Black matrix substrate and display device, and method for manufacturing black matrix substrate

The black matrix substrate with a transmittance adjustment layer and light-absorbing partition wall addresses stray light and external reflection issues, enhancing contrast and visibility in LED and organic EL displays.

JP7552039B2Active Publication Date: 2024-09-18TOPPAN HOLDINGS INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020038965
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-06
Publication Date
2024-09-18
Estimated Expiration
2040-03-06

AI Technical Summary

Technical Problem

Conventional display devices face issues with stray light entering adjacent pixels, reducing contrast and color purity, and external light reflection affecting visibility, particularly in LED and organic EL displays.

Method used

A black matrix substrate is developed with a transparent substrate, transmittance adjustment layer, black matrix, and light-absorbing partition wall, optimized for high visible light transmittance and low reflectance, incorporating carbon and silica fine particles to minimize stray light and external reflection.

Benefits of technology

The solution effectively reduces stray light impact on contrast and color purity, enhances visibility by minimizing external light reflection, and improves display quality in LED and organic EL displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552039000003
    Figure 0007552039000003
  • Figure 0007552039000008
    Figure 0007552039000008
  • Figure 0007552039000016
    Figure 0007552039000016
Patent Text Reader

Abstract

To provide a black matrix (BM) substrate forming a display device with improved visibility by relieving the decrease in contrast or the decrease in color purity because light enters the adjacent pixel as stray light in an LED display or an organic EL display, and provide a display device and a manufacturing method for the BM substrate.SOLUTION: In a BM substrate, a display device, and a manufacturing method for the BM substrate, a transparent substrate, a transmissivity adjustment layer, and BM including a plurality of first openings are stacked. On the BM, a protective layer and a light absorption partition wall including a second opening whose central axis coincides with that of the first opening are stacked in this order. The line width of the BM is wider than that of the light absorption partition wall. In a plan view, the light absorption partition wall is covered with the BM. The transmissivity adjustment layer is a resin diffused body containing carbon and silica microparticles. Preferably, the protective layer includes a third opening with the same shape as the first opening of the BM. The first opening and the third opening overlap at the same position in the plan view.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a display device that uses an LED or an organic electroluminescence (EL) element as a light source or an LED or an organic electroluminescence (EL) element as a display functional layer, and relates to a technique for improving display quality. [Background technology]

[0002] In recent years, a technology that uses direct-type backlights called mini-LEDs, which have a configuration in which multiple LED chips with sizes of, for example, 40 μm to 200 μm are arranged in a matrix, for use in liquid crystal display devices has been attracting attention. Mini-LEDs can be divided into two types: a method that uses three types of LED chips that emit red, green, and blue light to produce full color, and a method that uses a blue-emitting LED chip as a light source and converts the wavelength of the blue light to produce full color. In the following description, both micro-LEDs and mini-LEDs may be referred to as LED displays.

[0003] Also attracting attention is a technology that uses local dimming in which the light emission brightness of three types of LED chips is partially adjusted or light emission is partially stopped depending on the position of the display area on the display screen.

[0004] In such a liquid crystal display device using local dimming, the light emission on the display screen can be partially turned off, which can greatly improve the contrast of the display. In conventional liquid crystal display devices, the backlight is always on, so when the liquid crystal displays black, a small amount of light leaks, making it difficult to obtain a contrast comparable to that of an organic EL display. Liquid crystal display devices using local dimming have achieved the same contrast as an organic EL display, and are becoming superior display devices in terms of power consumption and lifespan.

[0005] Micro LEDs are display devices that have a structure in which LED chips, for example, 2 μm to 60 μm in size, are arranged in a matrix and display by driving each of the multiple LED chips individually. Such micro LEDs can display without using liquid crystal. The size of the LED chips is not limited to mini LEDs and micro LEDs.

[0006] Micro LEDs are broadly divided into two types: those that use three types of LED chips that emit red, green, and blue light, just like the mini LEDs mentioned above, and those that use only single-color LED chips that emit light in the blue wavelength range. In micro LEDs, each LED chip plays the role of a display function layer.

[0007] However, whether it is a micro LED, a mini LED, or an OLED, there is a concern that the light emitted from the light-emitting element may enter adjacent pixels as stray light, resulting in a decrease in display contrast and color purity. Such adverse effects on adjacent pixels become more pronounced as the resolution increases.

[0008] In LEDs and organic EL devices, which are light-emitting elements, a light-reflective electrode (hereinafter referred to as a reflective electrode) is generally provided at a position opposite the viewing side. In such a configuration, there is a problem that external light (sunlight or light from indoor lamps) incident from the viewing side is reflected and enters the observer's eyes, greatly reducing visibility. Usually, a circular polarizer is attached to the surface of the display device to cut the reflection of external light from the reflective electrode. However, circular polarizers are expensive, and an extra process of attaching the circular polarizer is required, so there is a demand to eliminate the circular polarizer.

[0009] 17 is a partial cross-sectional view of a conventional display device equipped with a light-emitting element 53, and shows a schematic diagram of the direction of light emitted from the light-emitting element. The light-emitting element may be an LED or an organic EL light-emitting element.

[0010] In the conventional display device shown in FIG. 17, among the emitted lights E20, E21, E22, E23, and E24, E20 and E24 enter adjacent pixels as stray light, causing adverse effects such as color mixing and contrast reduction in adjacent pixels.

[0011] Fig. 18 is a partial cross-sectional view showing a conventional display device, and illustrates the effect of external light (external light). Note that the display device shown here does not include (uses) a circular polarizer.

[0012] It can be seen that in the conventional display device shown in FIG. 18, oblique light In11 is reflected by the reflective electrode 51, and reflected light Re12 enters the viewer's eye 52, resulting in reduced visibility.

[0013] Patent Document 1 discloses a backlight device including a sheet that converts the wavelength of light emitted from a blue light-emitting element and a reflective partition wall, as described in claim 1. The main problem with Patent Document 1 is that the light becomes yellowish every time it passes through phosphor sheet 95, as described in paragraph

[0009] , and the solution is to make the surface of the reflective partition wall blue, as described in [Claim 4]. Also, FIG. 1 of Patent Document 1 shows an oxide semiconductor TFT as the TFT in display section 410 of the liquid crystal panel.

[0014] Patent Document 1 does not describe, for example, a technique for improving contrast or a technique for improving visibility when an observer views a liquid crystal panel. Patent Document 1 does not disclose a specific configuration including the electrodes of the blue light-emitting element used, and does not disclose, for example, the problem of external light reflection when a light-reflective reflective electrode is used for the lower electrode. Patent Document 1 hardly takes into account the technique for improving visibility, which is the most important for an observer.

[0015] Patent Document 2 discloses a full-color LED display panel in which a thin film that reflects or absorbs fluorescence is provided on the surface of a partition wall that surrounds a fluorescent light-emitting layer that converts wavelengths.

[0016] Patent Document 2 does not describe, for example, a technique for improving contrast or a technique for improving visibility when an observer views a full-color LED display device. Patent Document 2 does not disclose a specific configuration including an electrode of an LED that emits blue light, and does not disclose, for example, the problem of external light reflection when a light-reflective reflective electrode is used for the lower electrode. Patent Document 2 hardly takes into account the technique for improving visibility, which is the most important for an observer. [Prior art documents] [Patent documents]

[0017] [Patent Document 1] International Publication No. 2017 / 191714 Brochure [Patent Document 2] International Publication No. 2019 / 026826 Brochure Summary of the Invention [Problem to be solved by the invention]

[0018] The present invention has been made in consideration of the above problems, and has an object to provide a black matrix substrate that constitutes a display device with improved visibility by mitigating the decrease in contrast and color purity caused by stray light from light-emitting elements entering adjacent pixels in LED displays such as micro LEDs and mini LEDs, and further in organic EL displays, a display device using the same, and a method for manufacturing the black matrix substrate. [Means for solving the problem]

[0019] The black matrix substrate according to the first aspect of the present invention comprises: a transparent substrate, a transmittance adjusting layer, and a black matrix having a plurality of first openings are laminated in this order, and a protective layer and a light absorbing partition wall having second openings whose central axis coincides with that of the first openings are laminated in this order on the black matrix; The line width of the black matrix is Light-absorbing partition wider than the line width of and in a plan view, the light absorbing partition is covered with the black matrix, The transmittance adjusting layer is a black matrix resin dispersion containing carbon and silica fine particles. It is a trix board.

