Fireproof heat insulating composition, fireproof heat insulating composition slurry, fireproof heat insulating board and fireproof heat insulating structure

A fire-resistant heat-insulating composition using calcium sulfoaluminate and gypsum with fibrous minerals and inorganic powders addresses the challenge of achieving both heat insulation and fire resistance, ensuring structural integrity in fireproof insulation boards and structures.

JP7551064B2Active Publication Date: 2024-09-17JSP CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2022534060
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-01
Filing Date
2021-06-29
Publication Date
2024-09-17
Estimated Expiration
2041-06-29

AI Technical Summary

Technical Problem

Conventional insulation materials face challenges in achieving both good heat insulation and fire resistance, with organic resin foams being flammable and inorganic fiber aggregates having high thermal conductivity and poor workability, while existing fire-resistant materials do not meet fire-resistant structural specifications and lose integrity during fires.

Method used

A fire-resistant heat-insulating composition comprising calcium sulfoaluminate, gypsum, fibrous inorganic clay minerals, and inorganic powders with pores, which is used to create a fireproof insulation board by filling resin molded articles with a slurry that solidifies to provide both fire resistance and heat insulation.

Benefits of technology

The composition achieves both good heat insulation and fire resistance, maintaining board integrity during fires, and can be used to construct fireproof structures in buildings and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551064000009
    Figure 0007551064000009
  • Figure 0007551064000008
    Figure 0007551064000008
  • Figure 0007551064000010
    Figure 0007551064000010
Patent Text Reader

Abstract

Provided is a fire-resistant heat insulation composition whereby it is possible to achieve suitable heat insulation properties and fire resistance. The fire-resistant heat insulation composition includes: 5-100 parts by mass of gypsum with respect to 100 parts by mass of calcium sulfoaluminate including at least 40-70 mass% of hauyne and 5-30 mass% of belite; and 0.1-20 parts by mass of a fibrous inorganic clay mineral with a moisture content of at least 5% with respect to a total of 100 parts by mass of the calcium sulfoaluminate and the gypsum.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fireproof insulation composition, a fireproof insulation composition slurry, a fireproof insulation board, and a fireproof insulation structure for constructing a fireproof insulation structure of a building. [Background technology]

[0002] A variety of insulating and fireproofing materials are used in buildings. Insulating materials include polyurethane foam, polystyrene foam, phenol foam, and other resin foams that are highly insulating, lightweight, and easy to work with. In addition, inorganic fiber aggregates such as glass wool and rock wool, which are inexpensive, are also used.

[0003] Since resin foam is an organic material, it burns when a fire occurs and often causes damage by spreading the fire, so measures to prevent this are needed.

[0004] On the other hand, inorganic fiber aggregates such as glass wool and rock wool are mainly composed of non-flammable materials, but they tend to have higher thermal conductivity than resin foams, making them inferior in terms of insulation, and because they are fibrous, they feel punctured and are difficult to work with.Furthermore, in the past, the fiber aggregate was packed in a plastic bag and inserted between the pillars and exterior walls of the house, but this had issues such as gaps and the bag falling off over time.

[0005] On the other hand, thermal insulation materials in which non-combustibility is imparted to resin foam are already on the market. For example, there is a non-combustible insulation board in which one or both sides of a phenol foam board are laminated with non-combustible materials such as aluminum foil, aluminum hydroxide paper, and gypsum-based boards. However, in the case of such conventional non-combustible insulation boards, although the surface facing the flames does not burn in the event of a fire, the heat melts the phenol foam inside, creating a cavity, causing the board itself to fall off and spread the fire. This problem has not been solved, and the material does not meet the fire-resistant construction specifications stipulated in the Building Standards Act.

[0006] Examples of existing technologies for improving the flame resistance of resin foams include a technology for improving the flame resistance of polyurethane foam that relates to an insulating material in which a foam is formed from an alkali metal carbonate, isocyanates, water, and a reaction catalyst (Patent Document 1), and a technology for an injection material mainly for ground improvement of tunnels that is a curable composition consisting of one or more inorganic compounds selected from the group consisting of hydroxides, oxides, carbonates, sulfates, nitrates, aluminates, borates, and phosphates of metals selected from the group consisting of lithium, sodium, potassium, boron, and aluminum, water, and isocyanates (Patent Document 2).

[0007] However, the conventional technology of Patent Document 2 was developed for ground improvement and is not intended to obtain thermal insulation. In particular, in the conventional method of reacting an aqueous solution of 30% or more of an alkali metal carbonate with an isocyanate as in Patent Document 1, a large amount of water is used, and a large amount of unreacted water remains, so it must be dried before it can be used as a thermal insulation material, and the size of the bubbles in the resulting foam is large, so the thermal insulation is considered to be not great.

[0008] As techniques for coating synthetic resin foam to improve its flame resistance, there has been disclosed a technique relating to heat-insulating coated granules in which synthetic resin foam particles are surface-treated by forming a coating consisting of sepiolite and an aqueous organic binder mainly composed of a water-soluble resin, and then further coated with a coating material consisting of an aqueous inorganic binder containing inorganic powder and water glass mainly composed of an alkali metal silicate, and then dried and hardened (Patent Document 3); and a technique relating to an inorganic-containing synthetic resin foam in which the cell structure on at least a portion of the surface of the synthetic resin foam is filled with a silica-based inorganic material consisting of one or a mixture of two or more of calcium silicate, magnesium silicate, aluminum silicate, and aluminosilicate (Patent Document 4).

[0009] However, in conventional technologies that use these silicates, when the resin foam melts and the silicate filling it loses its binding strength and turns into powder, making it difficult to maintain its shape as an insulation board.

[0010] Known technologies include a foamed resin composite structure in which the interconnected voids formed between the foamed beads of a foamed resin made of bead-method polystyrene foam are filled with a filler material made of an organic substance having an oxygen index of more than 21 (Patent Document 5), and a composite molded body in which the voids in a thermoplastic resin foamed bead molded body having interconnected voids and a porosity of 5 to 60% are filled with a hardened product of cement or gypsum containing smectite (Patent Document 6).

[0011] However, in Patent Document 5, since the interconnected voids are filled with an organic filler material, an improvement in flame resistance to the level of non-combustibility cannot be expected. Patent Document 5 targets expanded polystyrene foam with very dense voids, with a void ratio of the foam of about 3%, and it is difficult to say that the voids are effectively utilized. Patent Document 6 describes that it is preferable for the cement to contain ettringite in the hardened product, gives examples of cements containing ettringite by trade name, and describes that the cement contains smectite, which is considered to be one of the materials for reducing separation of materials, but does not describe the calcium sulfoaluminate of the present invention as a cement that produces ettringite.

