Allylic flame-retardant prepolymer, resin composition, composite resin, prepreg and laminate

The resin composition combining allylbenzoxazine and allylphosphorus compounds with bismaleimide resin and fillers addresses flame retardancy and heat resistance issues, resulting in laminates with enhanced performance.

JP2024545352AActive Publication Date: 2024-12-05GUANGDONG HINNO TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024538969
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-31
Filing Date
2022-12-29
Publication Date
2024-12-05
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

Existing copper-clad laminates face challenges with insufficient flame retardancy, particularly when using bismaleimide resin, which affects heat resistance and high-temperature elastic modulus retention, and adding phosphorus-containing flame retardants compromises these properties.

Method used

A resin composition incorporating an allylbenzoxazine compound and an allylphosphorus-containing compound, combined with bismaleimide resin, cyanate ester resin, and inorganic fillers, enhances flame retardancy while maintaining high heat resistance and elastic modulus.

Benefits of technology

The laminate achieves UL-94V0 flame retardancy, high glass transition temperature, high peel strength, low water absorption, and strong dielectric properties, with improved toughness and reduced thermal expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545352000001
    Figure 2024545352000001
  • Figure 2024545352000002
    Figure 2024545352000002
  • Figure 2024545352000003
    Figure 2024545352000003
Patent Text Reader

Abstract

The present invention discloses an allyl-based flame-retardant prepolymer, a resin composition, a composite resin, a prepreg, and a laminate. The allyl-based flame-retardant prepolymer according to the present invention is obtained by prepolymerizing an allyl benzoxazine compound and an allyl phosphorus-containing compound having a mass ratio of 100:(20-80). The resin composition, composite resin, prepreg, and laminate produced using the allyl-based flame-retardant prepolymer according to the present invention have strong flame retardant performance, excellent high-temperature elastic modulus performance, excellent heat resistance and water absorption, and extremely excellent dielectric properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the technical field of copper-clad laminates, and specifically relates to an allylic flame-retardant prepolymer, a resin composition, a composite resin, a prepreg, and a laminate. [Background technology]

[0002] Copper clad laminates are plate-shaped materials manufactured by impregnating a reinforcing material with resin, coating one or both sides with copper foil, and hot pressing. In printed circuit boards, copper clad laminates can play the role of interconnection conduction, insulation, and support, and have a significant effect on the signal transmission speed, energy loss, and characteristic impedance of the circuit. With the further development of communication technology, the demands for copper clad laminates are becoming more diverse.

[0003] Bismaleimide resin (BMI) is a new high-performance resin material that has excellent heat resistance and high-temperature elastic modulus retention, but when used alone, it has disadvantages such as too high curing temperature and low solubility. Bismaleimide (BMI) after modification overcomes some of the above disadvantages and is widely used in the manufacture of copper-clad laminate substrates, but its flame retardancy is insufficient and cannot reach the UL-94V0 level. In order to achieve the flame retardant performance of copper-clad laminates, resins containing flame retardant elements, such as P, N, Si, etc., are generally added to the compounding components. The most flame retardant effect is achieved by adding phosphorus-containing flame retardants such as phosphorus-containing epoxy resins and phosphazene compounds. However, if the amount of phosphorus-containing flame retardant added is too high, it will have a negative effect on the heat resistance and high-temperature elastic modulus retention of the substrate.

[0004] Patent document CN109504087A discloses a resin composition made from modified bismaleimide prepolymer, the copper-clad laminate produced has a certain degree of heat resistance and flame retardancy, but lacks toughness and has low high-temperature elastic modulus retention.Patent document CN106336662A discloses a thermosetting resin composition containing an allyl-modified polyphenylene ether resin as a compounding component, the laminate produced has high flame retardancy, but has a low glass transition temperature (about 200°C), which is lower than the average value of BT resin substrates (200°C to 300°C), and the peel strength is not ideal.

[0005] In view of this, it is necessary to provide a resin composition having excellent overall performance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] China Patent Application Publication No. 109504087 [Patent Document 2] China Patent Application Publication No. 106336662 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention aims to provide an allylic flame-retardant prepolymer, a resin composition, and a composite resin, as well as a prepreg and a laminate produced therefrom, which have high flame retardancy, high peel strength, low water absorption, and high high-temperature elastic modulus retention. [Means for solving the problem]

[0008] The first aspect of the present invention comprises 100 parts by mass of an allylbenzoxazine-based compound and 20 to 80 parts by mass of an allyl phosphorus-containing compound, The structural formula of the allyl phosphorus-containing compound is [ka] and The allylbenzoxazine compound is at least one selected from the group consisting of compounds represented by the following structural formula: [ka] X is independently selected from -CHR1-, -CR2R3-, -SO2- or -O-; R1, R2, and R3 are each independently selected from -H or -CH3 to provide an allylic flame retardant prepolymer.