[0020] The black matrix substrate according to the present invention is The protective layer may be a black matrix substrate having a plurality of third openings having the same shape as the first openings of the black matrix, the first openings and the third openings overlapping at the same position in a planar view.

[0021] The black matrix substrate according to the present invention is The black matrix substrate may be one in which the protective layer has a visible light transmittance in the thickness direction of 95% or more and 99.5% or less in the wavelength range of 400 nm to 700 nm.

[0022] The black matrix substrate according to the present invention is The black matrix substrate may have a configuration in which a first transparent resin layer is inserted between the black matrix and the light absorbing partition wall.

[0023] The black matrix substrate according to the present invention is The second opening may be provided with a light wavelength conversion layer, which may be a black matrix substrate.

[0024] The black matrix substrate according to the present invention may be a black matrix substrate having a light scattering layer in the second opening.

[0025] The black matrix substrate according to the present invention may be a black matrix substrate in which the transmittance adjusting layer has a visible light transmittance in the thickness direction of 70% or more and 99.5% or less in the wavelength range of 400 nm to 700 nm.

[0026] The black matrix substrate according to the present invention may be a black matrix substrate in which at least one of a red filter, a green filter, and a blue filter is disposed in the plurality of first openings.

[0027] A display device according to a second embodiment of the present invention is a display device including a black matrix substrate according to the present invention.

[0028] The production method according to the third aspect of the present invention comprises the steps of: Of the black matrix substrates according to the first embodiment, this relates to one having a plurality of third openings. This manufacturing method is A step of applying and hardening a transmittance adjusting layer containing carbon and silica fine particles on a transparent substrate; A step of applying and hardening a black layer on the transmittance adjusting layer; applying an alkali-developable photosensitive protective layer onto the black layer and drying the same; exposing the protective layer to light using a photomask having a plurality of openings and developing the protective layer to form the third openings; and transferring the pattern of the plurality of third openings to a black layer by dry etching to form a black matrix while leaving a portion of the protective layer in a thickness direction. This is a method for manufacturing a black matrix substrate. Effect of the Invention

[0029] According to the present invention, it is possible to provide a black matrix substrate constituting a display device with improved visibility by mitigating the decrease in contrast and color purity caused by the light emitted from the light-emitting element entering adjacent pixels as stray light in an LED display such as a micro LED or a mini LED, and further an organic EL display, a display device using the same, and a manufacturing method for the black matrix substrate. In addition, by adjusting the carbon concentration of the transmittance adjusting layer, etc., it is possible to provide a display device with low light reflectance and further good visibility. [Brief description of the drawings]

[0030] [Figure 1]FIG. 3 is a partial cross-sectional view of the black matrix substrate according to the first embodiment of the present invention, taken along line AA' in FIG. 2 which will be described later. [Diagram 2] 2 is a partial plan view of the black matrix substrate according to the first embodiment of FIG. 1, viewed from above the first substrate side. [Diagram 3] 4 is a partial cross-sectional view of a modified example A of the black matrix substrate according to the first embodiment of the present invention. FIG. [Figure 4] FIG. 4 is a partial cross-sectional view of a modified example B of the black matrix substrate according to the first embodiment of the present invention. [Diagram 5] FIG. 11 is a partial cross-sectional view of a modified example C of the black matrix substrate according to the first embodiment of the present invention. [Figure 6] FIG. 11 is a partial cross-sectional view of modification D of the black matrix substrate according to the first embodiment of the present invention. [Figure 7] FIG. 1 is a partial plan view of a general driving circuit (active matrix driving) when the display function layer is a light emitting element such as an LED or an organic EL. [Figure 8] FIG. 11 is a partial cross-sectional view of a display device C according to a second embodiment of the present invention, which includes a black matrix substrate of modified example C of the first embodiment. [Figure 9] FIG. 1 is a partial cross-sectional view of a display device constructed using a black matrix substrate according to the present invention, and is a diagram illustrating one effect obtained by the black matrix substrate according to the present invention. [Figure 10] FIG. 11 is a partial cross-sectional view of a display device constructed using the black matrix substrate of the present invention, and is a diagram illustrating another effect obtained by the black matrix substrate of the present invention. [Figure 11] FIG. 11 is a partial cross-sectional view of a display device D including a black matrix substrate of modification D of the first embodiment, which relates to a modification of the second embodiment of the present invention. [Figure 12] FIG. 11 is a partial cross-sectional view of a display device E which relates to a modification of the second embodiment of the present invention and which includes a black matrix substrate of modification C of the first embodiment and uses a liquid crystal layer as a display function layer. [Figure 13]FIG. 1 is a partial plan view of a general driving circuit (active matrix driving) when the display function layer is a liquid crystal layer. [Figure 14] 5A to 5C are process diagrams illustrating a method for manufacturing a black matrix substrate according to a third embodiment of the present invention. [Figure 15] FIG. 11 is a partial cross-sectional view of a black matrix substrate manufactured by a method (A) for manufacturing a black matrix substrate according to a third embodiment of the present invention. [Figure 16] FIG. 11 is a partial cross-sectional view of a black matrix substrate manufactured by a method (B) for manufacturing a black matrix substrate according to a third embodiment of the present invention. [Figure 17] FIG. 1 is a partial cross-sectional view of a conventional display device, and shows a schematic view of the direction of light emission from a light-emitting element. [Figure 18] FIG. 1 is a partial cross-sectional view of a conventional display device, and illustrates the influence of external light (external light). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0032] In the following description, the same or substantially the same functions and components are given the same reference numerals, and their description is omitted or simplified, or is described only when necessary. In each drawing, the dimensions and ratios of each component are appropriately changed from the actual ones in order to make each component large enough to be recognized on the drawing. In addition, as necessary, elements that are difficult to illustrate, such as the structure of multiple layers constituting a conductive layer, wiring connections to a circuit section, switching elements (transistors), etc., are omitted or partially illustrated.

[0033] In each embodiment described below, characteristic features will be described, and descriptions of components that are the same as those used in a typical display device and the display device according to this embodiment will be omitted.

[0034] Ordinal numbers such as "first" and "second" are used to avoid confusion of components, such as the first substrate, the second substrate, and the first transparent resin layer, and do not limit the number. The matrix arrangement of light-emitting elements refers to an arrangement in which light-emitting units each containing one or more light-emitting elements are arranged in a matrix at a certain pitch in a plan view. Each light-emitting unit surrounded by a light-reflective partition contains one or more light-emitting elements that are light-emitting diodes. In a display device using the local dimming technology described below, the driving can be turned on and off in units of light-emitting units each containing, for example, three or more light-emitting elements, and the brightness of the light emitted can be adjusted in units of light-emitting units. In addition, in the local dimming technology, the number of pixels is greater than the number of light-emitting elements contained in the light-emitting unit in a plan view. In other words, the efficient display device driving due to the small number of light-emitting elements compared to the number of pixels can be said to be an advantage of local dimming.

[0035] The term "planar view" in the specification means a planar view in which an observer views the display device of the present invention in the normal direction from the first substrate side provided with a black matrix substrate.

[0036] In an embodiment of the present invention, the "display function layer" of the display device can be made of a plurality of light-emitting diode elements called LEDs (Light Emitting Diodes), a plurality of organic EL (Electro Luminescence) elements also called OLEDs (Organic Light Emitting Diodes), or a liquid crystal layer.

[0037] For LED chips, which are also light-emitting elements, vertical LED chips in which the electrodes (n-side electrode and p-side electrode) are separated into upper and lower parts in the thickness direction are preferred for high-definition applications. For large-sized display devices such as TVs, horizontal LED chips are also acceptable.

[0038] LEDs are generally manufactured by epitaxially growing the multilayer film that constitutes the element on a sapphire or silicon substrate via a buffer layer using a method such as MOCVD. The LED can be peeled off from the sapphire substrate by laser ablation and used as an LED chip.

[0039] [First embodiment: black matrix substrate] The black matrix substrate according to the present invention will now be described with reference to the drawings.

