Light Diffusion Film
A light diffusing film with a specific T/t ratio maintains half-value angle stability during high elongation processing, addressing the challenge of LED lighting devices' shape flexibility and diffusivity.
Patent Information
- Application Number
- JP2019199004
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-10-31
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-10-31
AI Technical Summary
LED lighting devices require light diffusion films that maintain a wide half-value angle even after processing with high elongation rates, especially when molded into curved or highly elongated shapes, as conventional films suffer from decreased diffusivity under such conditions.
A light diffusing film with a specific ratio (T/t) of average film thickness to average particle diameter of 3.0 or more, containing light diffusing particles and a resin binder, which maintains the half-value angle by balancing the contributions of particles and voids during stretching.
The film effectively suppresses a decrease in half-value angle even after high elongation processing, ensuring consistent light diffusion performance across various shapes and elongations.
Smart Images

Figure 0007553235000007 
Figure 0007553235000002 
Figure 0007553235000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a light diffusing film. [Background technology]
[0002] Conventionally, devices using light-emitting diodes (LEDs) have been known as light-emitting devices capable of emitting high-energy light with low power consumption. Since the light emitted from an LED has a strong directivity, it is required to highly disperse the light. Devices using light-emitting diodes are used as LED lighting devices such as automobile lights, refrigerators, microwave ovens, and indoor lights. High degree of dispersion is particularly required for LED lighting devices (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-041638 A Summary of the Invention [Problem to be solved by the invention]
[0004] Light diffusion films are used to diffuse light. Haze is sometimes used as an index to evaluate the light diffusion properties of light diffusion films. However, in LED lighting devices, even light diffusion films with high haze may not provide satisfactory light diffusion properties. Therefore, the half-value angle is used as an index of light diffusion properties in LED lighting devices. The half-value angle (degrees) is the half intensity I0 of the front light at an angle of 0 degrees from the light source that passes through the light diffusion film. 1 / 2 In other words, LED lighting devices require light diffusion films that exhibit a wide half-value angle (degrees).
[0005] On the other hand, LED lighting devices have a high degree of freedom in design, and many lighting devices with new shapes have been announced. Among them, parts such as the cover of an LED lighting device also require a degree of freedom in shape, and when molded from a flat sheet shape, there are cases where a curved surface with a high radius of curvature or a flat surface with a high elongation rate during molding exists. In order to meet this demand, it has become clear that molding a light diffusion film has a problem in that the light diffusion performance of the light diffusion film decreases in the case of a part with a high radius of curvature or a part with a high elongation rate. In particular, when the light diffusion film is stretched, the half-value angle is likely to decrease even if the decrease in haze is slight.
[0006] Therefore, an object of the present invention is to provide a light diffusing film capable of suppressing a decrease in the half-value angle even after processing at a high elongation rate. [Means for solving the problem]
[0007] The inventors have discovered that by using a light diffusion film having a light diffusion layer containing light diffusion particles and a resin binder, and by setting the ratio (T / t) of the average film thickness T of the light diffusion layer to the average particle diameter t of the light diffusion particles to be 3.0 or more, a light diffusion film can be obtained that can suppress the decrease in half-value angle even after processing at a high elongation rate. That is, the present invention relates to the following [1] to [5].
[0008] [1] A light diffusion film comprising a substrate film and a light diffusion layer containing light diffusion particles and a resin binder, A light diffusing film, wherein the ratio (T / t) of the average thickness T of the light diffusing layer to the average particle diameter t of the light diffusing particles is 3.0 or more.
