Joining member and manufacturing method thereof
The described method enhances joint strength and airtightness by laser welding metal members with a sheet-like brazing filler, addressing issues of thermal conductivity and defects in existing methods.
Patent Information
- Application Number
- JP2020195450
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-25
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Existing methods for joining metal members, such as brazing and laser welding, face issues with decreased joint strength, productivity, and poor airtightness and watertightness, particularly when working with materials like aluminum, which experience thermal conductivity and defects like solidification cracks.
A joining member and method that involves laser welding a first metal member with a second metal member using a sheet-like brazing filler metal, forming a base metal fusion zone that penetrates through both members and a brazing material fusion zone that seals the joint, enhancing strength and airtightness.
The method produces a joining member with improved joining strength, airtightness, and watertightness by integrating the metal members through a base metal and brazing material fusion zones, preventing solidification cracks and moisture ingress.
Smart Images

Figure 0007552290000016 
Figure 0007552290000034 
Figure 0007552290000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a joining member and a manufacturing method thereof. [Background technology]
[0002] In various fields, including transportation equipment such as automobiles, railways, and aircraft, as well as medical equipment, electronic components, chemical plants, and the like, it is common to manufacture large structural components by joining multiple metal members. Known methods for joining metal members include welding, pressure welding, brazing, and mechanical joining.
[0003] Of these, brazing is a technique in which a brazing filler metal, an alloy with a lower melting point than the parts to be joined (base material), is melted and used as an adhesive to join the parts to be joined without melting the parts themselves. Techniques such as furnace brazing and torch brazing are used to melt the brazing filler metal. Furnace brazing is a technique in which the parts are placed in a furnace and heated as a whole, while torch brazing is a technique in which the parts are locally heated and brazed using a gas torch.
[0004] In recent years, laser brazing, which uses laser light to perform brazing, has been proposed as a brazing method. In laser brazing, a laser light is irradiated and heated at the joining portion of the members to be joined, thereby melting the brazing material and joining the members together. For example, Patent Document 1 discloses a method for manufacturing a metal joining member, which includes a brazing process in which a plurality of metal members are brazed by laser brazing using flux and brazing material, a high-frequency laser pulse irradiation process in which flux remaining on the surface of the brazed portion is removed, and a chemical conversion treatment process in which a chemical conversion treatment is performed including the brazed portion (claim 1 of Patent Document 1).
[0005] As a welding method, laser welding that uses laser light is known. Laser welding is a method of melting and joining members by irradiating a high-energy laser light to the joining portion of the members to be joined, and differs from brazing in that the members to be joined themselves are melted. Laser welding has features such as high speed welding and little thermal deformation, and is used, for example, when manufacturing automobile parts and battery cases by joining aluminum alloy members.
[0006] Patent Document 2 describes a method for joining dissimilar materials, that is, laser welding without using brazing material, between an aluminum-based workpiece and an iron-based workpiece having a zinc-based coating layer on the surface (claims 1 and
[0013] of Patent Document 2). Patent Document 3 describes laser welding by irradiating a pulsed laser on an aluminum alloy plate for a battery case, which contains Fe, Mn, Ti, and Zr (claims 1,
[0009] , and
[0040] of Patent Document 3). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2013-176785 A [Patent Document 2] JP 2008-023562 A [Patent Document 3] Patent No. 5725344 Summary of the Invention [Problem to be solved by the invention]
[0008] Thus, although methods such as brazing and laser welding have been used to join metal components, there have been problems. In brazing methods, for example furnace brazing and torch brazing, when brazing components made of a material with high thermal conductivity such as aluminum, the components are heated to high temperatures over a wide area. This reduces the strength of the joint and reduces productivity. In addition, laser brazing requires the accurate feeding of a wire-shaped brazing material to a narrow melting area, and the brazing material reduces the temperature of the molten pool, slowing down the brazing speed. This has led to many problems in terms of production technology.
[0009] Furthermore, the laser welding method has the problem of defects occurring in the welded part (joint), degrading the joining characteristics. That is, depending on the material of the parts being joined, laser welding can cause defects such as solidification cracking and porosity in the welded part. Solidification cracking is a crack that occurs along the grain boundary, and when it occurs, the mechanical characteristics of the joint are significantly reduced. In addition, air and moisture can penetrate into the inside along the cracks, which can significantly deteriorate the airtightness and watertightness.
[0010] The present inventors have conducted extensive research in light of the above-mentioned problems, and have found that when joining metal members, by disposing a sheet-shaped brazing filler metal between plate materials and then performing laser welding so as to obtain a predetermined structure, a joined member having excellent joining strength as well as excellent airtightness and watertightness can be obtained.
[0011] The present invention has been completed based on such findings, and an object of the present invention is to provide a joint member having high joint strength and excellent airtightness and watertightness, and a method for manufacturing the same. [Means for solving the problem]
[0012] The present invention includes the following aspects (1) to (8). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."