[0040] Fig. 1 is a partial cross-sectional view of a black matrix substrate according to a first embodiment of the present invention, taken along line A-A' in Fig. 2 described later. That is, Fig. 2 is a partial plan view of the black matrix substrate according to the first embodiment of Fig. 1, viewed from above the first substrate side.

[0041] The black matrix substrate 100 includes a first substrate 10-1, a transmittance adjusting layer 1 formed on the first substrate 10-1, and a black matrix 6 having a first opening 19. A protective layer 4 is laminated on the block matrix 6, and further, a light-absorbing partition wall 2 is laminated thereon.

[0042] As shown in the figure, the black matrix 6 has a first opening 19, and the light absorptive partition 2 has a second opening 35. A central axis C1 of the first opening 19 and a central axis C2 of the second opening 35 approximately coincide with each other. In addition, a line width W1 of the black matrix 6 is wider than a line width W2 of the light absorptive partition 2, and as can be seen from FIG. 2, the light absorptive partition 2 is covered with the black matrix 6 in a plan view.

[0043] In addition to the above, the black matrix substrate 100 is characterized in that the transmittance adjusting layer 1 is a resin dispersion containing carbon and silica fine particles.

[0044] As described later, a color filter can be disposed in the first opening 19. A light scattering film, a wavelength conversion layer, or the like can be disposed in the second opening 35 of the light absorptive partition wall 2.

[0045] The protective layer 4 has a third opening 20 having the same shape as the first opening 19 of the black matrix 6, and it is preferable that the first opening 19 and the third opening 20 overlap at the same position in a planar view, from the viewpoint of simplicity of the manufacturing process described below.

[0046] Each layer constituting the black matrix substrate 100 will now be described.

[0047] (First board) The first substrate 10-1 can be made of a transparent substrate such as a glass substrate, a quartz substrate, a sapphire substrate, a plastic substrate, etc. When a display device is constructed by bonding a second substrate 10-2 having an array of thin film transistors (described later) and a black matrix substrate 100 facing each other, it is preferable that the first substrate 10-1 and the second substrate 10-2 are made of the same substrate material.

[0048] In particular, it is desirable that the thermal expansion coefficient of the substrate material constituting the second substrate is the same as that of the substrate material constituting the black matrix substrate 100. When different substrate materials are used for the array substrate and the black matrix substrate 100 described below, problems such as warping or peeling of the substrate may occur from the viewpoint of the thermal expansion coefficient.

[0049] (Black Matrix) A material that can be used for the black matrix 6 is an alkali-soluble photosensitive resist in which carbon having light-shielding properties is dispersed. The optical density (ΔOD) of the black matrix 6 may be 1 or more and 4 or less. The optical density of the black matrix 6 may be 4 or more, but in the configuration of the embodiment of the present invention, since the black matrix 6 and the light-absorbing partition wall 2 overlap, there is little need to increase the light-shielding properties of the black matrix alone. Carbon is also called carbon black. The film thickness of the black matrix 6 can be set to, for example, around 1 μm.

[0050] The material (photosensitive resist or thermosetting resist) used for the black matrix 6 has much in common with the materials for the transmittance adjusting layer 1 and the protective layer, and will be described in detail below in relation to the transmittance adjusting layer.

[0051] (Transmittance adjustment layer) The transmittance adjusting layer 1 is a dispersion containing carbon, silica fine particles which are optically isotropic fine particles, and a resin in which the carbon and silica fine particles are dispersed.

[0052] Basically, the transmittance adjusting layer 1 can be made of the same material as the black matrix. It is preferable to form the transmittance adjusting layer 1 with a resin dispersion containing carbon as the main pigment. It is preferable to set the light transmittance of the transmittance adjusting layer 1 to a range of 70% to 99.5% for visible light. In this transmittance range, the resin dispersion of carbon is preferably used. Adjust the amount added to your body.

[0053] Micro LED and OLED display devices often have a light-reflective electrode underneath the LED or OLED layer, which is the light-emitting element. In micro LED and OLED display devices with this structure, the re-reflection of external incident light by the light-reflective electrode reduces visibility. Usually, expensive circular polarizers are used in conjunction with the display device to eliminate the re-reflection of external incident light. Alternatively, many liquid crystal display devices use two polarizers in a crossed Nicol configuration (with polarization axes perpendicular to each other).

[0054] When using a circular polarizing plate or polarizing plate as described above, it is desirable to add inorganic fine particles to the transmittance adjusting layer 1 that do not cause polarization distortion, are optically isotropic, and are transparent in the visible range, in order to improve dispersibility or reduce the refractive index of the transmittance adjusting layer 1.

[0055] Optically isotropic fine particles are dispersed in the transmittance adjusting layer 1. For example, silica fine particles with a solid ratio of 18% by mass are used as the optically isotropic fine particles. The particle size of the silica fine particles can be selected from the range of 5 nm to 300 nm, for example. Two or more types of inorganic fine particles that are transparent in the visible range and have different particle sizes may be dispersed in the transmittance adjusting layer 1 together with carbon. The combined use of silica fine particles prevents the generation of secondary particles that tend to occur with carbon alone, and improves the dispersibility of the carbon.

[0056] In addition, "optically isotropic" means that the transparent fine particles applied to the embodiment of the present invention have a crystal structure in which the a-axis, b-axis, and c-axis are equal to each other, or are amorphous, and the propagation of light is isotropic without being affected by the crystal axis or crystal structure. Silica fine particles have a non-crystalline structure (amorphous). As fine particles of resin such as resin beads, fine particles having various properties including refractive index are known, and these fine particles can be used in combination. Fine particles of resin such as acrylic, styrene, urethane, nylon, melamine, and benzoguanamine may be used in combination.

[0057] The addition of the fine particles to the transmittance adjusting layer 1 is not for the purpose of imparting light scattering to the transmittance adjusting layer 1. When the scattering film, which is often applied to display devices, contains particles, it is preferable to use particles having an average particle size of, for example, 1.0 μm to 3.0 μm in microns. In other words, by using particles having a particle size larger than the wavelength of visible light, it is easy to obtain suitable light scattering properties as a scattering film. These particles having an average particle size of 1.0 μm to 3.0 μm in microns can be applied to the light scattering layer described below.

[0058] In addition, since the refractive index of silicon dioxide is smaller than that of carbon, the silicon dioxide fine particles have the effect of lowering the refractive index of the transmittance adjusting layer 1. The transmittance adjusting layer 1 having a low refractive index has the effect of suppressing light reflection at the interface between the transmittance adjusting layer 1 and the black matrix 6, thereby improving visibility.

[0059] For example, when the light transmittance of the transmittance adjusting layer 1 is in a high transmittance range such as 95% or more and 99.5% or less, ripples due to interference may occur in the light reflection at the interface between the black matrix 6 and the transmittance adjusting layer 1, and the black matrix 6 may be observed to be slightly colored in an iridescent manner. Such slight coloring caused by reflected light is easily observed when the display device is turned off and black is displayed.

[0060] In contrast, by forming the transmittance adjusting layer 1 using silica fine particles and carbon in combination, it is possible to obtain the effect of preventing the occurrence of such ripples. From the above viewpoint, the transmittance adjusting layer 1 containing silica fine particles that are optically isotropic and transparent in the visible range is useful. In the manufacturing method described later, the silica fine particles can be applied to end point management in dry etching. The emission spectrum caused by the Si group during dry etching does not occur when etching the protective layer 4 or the black matrix 6 of the display device of the present invention that does not contain silica fine particles, but occurs when etching progresses to the transmittance adjustment layer 1 that contains silica fine particles. Dry etching is stopped at the stage where the emission spectrum caused by the Si group is confirmed.

[0061] It is technically possible to apply a black dispersion with an organic pigment added to the transmittance adjustment layer 1, and further to the black matrix. However, in a transmittance adjustment layer that contains an organic pigment as a coloring material, the reflected light at the interface between the transmittance adjustment layer and the black matrix may appear yellowish. Furthermore, when the black matrix pattern is formed by dry etching, many organic pigments contain metal atoms, which may cause contamination during the dry etching process.