[0009] [2] Half-value angle H of light diffusion film at 40% elongation 40 is in the range of 25% lower than the value of the half-value angle H0 before stretching and 25% higher than the value of the half-value angle H0 before stretching. [3] The light diffusion film according to [1] or [2], wherein the loading amount of the light diffusion particles is 30% by mass or more and 80% by mass or less based on the total solid content of the light diffusion layer. [4] The light diffusing film according to any one of [1] to [3], wherein the light diffusing particles have an average particle diameter t of 0.5 to 10.0 μm. [5] The light diffusing film according to any one of [1] to [4], wherein the light diffusing layer has an average thickness T of 1.5 to 30 μm. Effect of the Invention
[0010] Therefore, according to the present invention, it is possible to provide a light diffusing film capable of suppressing a decrease in the half-value angle even after processing at a high elongation rate. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view of a light diffusion film 1 of the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of the light diffusion film 1 of this embodiment when stretched. [Diagram 3] FIG. 3 is a schematic cross-sectional view of the light diffusion film 1 of this embodiment when it is further stretched. [Figure 4] FIG. 4 is a schematic cross-sectional view showing the effect of a conventional light diffusing film C1 when it is stretched. [Diagram 5] FIG. 5 is an SEM photograph of a cross section of a light diffusing film at an elongation rate of 0%. [Figure 6] FIG. 6 is an SEM photograph of a cross section of a light diffusing film at an elongation rate of 40%. [Figure 7] FIG. 7 is an SEM photograph of a cross section of a light diffusing film at an elongation rate of 80%. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. The positional relationships such as up, down, left and right are based on the positional relationships shown in the drawings unless otherwise specified. The dimensional ratios of the drawings are not limited to the ratios shown. However, the following embodiments are examples for explaining the present invention, and the present invention is not limited to these, and can be implemented by arbitrarily changing them within the scope of the gist of the present invention. In this specification, for example, the expression of a numerical range such as "1 to 100" includes both the lower limit "1" and the upper limit "100". The same applies to the expression of other numerical ranges.
[0013] The light diffusion film according to the present embodiment includes a substrate film and a light diffusion layer containing light diffusion particles and a resin binder. In the present embodiment, the ratio (T / t) of the average thickness T of the light diffusion layer to the average particle diameter t of the light diffusion particles (hereinafter, simply referred to as "T / t ratio") is 3.0 or more. The light diffusion film according to the present embodiment can suppress the decrease in the half-value angle even after processing at a high elongation rate.
[0014] 1 is a schematic cross-sectional view of a light diffusion film 1 of this embodiment. The light diffusion film 1 of this embodiment includes a base film 2 and a light diffusion layer 3 provided on one surface 2a of the base film 2. In the light diffusion film 1, the light diffusion layer 3 is exposed at the outermost surface. Since the light diffusion layer 3 is exposed at the outermost surface, by stretching the light diffusion film 1, it becomes easier to form irregularities on the surface of the light diffusion layer 3, and it becomes easier to maintain the half-value angle after stretching.
[0015] The light diffusion layer 3 contains light diffusion particles 31 and a resin 32. The light diffusion layer 3 has therein voids B. The light diffusion layer 3 has a T / t ratio equal to or greater than a predetermined range, so that the light diffusion particles 31 are formed so as to be piled up in the thickness direction of the light diffusion layer 3.
[0016] Next, a method of using the light diffusion film 1 will be described. The light diffusion film 1 of this embodiment is used by, for example, molding under heating conditions to fit the curved shape of the surface of a transparent part. During this molding, the light diffusion film 1 stretches in accordance with the shape of the curved surface. The light diffusion film 1 of this embodiment can maintain the half-value angle due to light diffusion of the light diffusion film even through this stretching.
[0017] 1, when the light diffusion film 1 is not stretched, light is diffused by the light diffusion particles 31 in the light diffusion layer 3, the voids B, and the surface interfaces. Among these elements that diffuse light, the light diffusion particles 31 in the light diffusion layer 3 contribute greatly to the diffusion of light.
[0018] 2 is a schematic cross-sectional view of the light diffusion film 1 of this embodiment when stretched. When the light diffusion film 1 is stretched, the thickness of the light diffusion layer 3 decreases, and the contribution of the light diffusion particles 31 to light diffusion also decreases slightly, but the voids B inside the light diffusion film 1 expand, and the contribution to light diffusion increases. Note that the contribution of the light diffusion particles 31 to light diffusion decreases as the elongation rate increases, but the size of the voids B also increases as the elongation rate increases, and the contribution to light diffusion also increases. In this way, the light diffusion property before and after stretching is maintained.