[0013] (1) A joining member including: a first metal member having a first main surface and a second main surface; and a second metal member disposed on the second main surface side of the first metal member and joined to at least a portion of the first metal member via a laser weld, the joining member includes a sheet-shaped brazing material on a second main surface side of the first metal member, The laser welded portion includes a base material fusion portion formed of a molten and integrated product of the first metal member, the second metal member, and the sheet-shaped brazing material, and a brazing material fusion portion formed of a molten product of the sheet-shaped brazing material, the base material fusion portion is formed so as to penetrate from the first main surface to the second main surface of the first metal member and to be continuous to at least a part of the thickness of the second metal member; A joining member, wherein the brazing material molten portion is in close contact with the first metal member, the second metal member, and the base material molten portion.
[0014] (2) The joined member according to (1) above, wherein the first metal member and the second metal member are joined by forming a lap joint.
[0015] (3) The joined member according to (1) above, wherein the first metal member and the second metal member are joined to form a T-joint.
[0016] (4) The joining member according to any one of the above (1) to (3), wherein the first metal member and the second metal member are made of the same material.
[0017] (5) The joining member according to any one of the above (1) to (3), wherein the first metal member and the second metal member are made of different materials.
[0018] (6) The joining member according to any one of the above (1) to (5), wherein one or both of the first metal member and the second metal member are made of an aluminum-based metal.
[0019] (7) A method for producing a joint member according to any one of (1) to (6) above, comprising the following steps: A step of preparing a first metal member having a first main surface and a second main surface, a second metal member, and a sheet-shaped brazing material; A step of preparing a laminate in which the sheet-shaped brazing material and the second metal member are arranged in this order on a second main surface side of the first metal member prepared; and a step of irradiating a first main surface of a first metal member constituting the laminate with a laser beam to laser-weld the second metal member to at least a part of the first metal member via a joining interface; a method in which, in the laser welding process, the first metal member, the second metal member, and a portion of the sheet-shaped brazing material are melted and integrated to form a base material molten portion that penetrates the joint interface of the laser weld, and the sheet-shaped brazing material around the joint interface is melted to form a brazing material molten portion.
[0020] (8) The method according to (7) above, wherein the first metal member and the sheet-shaped brazing material are prepared by roll-bonding a first metal member and a sheet-shaped brazing material. Effect of the Invention
[0021] According to the present invention, there are provided a joint member having excellent joint strength as well as excellent airtightness and watertightness, and a method for manufacturing the same. [Brief description of the drawings]
[0022] [Figure 1] FIG. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of a joining member that forms a lap joint. [Diagram 3] FIG. 2 is a cross-sectional view showing an example of a joining member that forms a T-joint. [Figure 4] 1 is a diagram for explaining a laser welding process. [Diagram 5] FIG. 4 is a schematic cross-sectional view showing an example of a joining member that forms a cross joint. [Figure 6] FIG. 11 is a schematic cross-sectional view showing another example of a joining member that forms a cross joint. [Figure 7] FIG. 11 is a schematic cross-sectional view showing another example of a joining member that forms a cross joint. [Figure 8]FIG. 2 is a schematic cross-sectional view showing an example of a joining member that forms a corner joint. [Figure 9] FIG. 2 is a cross-sectional schematic diagram showing an example of a joining member that forms a scarf joint. [Figure 10] FIG. 2 is a schematic cross-sectional view showing an example of a joining member that forms an edge joint. [Figure 11] FIG. 2 is a schematic cross-sectional view showing an example of a joining member that forms a joint. [Figure 12] FIG. 11 is a schematic cross-sectional view showing another example of a joining member that forms a butt joint. [Figure 13] FIG. 11 is a schematic cross-sectional view showing another example of a joining member that forms a butt joint. [Figure 14] FIG. 11 is a schematic cross-sectional view showing yet another example of a joining member that forms a butt joint. [Figure 15] FIG. 2 is a schematic cross-sectional view showing an example of a joining member that forms a flare joint. [Figure 16] FIG. 4 is a schematic cross-sectional view showing another example of a joining member that forms a flare joint. [Figure 17] FIG. 4 is a schematic cross-sectional view showing an example of a joining member that forms a back plate joint. [Figure 18] FIG. 11 is a schematic cross-sectional view showing another example of a joining member that forms a back plate joint. [Figure 19] FIG. 2 is a schematic cross-sectional view showing an example of a joining member that forms a lap fillet joint. [Figure 20] 1 is a diagram showing a layer structure of a laminate in Example 1. [Figure 21] 1 is a diagram showing an embodiment of laser welding in Example 1. [Figure 22] 1 is a diagram showing a layer structure of a laminate in Example 2. [Diagram 23] 1 is a diagram showing an embodiment of laser welding in Example 2. [Figure 24] 1 is a diagram showing a layer structure of a laminate in Example 3. [Diagram 25] 1 is a diagram showing an embodiment of laser welding in Example 3. [Figure 26] 1 is a drawing showing a layer structure of a laminate in Example 4. [Figure 27] 1 is a diagram showing an embodiment of laser welding in Example 4. [Figure 28] 1 is an optical microscope image of a cross section of a bonded member in Example 1. [Figure 29] 1 is an optical microscope image of a cross section of a bonded member in Example 1. [Diagram 30] 1 is an optical microscope image of a cross section of a bonded member in Example 2. [Diagram 31] 1 is an optical microscope image of a cross section of a bonded member in Example 2. [Diagram 32] 1 is an optical microscope image of a cross section of a bonded member in Example 3. [Diagram 33] 1 is an optical microscope image of a cross section of a bonded member in Example 3. [Diagram 34] 1 is an optical microscope image of a cross section of a bonded member in Example 4. [Diagram 35] 1 is an optical microscope image of a cross section of a bonded member in Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.