[0009] In some embodiments of the present invention, in the allyl-based flame retardant prepolymer, the structural formula of the allylbenzoxazine-based compound is as follows: [ka]

[0010] In some embodiments of the present invention, the allyl-based flame-retardant prepolymer further comprises 10 to 20 parts by mass of a non-phosphorus type allyl compound, The phosphorus-free allyl compound is at least one selected from the group consisting of allyl bisphenol A, allyl bisphenol S, and allyl diphenyl ether.

[0011] In some embodiments of the present invention, the allyl-based flame-retardant prepolymer is obtained by mixing the allylbenzoxazine-based compound and the allyl phosphorus-containing compound, and heating the mixture at 100° C. to 130° C. for 1 to 3 hours.

[0012] A second aspect of the present invention provides a resin composition comprising, as components by mass, 10 to 30 parts of the allylic flame-retardant prepolymer according to the first aspect of the present invention, 50 to 100 parts of a bismaleimide resin, 30 to 80 parts of a cyanate ester resin, 5 to 30 parts of a functional resin, and 10 to 60 parts of an inorganic filler.

[0013] In some embodiments of the present invention, in the resin composition, the bismaleimide resin is selected from organic compounds containing two or more maleimide structures in their molecular structure, and / or The cyanate ester resin is at least one selected from the group consisting of bisphenol A type cyanate ester resins, novolac type cyanate ester resins, bisphenol F type cyanate ester resins, multifunctional type cyanate ester resins, bisphenol M type cyanate ester resins, bisphenol E type cyanate ester resins, and dicyclopentadiene bisphenol type cyanate ester resins, and / or The functional resin is at least one selected from the group consisting of epoxy resins, polyphenylene ethers, and hydrocarbon resins, and / or The inorganic filler is at least one selected from the group consisting of zirconium vanadate, zirconium tungstate, hafnium tungstate, crystallized glass, eucryptite, silica, quartz, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc powder, alumina, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay, and kaolin.

[0014] In some embodiments of the present invention, the resin composition further comprises 1 to 5 parts by mass of an auxiliary agent, and the auxiliary agent is at least one selected from the group consisting of a curing accelerator, a coupling agent, and a reinforcing agent.

[0015] A third aspect of the present invention provides a composite resin comprising the allylic flame-retardant prepolymer according to the first aspect of the present invention or the resin composition according to the second aspect of the present invention.

[0016] A fourth aspect of the present invention provides a prepreg comprising a reinforcing material and a resin material carried on the reinforcing material, the resin material being the composite resin according to the third aspect of the present invention.

[0017] A fifth aspect of the present invention provides a laminate comprising, as a manufacturing raw material, the prepreg according to the fourth aspect of the present invention. Effect of the Invention

[0018] Copper-clad laminates using bismaleimide as the main resin material have excellent heat resistance but insufficient flame retardancy. In order to improve the flame retardancy, a large amount of flame retardant or inorganic filler is added to the compounding components, or pretreatment such as modifying the raw resin is often performed. In the present invention, an appropriate amount of an allyl-based flame-retardant prepolymer is used to combine bismaleimide with other functional resins, inorganic fillers, auxiliary agents, and other components, thereby comprehensively improving the flame and heat resistance of the resin composition, and a laminate (copper-clad laminate) manufactured using the resin has not only flame retardancy but also excellent overall performance.

[0019] In the present invention, an allyl benzoxazine compound and an allyl phosphorus-containing compound are prepolymerized to obtain a flame-retardant prepolymer rich in allyl groups, which is then added to a bismaleimide resin and other components to form a resin composition. The allyl groups in the resin composition are bonded to each other to extend the linear chain of benzoxazine, reduce stress during the reaction process, improve the toughness of the resin composition, and reduce the expansion and contraction of the resin composition.

[0020] In the resin composition according to the present invention, the nitrogen and phosphorus elements exert a synergistic effect, and can further improve the flame retardant performance.