[0019] FIG. 3 is a schematic cross-sectional view of the light diffusion film 1 of the present embodiment when the light diffusion film 1 is further stretched. When the light diffusion film 1 is further stretched, the film thickness of the light diffusion layer 3 becomes smaller, and the contribution of the light diffusion particles 31 to light diffusion further decreases. However, in addition to the expansion of the voids B inside the light diffusion film 1, although not shown in the figure, the number of voids B may increase, and furthermore, recesses S are formed on the surface of the light diffusion layer 3. The recesses S are formed by the collapse of the light diffusion layer 3. However, since the value of T / t is equal to or greater than a predetermined value, roughness of the surface due to the exposure of the light diffusion particles 31 or roughness of the surface due to the formation of the recesses S themselves is formed, which contributes to an increase in light diffusibility. In this way, when the light diffusion film 1 is further stretched, elements that reduce light diffusibility and elements that increase light diffusibility coexist, so that the light diffusibility before and after stretching is maintained.
[0020] FIG. 4 is a schematic sectional view showing the operation when a conventional light diffusion film C1 is stretched. Here, the light diffusion film C1 will be described as a prior art. The light diffusion film C1 has, for example, a T / t of less than or equal to a predetermined value. The light diffusion film C1 includes a light diffusion layer C3 containing light diffusion particles C31 and a resin binder 32. When the light diffusion film C1 is stretched, the contribution of the light diffusion particles C31 to light diffusion becomes smaller. Although the size of the recesses is enlarged by stretching, the contribution of the recesses to light diffusion becomes smaller. Moreover, since the film thickness of the light diffusion particles C31 is not thick, almost no voids are formed in the light diffusion layer C3, and even when stretched, the contribution of the expansion of the voids B to light diffusion is small. For the above reasons, according to the diffusion film C1, since the contribution of each element that contributes to light diffusion becomes smaller due to stretching, the light diffusibility becomes smaller before and after stretching.
[0021] <T / t ratio> In the light diffusion film according to the present embodiment, the ratio (T / t) of the average film thickness T of the light diffusion layer to the average particle diameter t of the light diffusion particles is 3.0 or more. By having the T / t ratio, a light diffusion film capable of suppressing a decrease in the half-value angle even after processing at a high elongation rate can be obtained. The T / t ratio is preferably 3.0 or more, more preferably 3.3 or more, and even more preferably 3.8 or more. When the T / t ratio is equal to or more than the lower limit, the light diffusion particles tend to overlap easily in the light diffusion layer, and even when the light diffusion film is stretched, the half-value angle tends to be easily maintained. The upper limit of the T / t ratio is not particularly limited, but is preferably 20.0 or less, more preferably 15.0 or less, and even more preferably 10.0 or less. When the T / t ratio is equal to or less than the upper limit, the light diffusion layer is easily formed, and even when the film is stretched, the half-value angle is easily maintained.
[0022] The average particle diameter t of the light diffusing particles is preferably 0.5 to 10.0 μm, more preferably 1.0 to 8.0 μm, even more preferably 1.0 to 5.0 μm, and even more preferably 1.0 to 3.0 μm. When the average particle diameter t of the light diffusing particles is within this range, the half-value angle of the light diffusing film is improved, and when the average particle diameter t is within the range of 1.0 to 3.0 μm, the half-value angle of the light diffusing film is particularly high.
[0023] In this specification, the average particle diameter t of the light diffusing particles is the median diameter (D 50 ) and the median diameter (D 50 ) means the particle size at which the amount of particles in the particle distribution is 50 volume % when calculated cumulatively from the small particle size side.
[0024] The average thickness T of the light diffusion layer is preferably 1.5 to 30 μm, more preferably 3 to 20 μm, and even more preferably 5 to 15 μm. When the average thickness T of the light diffusion layer is within this range, the decrease in the half-value angle due to processing at a high elongation rate can be further suppressed. The method for measuring the average thickness T in this specification is the same as that described in the Examples.
[0025] The amount of light diffusing particles in the light diffusing layer is preferably 30% by mass or more and 80% by mass or less, more preferably 50% by mass or more and 75% by mass or less, even more preferably 65% by mass or more and 70% by mass or less, and even more preferably 65% by mass or more and 68% by mass or less, based on the total solid content of the light diffusing layer. When the amount of light diffusing particles is within this range, many light diffusing particles are filled in the light diffusing layer, and by stretching the light diffusing film, unevenness is easily formed on the surface of the light diffusing layer, and the half-value angle is easily maintained.