[0024] 1. Joining materials The joining member of this embodiment includes a first metal member having a first main surface and a second main surface, and a second metal member disposed on the second main surface side of the first metal member and joined to at least a part of the first metal member via a laser welded portion. The joining member also includes a sheet-shaped brazing material on the second main surface side of the first metal member. The laser welded portion includes a base material fusion portion constituted by a fused and integrated product of the first metal member, the second metal member, and the sheet-shaped brazing material, and a brazing material fusion portion constituted by a melted product of the sheet-shaped brazing material. The base material fusion portion penetrates from the first main surface to the second main surface of the first metal member and is formed continuously to at least a part of the thickness of the second metal member. The brazing material fusion portion is in close contact with the first metal member, the second metal member, and the base material fusion portion.
[0025] <Metal parts> The joining member of this embodiment includes a first metal member having a first main surface and a second main surface, and a second metal member disposed on the second main surface side of the first metal member and joined to at least a part of the first metal member via a laser welded portion. That is, the first metal member and the second metal member are joined via a laser welded portion. The shapes of the first metal member and the second metal member are not limited as long as they can constitute the joining member. They may be any of a plate material, an extruded material, and a bar material, or may have another shape.
[0026] The materials of the first metal member and the second metal member are not limited as long as they can be laser welded. For example, aluminum (Al), iron (Fe), copper (Cu), titanium (Ti), nickel (Ni), or alloys containing these metals are exemplified. The combination of the materials of the first metal member and the second metal member is also not limited. The first metal member and the second metal member may be made of the same material or different materials.
[0027] Preferably, one or both of the first metal member and the second metal member are made of an aluminum-based metal. The aluminum-based metal refers to pure aluminum or an aluminum alloy. Examples of pure aluminum include 1000-series alloys. Examples of aluminum alloys include 2000-series (Al-Cu-series) alloys, 3000-series (Al-Mn-series) alloys, 4000-series (Al-Si-series) alloys, 5000-series (Al-Mg-series) alloys, 6000-series (Al-Mg-Si-series) alloys, and 7000-series (Al-Zn-Mg-series) alloys. Particularly preferably, the first metal member is made of a 1000-series or 3000-series alloy.
[0028] <Brazing material> The joining member of this embodiment includes a sheet-shaped brazing material on the second main surface side of the first metal member. That is, the sheet-shaped brazing material is disposed on the second main surface side of the first metal member, in a gap with the second metal member or around the second metal member. The sheet-shaped brazing material is a component that assists in joining the first metal member and the second metal member during laser welding, and has a melting point lower than the melting points of the first metal member and the second metal member. This brazing material forms a base metal molten part together with the first metal member and the second metal member, and spreads around the joining interface to form a brazing material molten part.
[0029] The form of the brazing material is not limited as long as it is in a sheet form. For example, it may be a clad material bonded to the second main surface of the first metal member. It may also be a clad material bonded to the main surface of the second metal member. The clad material is a member obtained by clad rolling (pressing) a core material and a brazing material in a hot rolling process, and is also called a brazing sheet. Here, the first metal member and / or the second metal member correspond to the core material. The clad material may be a single-sided clad with the brazing material on one side of the core material, or a double-sided clad with the brazing material on both sides. However, the brazing material is not limited to the clad material. For example, it may be a coating formed on at least one main surface of the first metal member and / or the second metal member. The coating brazing material (16) may be formed by a known thick-film or thin-film forming method such as plating, sputtering, vapor deposition, or chemical vapor deposition. Furthermore, the brazing material may be a free-standing sheet, such as a foil, separate from the metal member.
[0030] The thickness of the brazing material is not limited. However, if the brazing material is too thin, the amount of brazing material required for laser welding will be small, which may cause poor joining. The thickness of the brazing material is preferably 5 μm or more.
[0031] The material of the brazing material depends on the materials of the first metal member and the second metal member, and therefore cannot be determined in general. When at least one of the first metal member and the second metal member is made of an aluminum-based metal, 4000 series (Al-Si) alloys, Al-Cu-Si, Al-Zn alloys, etc. are listed, among which 4000 series alloys are preferable. 4000 series alloys have high fluidity. An alloy with high fluidity spreads thinly in the gap between the first metal member and the second metal member during laser welding to form a brazing material molten part. Therefore, it is excellent in the effect of improving airtightness and watertightness, and can also be expected to have a stress relaxation effect on the joint.
[0032] <Laser welded part> The laser weld corresponds to a portion where at least a part of the first metal member and at least a part of the second metal member are joined. The laser weld is composed of a base metal fusion zone and a brazing filler metal fusion zone. Here, the base metal fusion zone and the brazing filler metal fusion zone are also called a weld bead and a fillet, respectively.