[0012] Patent Document 7 describes a composition containing calcium aluminate with a CaO content of 40 mass% or more, gypsum, inorganic powder having a hollow structure with an average particle size of 20 to 60 μm, and waste glass foam powder with an average particle size of 20 to 130 μm, but differs from the present invention in that calcium aluminate is the main component. The material described in Patent Document 8 is used for the purpose of covering the surface of steel frames to protect them from fire, and is not considered to have significant heat insulation properties.

[0013] It also contains isocyanate, an active hydrogen-containing compound, water, a reaction catalyst, and auyne hydrate, and has a density of 350 kg / m 3The insulating material described below is a hydrate obtained by mixing (1) cement, (2) an auyne-containing substance, and (3) water, and an insulating material is known in which the (2) auyne-containing substance is a substance containing free lime, anhydrous gypsum, auyne, and calcium aluminoferrite (Patent Document 9). However, this insulating material differs from the present invention in that the resulting auyne hydrate is used.

[0014] A fire-resistant coating composition characterized by containing ettringite as a main component and further containing inorganic compound powder and titanium oxide powder that release non-flammable gas at 100 to 1000°C (Patent Document 10) is also known.

[0015] A technology is disclosed relating to an unfired refractory insulating material consisting of heat-resistant aggregate, lightweight aggregate, alumina-based binder, silicon carbide, and reinforcing fibers, and shirasu balloons are described as the lightweight aggregate and calcium aluminate as the alumina-based binder (Patent Document 11). [Prior art documents] [Patent documents]

[0016] [Patent Document 1] Japanese Patent Application Publication No. 10-67576 [Patent Document 2] Japanese Patent Application Publication No. 8-92555 [Patent Document 3] JP 2001-329629 A [Patent Document 4] JP 2012-102305 A [Patent Document 5] Patent No. 4983967 [Patent Document 6] JP 2015-199945 A [Patent Document 7] JP 2017-77994 A [Patent Document 8] Japanese Patent Application Publication No. 7-48153 [Patent Document 9] JP 2016-160145 A [Patent Document 10] Japanese Patent Application Publication No. 7-61841 [Patent Document 11] Japanese Unexamined Patent Publication No. 62-41774 Summary of the Invention [Problem to be solved by the invention]

[0017] However, the prior arts of Patent Documents 10 and 11 described above are also based on the premise that they are used as fire-resistant insulation materials in high-temperature regions used in iron and steel manufacturing, and are insufficient in terms of both insulation properties under normal environments and fire resistance during fires. For this reason, a method that can achieve both good insulation and fire resistance has been desired. In view of the above, an object of the present invention is to provide a fireproof and heat insulating composition which is capable of achieving both good heat insulation and fire resistance. [Means for solving the problem]

[0018] As a result of extensive investigations, the present inventors have discovered that a fireproof and insulating composition that can solve the above-mentioned problems and achieve both good heat insulation and fire resistance can be obtained by using a specific composition, and have thus completed the present invention.

[0019] [1] A fireproof and insulating composition comprising 100 parts by mass of calcium sulfoaluminate containing at least 40 to 70% by mass of hauin and 5 to 30% by mass of belite, 5 to 100 parts by mass of gypsum, and 0.1 to 20 parts by mass of a fibrous inorganic clay mineral having a moisture content of 5% or more by mass per 100 parts by mass of the total of the calcium sulfoaluminate and the gypsum. [2] The fireproof and insulating composition according to [1], which contains an inorganic powder having voids. [3] The fireproof and insulating composition according to [1] or [2], which contains a setting retarder. [4] The fireproof and insulating composition according to any one of [1] to [3], further comprising a hydration accelerator. [5] A refractory heat insulating composition slurry obtained by mixing the refractory heat insulating composition according to any one of [1] to [4] with water. [6] A fireproof and insulating board obtained by filling and solidifying the slurry of the fireproof and insulating composition according to [5] into voids in a resin molding having a continuous void ratio of 25 to 70 volume %. [7] A fire-resistant insulation structure comprising the fire-resistant insulation board according to [6]. Effect of the Invention

[0020] According to the present invention, it is possible to provide a fireproof and heat insulating composition that can achieve both good heat insulation and fire resistance. Therefore, by using the fireproof and insulating composition of the present invention and a slurry thereof, a fireproof and insulating board having both good fire resistance and heat insulation properties can be obtained. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a schematic diagram of the crystal structure of a fibrous inorganic clay mineral (sepiolite). [Diagram 2] FIG. 2 is a side view showing the structure of the fireproof structure. [Diagram 3] FIG. 2 is a top view showing the structure of the fireproof structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described in detail below. In the present specification, parts and percentages are based on mass unless otherwise specified. Numerical ranges in the present specification include the upper and lower limits unless otherwise specified.

[0023] [Fireproof and heat-insulating composition] The fireproof and insulating composition according to an embodiment of the present invention (hereinafter sometimes simply referred to as "the composition") contains 5 to 100 parts by mass of gypsum per 100 parts by mass of calcium sulfoaluminate containing at least 40 to 70% by mass of auyn and 5 to 30% by mass of belite, and contains 0.1 to 20 parts by mass of a fibrous inorganic clay mineral having a moisture content of 5% or more per 100 parts by mass of the total of the calcium sulfoaluminate and gypsum.

[0024] (Calcium Sulfoaluminate) Calcium sulfoaluminate is a general term for a substance with hydration activity, whose main components are CaO, Al2O3, and SO3, obtained by mixing calcia raw materials, alumina raw materials, sulfur raw materials, etc., and firing them in a kiln or melting them in an electric furnace and cooling them.

[0025] The calcium sulfoaluminate is different from the calcium sulfoaluminate used as an expansive agent defined in JIS A 6202, although there is no particular limitation to this. It is similar in that it contains auin and uses ettringite as a hydration product, but differs from the expansive agent defined in JIS A 6202 in that the calcium sulfoaluminate contains belite, is used in a mixture with gypsum, and is used as a main component rather than as an admixture for cement.