[0026] The light diffusion particles in the light diffusion layer are preferably contained in an amount of 40 to 400 parts by mass, more preferably 100 to 300 parts by mass, even more preferably 180 to 240 parts by mass, and even more preferably 200 to 240 parts by mass, relative to 100 parts by mass of the resin binder. When the amount of the light diffusion particles is within this range, a large number of light diffusion particles are filled in the light diffusion layer, and by stretching the light diffusion film, unevenness is easily formed on the surface of the light diffusion layer, and the half-value angle is easily maintained.
[0027] Refractive index I of light diffusing particles p and the refractive index I of the resin binder r Difference with |I p -I r is preferably 0.01 to 0.50, more preferably 0.05 to 0.40, and further preferably 0.10 to 0.30. p -I r By increasing |, the internal diffusion in the light diffusion layer can be increased. However, depending on the expected elongation rate and the degree of surface diffusion at that elongation rate, the difference |Ip -I r The value of the refractive index I p is the refractive index I r It is preferable that the value is higher than .
[0028] The half-value angle H0 of the light diffusion film at an elongation rate of 0% is preferably 10 degrees or more, more preferably 20 degrees or more, even more preferably 30 degrees or more, and still more preferably 40 degrees or more. The upper limit of the half-value angle H0 is not particularly limited, but may be, for example, 70 degrees or less, or 60 degrees or less.
[0029] Half-value angle H of light diffusion film at 40% elongation 40 is preferably 10 degrees or more, more preferably 20 degrees or more, even more preferably 30 degrees or more, and still more preferably 40 degrees or more. 40 The upper limit of the angle is not particularly limited, but may be, for example, 70 degrees or less, or 60 degrees or less.
[0030] Half-value angle H of light diffusion film at 60% elongation 60 However, the half angle H is preferably 10 degrees or more, more preferably 20 degrees or more, even more preferably 30 degrees or more, and still more preferably 40 degrees or more. 60 The upper limit of the angle is not particularly limited, but may be, for example, 70 degrees or less, or 60 degrees or less.
[0031] Half-value angle H of light diffusion film at 80% elongation 80 However, the half angle H is preferably 10 degrees or more, more preferably 20 degrees or more, even more preferably 30 degrees or more, and still more preferably 40 degrees or more. 80 The upper limit of the angle is not particularly limited, but may be, for example, 70 degrees or less, or 60 degrees or less.
[0032] Half-value angle H of light diffusion film at 120% elongation 120However, the half angle H is preferably 10 degrees or more, more preferably 20 degrees or more, even more preferably 30 degrees or more, and still more preferably 40 degrees or more. 120 The upper limit of the angle is not particularly limited, but may be, for example, 70 degrees or less, or 60 degrees or less.
[0033] Half-value angle H of light diffusion film at 40% elongation 40 is preferably in the range of at least 25% lower than the value of the half-value angle H0 before stretching and not more than 25% higher than the value of the half-value angle H0 before stretching, more preferably in the range of at least 20% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, even more preferably in the range of at least 15% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, and even more preferably in the range of at least 10% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching.
[0034] Half-value angle H of light diffusion film at 60% elongation 60 However, it is preferably in the range of at least 25% lower than the value of the half-value angle H0 before stretching and not more than 25% higher than the value of the half-value angle H0 before stretching, more preferably in the range of at least 20% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, even more preferably in the range of at least 15% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, and even more preferably in the range of at least 10% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching.
[0035] Half-value angle H of light diffusion film at 80% elongation 80However, it is preferably in the range of at least 25% lower than the value of the half-value angle H0 before stretching and not more than 25% higher than the value of the half-value angle H0 before stretching, more preferably in the range of at least 20% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, even more preferably in the range of at least 15% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, and even more preferably in the range of at least 10% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching.
[0036] Half-value angle H of light diffusion film at 120% elongation 120 However, it is preferably in the range of at least 25% lower than the value of the half-value angle H0 before stretching and not more than 25% higher than the value of the half-value angle H0 before stretching, more preferably in the range of at least 20% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, even more preferably in the range of at least 15% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching, and even more preferably in the range of at least 10% lower than the value of the half-value angle H0 before stretching and not more than 20% higher than the value of the half-value angle H0 before stretching.
[0037] In this specification, the elongation ratio of the light diffusion film is a ratio represented by the following formula (1). Elongation rate (%) = [length after elongation – length before elongation] / [length before elongation] × 100 (1) The elongation conditions and half-value angles (degrees) in this specification are based on the test methods described in the Examples.