[0062] In contrast, the transmittance adjusting layer 1 containing carbon as the main pigment component has flat reflected light and is hardly colored. Flat reflected light means that in the visible range of 400 nm to 700 nm, for example, in a small range of 100 nm, there is no unevenness (fluctuation) of 2% or more in transmittance, and a nearly straight transmittance curve is obtained. Furthermore, by using carbon or silicon as the pigment component, metal contamination in the dry etching process can be avoided.

[0063] As a method for forming the transmittance adjustment layer 1 that can be applied to the embodiment of the present invention, it is preferable to form the transmittance adjustment layer 1 so as to be a fully coated film (a flat film in which no uneven pattern is formed within the effective display area). This allows the transmittance adjustment layer 1 to be formed easily. The film thickness of the transmittance adjustment layer 1 is not particularly specified, but can be selected, for example, from the range of 0.5 μm to 1.5 μm. A pixel opening can also be provided in a part of the transmittance adjustment layer 1 according to the size of the pixel opening of the display device.

[0064] The transmittance of the transmittance adjustment layer 1 for visible light (typically, the transmittance when the light has a wavelength of 550 nm) can be selected from the range of 70% to 99.5%. A transmittance adjustment layer 1 with a transmittance exceeding 99.5% is prone to ripples due to interference from external light reflection, as described above, impairing the display quality in "black display." If the transmittance of the transmittance adjustment layer 1 falls below 70%, this is undesirable since it leads to a decrease in the brightness of the display device. Furthermore, if the transmittance falls below 60%, low reflectivity cannot be obtained.

[0065] The transmittance of the transmittance adjusting layer 1 may be adjusted in the range of 70% to 99.5% depending on the film thickness and carbon content of the transmittance adjusting layer 1 used in the black matrix substrate. Furthermore, by providing the transmittance adjusting layer 1 described above on the black matrix 6, a low reflectance of 0.3% to 1% can be obtained at the interface between the first substrate 10-1 and the transmittance adjusting layer 1. Increasing the amount of carbon added to the transmittance adjusting layer 1 to increase the carbon concentration increases the refractive index of the transmittance adjusting layer 1, thereby increasing the reflectance of the transmittance adjusting layer 1. When the transmittance of the transmittance adjusting layer 1 becomes less than 60%, the refractive index increases and the reflectance increases.

[0066] Regarding the adjustment of the transmittance of the transmittance adjusting layer 1, when the total solid content including the resin, silica fine particles, and carbon constituting the dispersion used in the transmittance adjusting layer 1 is taken as 100% by mass, the carbon amount can be selected, for example, from the range of 0.5% to 15% by mass. A transmittance adjusting layer 1 with a carbon amount of 0.4% or less by mass has a reduced low reflection effect and is prone to the occurrence of interference colors due to the above-mentioned ripples. If the carbon amount exceeds 15% by mass, the optical density of the transmittance adjusting layer 1 increases, making it difficult to obtain the low reflection effect.

[0067] When the total solid content including the silica fine particles, carbon, and the resin described later is taken as 100% by mass, the amount of the silica fine particles added can be selected, for example, from the range of 1% by mass to 30% by mass. If the amount of carbon particles is 1% by mass or less, interference colors due to ripples are likely to appear. If the amount of carbon and silica particles added exceeds 45% by mass or even 50% by mass, the coating suitability of the resist described below is likely to decrease. If the amount of carbon and silica particles added is too small, the characteristics expected of the transmittance adjusting layer 1 cannot be obtained.

[0068] As the alkali-soluble resin applied to the resist that can be used when forming the transmittance adjusting layer 1 or the black matrix 6, for example, a resin synthesized to a molecular weight of about 5000 to 100000 using about 1 to 5 kinds of monomers selected from acrylic acid, methacrylic acid, alkyl acrylate or alkyl methacrylate such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, cyclic cyclohexyl acrylate or methacrylate, hydroxyethyl acrylate or methacrylate, styrene, etc. can be used. Furthermore, a normal photopolymerizable resin such as epoxy (meth)acrylate can also be used. A cardo resin with excellent patterning properties and heat resistance can also be used.

[0069] As the photopolymerization initiator applied to the resist used in forming the transmittance adjusting layer 1 or the black matrix 6, any known compound can be used as appropriate, but it is preferable to use an oxime ester compound, which can achieve high sensitivity even when used in a black photosensitive resin composition that does not transmit light.

[0070] The above shows a photosensitive alkali-soluble material as a resist applicable to the present invention, but is not limited thereto. A thermosetting compound can be added to a resin to be used in the form of a thermosetting resin. As the thermosetting compound, for example, one having at least one group selected from an epoxy group, an alkoxymethyl group, and an acyloxymethyl group can be used. Alternatively, as the thermosetting compound, (a) an epoxy compound, (b) a melamine compound, a guanamine compound, a glycoluril compound, or a urea compound substituted with at least one substituent selected from a methylol group, an alkoxymethyl group, and an acyloxymethyl group, and (c) a phenol compound, a naphthol compound, or a hydroxyanthracene compound substituted with at least one substituent selected from a methylol group, an alkoxymethyl group, and an acyloxymethyl group. Among them, a polyfunctional epoxy compound is preferable as the thermosetting compound.

[0071] There is an advantage to using a thermosetting method as the material applied to the black matrix 6. Unlike the photosetting method, the thermosetting method does not require light transmission, so the filling rate of the carbon pigment can be increased. With the photosetting method, the carbon content is limited to approximately 45% of the total solids including resin, but with the thermosetting method, the carbon content (solid content) can be around 65%. By increasing the carbon content, high light blocking properties can be obtained, and the productivity can be improved by a high etching rate in the dry etching process of the manufacturing process. A black matrix with a high carbon content can be made thinner, and the flatness can be improved in the subsequent process, for example, in laminating color filters.

[0072] (protective layer) The protective layer 4 laminated on the black matrix 6 can be formed using the same material as the transmittance adjusting layer. By lowering the carbon solid ratio and setting the visible light transmittance of the protective layer to 95% or more and 99.5%, it is possible to suppress internal reflection of light from the lower surface of the black matrix 6 within the display device. Note that the upper surface of the black matrix 6 refers to the surface that contacts the transmittance adjusting layer, and the lower surface of the black matrix 6 refers to the surface opposite to the upper surface.

[0073] When used in a display device, light reflected from the bottom surface of the black matrix 6 may enter the semiconductor layer (channel layer) of a thin film transistor that drives a light emitting element of an optical module, causing the thin film transistor to malfunction. The reflectance of the rack matrix 6 can be reduced, thereby reducing the amount of reflected light.

[0074] (Light-absorbing partition) It is convenient to use a light-absorbing partition wall 2 that contains carbon, which has low visible light wavelength selectivity, as a black pigment. Low visible light wavelength selectivity means that coloring of light absorbed or reflected in the light wavelength range of 400 nm to 700 nm is not observed, and the light appears black or gray.

[0075] When the light-absorbing partition 2 is formed by a photolithography technique, a carbon dispersion of the resin used for formation can be applied to the transmittance adjusting layer 1. In this case, the transmittance in the film thickness direction at the exposure wavelength (e.g., 365 nm) is desirably within a range of 0.1% to 10%. The transmittance is the transmittance in the film thickness direction of the light-absorbing partition 2 (in other words, the direction in which the exposure light enters). If it is less than 0.1%, the exposure light does not enter sufficiently, and the light-absorbing partition 2 is likely to peel off during alkaline development. If the transmittance exceeds 10%, visible light is likely to transmit to adjacent pixels, resulting in a decrease in color purity related to display.

[0076] Between adjacent light-absorptive partition walls 2, a light-scattering layer 28 or a wavelength-converting layer 25, 26, 27 can be disposed in the second opening 35. The average particle shape of the light-scattering particles or phosphor particles applied to the light-scattering layer or wavelength-converting layer is preferably larger than the wavelength of light in terms of scattering efficiency and conversion efficiency. For example, if the particle shape is within the range of 1 μm to 5 μm, the scattering effect and wavelength conversion efficiency are good. Therefore, assuming that about 2 to 5 light-scattering particles or phosphor particles are stacked vertically, the height H1 of the light-absorptive partition wall can be within the range of 2 μm to 25 μm, for example.

