Positive electrode material powder, positive electrode containing the same, and lithium secondary battery

A lithium nickel-based oxide powder with controlled single particle formation and coating addresses particle cracking and reactivity issues, improving high-temperature life and resistance characteristics in lithium secondary batteries.

JP2024545475AActive Publication Date: 2024-12-06LG ENERGY SOLUTION LTD

Patent Information

Application Number
JP2024539063
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-07
Filing Date
2023-01-06
Publication Date
2024-12-06
Estimated Expiration
2043-01-06

AI Technical Summary

Technical Problem

Conventional lithium nickel cobalt manganese oxides used in positive electrodes of lithium secondary batteries face issues such as particle cracking, increased gas generation, and reduced life characteristics due to high reactivity, especially at high temperatures, which are exacerbated by high nickel content for improved capacity.

Method used

A positive electrode material powder composed of lithium nickel-based oxide particles with a specific degree of single particle formation (0.3 to 0.8) is developed, characterized by a combination of single and pseudo-single particles, with controlled grain size and grain distribution, and optionally coated with elements like Al, Ti, and a coating layer to minimize electrolyte interaction.

Benefits of technology

The solution significantly reduces gas generation and maintains low resistance while enhancing high-temperature life and storage characteristics, ensuring excellent performance in lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545475000001_ABST
    Figure 2024545475000001_ABST
Patent Text Reader

Abstract

The present invention provides a positive electrode material powder that contains a lithium nickel-based oxide represented by chemical formula 1 and has a degree of monoparticulation represented by formula (1) of 0.3 to 0.8. [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2 In the above [Chemical Formula 1], M 1 is Mn, Al or a combination thereof, M 2 is at least one selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb and Mo, and 0.80≦a≦1.20, 0.55≦b<1, 0
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0002994, filed on January 7, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a positive electrode material powder for a lithium secondary battery, and a positive electrode and a lithium secondary battery including the same. More particularly, the present invention relates to a positive electrode material powder for a lithium secondary battery that can improve high-temperature performance while minimizing an increase in resistance, and a positive electrode and a lithium secondary battery including the same. [Background technology]

[0003] A lithium secondary battery generally comprises a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode and the negative electrode contain active materials capable of intercalating and deintercalating lithium ions.

[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMnO4, etc.), lithium iron phosphate compound (LiFePO4), etc. have been used as the positive electrode active material of lithium secondary batteries. Among them, lithium cobalt oxide has the advantage of high operating voltage and excellent capacity characteristics, but the raw material cobalt is expensive and the supply is unstable, making it difficult to commercially apply to large-capacity batteries. Lithium nickel oxide has low structural stability and is difficult to realize sufficient life characteristics. On the other hand, lithium manganese oxide has excellent stability but has a problem of low capacity characteristics. Therefore, lithium composite transition metal oxides containing two or more transition metals have been developed to compensate for the problems of lithium transition metal oxides containing Ni, Co, or Mn alone, and among them, lithium nickel cobalt manganese oxides containing Ni, Co, and Mn are widely used in the field of electric vehicle batteries.

[0005] Conventional lithium nickel cobalt manganese oxides are generally in the form of spherical secondary particles formed by agglomeration of tens to hundreds of primary particles. However, when lithium nickel cobalt manganese oxide in the form of secondary particles formed by agglomeration of many primary particles is used, there are problems in that primary particles are easily broken during the rolling process in the manufacture of the positive electrode, causing primary particles to fall off, and cracks are generated inside the particles during charging and discharging. When particle breakage or cracks occur in the positive electrode active material, the contact area with the electrolyte increases, and gas generation and active material degradation due to side reactions with the electrolyte increase, resulting in a problem of reduced life characteristics.

[0006] On the other hand, the demand for high-output, high-capacity batteries, such as those for electric vehicles, has recently been increasing, so the nickel content in the positive electrode active material is gradually increasing. As the nickel content in the positive electrode active material increases, the initial capacity characteristics improve, but the highly reactive Ni 4+ A large amount of ions are generated, causing the structure of the positive electrode active material to collapse, which increases the rate at which the positive electrode active material degrades, reducing the life characteristics and battery safety. In particular, performance degradation occurs rapidly when exposed to high temperatures.

[0007] In order to solve the above problems, a technology has been proposed to manufacture a single particle type positive electrode active material, not a secondary particle type, by increasing the sintering temperature during the manufacture of lithium nickel cobalt manganese oxide. In the case of a single particle type positive electrode active material, the contact area with the electrolyte is smaller than that of a conventional secondary particle type positive electrode active material, so there are fewer side reactions with the electrolyte, and the particle strength is excellent, so there is less particle cracking during electrode manufacture. Therefore, the application of a single particle type positive electrode active material has the advantage of excellent gas generation and life characteristics. However, there is a problem that the conventional single particle type positive electrode active material has high resistance, and when used, sufficient output performance cannot be obtained. Summary of the Invention [Problem to be solved by the invention]

[0008] In order to solve the above problems, an object of the present invention is to provide a positive electrode material powder for lithium secondary batteries which generates little gas at high temperatures, has excellent life characteristics, and at the same time, exhibits low resistance characteristics.