[0021] The laminate of the present invention has an overall flame retardancy level that can reach UL-94V0, a ​​high glass transition temperature (Tg>300°C), high peel strength, high high temperature elastic modulus retention (flexural modulus, storage modulus), a low coefficient of thermal expansion (CTE), low water absorption, and very strong dielectric properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be further described below with reference to the embodiments and examples. Note that these examples are merely for the purpose of illustrating the present invention and do not limit the scope of the present invention. In addition, after reading the contents of the present invention, those skilled in the art can make various changes and modifications to the present invention, and these equivalent forms are also included in the scope of the claims of this application.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. The terminology used herein is for the purpose of describing specific examples only and is not intended to be limiting of the invention.

[0024] [term] Terms or expressions used in this specification have the following meanings unless otherwise stated or contradicted:

[0025] The term "and / or", "or / and", and "and / or" as used herein includes any one item among two or more related listed items, and further includes any and all combinations of related listed items, including any two related listed items, any more related listed items, or all related listed items. It should be noted that when at least three items are connected by a combination of at least two conjunctions selected from "and / or", "or / and", and "and / or", it is understood that in this application, the technical means include all technical means connected by "logical AND" and further include all technical means connected by "logical OR". For example, "A and / or B" includes three meanings: A, B, and A+B. For example, a technical means of "A and / or B and / or C and / or D" includes any one of A, B, C, and D (i.e., all technical means connected by a "logical OR"), includes any and all combinations of A, B, C, and D, i.e., includes any combination of two or three of A, B, C, and D, and further includes four combinations of A, B, C, and D (i.e., all technical means connected by a "logical AND").

[0026] In this specification, it should be understood that the terms "preferably", "more preferably", and "even more preferably" are merely intended to describe more effective embodiments or examples, and are not intended to limit the scope of protection of the present invention.

[0027] In the present invention, the terms "further", "also further", "particularly" and the like are for explanatory purposes and indicate differences in content, but should not be construed as limiting the protection scope of the present invention.

[0028] In the present application, the terms "first", "second", "third", "fourth", "fifth", etc. in "first embodiment", "second embodiment", "third embodiment", "fourth embodiment", "fifth embodiment", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or quantity, nor should they be understood as implying the importance or quantity of the technical features shown. It should also be understood that "first", "second", "third", "fourth", "fifth", etc. serve the purpose of a non-exhaustive enumeration description only and do not constitute closed-type limitations on the numbers.

[0029] In the present invention, technical features described in an open format include both closed technical solutions consisting of the listed features and open technical solutions including the listed features.

[0030] In the present invention, for a numerical interval (i.e., a numerical range), unless otherwise specified, the selectable numerical distribution is considered to be continuous within the numerical interval, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical range, and each value between the two numerical endpoints. Unless otherwise specified, when a numerical interval refers only to integers within the numerical interval, it includes the integers at the two endpoints of the numerical range, and each integer between the two endpoints. In addition, when there are multiple ranges describing a feature or characteristic, they may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.

[0031] In the present invention, at least one is to be understood as one or more, inclusive of the number.

[0032] Unless otherwise specified, the temperature parameters in the present invention may be constant temperature treatments or may vary within a certain temperature range. It should be understood that the constant temperature treatments allow the temperature to vary within the precision range of the equipment control. For example, variations within the ranges of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0033] In the present invention, unless otherwise specified, size, particle size, and diameter generally refer to average values.

[0034] A first aspect of the present invention provides an allylic flame retardant prepolymer.

[0035] In the present invention, an allylbenzoxazine-based compound and an allylamine-based phosphorus-containing compound are prepolymerized into an allyl-based flame-retardant prepolymer, and then added to a resin composition, thereby obtaining excellent flame retardant effect, improving the toughness of the resin composition, and providing it with excellent overall performance.

[0036] The first aspect of the present invention comprises 100 parts by mass of an allylbenzoxazine-based compound and 20 to 80 parts by mass of an allyl phosphorus-containing compound, The structural formula of the allyl phosphorus-containing compound is [ka] and The allylbenzoxazine compound is at least one selected from the group consisting of compounds represented by the following structural formula: [ka] X is independently selected from -CHR1-, -CR2R3-, -SO2- or -O-; R1, R2, and R3 are each independently selected from -H or -CH3 to provide an allylic flame retardant prepolymer.

[0037] In some embodiments of the present invention, the ratio of parts by mass of the allyl benzoxazine-based compound to the allyl phosphorus-containing compound in the allyl-based flame retardant prepolymer is 100:(20-80), and may even be 100:(40-60). For example, the ratio of parts by mass is 100:20, 100:25, 100:30, 100:35, 100:40, 100:45, 100:50, 100:55, 100:60, 100:65, 100:70, 100:75, or 100:80, etc.