[0077] Incidentally, the height H1 of the light-absorptive partition wall 2 may be set to 25 μm or more. However, when a general coating device such as a curtain coater or a slit coater is used, it is somewhat difficult to form a coating film having a sufficient thickness after drying, and therefore it is appropriate to set the upper limit at 25 μm.

[0078] [Modification A of the first embodiment] 3 is a partial cross-sectional view of a modified example A of the first embodiment of the black matrix substrate of the present invention. The difference from the first embodiment is that a first transparent resin layer 21 is laminated on a protective layer 4, and a light absorbing partition wall 2 is laminated on this protective layer 4.

[0079] This modified example A has the advantage that the height H2 of the first transparent resin layer can supplement the height H1 of the light absorbing resin layer 2. In other words, the height H3 obtained by adding the height H2 of the first transparent resin layer and the height H1 of the light absorbing resin layer 2 can be set as the effective height of the light absorbing partition wall, and by optimizing this with the pixel opening width W3 (or the width of the first opening 19), the adverse effects of external light and stray light from the light emitting element, which will be described later, can be suppressed.

[0080] Furthermore, by adjusting the transmittance and further adjusting the refractive index of the transmittance adjusting layer 1 of this modification A, it is possible to adjust the reflectance and improve the image quality when the black matrix substrate 101 is used in a display device.

[0081] The reflectance is the reflectance when the reflected light occurring at the interface between the black matrix 6 and the first substrate 10-1 is taken as the numerator and, for example, an aluminum standard piece is taken as 100% (denominator). The measurement is performed by measuring the reflectance using a microspectrophotometer.

[0082] [Modification B of the First Embodiment] FIG. 4 is a partial cross-sectional view of modified example B of the first embodiment of the black matrix substrate of the present invention. The difference from modified example A of the first embodiment is that the transmittance adjusting layer 1 is not formed in the pixel opening 19. The transmittance adjusting layer 1 in the pixel opening 19 can be removed by a dry etching technique described later. Alternatively, the transmittance adjusting layer 1 can be formed only in the area where the black matrix is ​​to be formed by applying, exposing, and developing the layer using a well-known photolithography technique. is also good.

[0083] In the present invention, the height of the light absorbing partition is important as a factor for suppressing stray light to adjacent pixels and improving display quality. This point has been explained in the modification A of the first embodiment, but the same discussion can be applied to other embodiments of the present invention.

[0084] In order to prevent stray light from adjacent pixels, the height H1 of the light absorbing partition and the height H3 from the first substrate 10-1 to the light absorbing partition are important. In Fig. 4, the thickness (height) of the first transparent resin layer 21 including the thicknesses of the transmittance adjusting layer 1, the black matrix 6, and the protective layer 4 is designated as H2. Therefore, in Fig. 4, the substantial height H3 of the light absorbing partition from the viewpoint of preventing stray light is the total thickness (height) of H1 and H2.

[0085] 4, the thickness of the transmittance adjusting layer is included in the substantial height H3 of the light absorptive partition wall. However, in the first embodiment and modification A, the thickness of the transmittance adjusting layer is not added to the substantial height H3 of the light absorptive partition wall from the viewpoint of stray light suppression.

[0086] As described above, the height H1 of the light-absorptive partition wall is preferably within the range of 2 μm to 25 μm.

[0087] In the modified examples A and B, the substantial height H3 of the light absorptive partition wall can compensate for stray light suppression by the film thickness of the first transparent resin layer 21 and the line width W1 of the black matrix in addition to the light absorptive partition wall 2. By increasing the line width W1 of the black matrix, the height H1 of the light absorptive partition wall can be formed low.

[0088] [Modification C of the First Embodiment] FIG. 5 is a partial cross-sectional view of the modified example C of the first embodiment of the black matrix substrate of the present invention. A transmittance adjusting layer 1, a black matrix 6, and a protective layer 4 are laminated on a first substrate 10-1, and color filters (red filter R, green filter G, and blue filter B) are disposed in the opening of the black matrix 6. A first transparent resin layer 21 is provided so as to cover these components, and a light-absorbing partition wall 2 is laminated thereon. A light-scattering layer 28 is disposed in the second opening between the light-absorbing partition walls 2, forming a black matrix substrate 103 of the modified example C. The first transparent resin layer 21 may be omitted. The second opening of the light-absorbing partition wall 2 may be configured so that red, green, and blue wavelength conversion layers 25, 26, and 27 correspond to color filters of the same color. (Red filter, green filter, blue filter) As described above, in the black matrix substrate of the present invention, color filters such as red filters, green filters, and blue filters can be disposed in the openings of the black matrix. These are formed by dispersing the organic pigment described below in a resin such as acrylic.

[0089] Examples of red organic pigments that can be used in the red filter include CI Pigment Red 7, 14, 41, 48:2, 48:3, 48:4, 81:1, 81:2, 81:3, 81:4, 146, 168, 177, 178, 179, 184, 185, 187, 200, 202, 208, 210, 246, 254, 255, 264, 270, 272, and 279. Yellow pigments and orange pigments can also be used in the red layer R.

[0090] The yellow organic pigments applicable to the present invention are CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 1 17, 118, 119, 120, 123, 126, 127, 128, 129, 147, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 187, 188, 193, 194, 199, 198, 213, 214, etc.

[0091] Examples of orange organic pigments include CI Pigment Orange 36, 43, 51, 55, 59, 61, 71, and 73, with CI Pigment Orange 36 being preferred.

[0092] Green pigments that can be used for the green filter include CI Pigment Green 7, 10, 36, and 37, and can also be used in combination with a yellow pigment. Zinc phthalocyanine halide green pigments and aluminum phthalocyanine halide green pigments can be suitably used.

[0093] Examples of blue pigments that can be used for the blue filter include CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 60, and 64, and can also be used in combination with a violet pigment. Examples of violet pigments include CI Pigment Violet 1, 19, 23, 27, 29, 30, 32, 37, 40, 42, and 50.

[0094] The organic pigment as described above is dispersed in a transparent resin together with an organic solvent and a dispersant. The transparent resin is preferably a transparent resin having a visible transmittance of 90% or more, and is preferably an alkali-soluble photosensitive resin containing a resin precursor. The pigment can be contained in the resin in a range of 15% to 45% by mass.

[0095] As the photosensitive resin, a resin in which a photocrosslinkable group such as a (meth)acryloyl group or a styryl group is introduced into a linear polymer having a reactive substituent such as a hydroxyl group, a carboxyl group or an amino group by reacting the linear polymer with a (meth)acrylic compound having a reactive substituent such as an isocyanate group, an aldehyde group or an epoxy group or with cinnamic acid is used.

[0096] Examples of monomers and oligomers that are precursors of transparent resins include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, polyethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tricyclodecanyl (meth)acrylate, melamine (meth)acrylate, and epoxy (meth)acrylate, as well as various acrylic acid esters and methacrylic acid esters, (meth)acrylic acid, styrene, vinyl acetate, (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and acrylonitrile. These can be used alone or in combination of two or more. When curing by irradiation with ultraviolet light having a wavelength of 365 nm or the like, a photopolymerization initiator or the like is further added.

[0097] [Modification D of the First Embodiment] 6 is a partial cross-sectional view of a black matrix substrate of the present invention, showing a modified example D of the first embodiment. A transmittance adjusting layer 1, a black matrix 6, and a protective layer 4 are laminated on a first substrate 10-1. A first transparent resin layer 21 is provided so as to cover these components, and a light absorptive partition wall 2 is further laminated thereon. Wavelength conversion layers 25, 26, and 27 are disposed in second openings between the light absorptive partition walls 2, forming a black matrix substrate 103 of modified example D. The first transparent resin layer 21 may be omitted.

[0098] The wavelength conversion layers 25, 26, and 27 will be described in detail later in connection with a display device D of a second embodiment.

[0099] [Second embodiment, display device C] FIG. 8 relates to a second embodiment of the present invention and is a partial cross-sectional view of a display device C including a black matrix substrate 103 (FIG. 5) of the modification C of the first embodiment.