[0033] <Melted part of base material> The molten base material is composed of a molten and integrated product of the first metal member, the second metal member, and the sheet-shaped brazing material. That is, during laser welding, heat is generated on the first main surface of the first metal member irradiated with the laser light, and this heat is transferred to the brazing material and the second metal member. In the vicinity of the area irradiated with the laser light, the first metal member, the brazing material, and the second metal member reach a high temperature, and as a result, they melt to form a molten metal. Inside the molten metal, components diffuse and mix due to thermal convection. As the irradiated area of the laser light moves, the molten metal cools and solidifies to form the molten base material. Therefore, the molten base material is a solidified product containing components derived from the first metal member, the second metal member, and the brazing material. Each component in the molten base material may be distributed uniformly or unevenly. For example, the molten base material may contain a large amount of components derived from the first metal member depending on the location, and may also contain a large amount of components derived from the second metal member. Furthermore, the molten base material may contain a large amount of components derived from the brazing material at the joint.
[0034] The base material fusion zone penetrates from the first main surface to the second main surface of the first metal member, and is formed continuously to at least a part of the thickness of the second metal member. That is, the base material fusion zone exists over the entire thickness direction of the first metal member in the region near the laser welded portion, and further exists over a part or the entire thickness direction of the second metal member. It can also be said that the base material fusion zone is formed so as to straddle the first metal member and the second metal member and penetrate the interface between them. In this way, by forming the laser joint with the base material fusion zone as a fused and integrated product, and further forming it so as to penetrate the interface between the first metal member and the second metal member, it is possible to improve the strength of the joint. In this respect, it can be said that the base material fusion zone functions as the main joint.
[0035] The shape of the base material fusion zone is not particularly limited. Typically, the cross-sectional area decreases from the upper surface (first main surface) of the first metal member toward the lower surface of the second metal member. Examples of such shapes include a rotating body (cone) formed by rotating a triangle around a central axis, a rotating body (frustum of a cone) formed by rotating a trapezoid around a central axis, and a rotating body (parabolic rotating body) formed by rotating a parabola. In any case, there is no limitation as long as the shape is formed by laser welding.
[0036] <Brazing material melting part> The brazing material molten zone is composed of melted sheet-shaped brazing material. During laser welding, the first metal member and the second metal member around the molten metal that becomes the base metal molten zone do not reach a high enough temperature to melt. On the other hand, the brazing material melts because of its low melting point. The molten brazing material cools and solidifies to become the brazing material molten zone. Therefore, the brazing material molten zone is a solidification that mainly contains components derived from the brazing material. Even if it contains components derived from the first metal member or the second metal member, the amount is small. It is possible to distinguish the brazing material molten zone from the base metal molten zone by examining the composition and structure.
[0037] The brazing material molten portion is in close contact with the first metal member, the second metal member, and the base material molten portion. During laser welding, the brazing material is melted by heat transfer from the first metal member, the second metal member, and the base material molten portion to form the brazing material molten portion. At this time, the brazing material molten portion is formed so as to be in close contact with the first metal member, the second metal member, and the base material molten portion.
[0038] By providing the brazing material fusion zone, the joining strength of the joining member can be further improved. That is, the brazing material fusion zone is tightly joined to the first metal member and the second metal member around the base material fusion zone. The width of the joining portion is substantially increased, and the joining strength is increased. In this respect, the brazing material fusion zone can be said to function as an auxiliary joining portion.
[0039] Moreover, by providing a brazing material melting portion, it is possible to improve the airtightness and watertightness of the joint. This point will be explained with reference to Figs. 1(a) and 1(b). Fig. 1(a) is a cross-sectional view of a joint member without a brazing material and a brazing material melting portion, and Fig. 1(b) is a cross-sectional view of a joint member with a brazing material and a brazing material melting portion. In the case where there is no brazing material melting portion (Fig. 1(a)), the first metal member (12) and the second metal member (14) are joined only through the base material melting portion (22). In this case, air and moisture penetrate through the gap between the metal members (12, 14). As described above, solidification cracks (26) may occur in the base material melting portion (22) which is the laser welded portion. The solidification cracks (26) are a type of crack. When the solidification cracks (26) occur in the base material melting portion (22), air and moisture penetrate through the solidification cracks (26) into the upper part of the metal member (12). Therefore, it is not possible to ensure airtightness and watertightness of the joint. In contrast, when a brazing material fusion zone is provided (FIG. 1(b)), the periphery of the base metal fusion zone (22) is sealed with the brazing material (16) and the molten brazing material fusion zone (24). Therefore, even if a solidification crack (26) occurs, airtightness and watertightness are reliably ensured.
[0040] <Joining type> The type of joining between the first metal member and the second metal member is not limited as long as the two are joined via a laser joint. Any of the known types of joints may be used, including lap joints, T-joints, cross joints, corner joints, scarf joints, edge joints, edge joints, flare joints, backing plate joints, and lap fillet joints.