[0026] The content of auyne in calcium sulfoaluminate is 40 to 70%, preferably 45 to 70%, and more preferably 50 to 70%. If the content of auyne is less than 40%, the fire resistance is inferior, and even if it exceeds 70%, no further improvement in fire resistance can be expected. The belite content in calcium sulfoaluminate is 5 to 30%, preferably 5 to 20%, and more preferably 5 to 15%. If the belite content is less than 5%, it becomes difficult to ensure pot life and the long-term strength expression is low, resulting in poor fire resistance, whereas if it exceeds 30%, the fire resistance is poor.

[0027] Furthermore, as the calcium sulfoaluminate, compounds in which part of the CaO or Al2O3 in calcium sulfoaluminate is replaced with an alkali metal oxide, an alkaline earth metal oxide, silicon oxide, titanium oxide, iron oxide, an alkali metal halide, an alkaline earth metal halide, an alkali metal sulfate, an alkaline earth metal sulfate, or the like can also be used.

[0028] Furthermore, the calcium sulfoaluminate may contain up to 25% of minerals other than hauyne and belite, such as CaO, 12CaO·7Al2O3, 2CaO·Al2O3·SiO2, 3CaO·Al2O3, 4CaO·Al2O3·Fe2O3, and CaSO4. If the content is less than 25%, there is no adverse effect on the fire resistance and pot life.

[0029] The particle size of calcium sulfoaluminate is the best in terms of early strength development, with a Blaine specific surface area of ​​3,000 cm 2 / g or more is preferable, and 4,000 cm 2 / g or more is more preferable. 2 When the Blaine specific surface area is 1 / g or more, the early strength development is improved. Here, the Blaine specific surface area is a value measured in accordance with JIS R5201:2015 (physical testing method for cement).

[0030] (Gypsum) The gypsum contained in this composition can be any of anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum, and is not particularly limited. Anhydrous gypsum is a general term for calcium sulfate anhydrite, a compound with the molecular formula CaSO4, hemihydrate is a general term for compounds with the molecular formula CaSO4·1 / 2H2O, and dihydrate is a general term for compounds with the molecular formula CaSO4·2H2O.

[0031] The particle size of the gypsum is preferably an average particle size of 1 to 30 μm, more preferably 5 to 25 μm, in terms of non-combustibility, early strength development, and appropriate working time. Here, the average particle size is a value measured using a laser diffraction particle size distribution meter in a dispersed state using an ultrasonic device.

[0032] The content of gypsum in the composition is 5 to 100 parts by mass, and preferably 15 to 50 parts by mass, per 100 parts by mass of calcium sulfoaluminate. If the content of gypsum is less than 5 parts by mass or exceeds 100 parts by mass, sufficient fire resistance cannot be imparted.

[0033] (fibrous inorganic clay minerals) The fibrous inorganic clay mineral contained in the present composition (hereinafter, sometimes simply referred to as "fibrous mineral") must have a moisture content of at least 5% in order to obtain heat insulation and fire resistance. The fibrous inorganic clay mineral provides the composition with an effect of reducing material separation and also improves fire resistance.

[0034] A schematic diagram of the crystal structure of a fibrous inorganic clay mineral (sepiolite in FIG. 1) is shown (based on the structural model of Brauner and Preisinger; see JP-A-2004-59347 and JP-A-2002-338236). The fibrous mineral is a type of hydrous magnesium silicate mineral, and is a fibrous clay mineral that has a crystal structure as shown in FIG. 1 and is characterized by the presence of voids inside the crystals, with crystal water existing in the voids in the form of bound water or zeolite water.

[0035] According to Figure 1, two-dimensional crystal structures are stacked alternately like bricks to form a fibrous crystal structure. In this unit crystal structure, there are four hydroxyl groups bonded to Mg atoms, four bound waters bonded to Mg atoms, and eight zeolitic waters, as shown in Figure 1. Figure 1 shows eight zeolitic waters in the unit structure.

[0036] Fibrous minerals have a specific surface area of ​​50 to 500 m, depending on the type. 2 / g, the average fiber length is 0.1 to 50 μm, and the aspect ratio represented by the average fiber length / average fiber diameter is preferably 5 to 5000. Here, the specific surface area is a value measured according to the BET method and JIS Z8830:2013. The average fiber length and average fiber diameter are values ​​obtained by image analysis of SEM photographs.

[0037] Although there is no particular limitation on the fibrous mineral, a typical example is sepiolite ((OH2)4(OH)4Mg8Si 12 O 30 6~8H2O), palygorskite (attapulgite) ((OH2)4(OH)2Mg5Si8O 20.4H2O), wollastonite, loglinite, etc. Among these, one or more selected from sepiolite and palygorskite (attapulgite) are preferred.

[0038] The moisture content of the fibrous mineral is 5% or more, preferably 7% or more, and more preferably 9% or more, from the viewpoint of good fire resistance and heat insulation. The upper limit of the moisture content is not particularly limited, but is preferably 30% or less, for example. The fibrous mineral is heated from 30°C to 200°C using a thermogravimetric analyzer (TGA), and the moisture content W can be calculated from the following formula using the mass X before heating and the reduced mass (the mass reduced when heating from 30°C to 200°C) X1. The sample amount was 10 mg, the heating rate was 5.0°C / min, and the measurement was performed under air atmosphere conditions. Moisture content W (mass%)=(X1 / X)×100

[0039] The content of the fibrous mineral in the present composition is 0.1 to 20 parts, preferably 3 to 15 parts, per 100 parts of the total of calcium sulfoaluminate and gypsum. If the amount of the fibrous mineral is less than 0.1 part, the fire resistance and heat insulation may not be improved, and if it exceeds 20 parts, the fire resistance and heat insulation may be reduced. The fibrous mineral may be premixed with calcium sulfoaluminate and gypsum before use, or may be dispersed in water before use.

[0040] (Porous inorganic powder) In a preferred embodiment, the composition may further contain an inorganic powder having voids (hereinafter, sometimes simply referred to as "inorganic powder"). The inorganic powder is not particularly limited as long as it is a powder of an inorganic material having voids, and any inorganic powder can be used.

[0041] Representative examples of inorganic powders having voids include inorganic powders obtained from foams produced by heating volcanic deposits, such as volcanic ash balloons, at high temperatures; fly ash balloons generated from thermal power plants; inorganic powders obtained by burning obsidian, perlite, or shale; and waste glass foam powders (recycled glass balloons) obtained by crushing waste such as glass bottles, burning them, and adjusting the particle size. At least one of these can be used. When using fly ash balloons, it is preferable to use those with an ignition loss of 5% or less, since they contain less unburned carbon. In this specification, inorganic powders are defined to exclude the above-mentioned calcium sulfoaluminate, gypsum, and fibrous inorganic clay minerals.