[0038] In some embodiments of the present invention, the weight ratio of the allyl benzoxazine-based compound to the allyl phosphorus-containing compound in the allyl-based flame retardant prepolymer is 100:50.

[0039] In the present invention, in the allyl-based flame-retardant prepolymer, the allyl groups in the allyl benzoxazine compound and the allyl phosphorus-containing compound are bonded to each other, thereby extending the linear chain of benzoxazine, reducing stress during the reaction process, improving the toughness of the resin composition, and reducing the expansion and contraction of the resin composition.

[0040] In some embodiments of the present invention, in the allyl-based flame retardant prepolymer, the structural formula of the allylbenzoxazine-based compound is as follows: [ka]

[0041] In some embodiments of the present invention, the allyl-based flame-retardant prepolymer further comprises 10 to 20 parts by weight of a phosphorus-free allyl compound. In some embodiments, the phosphorus-free allyl compound is at least one selected from the group consisting of allyl bisphenol A, allyl bisphenol S, and allyl diphenyl ether.

[0042] In some embodiments of the present invention, the allyl-based flame retardant prepolymer further comprises 10 parts by weight of allyl bisphenol A.

[0043] In some embodiments of the present invention, the weight parts of the phosphorus-free allyl compound in the flame-retardant prepolymer is 10 to 20 parts, such as 10, 12, 15, 18, or 20 parts, relative to 100 parts by weight of the allylbenzoxazine compound.

[0044] In some embodiments of the present invention, an allyl-based flame-retardant prepolymer is obtained by mixing an allyl benzoxazine compound and an allyl phosphorus-containing compound and heating the mixture at 100°C to 130°C for 1 to 3 hours. In some embodiments, the allyl benzoxazine compound and the allyl phosphorus-containing compound are mixed and then heated at 100°C to 130°C, and the heating temperature may be selected from 100°C to 120°C, 100°C to 110°C, 100°C to 105°C, 110°C to 120°C, 120°C to 130°C, etc., and may be, for example, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, or 130°C. In some embodiments, the heating time is from 1 to 3 hours, and may be further selected from 1 to 3 hours, 1 to 2 hours, 1 to 1.5 hours, 2 to 3 hours, 2.5 to 3 hours, etc., such as 1 hour, 1.5 hours, 2 hours, 2.5 hours, or 3 hours.

[0045] In some embodiments of the present invention, the allyl benzoxazine-based compound and the allyl phosphorus-containing compound are mixed and heated at 120° C. for 2.5 hours to obtain the allyl-based flame-retardant prepolymer.

[0046] A second aspect of the present invention provides a resin composition (BT resin composition) having high flame retardant performance, high retention of high temperature elastic modulus, and extremely strong dielectric properties.

[0047] A second aspect of the present invention provides a resin composition comprising, as components by mass, 10 to 30 parts of the allylic flame-retardant prepolymer according to the first aspect of the present invention, 50 to 100 parts of a bismaleimide resin, 30 to 80 parts of a cyanate ester resin, 5 to 30 parts of a functional resin, and 10 to 60 parts of an inorganic filler.

[0048] In some embodiments of the present invention, the mass parts of the allyl-based flame-retardant prepolymer in the resin composition is 10 to 30 parts, or may be 10 to 20 parts, for example, 10, 12, 15, 18, 20, 22, 25, 28, or 30 parts, relative to 50 to 100 parts by mass of the bismaleimide resin.

[0049] In the present invention, the bismaleimide resin is selected from organic compounds containing two or more maleimide structures in the molecular structure.

[0050] In some embodiments of the present invention, the bismaleimide resin is at least one selected from the group consisting of an N-phenylmaleimide group, an N-(2-methylphenyl)maleimide group, an N-(4-methylphenyl)maleimide group, an N-(2,6-dimethylphenyl)maleimide group, a bis(4-maleimidophenyl)methane group, a 2,2-bis(4-(4-maleimidophenoxy)-phenyl)propane group, a bis(3,5-dimethyl-4-maleimidophenyl)methane group, a bis(3-ethyl-5-methyl-4-maleimidophenyl)methane group, a bis(3,5-diethyl-4-maleimidophenyl)methane group, a polyphenylmethane bismaleimide group, and a biphenyl structure-containing maleimide group.