[0041] 2(a) and (b) show schematic cross-sectional views of a joining member having a lap joint. FIG. 2(a) is an overall view of the joining member, and FIG. 2(b) is an enlarged view showing the vicinity of the joint. In this joining member (10), a first metal member (12) and a second metal member (14) form a lap joint. That is, a part of the second main surface of the first metal member (12) and a part of the main surface of the second metal member (14) are laser-joined via a joint (20). In addition, a sheet-shaped brazing material (16) is disposed on the second main surface of the first metal member (12), i.e., between the first metal member (12) and the second metal member (14). Furthermore, a base metal fusion portion (22) and a brazing material fusion portion (24) present around the base metal fusion portion (22) are formed in the joint (20).
[0042] 3(a) and (b) show schematic cross-sectional views of a joining member having a T-joint. FIG. 3(a) is an overall view of the joining member, and FIG. 3(b) is an enlarged view showing the vicinity of the joining portion. In this joining member (10), a first metal member (12) and a second metal member (14) are joined to form a T-joint. That is, a part of the second main surface of the first metal member (12) and an end face of the second metal member (14) are laser-joined via a joining portion (20). In addition, a sheet-shaped brazing material (16) is disposed on the second main surface of the first metal member. Furthermore, a base material fusion portion (22) and a brazing material fusion portion (24) existing around the base material fusion portion (22) are formed in the joining portion (20).
[0043] 2. Manufacturing method of joining components The manufacturing method of the joining member of the present embodiment includes the following steps: a step of preparing a first metal member having a first main surface and a second main surface, a second metal member, and a sheet-shaped brazing material (preparation step), a step of preparing a laminate in which the sheet-shaped brazing material and the second metal member are arranged in this order on the second main surface side of the prepared first metal member (lamination step), and a step of irradiating a laser beam to the first main surface of the first metal member constituting the laminate to laser-weld the second metal member to at least a part of the first metal member through the joining interface (laser welding step). In the laser welding step, the first metal member, the second metal member, and a part of the sheet-shaped brazing material are melted and integrated to form a base material molten part that penetrates the joining interface of the laser welded part, and the sheet-shaped brazing material around the joining interface is melted to form a brazing material molten part. Details of each step are described below.
[0044] <Preparation process> In the preparation step, a first metal member having a first main surface and a second main surface, a second metal member, and a sheet-shaped brazing material are prepared. The first metal member, the second metal member, and the sheet-shaped brazing material are as described above. For example, the first metal member and the sheet-shaped brazing material may be a clad material formed by rolling and bonding them together, in which case, the first metal member and the sheet-shaped brazing material may be prepared as an integrated body. The second metal member and the sheet-shaped brazing material may be a clad material formed by rolling and bonding them together, in which case, the second metal member and the sheet-shaped brazing material may be prepared as an integrated body. Furthermore, a foil-shaped brazing material may be used as a self-supporting sheet, in which case, the first metal member, the second metal member, and the sheet-shaped brazing material may be prepared separately.
[0045] <Lamination process> In the lamination step, a laminate is prepared in which a sheet-shaped brazing material and a second metal member are arranged in this order on the second main surface side of the prepared first metal member. In this case, preferably, a flux is arranged between the first metal member and the second metal member together with the sheet-shaped brazing material. The flux is a component that promotes the joining of the metal member and the brazing material. A natural oxide film may be formed on the surface of the metal member. Such an oxide film may hinder the metal contact between the metal member and the brazing material, causing a joining failure. If a flux with a melting point lower than that of the brazing material is used, the flux wets the surface of the metal member during welding and destroys the surface oxide film. Therefore, the joining failure can be suppressed.
[0046] The flux is not limited as long as it has a melting point lower than that of the brazing material and can destroy the surface oxide film of the metal member. Examples of such flux include noncorrosive fluoride-based flux and corrosive chloride flux, and noncorrosive flux is preferable. Noncorrosive flux does not corrode the metal member or brazing material. In addition, it is not necessary to wash the joining members after welding to remove the flux, which leads to a reduction in manufacturing costs. An example of noncorrosive flux is NOCOLOK (registered trademark).
[0047] The procedure for producing the laminate is not particularly limited. When using a clad material formed by rolling-bonding a first metal member and a sheet-shaped brazing material, a flux may be applied to the brazing material surface of the clad material, and a second metal member may be placed thereon. When using a clad material formed by rolling-bonding a second metal member and a sheet-shaped brazing material, a flux may be applied to the brazing material surface of the clad material, and a first metal member may be placed thereon. When using a foil-shaped brazing material as a self-supporting sheet, a flux may be applied to the brazing material surface, and then the first metal member, the brazing material, and the second metal member may be placed in this order. Alternatively, flux may be applied to the main surfaces of the first metal member and the second metal member, and the foil-shaped brazing material may be placed between the applied flux. Furthermore, a method may be considered in which a coating brazing material is formed on the surface of the first metal member using a known thin film formation method, and a flux is applied to the surface of the coating brazing material, and then the second metal member is placed.