[0042] Among these, at least one of the group consisting of shirasu balloons, fly ash balloons, and waste glass foam powder is preferred, since they are less likely to impair heat insulating properties when filled into the open cells of a foamed resin product.

[0043] The particle size of the inorganic powder is preferably an average particle size of 1 to 150 μm, more preferably 15 to 100 μm. Here, the average particle size is a value measured using a laser diffraction particle size distribution meter in a dispersed state using an ultrasonic device.

[0044] The content of the inorganic powder in the present composition is preferably 2 to 100 parts, more preferably 5 to 80 parts, per 100 parts of the total of calcium sulfoaluminate and gypsum. When the amount of the inorganic powder is 2 parts or more, the heat insulating property is improved, and when it is 100 parts or less, the fire resistance is improved.

[0045] (Retarder) In a preferred embodiment, the composition may further include a setting retarder. The setting retarder is a substance that adjusts the pot life of the refractory heat insulating composition slurry. Examples of the setting retarder include inorganic setting retarders and organic setting retarders. Examples of the inorganic setting retarder include phosphates, silicofluorides, copper hydroxide, boric acid or its salts, zinc oxide, zinc chloride, zinc carbonate, and the like. Examples of the organic setting retarder include oxycarboxylic acids (citric acid, gluconic acid, malic acid, tartaric acid, glucoheptonic acid, oxymalonic acid, lactic acid, etc.) or their salts (sodium salts, potassium salts, etc.), sugars, etc., as typified by sugar, and the like. One or more of these can be used. Furthermore, a mixture of an inorganic setting retarder such as a carbonate, bicarbonate, nitrate, hydroxide, silicate, etc., and the above-mentioned oxycarboxylic acids or their salts can also be used. Among these, hydroxycarboxylic acids or their salts alone or a mixture of an inorganic setting retarder and hydroxycarboxylic acids or their salts are preferred. In this specification, the setting retarder is defined to exclude the above-mentioned calcium sulfoaluminate, gypsum, fibrous inorganic clay minerals, and inorganic powders having voids.

[0046] The content of the setting retarder in the composition is preferably 0.02 to 2.0 parts, more preferably 0.05 to 1.0 parts, per 100 parts of the total of calcium sulfoaluminate and gypsum. When the amount of the setting retarder is 0.02 parts or more, it is easy to adjust the required pot life, and when it is 2.0 parts or less, the curing time is not too long and curing defects are unlikely to occur.

[0047] In a preferred embodiment, the composition may further contain a hydration accelerator. The hydration accelerator is a substance that promotes the reaction between calcium sulfoaluminate and gypsum, increases the amount of water of crystallization, and improves fire resistance, and is not particularly limited. Examples of the hydration accelerator include hydroxides such as calcium hydroxide, alkali metal silicates, aluminum sulfate such as anhydrous aluminum sulfate, alkali metal carbonates such as sodium carbonate, nitrates, nitrites, various Portland cements such as ordinary Portland cement, various inorganic filler fine powders, and the like, and one or more of these can be used. In this specification, the hydration accelerator excludes the above-mentioned calcium sulfoaluminate, gypsum, fibrous inorganic clay minerals, inorganic powders having voids, and setting retarders.

[0048] The content of the hydration accelerator in the present composition is preferably 0.1 to 15 parts by mass, more preferably 0.5 to 10 parts, per 100 parts of the total of calcium sulfoaluminate and gypsum. When the amount of the hydration accelerator is 0.1 part or more, a sufficient hydration acceleration effect is obtained, and when it is 15 parts or less, an effect of ensuring a sufficient pot life is obtained.

[0049] The content of calcium sulfoaluminate in the heat insulating fireproof composition according to the embodiment of the present invention is preferably 50 to 95%, more preferably 60 to 90%, from the viewpoint of fire resistance.

[0050] [Fireproof and heat insulating composition slurry] The refractory heat insulating composition slurry according to the embodiment of the present invention is prepared by mixing the refractory heat insulating composition and water. That is, the refractory heat insulating composition slurry can be prepared by using the refractory heat insulating composition and water (tap water, etc.). The amount of water used in preparing the slurry is not particularly limited, but is preferably 40 to 300 parts by mass, more preferably 80 to 250 parts by mass, per 100 parts by mass of calcium sulfoaluminate and gypsum in total. When the amount of water is 40 parts by mass or more, the voids are filled uniformly, improving the fire resistance, and when the amount of water is 300 parts by mass or less, the ettringite content in the hardened body in the voids increases, improving the fire resistance.

[0051] [Fireproof insulation board] The fireproof and insulating board according to an embodiment of the present invention is formed by filling and solidifying the fireproof and insulating composition slurry according to an embodiment of the present invention into voids in a resin molded body having a continuous void ratio of 25 to 70 volume %.

[0052] The fireproof and insulating composition slurry according to an embodiment of the present invention can be filled into the voids of a resin molded body (hereinafter sometimes simply referred to as a "resin molded body") having a continuous porosity of 25 to 70 volume % and solidified to produce the fireproof and insulating board according to an embodiment of the present invention.

[0053] The resin molded body is a resin having continuous voids, and has voids that can be filled with a slurry. Examples of the types of resin include foamed polyvinyl alcohol resin, foamed polyurethane resin, foamed polystyrene resin, foamed polyolefin resin, and foamed phenolic resin. The resin molded body can be obtained by filling a mold with granular foams having a diameter of several mm and having closed bubbles, which are made of these resins, and molding them under heat and pressure so that continuous voids are generated between the granular foams. The continuous void ratio of the resin molded body can be adjusted by the degree of pressure applied during production. For polystyrene resin, a resin molded body having continuous voids can be produced in accordance with the manufacturing method of polystyrene foam by the bead method. Among these, foamed polystyrene resin molded bodies are preferred in terms of versatility. If the continuous void ratio is 25% by volume or more, sufficient fire resistance can be imparted to the obtained board, and if it is 70% by volume or less, the board density is reduced, the thermal conductivity is reduced, and the heat insulation is improved. The continuous porosity V of the resin molded product can be determined, for example, by the following method. First, a rectangular sample is cut out from a resin molded body that has been left for 24 hours or more in an environment with a temperature of 23°C and a relative humidity of 50%, and the apparent volume (Va) is calculated from the external dimensions of the sample. Next, the sample is submerged in a measuring cylinder containing ethanol at a temperature of 23°C using a wire mesh tool, and the air present in the voids in the molded body is degassed by applying light vibration. Then, the rise in the water level is read taking into account the volume of the wire mesh tool, and the true volume (Vb) of the sample is measured. From the obtained apparent volume (Va) and true volume (Vb) of the sample, the continuous porosity (V) can be calculated using the following formula. Continuous porosity V(%)=[(Va-Vb) / Va]×100

[0054] The slurry filled into the continuous voids produces hydration products through a hydration reaction, which then solidifies (hardens). The continuous voids within the resin molding are filled with the hydration products. One example of the hydration product is ettringite, which is produced by the reaction of calcium sulfoaluminate and gypsum. Ettringite contains a large amount of water in its molecules as water of crystallization, so it dehydrates when heated, exhibiting a fire-extinguishing effect and imparting non-flammability to the resin molding.