[0009] Another object of the present invention is to provide a positive electrode and a lithium secondary battery containing the positive electrode material powder and having excellent resistance characteristics and high-temperature characteristics. [Means for solving the problem]

[0010] In one aspect, the present invention provides a positive electrode material powder comprising positive electrode active material particles including a lithium nickel-based oxide represented by the following chemical formula 1, and having a degree of single particle size represented by the following formula (1) of 0.3 to 0.8.

[0011] [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2 In the above [Chemical Formula 1], M 1 is Mn, Al or a combination thereof, M 2 is at least one selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb and Mo, and 0.80≦a≦1.20, 0.55≦b<1, 0 <c<0.45、0<d<0.45、0≦e≦0.20である。

[0012] Formula (1):

number

[0013] The positive electrode active material particles may be or include a single particle consisting of one nodule or a quasi-single particle which is a composite of 30 or less nodules. Preferably, the positive electrode material powder may be a combination of single particle and quasi-single particle positive electrode active material particles.

[0014] The average particle size of the nodules of the positive electrode material powder may be 0.8 μm to 4.0 μm, and the D 50 The average grain diameter may be 2.0 μm to 10.0 μm, and the average grain diameter may be 0.5 μm to 4.0 μm.

[0015] The positive electrode active material may further include a coating layer formed on the surface of the lithium nickel-based oxide and containing one or more coating elements selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb.Mo, Sr, Sb, Bi, Si, and S.

[0016] In another aspect, the present invention provides a positive electrode comprising the above-described positive electrode material powder, and a lithium secondary battery comprising the positive electrode. Effect of the Invention

[0017] The cathode powder according to the present invention is characterized in that the degree of monoparticulation represented by formula (1) is in the range of 0.3 to 0.8. In the case of a secondary battery using a cathode powder having a degree of monoparticulation of less than 0.3 represented by formula (1), the amount of gas generated during high-temperature storage is high, and high-temperature life characteristics are reduced. In the case of a secondary battery using a cathode powder having a degree of monoparticulation of more than 0.8, the high-temperature storage characteristics and high-temperature life characteristics are excellent, but the resistance is high, and output and capacity characteristics are reduced. In contrast, a secondary battery using a cathode powder having a degree of monoparticulation that falls within the range of the present invention is excellent in all of the high-temperature life characteristics, high-temperature storage characteristics, and resistance characteristics. [Brief description of the drawings]

[0018] [Figure 1] 1 is a scanning electron microscope image of the positive electrode material powders produced in Example 1 of the present invention and Comparative Examples 1 and 2. [Diagram 2] FIG. 2 is an EBSD analysis image of a cross section of an electrode manufactured using the cathode material powder manufactured in Example 1. [Diagram 3] FIG. 2 is a diagram showing an EBSD analysis image of a cross section of an electrode manufactured using the cathode material powder manufactured according to Comparative Example 1. [Figure 4] FIG. 13 is a diagram showing an EBSD analysis image of a cross section of an electrode manufactured using the positive electrode material powder manufactured according to Comparative Example 2. [Diagram 5] 1 is a graph showing the amount of gas generated during high-temperature storage of batteries manufactured using the positive electrode materials of Examples 1 to 4 and Comparative Examples 1 and 2. [Figure 6] 1 is a graph showing high-temperature life characteristics of lithium secondary batteries produced using the positive electrode materials of Examples 1 to 4 and Comparative Examples 1 and 2. [Figure 7] 1 is a graph showing resistance characteristics according to SOC (state of charge) of lithium secondary batteries manufactured using the positive electrode materials of Examples 1 to 4 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will now be described in more detail.

[0020] The terms and words used in this specification and the claims should not be interpreted limited to their ordinary and dictionary meanings, but should be interpreted in a way that is consistent with the technical ideas of the present invention, based on the principle that the inventor himself / herself can appropriately define the concepts of terms in order to explain the invention in the best possible way.

[0021] In the present invention, a "grain" is a particle unit having the same crystal orientation, and is the smallest particle unit that can be recognized as a single mass in an Electron Backscatter Diffraction (EBSD) map image. The size of the grain can be measured by image analysis of the EBSD map.

[0022] In the present invention, "single particle" means a particle consisting of one nodule, and "quasi-single particle" means a composite particle of 30 or less nodules.

[0023] The "nodule" is a lower particle unit constituting a single particle or a quasi-single particle, and may be a single crystal having no crystalline grain boundary, or a polycrystal having no apparent grain boundary when observed at a magnification of 5,000 to 20,000 using a scanning electron microscope.

[0024] In the present invention, the term "secondary particle" refers to a particle formed by agglomeration of a plurality of, for example, tens to hundreds of, primary particles. Specifically, the secondary particle may be an agglomeration of 50 or more primary particles.

[0025] In the present invention, the term "particle" is a concept including any one or all of a single particle, a quasi-single particle, a primary particle, a nodule, and a secondary particle.

[0026] In the present invention, the average particle size of the nodules or primary particles (D mean) refers to the arithmetic mean value calculated after measuring the particle size of nodules or primary particles observed from a scanning electron microscope image.

[0027] In the present invention, the "average particle size D 50 " means a particle size based on 50% of the volume cumulative particle size distribution of the positive electrode material powder, and can be measured using a laser diffraction method. For example, the positive electrode material powder is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT3000), and ultrasonic waves of about 28 kHz are irradiated at an output of 60 W, and a volume cumulative particle size distribution graph is obtained, and the particle size corresponding to 50% of the volume cumulative amount is obtained and measured.