[0048] <Laser welding process> In the laser welding step, a laser beam is irradiated onto a first main surface of a first metal member constituting the laminate, and a second metal member is laser-welded to at least a portion of the first metal member via a joint interface. In this process, the first metal component, the second metal component, and a portion of the sheet-shaped brazing material are melted and integrated to form a base material molten zone that penetrates the joint interface of the laser weld, and the sheet-shaped brazing material around the joint interface is melted to form a brazing material molten zone.
[0049] The laser welding process will be described with reference to Fig. 4. In this process, a laser beam (28) is irradiated onto a first main surface (upper surface in the figure) of a first metal member (12) constituting the laminate, and the second metal member (14) is laser-welded to at least a portion of the first metal member (12). The laser beam (28) moves in the direction indicated by the arrow in the figure. In this process, the first metal member (12), the second metal member (14), and a portion of the sheet-shaped brazing material (16) are melted and integrated to form a base material melted portion (22), and the surrounding sheet-shaped brazing material (16) is melted to form a brazing material melted portion (24).
[0050] When a laser beam is irradiated onto the main surface of a metal component, part of the laser energy is absorbed by the plate material, and the surface is rapidly heated. The generated heat is transferred into the plate material by conduction. The plate material surface instantly melts and vaporizes, forming a molten pool, and the components with high vapor pressure become evaporated material and are ejected, forming a depression on the surface of the molten pool. The laser beam irradiated onto the depression is absorbed by the molten pool, and the melting, vaporization, and ejection of evaporated material are repeated, forming a deep hole (keyhole) in the center of the molten pool. The keyhole moves as the laser beam moves. The molten pool is also rapidly cooled and solidified. The cooled and solidified molten pool is called the weld or weld bead. The depth of the molten part is called the penetration depth.
[0051] By adjusting the conditions of the laser irradiation, the penetration depth can be made greater than the thickness of the first metal member. In this case, the molten pool penetrates the first metal member and the brazing material and reaches the inside of the second metal member. That is, the first metal member, the second metal member, and a part of the brazing material are melted, and as a result, the first metal member and the second metal member can be lap-welded through the entire surface. The molten metal in the molten pool convects, and the components of the metal member and the brazing material that make up the molten metal mix together due to this convection. When the molten pool cools and solidifies, a molten base material part containing the components of the metal member and the brazing material is formed. The molten base material part is formed across the first metal member and the second metal member, so a joint is formed at the interface between the two. The interface where this joint is formed is the joint interface.
[0052] During laser welding, the metal components around the molten pool are affected by heat but do not melt. However, the brazing filler metal, which has a low melting point, does melt. In other words, the molten part formed by laser welding acts as a heat bridge, and heat is transferred to the brazing filler metal and flux, causing them to melt and spread, resulting in brazing. When creating a lap joint, the brazing filler metal spreads to fill the gap between the first and second metal components. The brazing filler metal that has spread is cooled to form a brazing filler metal molten part.
[0053] The molten base metal zone and the molten brazing filler metal zone can be examined by observing the structure and analyzing the composition of the cross section of the joining members. For example, the molten base metal zone has a different composition from the first metal member, the second metal member, and the brazing filler metal. Also, because it is rapidly cooled, its structure is different from other parts. Therefore, by examining the structure and composition, the areas of the molten base metal zone and the molten brazing filler metal zone can be determined.
[0054] The conditions of the laser welding are not particularly limited as long as the joining member of this embodiment can be manufactured. As the laser source, a known laser such as a CO2 laser, a YAG laser, a semiconductor laser, an LD-pumped solid-state laser, or a fiber laser can be used. The laser oscillation may be continuous oscillation or pulse oscillation. Furthermore, the conditions such as the laser output, the focal length, and the welding speed are not particularly limited as long as the joining member of this embodiment can be obtained.
[0055] The optimum conditions for laser welding cannot be determined in general because they depend on the material and thickness of the metal members and brazing material. For example, the welding speed may be set to 0.5 to 5 m / min, but is not limited to this.
[0056] If necessary, a cleaning process may be provided to clean the joining members that have been laser welded. In particular, when a corrosive flux is used, it is desirable to perform a cleaning process to remove residual flux. On the other hand, when a non-corrosive flux is used, the cleaning process may not be necessary.
[0057] In this manner, the joint member of the present embodiment can be obtained. Since the joint member after manufacture has both the base material fusion zone and the brazing material fusion zone, the strength of the joint is excellent. In addition, the airtightness and watertightness of the joint are reliably ensured.
[0058] In addition, examples of joining members for forming a cross joint, a corner joint, a scarf joint, a hem joint, a ridge joint, a flare joint, a back plate joint, and a lap fillet joint, and the direction of laser incidence in the method of laser irradiation for manufacturing these joining members are shown in Figs. EXAMPLES
[0059] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0060] (1) Preparation of joining members [Example 1] In Example 1, a joint member was produced by laser welding a clad material in which a first metal member and a brazing filler metal were joined to another clad material in which a second metal member and a brazing filler metal were joined to each other. The joint member was produced by the following procedure.