[0055] The method of filling the resin molded body with the fireproof heat insulating composition slurry is not particularly limited, but examples thereof include a method of filling by pressing with compressed air, a method of filling by suction after reducing pressure with a vacuum pump, a method of placing the resin molded body on a vibration table and filling into the gap while applying vibration of 30 to 60 Hz, etc. Among these, the method of filling into the gap while applying vibration is preferred from the viewpoint of quality stability.

[0056] The method of curing the fireproof insulation board after filling the gaps with the fireproof insulation composition slurry is not particularly limited, but examples include curing in air at room temperature after filling, or curing in air at room temperature after covering the board surface with a plastic film, etc. In order to shorten the curing time, the fireproof insulation board may be cured at a temperature of 30 to 50°C.

[0057] In some embodiments, the entire board may be further covered with a nonwoven fabric, a reinforcing material such as a lattice-like fiber sheet may be placed on one or both sides of the board, or a nonwoven fabric and a fiber sheet may be used in combination.

[0058] The shape of the fireproof and insulating board of the present invention is not particularly limited, but is preferably 500 to 1000 mm long, 1000 to 2000 mm wide, and 10 to 100 mm thick. The thickness is more preferably 50 to 100 mm. If the size is small, the fireproof and insulating board becomes lighter, and the workability during installation is improved.

[0059] In some embodiments, the present fireproof and insulating composition slurry may further contain one or more additives, provided they do not affect the performance of the composition, such as surfactants, air entraining agents, carbonization promoters, flame retardant agents, fire spread inhibitors, inorganic substances, rust inhibitors, antifreeze agents, shrinkage reducing agents, clay minerals, anion exchangers, etc.

[0060] The density of the fireproof and insulating board according to the embodiment of the present invention is 100 to 800 kg / m3 so as not to impair the fireproof and insulating properties. 3 is preferable, and 200 to 500 kg / m 3 More preferably, 100 kg / m 3 If the resistance is more than 800kg / m, sufficient fire resistance is ensured. 3 If the thickness is less than this, sufficient heat insulation can be obtained.

[0061] [Fireproof and heat-insulating structure] The fireproof and heat-insulating structure according to the embodiment of the present invention includes a fireproof and heat-insulating board. That is, the fireproof structure of a building can be constructed using the above-mentioned fireproof and heat-insulating board. For example, such a fireproof structure is a structure consisting of layers in the order of siding board, moisture-permeable waterproof sheet, fireproof and heat-insulating board, structural plywood, and fireproof and heat-insulating board, in the layer structure from the exterior wall side, with a space of about 100 mm (space for insulating material such as glass wool) between the structural plywood and the fireproof and heat-insulating board by a stud (stud in FIG. 3). A furring strip may be provided between the siding board and the moisture-permeable waterproof sheet (see FIG. 3).

[0062] According to an embodiment of the present invention, a fire-resistant and insulating structure including a fire-resistant insulating board is obtained. When constructing a fire-resistant structure, depending on the required fire resistance specifications, the fire-resistant insulating board may be laminated in a plurality of sheets, or the fire-resistant insulating board may be used in combination with a reinforced gypsum board. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.

[0064] "Experimental Example 1" The lower part of the thickness direction of the foamed resin molded body A (size: length 20 cm × width 20 cm × thickness 5 cm) having continuous voids was reinforced with alkali-resistant glass fiber, and polyester nonwoven fabric was further layered. This was set in a vibration impregnation device, and the fireproof heat insulating composition slurry of the composition shown in Table 1 was poured onto the upper surface of the molded body, and vibration of 60 Hz was applied for 1 minute to impregnate the fireproof heat insulating composition slurry into the voids, thereby producing a fireproof heat insulating board. After filling, the fireproof heat insulating board was removed from the device and cured at room temperature for 3 days. The cured fireproof heat insulating board was evaluated for the content of crystal water, fire resistance, shape retention, shape retention rate, and thermal conductivity. The results are shown in Table 1.

[0065] (Materials used) Foamed resin molded product A: Commercially available polystyrene foam beads (diameter 1-5 mm) were filled into a molding machine (VS-500, manufactured by Daisen Kogyo Co., Ltd.), heated with steam, and fused together with voids between the foamed beads. The continuous void ratio was controlled by adjusting the degree of pressure. The continuous void ratio was 36.8%, and the density of the polystyrene foamed beads was 10.5 kg / m 3 , Thermal conductivity of polystyrene foam beads is 0.033W / (m K)

[0066] Calcium sulfoaluminate 1 (CSA1): CaO raw material, Al2O3 raw material and CaSO4 raw material were mixed and crushed, then heat treated at 1300℃ for 3 hours in an electric furnace to synthesize clinker, which was then crushed in a ball mill. Haoyne: 69%, belite: 10%, other minerals: 12%, Blaine specific surface area: 4800cm 2 / g

[0067] Calcium sulfoaluminate 2 (CSA2): CaO raw material, Al2O3 raw material and CaSO4 raw material were mixed and crushed, then heat treated at 1300℃ for 3 hours in an electric furnace to synthesize clinker, which was then crushed in a ball mill. Haoyne: 55%, belite: 24%, other minerals: 16%, Blaine specific surface area: 4900cm 2 / g

[0068] Calcium sulfoaluminate 3 (CSA3): CaO raw material, Al2O3 raw material and CaSO4 raw material were mixed and crushed, then heat treated at 1300℃ for 3 hours in an electric furnace to synthesize clinker, which was then crushed in a ball mill. Haoyne: 42%, belite: 29%, other minerals: 25%, Blaine specific surface area: 4950cm 2 / g

[0069] Ettringite 1 (ET1): Ettringite powder obtained by hydrothermal synthesis using hydrated lime, aluminum sulfate, and gypsum as starting materials, filtering, and drying the product. Water of crystallization: 46%