[0028] The inventors conducted extensive research to develop a cathode material for lithium secondary batteries that is excellent in both high temperature and resistance characteristics, and discovered that the average particle size of the cathode material powder is D 50 The inventors have found that when the grain size satisfies a specific relationship, it is possible to minimize an increase in resistance and realize excellent high temperature characteristics, and have completed the present invention.

[0029] Specifically, the positive electrode material powder according to the present invention satisfies the degree of monoparticle size represented by the following formula (1) of 0.3 to 0.8.

[0030] Formula (1):

number

[0031] The n is the total number of grains measured through the electron backscatter diffraction (EBSD) analysis, and may be 350 to 450, preferably 380 to 430, and more preferably 390 to 410. If the total number of grains measured is too small, it may not represent the grain size tendency in the entire cathode material powder, and if it is too large, the measurement accuracy may decrease.

[0032] Electron Backscatter Diffraction (EBSD) analysis is a method to measure the crystallographic phase and crystallographic orientation of a sample using the diffraction pattern of the sample, and to analyze the crystallographic information of the sample based on the measurement. When the sample is tilted at a large angle to the direction of the electron beam in a scanning electron microscope, the incident electron beam is scattered within the sample, and a diffraction pattern is displayed in the direction of the surface of the sample, which is called an electron backscattered diffraction pattern (EBSP). The electron backscattered diffraction pattern responds to the crystal orientation of the area irradiated with the electron beam, so it can be used to accurately measure the crystal orientation of the sample and obtain an EBSD IPF map (inverse pole figure map) that shows the grains with the same crystal orientation divided into sections. In addition, the IPF map can be image-analyzed using the EBSD software to obtain information such as grain size, pattern, and orientation.

[0033] In the present invention, for the EBSD analysis of the cathode material powder, an electrode for EBSD analysis is manufactured using the cathode material powder to be analyzed, and then the manufactured electrode is cut by ion milling, and the cut electrode cross section is irradiated with an electron beam to perform the EBSD analysis. Specifically, the electrode for EBSD measurement can be manufactured by mixing the cathode material powder to be analyzed, a conductive material, and a binder in N-methylpyrrolidone to manufacture an electrode slurry, applying the electrode slurry on an aluminum current collector, and drying it. Meanwhile, a rolling process is not performed when manufacturing the electrode for EBSD analysis. This is because the rolling process may cause deformation and cracking of the cathode active material particles.

[0034] 2 to 4 show IPF map images obtained by EBSD analysis of the cross section of the electrodes manufactured using the cathode powders of Example 1 and Comparative Examples 1 and 2, which will be described later, cut by ion milling. As shown in Fig. 2 to 4, images divided into grain units can be obtained through the EBSD analysis.

[0035] On the other hand, the above D 50 is the average particle size of the cathode material powder measured using a laser diffraction particle size analyzer, specifically, it means the particle size at a point where the volume cumulative amount is 50% in a volume cumulative particle size graph measured using a laser diffraction particle size analyzer.

[0036] The above formula (1) is calculated by dividing the sum of the volumes of the spheres whose diameter is the diameter of each grain measured through EBSD analysis by the number of grains, and then dividing the sum by the average particle diameter D of the cathode powder. 50 The degree of monoparticleization represented by the formula (1) is calculated by dividing the degree of monoparticleization by the degree of monoparticleization, and the closer the degree of monoparticleization represented by the formula (1) is to 1, the fewer the number of grains in the powdered positive electrode active material, i.e., the more particles in the form of monoparticles, and the closer the degree of monoparticleization is to 0, the more the positive electrode active material contains a large number of grains, i.e., the more particles in the form of secondary particles.

[0037] On the other hand, D substituted into the above formula (1) 50and grain radius are values ​​measured on a micrometer (μm) scale, but are dimensionless numbers that do not include units.

[0038] According to the research of the present inventors, it has been shown that when the degree of monoparticulation represented by the above formula (1) satisfies a specific range, it is possible to obtain the effects of simultaneously improving high-temperature storage characteristics, high-temperature life characteristics, and resistance characteristics.

[0039] Specifically, it was found that when a secondary battery is manufactured using a cathode powder having a degree of monoparticulation of 0.3 to 0.8, preferably 0.3 to 0.6, the amount of gas generated after high-temperature storage is significantly reduced and the high-temperature life characteristics are significantly improved compared to when a conventional cathode material having a secondary particle form is used, while the resistance characteristics are maintained at the same level, and the high-temperature storage characteristics, high-temperature life characteristics, and resistance characteristics are all excellent. When a cathode powder having a degree of monoparticulation of less than 0.3 is used, there is no effect of improving gas generation and life characteristics during high-temperature storage, and when the degree of monoparticulation exceeds 0.8, there is an effect of improving the high-temperature life characteristics and high-temperature storage characteristics, but the resistance increases and the output and capacity characteristics decrease.

[0040] Meanwhile, the positive electrode material powder according to the present invention contains positive electrode active material particles that include a lithium nickel-based oxide represented by the following [chemical formula 1].

[0041] [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2 In the above [Chemical Formula 1], the M 1 may be Mn, Al or a combination thereof, preferably Mn or a combination of Mn and Al.