[0038] <Base film> The base film preferably contains a thermoplastic resin. Examples of resins constituting the base film include polycarbonate resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene naphthalate resin, acrylic resin, polyvinyl chloride resin, polyethylene resin, polypropylene resin, polystyrene resin, polyurethane resin, triacetyl cellulose resin, and norbornene resin. Among these, one type may be used alone, or two or more types may be used in combination. Among these, the base film preferably contains at least one selected from the group consisting of polycarbonate resin, polyethylene terephthalate resin, polyacrylic resin, polyvinyl chloride resin, and polyurethane resin, and more preferably contains a polycarbonate resin.
[0039] From the viewpoint of stretching the light diffusion film, it is preferable that the base film is a non-stretched film that has not been subjected to stretching, particularly biaxial stretching. Here, when the base film is rolled, it may be slightly stretched, but when it has not been stretched or biaxially stretched, it is included in the non-stretched film in this specification.
[0040] In order to improve adhesion to the light diffusing layer, the surface of the substrate may be subjected to a corona discharge treatment or may have an easy-adhesion layer.
[0041] The glass transition temperature of the resin of the base film is preferably 100 to 200° C., more preferably 120 to 180° C., and even more preferably 140 to 155° C. When the glass transition temperature of the resin of the base film is within this range, stretching processing under heating conditions can be easily performed.
[0042] The thickness of the substrate film is preferably from 10 to 500 μm, more preferably from 100 to 400 μm, and further preferably from 150 to 300 μm.
[0043] <Light diffusing layer> The light diffusing layer includes light diffusing particles and a resin binder.
[0044] (Light Diffusion Particles) The light diffusing particles according to this embodiment are blended in the light diffusing layer to diffuse light. In this embodiment, the light diffusing particles refer to particles having an average particle diameter of 0.4 μm or more. Here, the average particle diameter can be measured in the same manner as the above-mentioned average particle diameter t.
[0045] The light diffusion particles are preferably particles having a glass transition temperature higher than the glass transition temperature of the resin of the substrate film, and more preferably thermoplastic resin particles or thermosetting resin particles having the above-mentioned glass transition temperature. In the case of thermoplastic resin particles, the melting temperature of the thermoplastic resin particles is preferably 20° C. higher than the glass transition temperature of the resin of the substrate film, more preferably 40° C. higher than the glass transition temperature of the resin of the substrate film, and even more preferably 50° C. higher than the glass transition temperature of the resin of the substrate film. By using the thermoplastic resin particles or thermosetting resin particles, the shape of the light diffusion particles can be maintained when the light diffusion film is stretched under heating temperature conditions, and the maintenance rate of the half-value angle after stretching can be increased.
[0046] Examples of resins used in the light-diffusing particles include benzoguanamine resin, acrylic resin, styrene resin, urethane resin, nylon resin, silicone resin, melamine resin, epoxy resin, polycarbonate resin, and thiophene resin. Of these, one type may be used alone, or two or more types may be used in combination. Among these, benzoguanamine resin, acrylic resin, styrene resin, and melamine resin are preferred. In addition, the light-diffusing particles may be solid particles or hollow particles.
[0047] The light diffusing particles may contain inorganic oxides such as silica and alumina, ultraviolet absorbing agents, and other components.
[0048] The average particle diameter t of the light diffusing particles is as described above. The light diffusing particles may have a high refractive index or a low refractive index. In the case of a high refractive index, the refractive index of the light diffusing particles is preferably 1.40 to 1.70, more preferably 1.50 to 1.70, and even more preferably 1.55 to 1.70. In the case of a low refractive index, the refractive index of the light diffusing particles is preferably 1.26 to 1.36, more preferably 1.28 to 1.34, and even more preferably 1.30 to 1.32.