[0100] The substrate material applicable to the first substrate 10-1 and the second substrate 10-2 may be a transparent substrate such as a glass substrate, a quartz substrate, a sapphire substrate, or a plastic substrate. It is desirable that the substrate materials constituting the first substrate 10-1 and the second substrate 10-2 have the same thermal expansion coefficient. When different substrate materials are used for the second substrate (array substrate) and the first substrate 10-1, problems such as warping or peeling of the substrate may occur from the viewpoint of the thermal expansion coefficient.

[0101] An array substrate is a substrate on which thin-film transistors that drive display function layers such as light-emitting elements and liquid crystal layers are arranged in a matrix. In this case, one or more thin-film transistors are arranged for each pixel, which is the smallest unit of display. Usually, one thin-film transistor is arranged for each pixel to drive the liquid crystal layer, but for light-emitting elements such as organic electroluminescence, seven thin-film transistors may be arranged for each pixel.

[0102] The optical module 105 shown in Fig. 8 includes a light-emitting element 3, which is an LED, on a second substrate 10-2. Each of the light-emitting elements 3 is driven by a first thin-film transistor 67 and a second thin-film transistor 68 shown in Fig. 7. Note that Fig. 7 is a general circuit diagram in which an array of the first thin-film transistor 67 and the second thin-film transistor 68 is controlled by a video signal circuit 81 and a scanning signal circuit 82, and therefore a detailed description thereof will be omitted.

[0103] The light-reflective partitions 5 are disposed on the second substrate 10-2, and one or more light-emitting elements (blue light-emitting element 3B, green light-emitting element 3G, red light-emitting element 3R in FIG. 8) are disposed in the third openings 20 between the light-reflective partitions 5. The black matrix substrate 103 and the optical module 105 are bonded to each other so as to face each other via the planarizing resin layer 23, which also serves as an adhesive layer.

[0104] In addition, the black matrix 6, the light absorptive partition 2, and the light reflective partition 5 overlap in plan view. Of the fourth opening 41, the second opening 35, and the first opening 19, the width of the first opening 19 is the narrowest.

[0105] 8, the light emitting elements include a blue light emitting element 3B, a green light emitting element 3G, and a red light emitting element 3R, which are disposed in the fourth opening 41. These light emitting elements may be white light emitting elements.

[0106] [Light reflective partition wall] The light-reflective partition 5 is formed by, for example, depositing aluminum or silver, which has a high visible light reflectance, on the surface of a column made of resin. The aluminum or silver may be an alloy containing 0.5 at % or more and 5 at % or less of a different element.

[0107] When silver is used, the adhesion between silver and resin is low, so a three-layer structure in which silver (alloy) is sandwiched between conductive oxides is desirable. The resin pillars can be formed by using an alkali-soluble photosensitive resin and a well-known photolithography method. Alternatively, a thermosetting resin film can be etched by a dry etching method.

[0108] The height of the resin pillar can be set within a range of, for example, 1 μm to 30 μm. The light emitting element formed on the sapphire substrate via a buffer layer or the like becomes tall in the thickness direction. In this way, when the light emitting elements (blue light emitting element 3B, green light emitting element 3G, and red light emitting element 3R in FIG. 8) are tall, the height of the pillar may be greater than 30 μm.

[0109] As the photosensitive resin, similar to the transparent resin for dispersing an organic pigment described above, a resin is used in which a photocrosslinkable group such as a (meth)acryloyl group or a styryl group is introduced into a linear polymer having a reactive substituent such as a hydroxyl group, a carboxyl group or an amino group by reacting the linear polymer with a (meth)acrylic compound having a reactive substituent such as an isocyanate group, an aldehyde group or an epoxy group or cinnamic acid.

[0110] As the monomer and oligomer which are the precursors of the transparent resin, the same materials as those used for the transparent resin in which the organic pigment is dispersed, as described above, can be used.

[0111] [Effect 1 of the light-absorbing partition and transmittance adjusting layer provided in the display device of the present invention] 9 is a partial cross-sectional view of a display device using a black matrix substrate having light absorbing partitions 2 according to the present invention, and is a diagram for explaining one effect obtained by the black matrix substrate of the present invention. The effect can be compared with the explanation of the conventional display device shown in FIG.

[0112] In the display device of the present invention shown in Fig. 9, the emitted light from the light-emitting element 3 is indicated by E0, E1, E2, E3, and E4. Of these emitted light, the emitted light E0 and E4 are cut by the light-absorbing partition 2 and do not affect adjacent pixels. Therefore, the light-reflective partition 5 provided in the display device of the present invention can effectively utilize the emitted light from the light-emitting element.

[0113] [Effects 2 of the light-absorbing partition and transmittance adjusting layer provided in the display device of the present invention] Fig. 10 is a partial cross-sectional view of a display device using a black matrix substrate having a transmittance adjusting layer 1 according to the present invention, and is also a diagram for explaining another effect obtained by the black matrix substrate of the present invention. The effect can be compared with the explanation of the conventional display device shown in Fig. 18, which has already been described. Note that Fig. 10 also shows a display device that does not have (use) a circular polarizer, just like Fig. 18.

[0114] In the display device of the present invention shown in FIG. 10, obliquely incident light In1 from the outside is blocked by the light-absorbing partition 2, and reflected light Re4 does not enter the eye 50 of the observer.

[0115] 10 also explains that incident light In2 from the normal direction (perpendicular to the first substrate 10-1) is attenuated by the transmittance adjustment of the transmittance adjustment layer 1. That is, in FIG. 10, when external light In2 is incident from the normal direction, for example, if the transmittance adjustment layer 1 has a visible light transmittance of 70%, the amount of external light In2 that passes through the pixel opening is reduced by the transmittance adjustment layer 1, and reaches the reflective electrode 31 at 70% of its light amount.

[0116] The light is reflected by the reflective electrode 31, generating reflected light, which again passes through the transmittance adjustment layer 1 to become reflected light Re3. The amount of reflected light Re3 that passes through the transmittance adjustment layer 1 again is 49% of the original amount of light (100%), and the transmittance adjustment layer 1 can suppress the reflected light.

[0117] As described above, the technology according to the present invention is useful for display devices that use light-emitting elements such as LEDs and organic EL as light sources and have a reflective electrode or a light-reflecting film as the underside of the light sources. In other words, the configuration of the transmittance adjusting layer 1, black matrix 6, light-absorbing partition 2, and light-reflective partition 5 according to the present invention shown in Fig. 9 can greatly improve the display quality of a display device that uses light-emitting elements such as LEDs and organic EL as light sources.

[0118] [Second embodiment, display device D] 11 is a partial cross-sectional view of a display device D including a black matrix substrate according to the modification D of the first embodiment of the present invention, which relates to a modification of the second embodiment of the present invention. The black matrix substrate 104 described in the modification D of the first embodiment and an optical module 105 are bonded to each other so as to face each other.

[0119] For the wavelength conversion layers 25, 26, 27, quantum dots or organic fluorescent dyes can be used, but from the viewpoint of conversion efficiency, it is preferable to use phosphors having a diameter in the range of 1 μm to 20 μm, for example.

[0120] When the light-emitting element is, for example, a blue-emitting LED in the range of 380 nm to 500 nm, a blue phosphor can be used for wavelength conversion layer 27, a green phosphor for wavelength conversion layer 26, and a red phosphor for wavelength conversion layer 25. If the emission wavelength of the blue-emitting LED is the desired blue wavelength, wavelength conversion layer 27 can simply be a light scattering layer. When a light-emitting element emitting light in the near-ultraviolet region of 365 nm or 395 nm is used as the blue-emitting LED, it is necessary to use a blue phosphor for wavelength conversion layer 27 in the blue pixel opening.

[0121] The blue phosphor is Sr 2 P 2 O 7 :Sn 4+ , Sr 4 Al 14 O 25 :EU 2+ , BaMgAl 10 O 17 :EU 2+ , SrGa 2 S 4 :Ce 3+ , CaGa 2 S 4 :Ce 3+ , (Ba,Sr)(Mg,Mn)Al 10 O 17 :EU 2+ , (Sr, Ca, Ba 2 , Mg) 10 (PO 4 ) 6 Cl 2 :EU 2+ , BaAl2 SiO 8 :Eu 2+ 、Sr 2 P 2 O 7 :Eu 2+ 、Sr 5 (PO 4 ) 3 Cl:Eu 2+ 、(Sr,Ca,Ba) 5 (PO 4 ) 3 Cl:Eu 2+ 、BaMg 2 Al 16 O 27 :Eu 2+ 、(Ba,Ca) 5 (PO 4 ) 3 Cl:Eu 2+ 、Ba 3 MgSi 2 O 8 :Eu 2+ 、Sr 3 MgSi 2 O 8 :Eu 2+ and the like can be mentioned.