[0042] Said M 2is one or more selected from the group consisting of Ba, Ca, Zr, Y, Ti, Mg, Ta, Nb, and Mo, preferably one or more selected from the group consisting of Zr, Y, Mg, and Ti, and more preferably Zr, Y, or a combination thereof. Element M2 is not necessarily included, but when included in an appropriate amount, it can play a role in promoting particle growth during firing or improving the stability of the crystal structure.

[0043] Said a represents the molar ratio of lithium in the lithium nickel-based oxide, and may be 0.80 ≦ a ≦ 1.20, 0.90 ≦ a ≦ 1.10, or 0.95 ≦ a ≦ 1.15. When the molar ratio of lithium satisfies the above range, a stable layered crystal structure can be formed.

[0044] Said b represents the molar ratio of nickel in all metals excluding lithium in the lithium nickel-based oxide, and may be 0.55 ≦ b < 1, 0.60 ≦ b < 1, 0.80 ≦ b < 1, or 0.82 ≦ b < 1. When the molar ratio of nickel satisfies the above range, excellent capacity characteristics appear. In particular, when the molar ratio of nickel is 0.80 or more, more excellent capacity characteristics can be realized.

[0045] Said c represents the molar ratio of cobalt in all metals excluding lithium in the lithium nickel-based oxide, and may be 0 < c < 0.45, 0 < c < 0.40, 0 < c < 0.20, or 0 < c < 0.18.

[0046] Said d represents the molar ratio of element M in all metals excluding lithium in the lithium nickel-based oxide 1 and may be 0 < d < 0.45, 0 < d < 0.40, 0 < d < 0.20, or 0 < d < 0.18.

[0047] Said e represents the molar ratio of element M in all metals excluding lithium in the lithium nickel-based oxide 2 and may be 0 ≦ e ≦ 0.20, 0 ≦ e ≦ 0.15, or 0 ≦ e ≦ 0.10.

[0048] More preferably, the lithium nickel-based oxide may be represented by the following [Chemical Formula 1-1].

[0049] [Chemical Formula 1-1] Li a1 Ni b1 Co c1 Mn d1 Al d2 M 2 e1 O2 In the above [Chemical Formula 1-1], M 2 is one or more selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo, and 0.80 ≦ a1 ≦ 1.20, 0.82 ≦ b1 < 1, 0 < c1 < 0.18, 0 < d1 < 0.18, 0 ≦ d2 < 0.18, 0 ≦ e1 ≦ 0.20, and preferably 0.80 ≦ a1 ≦ 1.20, 0.82 ≦ b1 < 1, 0 < c1 < 0.15, 0 < d1 < 0.15, 0 < d2 < 0.15, 0 ≦ e1 ≦ 0.10. When the lithium nickel-based oxide has the composition of the above [Chemical Formula 1-1], the structural stability and capacity characteristics of the positive electrode active material are excellently exhibited.

[0050] On the other hand, the positive electrode active material may further include a coating layer formed on the surface of the lithium nickel-based oxide and containing one or more coating elements selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, and S.

[0051] When a coating layer is present on the surface of the lithium nickel-based oxide, the contact between the electrolyte and the lithium nickel-based oxide is suppressed by the coating layer, so that the effects of reducing the elution of transition metals and gas generation due to side reactions with the electrolyte can be obtained.

[0052] Preferably, the coating element may include Co. When a coating layer containing Co is formed on the surface of the lithium nickel-based oxide particles, the effects of suppressing side reactions with the electrolytic solution, improving the output, and reducing the resistance can be obtained.

[0053] Meanwhile, the positive electrode active material particles of the present invention may be a single particle consisting of one nodule and / or a quasi-single particle which is a composite of 30 or less nodules, preferably 2 to 20 nodules, more preferably 2 to 10 nodules, or may have a form including these. Preferably, the positive electrode material powder according to the present invention may be a combination of single particles and positive electrode active material particles in the form of quasi-single particles. If the number of nodules constituting the positive electrode active material particles exceeds 30, particle cracking increases during electrode manufacturing, and the occurrence of internal cracks due to volume expansion / contraction of the nodules during charging / discharging increases, which may reduce the effect of improving high-temperature life characteristics and high-temperature storage characteristics.

[0054] Meanwhile, the cathode powder according to the present invention may have an average grain diameter measured by EBSD of about 0.5 μm to 4 μm, preferably about 0.8 μm to 2 μm, and more preferably about 0.8 μm to 1.8 μm. When the average grain diameter of the cathode powder satisfies the above range, the rock salt phase in the lithium nickel oxide is small, and thus the resistance characteristics are more excellent.

[0055] On the other hand, the positive electrode powder D 50 The diameter of the positive electrode material powder may be 2.0 μm to 10.0 μm, preferably 2.0 μm to 8.0 μm. More preferably, the diameter of the positive electrode material powder is about 3.0 μm to 7.0 μm. 50 If the D is very small, the processability during electrode manufacturing may decrease, the electrolyte impregnation may decrease, and the electrochemical properties may increase. 50 If the resistance is too large, the output characteristics will decrease due to an increase in resistance.