[0049] (Resin binder) The resin binder may be a thermoplastic resin or a thermosetting resin, but preferably contains a thermoplastic resin. Examples of the thermoplastic resin include ABS resin, norbornene resin, silicone resin, nylon resin, polyvinyl acetal resin, polycarbonate resin, modified polyphenylene ether resin, polybutylene terephthalate resin, polyethylene terephthalate resin, sulfone resin, imide resin, fluororesin, styrene resin, acrylic resin, vinyl chloride resin, vinyl acetate resin, vinyl chloride-vinyl acetate copolymer resin, polyester resin, urethane resin, rubber resin, polyvinyl ether resin, polyvinyl alcohol resin, polyvinyl butyral resin, polyvinyl pyrrolidone resin, and polyethylene glycol resin. Among these, one type may be used alone, or two or more types may be used in combination. The thermoplastic resin binder preferably contains at least one selected from the group consisting of polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl alcohol resin, polyvinyl acetal resin, polyvinyl butyral resin, polystyrene resin, acrylic resin, urethane resin, silicone resin, and fluororesin, and more preferably contains at least one selected from the group consisting of polyvinyl acetal resin and acrylic resin.
[0050] The glass transition temperature of the resin of the resin binder is preferably lower than the glass transition temperature of the resin of the base film, more preferably 80 to 200°C, even more preferably 90 to 150°C, and even more preferably 100 to 120°C.
[0051] The content of the resin binder is preferably 25% by mass or more and 70% by mass or less, more preferably 30% by mass or more and 50% by mass or less, and even more preferably 32% by mass or more and 35% by mass or less, based on the total solid content of the light diffusion layer.
[0052] The content of the thermoplastic resin is preferably 60% by mass or more and 100% by mass or less, more preferably 70% by mass or more and 100% by mass or less, and even more preferably 80% by mass or more and 100% by mass or less, based on the total amount of the resin binder.
[0053] The light diffusion layer according to this embodiment may contain inorganic particles having an average particle diameter of less than 0.4 μm (hereinafter, simply referred to as "inorganic fine particles"). The average particle diameter can be measured in the same manner as the average particle diameter t described above. Note that an average particle diameter of less than 0.4 μm makes almost no contribution to light diffusion. The inorganic fine particles are preferably inorganic oxide fine particles.
[0054] The inorganic fine particles are used, for example, to adjust the refractive index. In this case, the refractive index of the inorganic fine particles is preferably 1.9 or more, more preferably 2.0 or more, and even more preferably 2.3 or more. Examples of inorganic oxides contained in the inorganic oxide fine particles include lead hydroxycarbonate (2PbCO3Pb(OH)2) (refractive index 1.94 to 2.09), titanium oxide (refractive index 2.71), zirconium oxide (refractive index 2.4), zinc oxide (refractive index 1.95), and aluminum oxide (refractive index 1.76). Of these, one type may be used alone, or two or more types may be used in combination.
[0055] The inorganic fine particles may be white. By using inorganic fine particles exhibiting white color, the light diffusion film exhibits white color, and the effect of reducing uneven brightness near the light source of the backlight device and making light leakage at the end of the light guide plate less noticeable can be enhanced. Examples of inorganic fine particles exhibiting whiteness include zirconium oxide, titanium oxide, and zinc oxide. Of these, one type may be used alone, or two or more types may be used in combination. Among these, zirconium oxide and titanium oxide are preferred.
[0056] The primary particle diameter of the inorganic fine particles is preferably 10 to 50 nm. When such nanometer-order particles are dispersed in the light diffusion layer, most of them are contained in the light diffusion layer as aggregates.
[0057] The content of the inorganic fine particles is preferably 40 to 500 parts by mass, more preferably 120 to 300 parts by mass, and further preferably 160 to 240 parts by mass, based on 100 parts by mass of the resin binder.
[0058] The light diffusing layer may further contain additives such as a leveling agent, a surfactant such as a defoaming agent, an antioxidant, and an ultraviolet absorbing agent.
[0059] <Other properties of light diffusion film> (Total light transmittance) The total light transmittance Tt0 of the light diffusion film at an elongation rate of 0% is preferably 50% or more, more preferably 60% or more, even more preferably 65% or more, and even more preferably 70% or more. The upper limit of the total light transmittance Tt0 is not particularly limited, and may be, for example, less than 99%, less than 95%, less than 85%, or less than 80%.
[0060] Total light transmittance (Tt) of light diffusion film at 120% elongation 120 is preferably 50% or more, more preferably 60% or more, even more preferably 65% or more, and still more preferably 70% or more. 120The upper limit is not particularly limited, and may be, for example, less than 99%, less than 95%, less than 90%, less than 85%, less than 80%, or less than 70%.