[0051] In some embodiments of the present invention, the bismaleimide resin is N,N'-(4,4'-methylenediphenyl)bismaleimide.

[0052] In some embodiments of the present invention, the mass parts of the bismaleimide resin in the resin composition is 50 to 100 parts, or may be 50 to 75 parts, for example, 50, 55, 60, 65, 70, 75, 85, 90, or 100 parts, relative to 10 to 30 parts by mass of the allyl-based flame-retardant prepolymer.

[0053] In some embodiments of the present invention, the cyanate ester resin is at least one selected from the group consisting of bisphenol A type cyanate ester resins, novolac type cyanate ester resins, bisphenol F type cyanate ester resins, multifunctional type cyanate ester resins, bisphenol M type cyanate ester resins, bisphenol E type cyanate ester resins, and dicyclopentadiene bisphenol type cyanate ester resins.

[0054] In some embodiments of the present invention, the cyanate ester resin is a bisphenol A type cyanate ester.

[0055] In some embodiments of the present invention, the mass parts of the allyl-based flame-retardant prepolymer in the resin composition is 30 to 80 parts, or may be 30 to 60 parts, for example, 30, 35, 40, 45, 50, 55, 60, 70, or 80 parts, relative to 50 to 100 parts by mass of the bismaleimide resin.

[0056] In some embodiments of the present invention, the functional resin is at least one selected from the group consisting of epoxy resins, polyphenylene ethers, and hydrocarbon resins.

[0057] In some embodiments of the present invention, the functional resin is an epoxy resin.

[0058] In some embodiments of the present invention, the mass parts of the functional resin in the resin composition is 5 to 30 parts, or may be 5 to 20 parts, for example, 5, 8, 10, 12, 15, 17, 20, 25, or 30 parts, relative to 50 to 100 parts by mass of the bismaleimide resin.

[0059] In some embodiments of the present invention, the inorganic filler is at least one selected from the group consisting of zirconium vanadate, zirconium tungstate, hafnium tungstate, crystallized glass, eucryptite, silica, quartz, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc powder, alumina, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay, and kaolin.

[0060] In some embodiments of the present invention, the inorganic filler is silica.

[0061] In some embodiments of the present invention, the mass parts of the inorganic filler in the resin composition is 10 to 60 parts, or may be 40 to 50 parts, for example, 10, 20, 30, 35, 38, 40, 42, 45, 50, 55, or 60 parts, relative to 50 to 100 parts by mass of the bismaleimide resin.

[0062] In the present invention, the resin composition may or may not contain an auxiliary agent.

[0063] In some embodiments of the present invention, the coagent is at least one selected from the group consisting of accelerators, coupling agents, and toughening agents.

[0064] In some embodiments of the present invention, the coagent is a curing accelerator, and the curing accelerator may be selected from imidazoles, such as 2-methylimidazole, 2-phenylimidazole, and 2-ethyl-4 methylimidazole, and may be at least one selected from the group consisting of organometallic salts, such as zinc octoate, zinc isooctanoate, stannous octoate, dibutyltin dilaurate, zinc naphthenate, cobalt naphthenate, aluminum acetylacetonate, cobalt acetylacetonate, and copper acetylacetonate. The coupling agent may be at least one selected from the group consisting of silane coupling agents, titanate coupling agents, aluminate coupling agents, and organochromium complex coupling agents. The reinforcing agent may be at least one selected from the group consisting of rubber, silicone resin, and polybutadiene.

[0065] In some embodiments of the present invention, the coagent is a 2-methylimidazole cure accelerator.

[0066] In some embodiments of the present invention, the amount of the auxiliary in the resin composition is 1 to 5 parts by mass, or may be 2 to 5 parts, for example, 1, 2, 3, 4, 5, 6, 7, or 8 parts, relative to 50 to 100 parts by mass of the bismaleimide resin.

[0067] In some embodiments, the resin composition includes, as components, in parts by weight, 10-30 parts of an allyl-based flame-retardant prepolymer, 50-100 parts of a bismaleimide resin, 30-80 parts of a cyanate ester resin, 5-30 parts of a functional resin, 10-60 parts of an inorganic filler, and 0-5 parts of an auxiliary. The parts by weight of the allyl-based flame-retardant prepolymer may be independently 10-30 parts, such as 10, 12, 15, 18, 20, 25, 28, or 30 parts, the parts by weight of the bismaleimide resin may be independently 50-100 parts, such as 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100 parts, and the parts by weight of the cyanate ester resin may be independently 30-80 parts, such as 30, 40, 50, 60, 70, or 80 parts. The parts by mass of the functional resin may be independently 5 to 30 parts, for example, 5, 8, 10, 12, 15, 18, 20, 25, 28, or 30 parts, the parts by mass of the inorganic filler may be independently 10 to 60 parts, for example, 10, 20, 30, 50, 50, or 60 parts, and the parts by mass of the auxiliary may be independently 0 to 5 parts, further 1 to 5 parts, or further 2 to 5 parts, for example, 0, 1, 2, 3, 4, or 5 parts.