[0056] The average particle size of the nodules in the positive electrode material powder may be 0.8 μm to 4.0 μm, preferably 0.8 μm to 3 μm, and more preferably 1.0 μm to 3.0 μm. When the average particle size of the nodules is within this range, particle cracking during electrode manufacturing can be minimized, and an increase in resistance can be more effectively suppressed. Here, the average particle size of the nodules refers to a value obtained by measuring the particle size of each nodule observed in an SEM image obtained by analyzing the positive electrode material powder with a scanning electron microscope, and then calculating the arithmetic average of the measured values.

[0057] The cathode powder of the present invention as described above can be prepared by mixing a cathode active material precursor and a lithium source material, and then calcining the mixture.

[0058] In this regard, the positive electrode active material precursor may be a commercially available positive electrode active material precursor, or may be prepared by a method for preparing a precursor known in the art.

[0059] For example, the precursor may be prepared by introducing an aqueous solution of a transition metal, an ammonium cation complex forming compound, and a basic compound into a reactor and stirring the mixture to carry out a coprecipitation reaction.

[0060] The transition metal aqueous solution may be prepared by dissolving a transition metal-containing source material in a solvent such as water, for example, by dissolving a nickel-containing source material, a cobalt-containing source material, or a manganese-containing source material in water. If necessary, the transition metal aqueous solution may further include an aluminum-containing source material.

[0061] Meanwhile, the transition metal-containing source material may be an acetate, carbonate, nitrate, sulfate, halite, sulfide, or oxide of a transition metal.

[0062] Specifically, the nickel-containing source material may be, for example, NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, nickel halides, or combinations thereof.

[0063] The cobalt-containing source material can be, for example, CoSO4, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4·7H2O, or combinations thereof.

[0064] The manganese-containing source material can be, for example, Mn2O3, MnO2, Mn3O4MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halides, or combinations thereof.

[0065] The aluminum-containing source material may be, for example, Al2O3, Al(OH)3, Al(NO3)3, Al2(SO4)3, (HO)2AlCH3CO2, HOAl(CH3CO2)2, Al(CH3CO2)3, aluminum halide, or a combination thereof. However, in the case of Al, it does not matter if it is added together with the lithium source material in the firing step described below, without being added to the transition metal aqueous solution.

[0066] In this case, the amount of each of the transition metal-containing raw materials to be added may be determined in consideration of the molar ratio of the transition metal in the cathode material to be finally produced. For example, in the present invention, the transition metal-containing raw materials may be added in an amount such that the molar ratio of cobalt to manganese in all transition metals contained in the aqueous transition metal solution is 0.5 or more and less than 1.

[0067] Meanwhile, the ammonium cation complexing agent may include at least one compound selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and (NH4)2CO3, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent. In this case, the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0068] The basic compound may be at least one compound selected from the group consisting of NaOH, KOH, and Ca(OH)2, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent. In this case, the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol) that is uniformly miscible with water.

[0069] When the aqueous transition metal solution, the ammonium cation complex former, and the basic compound are charged into a reactor and stirred as described above, the transition metal in the aqueous transition metal solution is coprecipitated to produce precursor particles in the form of transition metal hydroxide.

[0070] In this case, the transition metal aqueous solution, the ammonium cation complex forming agent, and the basic compound are added in amounts such that the pH of the reaction solution falls within a desired range.

[0071] When the precursor particles are formed by the above method, the positive electrode active material precursor is separated from the reaction solution to obtain the positive electrode active material precursor. For example, the reaction solution is filtered to separate the positive electrode active material precursor from the reaction solution, and the separated positive electrode active material precursor is washed with water and dried to obtain the positive electrode active material precursor. In this case, a process such as pulverization and / or classification may be performed as necessary.

[0072] Next, the positive electrode active material precursor and a lithium raw material are mixed and then calcined to prepare a lithium nickel-based oxide. 1 The metal-containing raw materials may be mixed together and calcined.

[0073] The lithium source material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a mixture thereof.

[0074] Meanwhile, the lithium source material and the positive electrode active material precursor may be mixed so that the molar ratio of Li:total metals in the precursor is 1:1 to 1.2:1, preferably 1:1 to 1.1:1. When the mixing ratio of the lithium source material and the metals in the positive electrode active material precursor satisfies the above range, the layered crystal structure of the positive electrode active material is developed, and a positive electrode material having excellent capacity characteristics and structural stability can be produced.

[0075] Meanwhile, the calcination is carried out under conditions that allow the grains of the positive electrode active material to grow so as to satisfy the range of the single particle degree of the present invention. The preparation of a positive electrode active material powder having a single particle and / or quasi-single particle form with a desired single particle degree is affected by the calcination conditions, which are affected by the properties of the positive electrode active material precursor, such as the composition and molar ratio of components in the precursor, and the presence of any additives. For example, if the calcination temperature is not an appropriate temperature corresponding to the precursor composition, the resulting positive electrode active material powder may not be in a single particle and / or quasi-single particle form and may not satisfy the desired single particle degree.

[0076] Specifically, the appropriate sintering temperature for producing a positive electrode active material powder having a desired degree of single particle size may vary depending on the metal composition in the precursor. For example, when the content of nickel (Ni) is 80 mol% or more, the sintering temperature may be about 790°C to 950°C, preferably about 800°C to 900°C.

[0077] The firing may be performed for 5 to 35 hours in an oxygen atmosphere. In this specification, the oxygen atmosphere means an atmosphere containing a sufficient amount of oxygen for firing, including an air atmosphere. In particular, it is preferable to perform the firing in an atmosphere having an oxygen partial pressure higher than that of the air atmosphere.