[0061] <Preparation process> As the upper material, a plate-shaped clad material was prepared by joining A3003 material (Al-Mn alloy) and A4343 material (Al-Si alloy) by hot rolling. This clad material had a total thickness of 1.6 mm, and the thickness of the A4343 material was approximately 7% of the total thickness. In addition, the same clad material as the upper material was prepared as the lower material. The A3003 material of the upper material (clad material) corresponds to the first metal member, and the A4343 material corresponds to the brazing material. The A3003 material of the lower material (clad material) corresponds to the second metal member, and the A4343 material corresponds to the brazing material.
[0062] <Lamination process> The upper and lower materials were laminated with flux interposed therebetween, as shown in Fig. 20. Specifically, NOCOLOK flux was applied to the brazing material surface of the upper material. Next, the upper and lower materials were laminated so that the flux-coated surface of the upper material and the brazing material surface of the lower material faced each other. The obtained laminate had a layer structure from top to bottom of the upper material [A3003 (first metal member) / A4343 (brazing material)] / flux / lower material [A4343 (brazing material) / A3003 (second metal member)].
[0063] <Laser welding process> The laminate was irradiated with a laser as shown in Figure 21 to bond the upper and lower members. Specifically, the laser was irradiated while scanning the approximate center of the surface of the upper member constituting the laminate. The irradiation was performed under the condition of a laser output of 2.0 kW. As a result, a bonded member was obtained in which the upper and lower members were bonded at the laser irradiated portion.
[0064] [Example 2] In Example 2, a joint member was produced by laser welding a clad material in which a first metal member and a brazing filler metal were joined to a second metal member. The joint member was produced by the following procedure.
[0065] <Preparation process> A plate-shaped clad material was prepared as the upper material by joining A3003 and A4343 materials by hot rolling. The total thickness of this clad material was 2.0 mm, and the thickness of the A4343 material was approximately 7% of the total thickness. An A6063 extrusion material was prepared as the lower material. The A3003 material of the upper material (clad material) corresponds to the first metal member, and the A4343 material corresponds to the brazing material. The lower material (A6063 extrusion material) corresponds to the second metal member.
[0066] <Lamination process> The upper and lower materials were laminated with flux interposed therebetween, as shown in Fig. 22. Specifically, NOCOLOK flux was applied to the brazing material surface of the upper material. Next, the upper and lower materials were laminated so that the flux-coated upper and lower material surfaces faced each other. The obtained laminate had a layer structure from top to bottom of the upper material [A3003 (first metal member) / A4343 (brazing material)] / flux / lower material [A6003 (second metal member)].
[0067] <Laser welding process> The laminate was irradiated with a laser to bond the upper and lower members as shown in Fig. 23. The irradiation was performed under the condition of a laser output of 2.6 kW. As a result, a bonded member was obtained in which the upper and lower members were bonded at the laser irradiated portion.
[0068] [Example 3] In Example 3, the first metal member and the second metal member were laser-welded via a foil-shaped brazing material. The joining member was produced by the following procedure.
[0069] <Preparation process> A3003 plate material (thickness 2.0 mm) was prepared as the upper material, and A6063 extrusion material (thickness 2.0 mm) was prepared as the lower material. The A3003 plate material (upper material) corresponds to the first metal member, and the A6063 extrusion material (lower material) corresponds to the second metal member. In addition, A4045 foil material (thickness 0.06 mm) was prepared as the brazing material.
[0070] <Lamination process> The upper and lower materials were laminated with the brazing material and flux interposed therebetween, as shown in Fig. 24. Specifically, NOCOLOK flux was applied to the surfaces of the upper and lower materials. The upper and lower materials were laminated so that the upper material surface coated with the flux faced the brazing material surface not coated with the flux, and the brazing material and the lower material were laminated so that the brazing material surface coated with the flux faced the lower material surface. The obtained laminate had a layer structure from top to bottom of the upper material [A3003 sheet material (first metal member)] / flux / A4045 foil material (brazing material) / flux / lower material [A6063 extrusion material (second metal member)].
[0071] <Laser welding process> The laminate was irradiated with a laser to bond the upper and lower members as shown in Fig. 25. The irradiation was performed under the condition of a laser output of 2.4 kW. As a result, a bonded member was obtained in which the upper and lower members were bonded at the laser irradiated portion.
[0072] [Example 4 (Comparison)] In Example 4, the first metal member and the second metal member were laser-welded together without using any brazing material or flux. The joining members were produced in the following procedure.
[0073] <Preparation process> An A3003 plate (thickness 2.0 mm) was prepared as the upper material, and an A6063 extrusion (thickness 2.0 mm) was prepared as the lower material. The A3003 plate (upper material) corresponds to the first metal member, and the A6063 extrusion (lower material) corresponds to the second metal member.
[0074] <Lamination process> The upper and lower members were laminated as shown in Fig. 26. The obtained laminate had a layer structure from top to bottom of upper member [A3003 plate material (first metal member)] / lower member [A6063 extruded material (second metal member)].
[0075] <Laser welding process> The laminate was irradiated with a laser to bond the upper and lower members as shown in Fig. 27. The irradiation was performed under the condition of a laser output of 2.2 kW. As a result, a bonded member was obtained in which the upper and lower members were bonded at the laser irradiated portion.