[0070] Gypsum 1 (CS1): Type II anhydrous gypsum manufactured by Noritake Company, product name D-101A, purity 95%, average particle size 20 μm

[0071] Gypsum 2 (CS2): β-type hemihydrate manufactured by Noritake Company, product name FT-2, purity 95%, average particle size 20 μm

[0072] Gypsum 3 (CS3): Gypsum dihydrate manufactured by Noritake Company, product name P52B, purity 95%, average particle size 20 μm

[0073] Fibrous mineral (F1): Sepiolite manufactured by TOLSA, product name: PANGEL AD, moisture content: 13.2%, average fiber length: 5 μm, average fiber diameter: 0.1 μm, specific surface area: 320 m 2 / g

[0074] Fibrous mineral (F2): Active Minerals International palygorskite (attapulgite), product name: MIN-U-GEL 200, moisture content: 9.8%, average fiber length: 5 μm, average fiber diameter: 0.1 μm, specific surface area: 270 m 2 / g

[0075] Fibrous mineral (F3): Wollastonite manufactured by Kansai Matec Co., Ltd., product name: KTP-H02, moisture content: 2.0%, average fiber length: 75 μm, average fiber diameter: 10 μm, specific surface area: 4200 cm 2 / g

[0076] Non-fibrous mineral (N1): Bentonite manufactured by Kunimine Industries, product name: Kunigel V1, crystal water rate: 3.5%, specific surface area: 60 m 2 / g, layered

[0077] Water: Tap water

[0078] (Preparation of refractory heat insulating composition slurry and amount of charge) (1) When calcium sulfoaluminate is used A mixture was prepared by adding gypsum in the amount shown in Table 1 to 100 parts by mass of calcium sulfoaluminate (CSA1 to 3), and then adding fibrous minerals (F1 to F3) or non-fibrous minerals (N1) in the types and amounts shown in Table 1 and 100 parts by mass of water to 100 parts by mass of the mixture, and stirring was performed for 5 minutes to prepare a slurry (fireproof heat insulating composition slurry). The prepared slurry had a volume of 810 cm 3 It was poured onto the top surface of the foamed resin molded body so that the volume was 1.1 times the void volume of the resin molded body.

[0079] (2) When synthetic ettringite is used When synthetic ettringite (ET1) was used, a mixture was prepared by mixing 100 parts by mass of the synthetic ettringite with fibrous mineral (F1) in a predetermined ratio shown in Table 1, and 100 parts by mass of water was added to the mixture, and the mixture was stirred for 5 minutes to prepare a slurry (fireproof heat insulating composition slurry). The prepared slurry had a volume of 810 cm 3 It was poured onto the top surface of the foamed resin molded body so that the volume was 1.1 times the void volume of the resin molded body.

[0080] (Measurement method) Continuous porosity: The continuous porosity of the foamed resin molded body was determined as follows. First, the apparent volume (Va) was determined from the external dimensions (10 cm long x 10 cm wide x 5 cm thick) of the foamed resin molded body that had been left for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%, and the sample was submerged in a measuring cylinder containing ethanol at a temperature of 23°C using a wire mesh tool, and the air present in the voids in the molded body was degassed by applying light vibration. Then, the water level rise was read taking into account the volume of the wire mesh tool, and the true volume (Vb) of the sample was measured. From the obtained apparent volume (Va) and true volume (Vb) of the sample, the continuous porosity (V) was calculated using the following formula.

[0081] Continuous porosity V(%)=[(Va-Vb) / Va]×100

[0082] Content of water of crystallization (amount of water of crystallization): 20 g of sample was taken from the fireproof insulation board, and the free water and foam in the hardened body were dissolved with acetone. After filtering, the residue was thoroughly washed with acetone and vacuum dried in a desiccator for 48 hours in an environment of 25°C. The amount of water of crystallization was determined by measuring the mass loss rate (%) of the dried hardened body (residue) in the range of 50 to 200°C using a thermal analyzer (heating rate: 10°C / min, in air). In this specification, the term "water of crystallization" refers to water that is chemically or physically bound in the fireproof and insulating board, excluding free water that can be removed by drying with acetone or the like.

[0083] Fire resistance: A heat generation test was carried out using a cone calorimeter as specified in ISO-5660-1:2002 to simply evaluate fire resistance. A test specimen measuring 10cm length x 10cm width x 5cm thickness obtained from a fire-resistant insulation board was used, and the total heat generation after heating for 20 minutes was 8MJ / m 2 It is preferable that the thickness is not more than 100 nm in terms of fire resistance (non-combustible).

[0084] Thermal conductivity: Measurements were taken with a rapid thermal conductivity meter (box probe method) using a test specimen of 10 cm length x 5 cm width x 5 cm thickness obtained from a fireproof insulation board. The lower the thermal conductivity, the higher the heat insulating property. The thermal conductivity is preferably 0.070 W / mK or less.

[0085] Shape retention: After a combustion test (fire resistance test) using a cone calorimeter, the test specimen was rated as ◯ if it had no cracks, breaks, collapse, missing parts, or shrinkage, and rated as × if it had any cracks, breaks, collapse, or missing parts.

[0086] Shape retention rate: The shape retention rate ((volume of specimen after test / volume of specimen before test) x 100(%)) was measured by comparing the volume of the specimen after the combustion test (fire resistance test) using a cone calorimeter with the volume of the specimen before the test.

[0087] [Table 1]

[0088] The amount of gypsum (CS) in Table 1 above is the part by mass relative to 100 parts by mass of calcium sulfoaluminate (CSA). The amount of fibrous mineral (F) is the part by mass relative to 100 parts by mass of a mixture of calcium sulfoaluminate (CSA) and gypsum (CS). In addition, in Experiment No. 1-22, 5 parts by mass of fibrous mineral (F1) and 5 parts by mass of fibrous mineral (F2) were mixed with 100 parts by mass of a mixture of calcium aluminate (CA) and gypsum (CS).

[0089] From Table 1, it can be seen that the amount of crystallization water in the filled hardened body, for example, the amount of crystallization water in ettringite, is greatly increased by using calcium sulfoaluminate, gypsum, and fibrous minerals that satisfy the specified conditions. In other words, since the fibrous minerals contribute to the reaction between calcium sulfoaluminate and gypsum, the content ratio of ettringite increases, and the fire resistance, shape retention, and thermal conductivity can be improved. On the other hand, in the comparative example in which synthetic ettringite was used, it can be seen that the amount of crystallization water is not increased by using the fibrous minerals. In this comparative example, most of the water added when preparing the slurry exists as free water, not as crystallization water, so that the free water is easily lost when dried or heated over time, and it is considered that the effect of the examples cannot be obtained.