[0068] A third aspect of the present invention provides a composite resin comprising the allyl-based flame-retardant prepolymer according to the first aspect of the present invention or the resin composition according to the second aspect of the present invention. The composite resin has excellent flame retardancy and heat resistance, and is excellent in high-temperature elastic modulus performance.

[0069] A fourth aspect of the present invention provides a prepreg comprising the composite resin according to the third aspect of the present invention.

[0070] In some embodiments of the present invention, the prepreg includes a reinforcing material and a resin material supported on the reinforcing material, and the resin material may be the composite resin described above.

[0071] A fifth aspect of the present invention provides a laminate comprising a prepreg according to the fourth aspect of the present invention.

[0072] In the present invention, the flame retardant level of the laminate reaches UL94V0, and has excellent overall performance. In some embodiments, the glass transition temperature Tg of the laminate is >250°C, and furthermore, Tg >280°C. In some embodiments, the peel strength of the laminate is >5.6 lb / in. In some embodiments, the tin plating heat resistance of the laminate is >300s. In some embodiments, the laminate passes the saturated vapor pressure test (PCT). In some embodiments, the 200°C storage modulus of the laminate is >30 Gpa. In some embodiments, the water absorption of the laminate is 0.1% to 0.12%. Specific examples are shown below. EXAMPLES

[0073] For experimental parameters not described in the following specific examples, reference should be made to the guide described in this application, to experimental manuals in the field or other experimental methods known in the field, or to experimental conditions recommended by manufacturers.

[0074] The materials and reagents in the following specific examples are either commercially available or can be prepared according to known procedures by those skilled in the art.

[0075] Raw materials: The bismaleimide resin is BMI-01 manufactured by Honghu Soumaba. The cyanate ester resin is BA-3000S manufactured by Lonza Group. The phosphorus-containing epoxy resin is 589K75 manufactured by Kosho Electronics. The phosphazene compound is SPB100 manufactured by Otsuka Chemical Co., Ltd. The epoxy resin is NC3000H manufactured by Nippon Kayaku Co., Ltd.

[0076] Preparation of aryl phosphorus-containing compounds: In step 1, 1 mol of 2-methylallylamine was taken, mixed with a solvent, heated to 80°C to 120°C, 0.5 mol of terephthalaldehyde was added, and the mixture was reacted for 3 to 8 hours under a nitrogen atmosphere.

[0077] In step 2, the reaction solution was cooled to room temperature and filtered by suction to obtain a crude product, which was then recrystallized from water (4 to 7 times). The recrystallized product was then dried at 60°C to 90°C for 24 hours to obtain an intermediate product.

[0078] In step 3, 0.5 mol of the intermediate product, 1 mol of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and a solvent were mixed, heated to 100°C to 150°C, and reacted for 5 to 7 hours under a nitrogen atmosphere. The reaction solution was then cooled to room temperature and recrystallized in water (4 to 7 times). The recrystallized product was then dried at 60°C to 90°C for 24 hours to obtain an allyl phosphorus-containing compound.

[0079] Preparation of allyl-based flame-retardant prepolymer 1: 100 parts by mass of an allyl benzoxazine-based compound and 50 parts by mass of an allyl phosphorus-containing compound were placed in a three-neck flask, an organic solvent was added and mixed, and the mixture was heated to 120°C in an oil bath and stirred for 2.5 hours to obtain an allyl-based flame-retardant prepolymer 1.

[0080] The structural formula of the allylbenzoxazine compound is shown below. [ka]

[0081] Preparation of allyl-based flame-retardant prepolymer 2: 100 parts by mass of an allyl benzoxazine-based compound, 50 parts by mass of an allyl phosphorus-containing compound, and 10 parts by mass of allyl bisphenol A were placed in a three-neck flask, an organic solvent was added and mixed, and the mixture was heated to 120°C in an oil bath and stirred for 2.5 hours to obtain an allyl-based flame-retardant prepolymer 2.