[0076] For Examples 1 to 4, Tables 1 and 2 show the materials used in producing the joined members and the chemical compositions of the aluminum alloys.
[0077] [Table 1]
[0078] [Table 2]
[0079] (2) Evaluation of joining materials The cross sections of the joints of the joint members obtained in Examples 1 to 4 were observed. First, the joint members were cut in a direction perpendicular to the joint surface using a wet grindstone cutter, and then polished to prepare samples for observing the joints. The cut surfaces of the samples were observed using an optical microscope.
[0080] (3) Evaluation results Optical microscope images of the cross section of the bonded member of Example 1 are shown in Figures 28 and 29. Figure 28 shows the entire bonded member, and Figure 29 shows the vicinity of the bonded portion. Similarly, optical microscope images of the cross section of the bonded member of Example 2 are shown in Figures 30 and 31, optical microscope images of the cross section of the bonded member of Example 3 are shown in Figures 32 and 33, and optical microscope images of the cross section of the bonded member of Example 4 are shown in Figures 34 and 35.
[0081] As shown in Figures 28 and 29, the joint member of Example 1 had a base material molten zone formed at the joint where the core material (A3003 material) and the skin material (A4343 material) had melted and solidified. This base material molten zone firmly joined the core materials of the upper and lower plates so as to be integrated. In addition, a brazing material molten zone formed around the base material molten zone where the skin material (A4343) had melted and solidified. This brazing material molten zone sealed the base material molten zone. The same results as in Example 1 were obtained for the joint members of Examples 2 and 3, and the base material molten zone and the brazing material molten zone that sealed the periphery were formed at the joint.
[0082] On the other hand, in the joint member of Example 4, which did not use brazing material or flux, a structure similar to the molten base material where the metallic members were melted and solidified was observed in the joint, but no molten brazing material was observed around it. Therefore, the structure similar to the molten base material was not sealed and was exposed to the atmosphere.
[0083] From the above results, it can be seen that according to this embodiment, a joint member having excellent joint strength, as well as excellent airtightness and watertightness can be obtained. [Explanation of symbols]
[0084] 10 Joining materials 12 First metal member 14 Second metal member 16 Brazing sheet material 18 Joint interface 20 Laser Welding 22 Base material fusion zone 24 Brazing material melting part 26 Solidification cracking 28 Laser Light
Claims
1. A joining member including: a first metal member having a first main surface and a second main surface; and a second metal member disposed on the second main surface side of the first metal member and joined to at least a portion of the first metal member via a laser weld, the joining member includes a sheet-shaped brazing material on a second main surface side of the first metal member, The laser welded portion includes a base material fusion portion formed of a molten and integrated product of the first metal member, the second metal member, and the sheet-shaped brazing material, and a brazing material fusion portion formed of a molten product of the sheet-shaped brazing material, one or both of the first metal member and the second metal member are made of an aluminum-based metal, The material of the brazing material is a 4000 series (Al-Si series) alloy, an Al-Cu-Si series, or an Al-Zn series, the base material fusion portion is formed so as to penetrate from the first main surface to the second main surface of the first metal member and to be continuous to at least a part of the thickness of the second metal member, A joining member, wherein the brazing material molten portion is in close contact with the first metal member, the second metal member, and the base material molten portion, and the periphery of the base material molten portion is sealed by the sheet-shaped brazing material and the brazing material molten portion.
2. The joint member according to claim 1 , wherein the first metal member and the second metal member are joined to each other by forming a lap joint.
3. The joint member according to claim 1 , wherein the first metal member and the second metal member are joined to form a T-joint.
4. The joining member according to any one of claims 1 to 3, wherein the first metal member and the second metal member are made of the same material.
5. The joining member according to any one of claims 1 to 3, wherein the first metal member and the second metal member are made of different materials.
6. A method for producing a joint member according to any one of claims 1 to 5, comprising the following steps: preparing a first metal member having a first main surface and a second main surface, a second metal member, and a sheet-shaped brazing material; A step of preparing a laminate in which the sheet-shaped brazing material and the second metal member are arranged in this order on a second main surface side of the prepared first metal member; and a step of irradiating a first main surface of a first metal member constituting the laminate with laser light to laser-weld the second metal member to at least a portion of the first metal member via a joining interface; a method in which, in the laser welding process, the first metal member, the second metal member, and a portion of the sheet-shaped brazing material are melted and integrated to form a base material molten portion that penetrates the joint interface of the laser weld, and the sheet-shaped brazing material around the joint interface is melted to form a brazing material molten portion.
7. The method according to claim 6 , further comprising the steps of: preparing a clad material in which the first metal member and the sheet-shaped brazing material are roll-bonded to each other;
Citation Information
Patent Citations
Storage and transportation of polyolefin powder
JP1982025344A
Method for joining different kinds of materials
JP2008023562A
Heat radiator
JP2010171279A
Clad material for cooler, and cooler for heating element
JP2013036098A
Method for manufacturing metal joined member and metal joined member
JP2013176785A
Cited By
Method for manufacturing weldment
WO2026225614A1