[0061] The total light transmittance can be measured by a method in accordance with JIS K7361-1:1997.
[0062] (Hayes) The haze Hz0 of the light diffusion film at an elongation rate of 0% is preferably 90%, more preferably 95%, even more preferably 96%, and still more preferably 97%. The upper limit of the haze Hz0 is not particularly limited, but may be, for example, less than 100%.
[0063] Haze (Hz) of light diffusion film at 120% elongation 120 is preferably 90%, more preferably 95%, even more preferably 97%, and even more preferably 98%. 120 The upper limit is not particularly limited, but may be, for example, less than 100%.
[0064] The haze can be measured by a method in accordance with JIS K7136:2000.
[0065] (Arithmetic mean roughness (Ra)) The light diffusion film has an arithmetic mean roughness Ra0 at an elongation rate of 0% of preferably 1000 nm or less, more preferably 800 nm or less, and even more preferably 600 nm or less. The lower limit of the arithmetic mean roughness Ra0 is not particularly limited, but may be 200 nm.
[0066] Arithmetic mean roughness Ra of light diffusion film at 120% elongation 120 is preferably 1500 nm or less, more preferably 1000 nm or less, and even more preferably 800 nm or less. 120 The lower limit of the thickness is not particularly limited, but may be 300 nm.
[0067] By having an arithmetic mean roughness (Ra) in this range, a good balance between surface diffusion and internal diffusion is maintained, making it easier to maintain the half-value angle. The arithmetic mean roughness (Ra) can be determined using an atomic force microscope "Nanocute System" (product name, manufactured by Hitachi High-Tech Science Corporation, probe: Si single crystal probe, measurement mode: DFM mode, image processing: flat processing (XY) once) using a measurement method that complies with JIS B0601:2001.
[0068] [Method of manufacturing light diffusion film] The light diffusion film can be obtained, for example, by applying a coating liquid containing light diffusion particles and a resin binder onto a substrate film, although the manufacturing method thereof is not particularly limited. The amounts of light diffusion particles and resin binder contained in the coating liquid are as described above, and these components are diluted with a solvent to adjust the viscosity to an appropriate level, and then coated onto the substrate film.
[0069] [How to use light diffusion film] The light diffusion film is disposed on the surface of a transparent member. Examples of the method of using the light diffusion film include: (a) A preform method in which a light diffusing film is pressed onto the surface of a transparent material; (b) An insert molding method in which a light diffusion film is placed inside a mold and a transparent resin is poured into the mold. (c) A three-dimensional surface decoration molding method in which a light-diffusing film is laminated to an adherend by pressing it to one side of a transparent material in a non-contact manner under reduced pressure. The three-dimensional surface decoration molding method can be performed, for example, by using a TOM molding machine "NGF-5012-RS" (manufactured by Fuse Vacuum Co., Ltd.). Among these, (b) the insert mold molding method or (c) the three-dimensional surface decoration molding method is preferred, and (b) the insert mold molding method is more preferred.
[0070] In this embodiment, the temperature when laminating the light diffusion film onto the adherend (for example, the temperature of the molding chamber of a decorative molding machine) is preferably 70 to 200°C. The above temperature is more preferably 100 to 160°C, and further preferably 130 to 160°C. By performing molding within the above temperature range, the light diffusion film is stretched to conform to the surface of the resin molded body. Even if the resin molded body has a shape that results in a high elongation rate of 80% or 120% or more, the light diffusion film according to this embodiment can suppress a decrease in the half-value angle due to the molding.
[0071] The light diffusion film according to this embodiment is used for diffusing light in LED lighting devices such as automobile lights, for example.
[0072] As described above, the present specification discloses the following embodiments. <1> A light diffusion film comprising a substrate film and a light diffusion layer containing light diffusion particles and a resin binder, A light diffusing film, wherein the ratio (T / t) of the average thickness T of the light diffusing layer to the average particle diameter t of the light diffusing particles is 3.0 or more. <2> Half-value angle H of light diffusion film at 40% elongation 40 is in the range of 25% lower than the value of the half-value angle H0 before elongation and 25% higher than the value of the half-value angle H0 before elongation. <1> The light diffusion film according to claim 1.