[0090] "Experimental Example 2" To 100 parts by mass of calcium sulfoaluminate (CSA1), 50 parts by mass of gypsum (CS1), and 100 parts by mass of a mixture of calcium sulfoaluminate and gypsum, inorganic powders of the types and amounts shown in Table 2, 7 parts by mass of fibrous mineral (F1), and 100 parts by mass of water were added, and a fireproof and insulating composition slurry was prepared in the same manner as in Experimental Example 1, and its performance was evaluated. The results are shown in Table 2.

[0091] (Materials used) Inorganic powder 1 (P1): Shirasu Balloon manufactured by Axes Chemical Co., Ltd., product name: MSB-301, average particle size 50 μm Inorganic powder 2 (P2): Shirasu Balloon manufactured by Axes Chemical Co., Ltd., product name: ISM-F015, average particle size 22 μm Inorganic powder 3 (P3): Shirasu Balloon manufactured by Axes Chemical Co., Ltd., product name: MSB-5011, average particle size 96 μm Inorganic powder 4 (P4): Tomoe Engineering Co., Ltd. fly ash balloon, product name: Senolite SA, average particle size 80 μm Inorganic powder 5 (P5): Waste glass foam powder manufactured by DENNERT PORAVER GMBH, product name: Poraver (0.04-0.125 mm particle size), average particle size 90 μm

[0092] [Table 2]

[0093] In Table 2, the amount of inorganic powder (P) is the part by mass relative to 100 parts by mass of the mixture of calcium sulfoaluminate (CA) and gypsum (CS). In Experiment No. 2-13, 7 parts by mass of inorganic powder (P1) and 7 parts by mass of inorganic powder (P4) were mixed with 100 parts by mass of the mixture of calcium sulfoaluminate (CA) and gypsum (CS).

[0094] From Table 2, it can be seen that by further containing an inorganic powder, the fireproof and heat insulating composition can improve heat insulating properties while maintaining excellent fire resistance and shape retention.

[0095] "Experimental Example 3" To 100 parts by mass of calcium sulfoaluminate (CSA1), 50 parts by mass of gypsum (SC1), and 100 parts by mass of a mixture of calcium aluminate and gypsum, the type and amount of a setting retarder shown in Table 3, 7 parts by mass of a fibrous mineral (F1), and 100 parts by mass of water were added, and a refractory heat insulating composition slurry was prepared in the same manner as in Experimental Example 1, and its performance was evaluated. The gelation time was also evaluated. The results are shown in Table 3.

[0096] (Materials used) Coagulation retarder (R1): Reagent grade 1 sodium citrate Set retarder (R2): Reagent grade 1 tartaric acid Coagulation retarder (R3): Reagent grade 1 sodium gluconate

[0097] (Measurement method) Gel time: The prepared fireproof and heat insulating composition slurry was placed in a plastic beaker, which was then placed in an insulated container, and a resistance thermometer was inserted. The gel time was determined as the time it took for the temperature to rise by 2°C due to the heat generated by the hardening of the mortar, compared to the temperature immediately after the end of kneading, as recorded by a recorder.

[0098] [Table 3]

[0099] In Table 3 above, the amount of the setting retarder (R) is expressed in parts by mass relative to 100 parts by mass of the mixture of calcium sulfoaluminate (CSA) and gypsum (CS).

[0100] From Table 3, it can be seen that by further containing a setting retarder, the pot life can be adjusted while maintaining excellent fire resistance, shape retention, and heat insulation properties.

[0101] "Experimental Example 4" To 100 parts by mass of calcium sulfoaluminate (CSA1), 50 parts by mass of gypsum (SC1), and to 100 parts by mass of a mixture of calcium sulfoaluminate and gypsum, 0.07 parts by mass of a setting retarder, the types and amounts of hydration accelerators shown in Table 4, 7 parts by mass of fibrous mineral (F1), and 100 parts by mass of water were added, and a refractory heat insulating composition slurry was prepared in the same manner as in Experimental Example 1, and the performance was evaluated. The gelation time was also evaluated. The results are shown in Table 4.

[0102] (Materials used) Hydration accelerator 1 (ACC1): Calcium hydroxide, first-grade reagent Hydration accelerator 2 (ACC2): Denka ordinary Portland cement Hydration accelerator 3 (ACC3): Reagent grade 1 sodium carbonate Hydration accelerator 4 (ACC4): Reagent grade 1 anhydrous aluminum sulfate

[0103] [Table 4]

[0104] In Table 4 above, the amount of hydration accelerator (ACC) is expressed in parts by mass relative to 100 parts by mass of the mixture of calcium sulfoaluminate (CSA) and gypsum (CS).

[0105] From Table 4, it is seen that by further containing a hydration promoter in the fireproof and heat insulating composition, the amount of water of crystallization can be increased, and fire resistance can be improved while maintaining excellent heat insulating properties and shape retention.

[0106] "Experimental Example 5" A mixture was prepared by adding 50 parts by mass of gypsum (CS1) to 100 parts by mass of calcium sulfoaluminate (CSA1), and 7 parts by mass of fibrous mineral (F1) and water in the amounts shown in Table 5 were added to 100 parts by mass of the mixture of calcium sulfoaluminate and gypsum to prepare a fireproof and insulating composition slurry in the same manner as in Experimental Example 1, and the performance was evaluated. The results are shown in Table 5.

[0107] [Table 5]

[0108] In Table 5 above, the amount of water is expressed in parts by mass relative to 100 parts by mass of the mixture of calcium aluminate (CA) and gypsum (CS).

[0109] From Table 5, it is seen that by preparing a fireproof and heat insulating composition slurry with an appropriate amount of water, excellent fire resistance, shape retention, and heat insulating properties are exhibited.

[0110] "Experimental Example 6" 50 parts by mass of gypsum (CS1) was added to 100 parts by mass of calcium sulfoaluminate (CSA1), and 7 parts by mass of fibrous mineral (F1) and 100 parts by mass of water were added to 100 parts by mass of the mixture of calcium sulfoaluminate and gypsum, and the porosity of the foamed resin molded body was changed as shown in Table 6. A fireproof and heat insulating composition slurry was prepared in the same manner as in Experimental Example 1, and the performance was evaluated. The results are shown in Table 6. The porosity was changed by using foamed resin molded bodies B to E having different porosities.