[0082] The structural formula of the allylbenzoxazine compound is shown below. [ka]

[0083] Preparation of allyl-based flame-retardant prepolymer 3: 100 parts by mass of an allyl benzoxazine-based compound and 100 parts by mass of an allyl phosphorus-containing compound were placed in a three-neck flask, an organic solvent was added and mixed, and the mixture was heated to 120°C in an oil bath and stirred for 2.5 hours to obtain an allyl-based flame-retardant prepolymer 3.

[0084] The structural formula of the allylbenzoxazine compound is shown below. [ka]

[0085] Prepreg Manufacturing: The raw materials were mixed uniformly according to the compounding ratio of each component in Table 1 to obtain an emulsion liquid. Then, a 2116 glass cloth was immersed in the emulsion liquid and baked in an oven at 160°C for 3 minutes to obtain a prepreg with an emulsion content of 55%.

[0086] [Table 1]

[0087] Laminate manufacturing: Ten prepregs were laminated, and each of the top and bottom surfaces of the laminate was covered with a sheet of electrolytic copper foil having a thickness of 18 μm. The laminate was then placed in a vacuum press with programmable temperature and pressure controls, and subjected to a pressure of 30 kgf / cm. 2 The laminate was heated and cured in stages under a vacuum pressure (vacuum level <10 mBar), first at 180°C for 1 hour, then heated to 220°C and continued to be heated for 2 hours, then heated to 240°C and continued to be heated for 2 hours, and then cooled to obtain a copper foil-clad laminate with a thickness of 1.0 mm.

[0088] Performance test: Performance tests were carried out on the laminates produced in Examples 1 to 3 and Comparative Examples 1 to 4 according to the following test standards.

[0089] The glass transition temperature (Tg) / storage modulus was tested according to IPC-TM650 2.4.25D.

[0090] The peel strength test was performed in accordance with IPC-TM-650 2.4.8.

[0091] The heat resistance of the tin plating was tested in accordance with IPC-TM650 2.4.6.

[0092] PCT was tested in accordance with IPC-TM650 2.6.23.

[0093] Flexural modulus was tested in accordance with IPC-TM650 2.4.4.

[0094] The flame retardant level was tested in accordance with IPC-TM650 2.3.10.

[0095] Water absorption was tested in accordance with IPC-TM650 2.6.2.1.

[0096] Dielectric properties were tested in accordance with IPC-TM650 2.5.5.9.

[0097] The test results of the above tests are shown in Table 2.

[0098] [Table 2]

[0099] As can be seen from the data in Table 2, the resin composition using the allylic flame-retardant prepolymer of the present invention has strong flame retardancy, which can reach the UL94V0 level, high heat resistance and moisture resistance, low rate of change in high temperature elastic modulus, low water absorption, and extremely strong dielectric properties.

[0100] As can be seen from the data in Table 2, changing the composition of the prepolymer reduces the peel strength, increases the water absorption rate, and also affects the elastic modulus performance. Adding allyl bisphenol A to the compounding components can improve the viscosity and improve the peel strength, but if the amount of allyl-based flame-retardant prepolymer added is too large, the high temperature elastic modulus performance will be significantly reduced and the water absorption rate will increase, which will seriously affect the overall performance of the laminate. If the allyl-based flame-retardant prepolymer of the present invention is not used or if a normal phosphorus-containing resin is used as a flame-retardant additive, the water absorption rate will be significantly increased and the elastic modulus performance and dielectric properties will be significantly reduced.

[0101] All documents mentioned in the present invention are incorporated herein by reference in their entirety, as if each document were individually incorporated by reference. Unless inconsistent with the purpose and / or technical means of the present invention, the cited documents of the present invention are incorporated herein in their entirety and for all purposes. In the present invention, when a cited document is mentioned, the definitions of related technical features, terms, nouns, phrases, etc. in the cited document are also incorporated. In the present invention, when a cited document is mentioned, examples of related technical features incorporated, preferred embodiments may also be incorporated by reference into the present application, but are limited to those that can implement the present invention. In the case where the cited content is inconsistent with the description of the present application, it should be understood that the content is adaptively modified based on or in accordance with the description of the present application.

[0102] The technical features of the above embodiments and examples can be combined in any combination. For the sake of brevity, not all possible combinations of the technical features in the above embodiments and examples are described, but as long as there is no contradiction in the combinations of these technical features, all of them should be considered within the scope of this specification.