[0078] Meanwhile, when preparing a positive electrode active material having a coating layer, the calcination may be followed by a step of mixing the lithium composite transition metal oxide prepared by calcination with a coating raw material, followed by a heat treatment. In this case, the mixing may be a solid-phase mixing or a liquid-phase mixing, and the heat treatment may be performed at a suitable temperature depending on the coating raw material. For example, the heat treatment in the coating process may be performed at a temperature of 200°C to 700°C, or 300°C to 600°C, but is not limited thereto.

[0079] Meanwhile, in the manufacture of the cathode powder of the present invention, it is preferable not to perform a water washing process after the calcination. In the past, in the manufacture of high-nickel (High-Ni) NCM-based lithium nickel oxides having a nickel (Ni) content of 80 mol% or more, a water washing process was generally performed after calcination to reduce the content of lithium by-products. However, according to the research of the present inventors, it was shown that if a water washing process is performed in the manufacture of a lithium nickel oxide in the form of a single particle or pseudo-single particle, the surface characteristics of the lithium nickel oxide are deteriorated during the water washing process, and the resistance increases. Therefore, in the manufacture of the cathode powder of the present invention, it is preferable not to perform water washing, but to consume the residual lithium on the surface of the lithium nickel oxide through the process of forming a coating layer. In this way, when the cathode material is manufactured without washing the lithium nickel oxide with water, the increase in resistance due to surface defects can be suppressed.

[0080] positive electrode Next, the positive electrode according to the present invention will be described.

[0081] The positive electrode according to the present invention includes a positive electrode active material layer containing the positive electrode material powder according to the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and containing the positive electrode material powder. Since the positive electrode material powder has been described above, a description of the positive electrode material powder is omitted, and the following describes components other than the positive electrode material powder.

[0082] In the positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive and does not induce chemical changes in the battery, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may generally have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0083] The positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode material powder.

[0084] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing a chemical change in the battery that is constructed. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these may be used alone or in combination. The conductive material may be usually contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.

[0085] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.

[0086] The positive electrode may be manufactured by a typical method for manufacturing a positive electrode, for example, by mixing a positive electrode material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling the same.

[0087] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to have a viscosity that allows excellent thickness uniformity when the slurry is applied to manufacture a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.

[0088] Alternatively, the positive electrode may be manufactured by casting the positive electrode slurry on a separate support, peeling the positive electrode slurry from the support, and laminating the resulting film on a positive electrode current collector.

[0089] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.

[0090] The lithium secondary battery of the present invention includes the positive electrode according to the present invention. Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator and an electrolyte interposed between the positive electrode and the negative electrode, and the positive electrode is as described above. In addition, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0091] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0092] The negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of typically 3 to 500 μm, and may have fine irregularities formed on the surface of the current collector to enhance the binding force of the negative electrode active material, as in the case of the positive electrode current collector. For example, the negative electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0093] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.

[0094] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, among which any one or a mixture of two or more may be used.

[0095] Also, a metallic lithium thin film may be used as the negative electrode active material. Also, as the carbon material, both low crystalline carbon and high crystalline carbon may be used. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, scaly, spherical or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0096] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing a chemical change in the battery that is constructed. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these may be used alone or in combination. The conductive material may be usually contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.

[0097] The binder serves to improve the adhesion between the negative electrode active material particles and the adhesive strength between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.

[0098] For example, the negative electrode active material layer may be manufactured by coating a negative electrode slurry including a negative electrode active material and, optionally, a binder and a conductive material on a negative electrode current collector and drying the coated negative electrode slurry, or by casting the negative electrode slurry on a separate support and then peeling the negative electrode slurry from the support to obtain a film, which may then be laminated on the negative electrode current collector.

[0099] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery may be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and excellent electrolyte humidification ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymeric material may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single layer or multilayer structure.

[0100] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0101] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0102] The organic solvent may be any organic solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, or the like; dibutyl ether; ether-based solvents such as ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylenecarbonate (EC), and propylenecarbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2-C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond-directed ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes. Among these, carbonate-based solvents are preferred, and mixtures of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and low-viscosity linear carbonate-based compounds (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) are more preferred.

[0103] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within a range of 0.1 to 5.0M, and more preferably 0.1 to 3.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore excellent electrolyte performance can be exhibited, and lithium ions can be effectively transferred.

[0104] In addition to the constituents of the electrolyte, the electrolyte may further contain additives for the purpose of improving the life characteristics of the battery, suppressing the decrease in the battery capacity, improving the discharge capacity of the battery, etc. For example, the additives may be haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, which may be used alone or in combination, but are not limited thereto. The additives may be contained in an amount of 0.1% by weight to 10% by weight, preferably 0.1% by weight to 5% by weight, based on the total weight of the electrolyte.

[0105] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, and is therefore useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0106] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0107] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0108] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the exemplary embodiments set forth herein.

[0109] Example 1 Nickel-cobalt-manganese hydroxide powder with a Ni:Co:Mn molar ratio of 83:11:6 and lithium hydroxide were mixed so that the transition metal (Ni+Co+Mn):Li molar ratio was 1:1.05, and then calcined at 870°C for 10 hours to produce a cathode powder.