[0122] In addition, as green phosphors, (BaMg)Al 6 O 27 :Eu 2+ ,Mn 2+ 、Sr 4 Al 14 O 25 :Eu 2+ 、(SrBa)Al 12 Si 2 O 8 :Eu 2+ 、(BaMg) 2 SiO 4 :Eu 2+ 、Y 2 SiO 5 :Ce 3+ ,Tb 3+ 、Sr 2 P 2 O 7 -Sr 2 B 2 O 5 :Eu 2+ 、(BaCaMg) 5 (PO4 ) 3 Cl:Eu 2+ , Sr 2 Si 3 O 8 -2SrCl 2 :Eu 2+ , Zr 2 SiO 4 , MgAl 11 O 19 :Ce 3+ , Tb 3+ , Ba 2 SiO 4 :Eu 2+ , Sr 2 SiO 4 :Eu 2+ , (BaSr)SiO 4 :Eu 2+ etc. can be mentioned.

[0123] Also, as red phosphors, Y 2 O 2 S:Eu 3+ , YAlO 3 :Eu 3+ , Ca 2 Y 2 (SiO 4 ) 6 :Eu 3+ , LiY 9 (SiO 4 ) 6 O 2 :Eu 3+ , YVO 4 :Eu 3+ , CaS:Eu 3+ , Gd 2 O 3 :Eu 3+ , Gd 2 O 2 S:Eu 3+ , Y(P,V)O 4 :Eu 3+ , Mg 4 GeO 5 . 5 F:Mn 4+ , Mg 4 GeO 6 :Mn 4+ , K 5 Eu 2.5 (WO 4 ) 6.25, Na 5 EU 2.5 (WO 4 ) 6.25 , K 5 EU 2.5 (MoO 4 ) 6.25 , Na 5 EU 2.5 (MoO 4 ) 6.25 etc.

[0124] [Second embodiment, display device E] Figure 12 relates to a modified example of the second embodiment of the present invention, and is a partial cross-sectional view of a display device E (mini LED) that has a black matrix substrate of modified example C of the first embodiment and uses a liquid crystal layer as a display function layer.

[0125] FIG. 13 is a partial plan view of a general active matrix driving circuit when the display function layer is a liquid crystal layer.

[0126] The liquid crystal layer 9 is driven by a voltage applied between pixel electrodes 7 and a common electrode 8 provided on an array substrate 108 having thin film transistors on a third substrate 10-3. Both the pixel electrodes 7 and the common electrode 8 are formed of a transparent conductive film such as ITO. Each pixel electrode 7 is driven by a third thin film transistor 71 shown in Fig. 13. Note that Fig. 13 is a general circuit diagram in which an array of third thin film transistors 71 is controlled by a scanning signal circuit 72 and a video signal circuit 73, and therefore a detailed description will be omitted.

[0127] The basic configuration of the optical module 107 is almost the same as that of the optical module 105 of the first embodiment. In the optical module 107 of the second embodiment, the light-emitting element 3 is three types of LEDs, namely, a blue light-emitting element, a green light-emitting element, and a red light-emitting element, each of which is disposed in the light-emitting unit 74.

[0128] For example, each of the light-emitting elements 3 arranged in the light-emitting unit 74 may be driven by a first thin film transistor and a second thin film transistor. A plurality of light-emitting elements in a light-emitting unit may be driven by one thin film transistor. The light-emitting element 74 is an area surrounded by the light-reflective partition 5, in which one or more light-emitting elements are arranged.

[0129] The liquid crystal layer 9, which is a display function layer, uses horizontally aligned liquid crystal and is driven by the FFS (fringe field switching) method. Note that in Fig. 12, illustrations of a cover glass, a touch panel, light control elements such as a polarizing plate, an alignment film, etc. are omitted.

[0130] [Third embodiment, manufacturing method of black matrix substrate] 14 is a process diagram showing a method for manufacturing a black matrix substrate according to a third embodiment of the present invention. The black matrix substrate of the present invention includes light absorbing partition walls, but the method for manufacturing a black matrix substrate of the present invention is characterized by a process performed before the light absorbing partition walls are formed.

[0131] In addition, the expression "dispersion" described below refers to a coating liquid in which silica particles, carbon, etc. are dispersed in an acrylic resin together with an organic solvent, a dispersant, etc. "Coating" refers to coating with a normal coating device such as a curtain coater or a spin coater, and "drying" refers to drying on a hot plate at about 80°C, for example. "Curing" refers to thermal curing of the coating film after drying, for example, in the range of 180°C to 250°C. "Exposure" refers to normal exposure using a photomask and a wavelength of 365 nm. In addition, "black layer" refers to a coating film of a black dispersion after drying before forming a pattern of a black matrix. In addition, the "resist" used to form the protective layer refers to the alkali-soluble negative photosensitive resist described in the first embodiment.

[0132] (Manufacturing method of black matrix substrate (A)) FIG. 15 is a partial cross-sectional view of a black matrix substrate manufactured by the manufacturing method (A) of a black matrix substrate according to the third embodiment of the present invention, in which the transmittance adjusting layer remains.

[0133] The black matrix substrate produced by the method (A) for producing a black matrix substrate of the present invention can be produced, for example, by including the following steps (1) to (5). (1) A transmittance adjustment layer was applied onto a transparent substrate, which was the first substrate 10-1, using a dispersion containing carbon and silica particles. The dispersion was prepared as a negative photosensitive resist, and after drying, it was hardened at 365 nm. The thickness of the transmittance adjustment layer after drying was 0.6 μm. The silica particles in the dispersion were 18 mass % and carbon 3 mass % in solid ratio. (2) On the hardened transmittance adjusting layer, a carbon dispersion was applied as a black layer to a thickness of 0.8 μm after drying, and hardened by exposure. The carbon was also 45% in solid ratio. (3) A protective layer was applied using a carbon dispersion (carbon was 3% by mass in solid ratio) prepared as a negative resist, and then dried. The film thickness of the protective layer after drying was 1.5 μm. (4) A photomask with a black matrix pattern was used for exposure, followed by alkaline development to form a protective layer pattern before the next process. This pattern was a 3 μm-3 μm line and space pattern for the effective display area used for display, and included a 0.5 mm wide frame pattern surrounding the four sides of this effective display area. Upon development, the black layer was exposed between the 3 μm-3 μm lines and spaces. (5) Using a dry etching device and CF 4 and C. 3 F 8 The black layer was dry etched by introducing freon gas of 1000 g.

[0134] Dry etching was performed until the transmittance adjusting layer was exposed, and was stopped when the emission spectrum of the Si group originating from the silica fine particles was detected.

[0135] After dry etching, a black matrix can be formed in which the protective layer and the black layer have the same 3 μm line and space and frame pattern.

[0136] By carrying out the above steps (1) to (5), a black matrix substrate 100a in which the transmittance adjusting layer 1 remains on the substrate 10-1 is obtained, as shown in FIG.

[0137] (Manufacturing method of black matrix substrate (B)) Figure 16 is a partial cross-sectional view of a black matrix substrate manufactured by a manufacturing method (B) of a black matrix substrate which is the third embodiment of the present invention, in which the transmittance adjustment layer 1 of the first opening 19 has been removed and the surface of the first substrate 10-1 is exposed.

[0138] The manufacturing method (B) of a black matrix substrate is the same as the manufacturing method (A) of a black matrix substrate in steps (1), (2), and (4), except for the thickness of the protective layer in step (3) and the depth of the dry etching in step (5).

[0139] Since the emission spectrum intensity of the Si group associated with the silica microparticles contained in the transmittance adjusting layer 1 differs significantly from the emission spectrum intensity of the Si group from the first substrate when it is a glass substrate, the depth of dry etching can be determined from the intensity difference between these emission spectra, and dry etching can be stopped at the surface of the first substrate.

