layer, the cross-linked insulating layer comprising: (a) (1) ethylene monomer, (2) an optional α-olefin comonomer; (3) an ethylene-based polymer, optionally including an organosiloxane comonomer; and (b) dicumyl peroxide (DCP); and (c) a Si—H containing (AP) scavenger; and (d) an optional curing coagent; and (e) an optional antioxidant.

9. The Si—H-containing (AP) scavenger is selected from the following (s1) to (s20): 【Chemistry 2】 9. The cable of claim 8, wherein the cable is selected from the group consisting of: and combinations thereof.

10. The cross-linked insulating layer is 95% to 99.9% by weight of an ethylene homopolymer; 0.1% to 1.0% by weight of said Si-H containing (AP) scavenger.

11. The cable of claim 10 comprising 0.1% to 1.0% by weight of a curing aid.

12. The cross-linked insulating layer is 95% to 99.9% by weight of an ethylene / organosiloxane copolymer; 0.1% to 1.0% by weight of said Si-H containing (AP) scavenger.

13. The cable core is 1. A cooling cable core comprising a crosslinked insulation layer comprising decomposition by-products selected from the group consisting of cumyl alcohol (CA), acetophenone (AP), methane, alpha methyl styrene, and combinations thereof; The crosslinked insulation layer of the cooled cable core has an R of less than 0.57 from 1 minute after the crosslinking procedure and cooling to ambient temperature to 60 minutes after the crosslinking procedure and cooling to ambient temperature and before the degassing procedure. AP/CA A cable according to any one of claims 8 to 12, having a value.

14. the cooling cable core having the crosslinked insulation layer is a composition (C), A similar composition (SC) is defined as a composition identical to (C) except that it does not contain component (c), i.e., the Si—H containing (AP) scavenger; The composition (C) is R AP/CA (C), and the composition (SC) has R AP/CA (SC), The composition (C) is R AP/CA This has a reduction in Formula 5 R AP/CA % decrease in = [(R AP/CA (C)-R AP/CA (SC)) / R AP/CA (SC)] × 100% When determined by AP/CA 14. The cable of claim 13, wherein the S is at least 2.0% greater than (SC).

15. a first crosslinked polymer semiconducting layer; and an optional second crosslinked polymeric semiconducting layer.

Citation Information

Patent Citations

  • electrical insulating material with high electrical creep strength

    DE3717971A1

  • Method for preparing cable with cross-linked insulating layer and cable therefor

    JP2018518804A