[0110] Example 2 A positive electrode material powder was produced in the same manner as in Example 1, except that the sintering was carried out at 890°C.

[0111] Example 3 A positive electrode material powder was produced in the same manner as in Example 1, except that the sintering was carried out at 910°C.

[0112] Example 4 A positive electrode material powder was produced in the same manner as in Example 1, except that the firing was carried out at 930°C.

[0113] Comparative Example 1 A positive electrode material powder was produced in the same manner as in Example 1, except that the firing was carried out at 770°C.

[0114] Comparative Example 2 A positive electrode material powder was produced in the same manner as in Example 1, except that the firing was carried out at 950°C.

[0115] Experimental Example 1:D 50 and measurement of nodule / primary particle size 0.1 g of each of the cathode powders produced in Examples 1 to 4 and Comparative Examples 1 to 2 was dispersed in a dispersion medium, and then introduced into a laser diffraction particle size measuring device (Microtrac MT3000). Ultrasonic waves of about 28 kHz were irradiated at an output of 60 W to measure the D of each of the cathode powders. 50 The measurement results are shown in Table 1 below.

[0116] In addition, a scanning electron microscope was used to obtain SEM images of each of the positive electrode material powders produced in Examples 1 to 4 and Comparative Examples 1 and 2.

[0117] Then, the particle size of the nodules / primary particles identified from the measured SEM images was measured, and the arithmetic mean value was calculated to obtain the average particle size (D mean The measurement results are shown in Table 1 below.

[0118] FIG. 1 shows SEM images of the positive electrode material powders of Example 1 and Comparative Examples 1 and 2.

[0119] Experimental Example 2: Measurement of grain size and monoparticle size The cathode powders produced in Examples 1 to 4 and Comparative Examples 1 and 2 were mixed with carbon black and a PVDF binder in a weight ratio of 95:2:3 in N-methylpyrrolidone to produce an electrode slurry. The electrode slurry was applied to one side of an aluminum current collector and then dried at 130° C. to produce an electrode for EBSD analysis. No rolling was performed during the production of the cathode.

[0120] The cathode was cross-sectioned using an ion milling device (HITACHI IM-500, accelerating voltage 6 kV), and an electron backscatter diffraction (EBSD) analysis was performed on the cross-section of the cathode using a FE-SEM (JEOL JSM7900F) equipped with an EBSD analyzer. The EBSD analysis was performed at an accelerating voltage of 15 kV, a WD of 15 mm, and a scale with a total number of grains of about 400 + / - 10.

[0121] The grain diameter of each particle observed from the cross section of each positive electrode was measured through EBSD analysis, and the grain radius was calculated as 1 / 2 of the maximum diameter of the measured grain, and the arithmetic mean value of the measured grain diameters was calculated as the average grain diameter. In addition, the grain radius and the D measured in Experimental Example 1 were 50 The degree of monoparticle size was calculated by substituting the above into formula (1). The measurement results are shown in Table 1 below.

[0122] 2 to 4 show EBSD maps of cross sections of electrodes manufactured using the positive electrode material powders of Example 1 and Comparative Examples 1 and 2. FIG.

[0123] [Table 1]

[0124] <Manufacturing lithium secondary batteries> The cathode powders prepared in Examples 1 to 4 and Comparative Examples 1 to 2, carbon black conductive material, and PVDF binder were mixed in a weight ratio of 95:2:3 in N-methylpyrrolidone to prepare a cathode slurry. The cathode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare a cathode.

[0125] Anode active material graphite, conductive material super C, and binder SBR / CMC were mixed in a weight ratio of 95.6:1.0:3.4 to prepare anode slurry, which was then applied to one side of a copper current collector, dried at 130°C, and rolled to prepare anode.

[0126] A separator was interposed between the positive and negative electrodes to prepare an electrode assembly, which was then placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. The electrolyte was prepared by dissolving LiPF6 at a concentration of 1M in a mixed organic solvent in which ethylene carbonate / dimethyl carbonate / diethyl carbonate were mixed in a volume ratio of 1:2:1, and adding 2 wt% vinylene carbonate (VC).

[0127] Experimental example 3: Evaluation of high-temperature storage characteristics Each of the lithium secondary batteries prepared above was charged to 4.2 V at 1C in CC-CV mode, and then the secondary battery was disassembled to separate the positive electrode. Then, 400 mg of the positive electrode and 400 μL of electrolyte were placed in a pouch-type battery case and sealed to prepare a cell. The cell was stored at 60° C. for 10 weeks, and the change in cell volume (ΔCell volume, unit: ΔmL) before and after high-temperature storage was measured. The change in cell volume was measured by placing the cell in water and measuring the change in the volume of the water. The measurement results are shown in FIG. 5 and Table 2.

[0128] Experimental example 4: Evaluation of high temperature life characteristics Each of the lithium secondary batteries prepared above was charged at 45° C. in CC-CV mode at 1 C to 4.25 V, and discharged at a constant current of 0.05 C to 2.5 V, which constitutes one cycle. After 300 charge-discharge cycles, the capacity retention rate was measured to evaluate the life characteristics. The measurement results are shown in FIG. 6 and Table 2.