[0103] The above examples only describe some embodiments of the present invention, and should not be understood as limiting the scope of the patent of the present invention. It should be noted that those skilled in the art can make various modifications and improvements to the present invention without departing from the spirit of the present invention, and these modifications and improvements also belong to the scope of the present invention. It can also be understood that after reading the above description of the present invention, those skilled in the art can make various changes and modifications to the present invention, and these equivalent forms are also included in the scope of protection of the present invention. It should be understood that any technical means obtained by those skilled in the art through logical analysis, reasoning, or limited experiments based on the technical means provided by the present invention are within the scope of the claims attached to the present invention. Therefore, the scope of protection of the patent of the present invention depends on the scope of the attached claims, and the specification is intended to explain the content of the claims.

Claims

1. 100 parts by weight of an allyl benzoxazine-based compound and 20 to 80 parts by weight of an allyl phosphorus-containing compound, The structural formula of the allyl phosphorus-containing compound is 【Chemistry 1】 and The allylbenzoxazine compound is at least one selected from the group consisting of compounds represented by the following structural formula: 【Chemistry 2】 X is independently -CHR 1 -, -CR 2 R 3 -, -SO 2 - or -O-, R 1 , R 2 , R 3 are each independently -H or -CH 3 An allylic flame-retardant prepolymer, characterized in that it is selected from the following:

2. 2. The allyl-based flame-retardant prepolymer according to claim 1, wherein the structural formula of the allylbenzoxazine compound is as follows: 【Chemistry 3】

3. Further comprising 10 to 20 parts by weight of a phosphorus-free allyl compound; 3. The allyl-based flame-retardant prepolymer according to claim 1, wherein the non-phosphorus type allyl compound is at least one selected from the group consisting of allyl bisphenol A, allyl bisphenol S, and allyl diphenyl ether.

4. The allyl-based flame-retardant prepolymer according to claim 1, which is obtained by mixing the allyl benzoxazine compound and the allyl phosphorus-containing compound and heating the mixture at 100°C to 130°C for 1 to 3 hours.

5. A resin composition comprising, as components by mass, 10 to 30 parts of the allyl-based flame-retardant prepolymer according to any one of claims 1 to 4, 50 to 100 parts of a bismaleimide resin, 30 to 80 parts of a cyanate ester resin, 5 to 30 parts of a functional resin, and 10 to 60 parts of an inorganic filler.

6. The bismaleimide resin is selected from organic compounds containing two or more maleimide structures in the molecular structure, and / or The cyanate ester resin is at least one selected from the group consisting of bisphenol A type cyanate ester resins, novolac type cyanate ester resins, bisphenol F type cyanate ester resins, polyfunctional type cyanate ester resins, bisphenol M type cyanate ester resins, bisphenol E type cyanate ester resins, and dicyclopentadiene bisphenol type cyanate ester resins, and / or The functional resin is at least one selected from the group consisting of epoxy resins, polyphenylene ethers, and hydrocarbon resins, and / or The resin composition according to claim 5, characterized in that the inorganic filler is at least one selected from the group consisting of zirconium vanadate, zirconium tungstate, hafnium tungstate, crystallized glass, eucryptite, silica, quartz, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc powder, alumina, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay, and kaolin.

7. The resin composition according to claim 5, further comprising 1 to 5 parts by mass of an auxiliary agent, the auxiliary agent being at least one selected from the group consisting of a curing accelerator, a coupling agent, and a reinforcing agent.

8. A composite resin comprising the allyl-based flame-retardant prepolymer according to any one of claims 1 to 4, or the resin composition according to any one of claims 5 to 7.

9. A prepreg comprising a reinforcing material and a resin material carried on the reinforcing material, the resin material being the composite resin according to claim 8.

10. A laminate comprising the prepreg according to claim 9 as a production raw material.

Citation Information

Patent Citations

  • Resin compound, prepreg and laminated board prepared from resin compound

    CN109504087A

  • Allyl flame-retardant prepolymer, resin composition, composite resin, prepreg and laminated board

    CN114316115A

  • DOPO derivative and epoxy resin composition applied in high-frequency substrate

    JP2017110014A

  • Thermosetting resin composition, resin film with carrier, pre-preg, metal-clad laminate sheet, resin substrate, printed wiring substrate and semiconductor device

    WO2017170643A1

  • Resin composition, prepreg, laminate, metal foil clad laminate, printed wiring board, and multilayer printed wiring board

    WO2018124164A1