[0140] In addition, in flexible displays such as organic electroluminescence displays, the first substrate may be made of resin. A thin film of silicon dioxide or silicon nitride is formed on the resin substrate of such flexible displays to prevent moisture and oxygen from passing through. Therefore, even when the first substrate is made of resin, the etching depth can be set by the difference in emission spectrum intensity of the Si group in the etching depth direction.

[0141] The method for manufacturing a black matrix substrate disclosed in the third embodiment has the following new effects.

[0142] When forming a highly light-shielding black matrix using photolithography alone, it is extremely difficult to reproduce pixels with a pitch of 10 μm or less, for example, with a line width of 4 μm or even 3 μm or less. It is difficult to stably reproduce a fine line pattern with a line width of 4 μm or less for high-definition pixels using photolithography alone due to shape variations and pixel peeling. In particular, there is a problem with the corners of the pixel opening becoming rounded. For example, in a stripe pattern with an 8 μm pitch and a 4 μm line width, two photomasks are used: a photomask for the stripe pattern and a photomask for the frame pattern surrounding the four sides of the matrix-shaped pixels in the effective display area, and the photolithography process is also divided into these two patterns.

[0143] The dry etching method allows for the integral formation of a 3 μm-3 μm line and space pattern and a frame portion with a single photomask. Furthermore, the dry etching method disclosed in the third embodiment is extremely effective for reproducing a matrix pattern (not a stripe pattern, but a black matrix formed in a vertical and horizontal grid) that is effective for stray light countermeasures with high-resolution pixels of, for example, 500 ppi or more.

[0144] In addition, in a stripe pattern, external light reflected from the direction of the stripes often enters the eye through the reflective electrode, reducing visibility. To improve contrast in high-definition pixels, a black matrix pattern in a vertical and horizontal grid is preferable, rather than a stripe pattern.

[0145] The above-described embodiments may be freely combined and used. It is preferable that an antenna is further mounted on an electronic device equipped with a display device according to an embodiment of the present invention to perform communication and contactless power supply and reception.

[0146] Although preferred embodiments of the present invention have been described and illustrated above, it should be understood that these are illustrative of the present invention and should not be considered as limiting. Additions, omissions, substitutions, and other modifications can be made without departing from the scope of the present invention. Thus, the present invention should not be considered as limited by the foregoing description, but is defined by the claims. [Industrial Applicability]

[0147] A display device including the black matrix substrate of the present invention can be used in various applications. Examples of electronic devices to which the display device according to the above-described embodiment can be applied include electronic devices such as mobile phones, portable game devices, portable information terminals, personal computers, electronic books, video cameras, digital still cameras, head-mounted displays, navigation systems, audio playback devices (car audio, digital audio players, etc.), copiers, facsimiles, printers, multifunction printers, vending machines, automated teller machines (ATMs), personal authentication devices, optical communication devices, and IC cards. [Explanation of symbols]

[0148] 1... Transmittance adjustment layer 2. Light-absorbing partition 3. Light-emitting (diode) element 3B: Blue light emitting element 3G: Green light emitting element 3R: Red light emitting element 4... Protective layer 5... Light reflective partition wall 6. Black matrix 7 Pixel electrode (ITO) 8 ··· Common electrode (ITO) 9. Liquid crystal layer 10-1: First board 10-2: Second board 10-3 Third board 19 First opening 20 Third opening 21 ... 1st transparent resin layer 23 ... Flattened resin layer 25 Red wavelength conversion layer 26 Green wavelength conversion layer 27 Blue wavelength conversion layer 28 ... light scattering layer 31...Reflecting electrode 35 Second opening 40 Observer direction 41 Fourth opening 50, 52... Observer (eye) 51...Reflecting electrode 53 Light emitting element 56 Black Matrix 63 Liquid crystal layer 64, 84... Scanning signal lines (gate lines) 65, 83: Video signal line (source line) 67 First thin film transistor 68 Second thin film transistor 71 Third thin film transistor 72 Scanning signal control circuit 73 Video signal control circuit 74 Light Emitting Unit 81 Video signal control circuit 82 Scanning signal control circuit 85... Power line 86 Grand 87 Capacitive element 100, 101, 102, 103, 104... Black matrix substrate 100a: Black matrix substrate manufactured by manufacturing method (A) 100b: Black matrix substrate manufactured by manufacturing method (B) 105 Optical module (array substrate having light-emitting elements arranged thereon) 106: Optical module (array substrate having light-emitting elements arranged thereon) 107: Optical module (backlight unit having light-emitting elements) 108 Array substrate (having thin film transistors for driving the liquid crystal layer) 110...Display device C 120...Display device D 130...Display device E E0, E1, E2, E3, E4, E20, E21, E22, E23, E24...Outgoing light In1, In11...Diagonal incident light In2, In21: External incident light (incident light from the normal direction) Re3, Re4, Re12, Re22... Reflected light R Red filter G: Green filter B: Blue filter H1: Height of light-absorbing partition H2: Thickness of the first transparent resin layer H3: Effective height of light-absorbing partition C1: Central axis of the first opening 19 C2: central axis of the second opening 35 W1: Black matrix line width W2: Line width of light-absorbing partition PX: Configuration of one pixel's TFT unit

Claims

1. a transparent substrate, a transmittance adjusting layer, and a black matrix having a plurality of first openings are laminated in this order; laminating, in this order, a protective layer and a light-absorbing partition wall having a plurality of second openings whose central axes are substantially aligned with the first openings on the black matrix; the line width of the black matrix is ​​wider than the line width of the light absorbing partition wall, and in a plan view, the light absorbing partition is covered with the black matrix, The transmittance adjusting layer is a resin dispersion containing carbon and silica fine particles.

1. A black matrix substrate comprising:

2. the protective layer includes a plurality of third openings having the same shape as the first openings of the black matrix, the first openings and the third openings overlap at the same position in a plan view; 2. The black matrix substrate according to claim 1,

3. The protective layer has a visible light transmittance in a thickness direction of 95% or more and 99.5% or less in a wavelength range of 400 nm to 700 nm.

3. The black matrix substrate according to claim 1, wherein the first and second electrodes are arranged in a first direction.

4. a first transparent resin layer is inserted between the black matrix and the light absorbing partition wall; 4. The black matrix substrate according to claim 1, wherein the first insulating layer is a black matrix substrate.

5. The second opening is provided with a wavelength conversion layer for light.

5. The black matrix substrate according to claim 1, wherein the first insulating layer is a black matrix substrate.

6. The second opening is provided with a light scattering layer.

5. The black matrix substrate according to claim 1, wherein the first insulating layer is a black matrix substrate.

7. The transmittance of the transmittance adjusting layer in the thickness direction of the visible light is 70% or more and 99.5% or less in the wavelength range of 400 nm to 700 nm.

7. The black matrix substrate according to claim 1, wherein the first insulating layer is a black matrix substrate.

8. At least one of a red filter, a green filter, and a blue filter is disposed in the first openings.

8. The black matrix substrate according to claim 1, wherein the first insulating layer is a black matrix substrate.

9. The black matrix substrate according to any one of claims 1 to 8 is provided. A display device comprising:

10. A method for manufacturing a black matrix substrate according to claim 2, comprising the steps of: A step of applying and hardening a transmittance adjusting layer containing carbon and silica fine particles on a transparent substrate; A step of applying and hardening a black layer on the transmittance adjusting layer; applying an alkali-developable photosensitive protective layer onto the black layer and drying the same; exposing the protective layer to light using a photomask having a plurality of openings and developing the protective layer to form the plurality of third openings; and transferring the pattern of the plurality of third openings to a black layer by dry etching to form a black matrix while leaving a portion of the protective layer in a thickness direction thereof.

2. A method for manufacturing a black matrix substrate comprising the steps of:

Citation Information

Patent Citations

  • Image display device

    JP2006093053A

  • Manufacturing method of color conversion filter

    JP2009230889A

  • Face panel for color image display, panel for color image display using the face panel, and color image display equipped with the panel

    JP2010055947A

  • Color filter forming substrate and organic el display device

    JP2014142610A

  • Method for manufacturing laminate, method for manufacturing color filter, laminate, and color filter