[0111] (Materials used) Foamed resin molded body B: Commercially available polystyrene foam beads (diameter 1-5 mm) were filled into a molding machine (VS-500, manufactured by Daisen Kogyo Co., Ltd.) and heated with steam to fuse the foamed beads together while leaving voids between them. The continuous void ratio was controlled by adjusting the degree of pressure. The continuous void ratio was 25.3%, and the density of the polystyrene foam beads was 10.5 kg / m 3 , Thermal conductivity of polystyrene foam beads is 0.033W / m K

[0112] Foamed resin molded product C: Commercially available polystyrene foam beads (diameter 1-5 mm) were filled into a molding machine (VS-500, manufactured by Daisen Kogyo Co., Ltd.), heated with steam, and fused together with voids between the foamed beads. The continuous void ratio was controlled by adjusting the degree of pressure. The continuous void ratio was 43.9%, and the density of the polystyrene foamed beads was 10.5 kg / m 3 , Thermal conductivity of polystyrene foam beads is 0.033W / m K

[0113] Foamed resin molded product D: Commercially available polystyrene foam beads (diameter 1-5 mm) were filled into a molding machine (VS-500, manufactured by Daisen Kogyo Co., Ltd.), heated with steam, and fused together with voids between the foamed beads. The continuous void ratio was controlled by adjusting the degree of pressure. The continuous void ratio was 58.7%, and the density of the polystyrene foamed beads was 10.5 kg / m 3 , Thermal conductivity of polystyrene foam beads is 0.033W / m K

[0114] Foamed resin molded product E: Commercially available polystyrene foam beads (diameter 1-5 mm) were filled into a molding machine (VS-500, manufactured by Daisen Kogyo Co., Ltd.), heated with steam, and fused together with voids between the foamed beads. The continuous void ratio was controlled by adjusting the degree of pressure. The continuous void ratio was 69.4%, and the density of the polystyrene foamed beads was 10.5 kg / m 3 , Thermal conductivity of polystyrene foam beads is 0.033W / m K

[0115] [Table 6]

[0116] From Table 6, it can be seen that the use of a foamed resin molded product having appropriate continuous voids provides excellent non-flammability, shape retention, and heat insulation.

[0117] "Experimental Example 7" Fireproof and insulating boards (length 1000 mm×width 1000 mm×thickness 25 mm) were produced in the same manner as in Experimental Example 1 using the fireproof and insulating composition slurries of Experiment Nos. 1-1, 1-2, 2-5 and 4-1. The fireproof insulation boards thus prepared were assembled into the fireproof structure shown in Figures 2 and 3, and then placed in a fireproof furnace. The fireproof structure has a structure in which the ceramic siding board is fixed to a laminated board consisting of a moisture-permeable waterproof sheet, a fireproof insulation board, and structural plywood via furring strips, and the structural plywood of the laminated board is fixed to the fireproof insulation board via columns, as shown in Figure 3. Then, this fireproof structure was placed in a fireproof furnace so that the ceramic siding board side was the heating surface.

[0118] The size of the fireproof structure was 2200mm wide x 1200mm long. The test was carried out by changing the type and thickness of the fireproof insulation composition of the fireproof insulation board and checking the burning state of the fireproof structure after the test. When installing boards with different thicknesses, the number of boards installed was also changed. The results are shown in Table 7. Details of the materials used are as follows:

[0119] (Materials used) Ceramic siding board: Nichiha, Moen siding, thickness 16mm Breathable waterproof sheet: Fukubi Chemical Co., Ltd., Super Airtex KD Structural plywood: polyethylene, JAS standard, special grade, thickness 9mm Pillar (stud): Wood (cedar), length 15mm Furring strip: Wood (cedar), length 105mm

[0120] (Fire resistance test method) As shown in the side view of Figure 2 and the top view of Figure 3, which show the internal structure, the fireproof structure was placed in a fireproof furnace and heated on the side of the ceramic siding board that simulated the exterior wall, with gas burners (a total of five) igniting the fireproof structure for one hour according to the standard overheating curve in accordance with ISO 834. After that, the heating was stopped and the structure was left in the fireproof furnace for three hours. The structure was removed from the furnace and the fireproof insulation board was peeled off to check the burning state of the pillars.

[0121] [Table 7]

[0122] From Table 7, it can be seen that when a fire-resistant structure is made using the fire-resistant insulation board according to the embodiment of the present invention, the fire resistance is improved. [Industrial Applicability]

[0123] By using the fireproof and heat-insulating composition and its slurry according to the embodiment of the present invention, a fireproof and heat-insulating board having fire resistance and heat insulation properties can be obtained. In addition, when the board is used to construct a structure such as a wall or a pillar, the shape can be maintained even when exposed to flames, so that the board has the effect of preventing the spread of fire. Therefore, the embodiment of the present invention can contribute to the construction of buildings, vehicles, aircraft, ships, refrigeration equipment, and refrigeration equipment with high fire safety.

Claims

1. The calcium sulfoaluminate contains at least 40 to 70% by mass of auin and 5 to 30% by mass of belite, and contains 5 to 100 parts by mass of gypsum. the calcium sulfoaluminate contains minerals other than the auyne and the belite in an amount of 25% or less; The refractory heat insulating composition comprises 0.1 to 20 parts by mass of a fibrous inorganic clay mineral having a moisture content of 5% by mass or more per 100 parts by mass of the calcium sulfoaluminate and the gypsum combined.

2. 2. The heat insulating fire resistant composition of claim 1, further comprising an inorganic powder having voids.

3. 3. The heat insulating fireproof composition of claim 1, further comprising a set retarder.

4. The heat insulating fireproof composition according to any one of claims 1 to 3, further comprising a hydration accelerator.

5. A refractory heat insulating composition slurry comprising the refractory heat insulating composition according to any one of claims 1 to 4 and water.

6. A fireproof and insulating board obtained by filling the voids of a resin molded body having a continuous void ratio of 25 to 70 volume % with the fireproof and insulating composition slurry according to claim 5 and solidifying it.

7. A fire-resistant and insulating structure comprising the fire-resistant insulation board of claim 6.

Citation Information

Patent Citations

  • JP1974083967A

  • Non-burnt refractory heat insulator

    JP1987041774A

  • Fire-resistant coating material

    JP1995048153A

  • Composition for fire-resistant coating

    JP1995061841A

  • Curable composition

    JP1996092555A