[0129] [Table 2]

[0130] Experimental Example 5: Evaluation of resistance characteristics The cathode powders prepared in Examples 1 to 4 and Comparative Examples 1 to 2, carbon black conductive material, and PVDF binder were mixed in a weight ratio of 95:2:3 in N-methylpyrrolidone to prepare a cathode slurry. The cathode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare a cathode.

[0131] A lithium metal electrode was used as the negative electrode.

[0132] An electrode assembly was prepared by interposing a separator between the positive and negative electrodes, and then the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a coin-half cell. The electrolyte was prepared by dissolving LiPF6 at a concentration of 1M in a mixed organic solvent of ethylene carbonate / dimethyl carbonate / diethyl carbonate in a volume ratio of 1:2:1, and adding 2 wt% vinylene carbonate (VC).

[0133] The coin half-cell was charged and discharged once at 2.5 to 4.25 V under the condition of 0.1 C / 0.1 C, and then charged again to 4.25 V, and the resistance (unit: Ω) was measured according to the SOC while discharging 10% of the cell discharge capacity at each time. At this time, the resistance was measured from the voltage change when a current density of 1.0 C was applied for 10 seconds at each SOC. The measurement results are shown in FIG. 7.

[0134] It can be seen from Table 2 and FIGS. 5 to 7 that the batteries employing the cathode material powders of Examples 1 to 4, in which the degree of monoparticle size of Formula (1) falls within the range of the present invention, have significantly better high-temperature life characteristics and high-temperature storage characteristics than the battery employing the cathode material powder of Comparative Example 1, and have resistance characteristics equivalent to those of the battery of Comparative Example 1, with almost no increase in resistance.

[0135] In contrast, in the case of the battery using the cathode material powder of Comparative Example 2, the high-temperature life characteristics and high-temperature storage characteristics were at the same level as those of the battery using the cathode material powder of Example 1, but it was confirmed that the resistance increased significantly.

Claims

1. The lithium nickel-based oxide is represented by the following formula 1: A positive electrode material powder having a monoparticle degree represented by the following formula (1) of 0.3 to 0.8: [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O 2 In the above [Chemical Formula 1], M 1 is Mn, Al or a combination thereof, M 2 is one or more elements selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo, and 0.80≦a≦1.20, 0.55≦b<1, 0<c<0.45, 0<d<0.45, and 0≦e≦0.

20. Formula (1): [0010] In the formula (1), Ri is a radius of an i-th grain measured when an electrode manufactured using the positive electrode material powder is subjected to an ion milling process and then the electrode is analyzed by electron backscatter diffraction (EBSD), n is the total number of grains measured through the electron backscatter diffraction (EBSD) analysis, and is 350 to 450; The above D 50 is the volume cumulative average particle size of the positive electrode material powder measured via a particle size analyzer.

2. 2. The cathode material powder of claim 1, wherein the cathode active material powder comprises at least one of a single particle consisting of one nodule and a quasi-single particle which is a composite of 30 or less nodules.

3. 2. The cathode material powder of claim 1, wherein the cathode material powder is a combination of single-particle and quasi-single-particle morphology cathode active material particles.

4. The cathode material powder according to claim 1, wherein the average grain diameter of the cathode material powder is 0.5 μm to 4 μm.

5. D of the positive electrode material powder 50 The positive electrode material powder according to claim 1, wherein the particle size is 2.0 μm to 10.0 μm.

6. 2. The cathode material powder according to claim 1, wherein the average particle size of the nodules of the cathode material powder is 0.8 μm to 4.0 μm.

7. The cathode material powder according to claim 1, wherein the cathode material powder has a degree of monoparticle size represented by formula (1) of 0.3 to 0.

6.

8. 2. The positive electrode material powder according to claim 1, wherein in the [Chemical Formula 1], 0.80≦b<1, 0<c<0.20, 0<d<0.20, and 0≦e≦0.

10.

9. The lithium nickel-based oxide is represented by the following [Chemical Formula 1-1]: [Chemical formula 1-1] Li a1 Ni b1 Co c1 Mn d1 Al d2 M 2 e1 O 2 In the above [Chemical Formula 1-1], M 2 is one or more selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo, and 0.80≦a1≦1.20, 0.82≦b1<1, 0<c1<0.18, 0<d1<0.18, 0≦d2<0.18, and 0≦e1≦0.

20.

10. The positive electrode active material according to claim 1, further comprising a coating layer formed on the surface of the lithium nickel-based oxide and containing one or more coating elements selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb.Mo, Sr, Sb, Bi, Si and S.

11. A positive electrode comprising the positive electrode material powder according to any one of claims 1 to 10; and a current collector.

12. A lithium secondary battery comprising the positive electrode according to claim 11; and a negative electrode.

Citation Information

Patent Citations

  • Method for manufacturing positive electrode active material for secondary battery and positive electrode active material for secondary battery manufactured by the same

    JP2019508869A

  • Semiconductor light-receiving element

    JP2021141112A

  • Non-aqueous electrolyte secondary battery

    JP2021163542A

  • Positive electrode active material for secondary battery, method for producing the same, and lithium secondary battery including the same

    JP2021516424A

  • Apparatus and method for drying electrode sheet for battery

    KR102388446B1

Cited By

  • Cathode material powder and method for manufacturing cathode material powder

    JP2026532458A

  • Cathode material powder and method for manufacturing cathode material powder

    JP7935262B2