[0073] <3> A light diffusion film comprising a substrate film and a light diffusion layer containing light diffusion particles and a resin binder, The half-value angle H of the light diffusion film at an elongation rate of 40% 40 is in the range of 25% lower than the value of the half-value angle H0 before stretching and 25% higher than the value of the half-value angle H0 before stretching.
[0074] <4> Half-value angle H of light diffusion film at 60% elongation 60is in the range of 25% lower than the value of the half-value angle H0 before elongation and 25% higher than the value of the half-value angle H0 before elongation. <1> ~ <3> 13. The light diffusion film according to claim 12 . <5> Half-value angle H of light diffusion film at 80% elongation 80 is in the range of 25% lower than the value of the half-value angle H0 before elongation and 25% higher than the value of the half-value angle H0 before elongation. <1> ~ <4> 13. The light diffusion film according to claim 12 . <6> The filling amount of the light diffusing particles is 30% by mass or more and 80% by mass or less with respect to the total solid content of the light diffusing layer. <1> ~ <5> 13. The light diffusion film according to claim 12 . <7> The filling amount of the light diffusing particles is 50% by mass or more and 75% by mass or less with respect to the total solid content of the light diffusing layer. <1> ~ <6> 13. The light diffusion film according to claim 12 . <8> The light diffusing particles are contained in an amount of 40 parts by mass or more and 250 parts by mass or less relative to 100 parts by mass of the resin binder. <1> ~ <7> 13. The light diffusion film according to claim 12 .
[0075] <9> The light diffusing layer is exposed on the outermost surface. <1> ~ <8> 13. The light diffusion film according to claim 12 . <10> The light diffusing particles include thermosetting resin particles. <1> ~ <9> 13. The light diffusion film according to claim 12 . <11> The resin binder comprises a thermoplastic resin. <1> ~ <10> 13. The light diffusion film according to claim 12 . <12> The resin binder contains at least one selected from the group consisting of polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl alcohol resin, polyvinyl acetal resin, polyvinyl butyral resin, polystyrene resin, acrylic resin, urethane resin, silicone resin, and fluororesin. <1> ~ <11> 13. The light diffusion film according to claim 12 .
[0076] <13> The light diffusing particles have an average particle size t of 0.5 to 10.0 μm. <1> ~ <12> 13. The light diffusion film according to claim 12 . <14> The light diffusing layer has an average thickness T of 1.5 to 30 μm. <1> ~ <13> 13. The light diffusion film according to claim 12 . <15> The base film contains at least one resin selected from the group consisting of polycarbonate resin, polyethylene terephthalate resin, acrylic resin, polyvinyl chloride resin, and urethane resin. <1> ~ <14> 13. The light diffusion film according to claim 12 . <16> The refractive index I of the light diffusing particles p and the refractive index I of the resin binder r Difference with |I p -I r | is between 0.01 and 0.5, <1> ~ <15> 13. The light diffusion film according to claim 12 .
[0077] <17> Half-value angle H of light diffusion film at 40% elongation 40 is 10 degrees or more, <1> ~ <16> 13. The light diffusion film according to claim 12 . <18> Half-value angle H of light diffusion film at 60% elongation 60 is 10 degrees or more, <1> ~ <17> 13. The light diffusion film according to claim 12 . <19> Half-value angle H of light diffusion film at 80% elongation 80 is 10 degrees or more, <1> ~ <18> 13. The light diffusion film according to claim 12 . EXAMPLES
[0078] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0079] [Measurement method] <Average thickness T of light diffusion layer> The cross section of the light diffusion film was observed at five locations at a magnification of 2,000 times using a SEM (Scanning Electron Microscope), and the average value of 10 locations on each cross section, a total of 50 locations, was determined as the average film thickness T of the light diffusion layer.
[0080] <Half-value angle> Measurements were carried out using an optical scattering measuring device "MiniDiff V2" (product name, manufactured by Light Tec). A diffusion film was placed on top of a transmitted light source so that light would enter the diffusion layer, and the light receiving unit was placed on top of that. Measurement conditions were that the incident light source was G (525 nm) and the angle of the incident light was perpendicular to the diffusion film, and the intensity of the transmitted light in the measurement field of view (-75 degrees to 75 degrees) was measured. The intensity I 1 / 2 The angle at which the intensity was more than half was measured, and the angular range at which the intensity was more than half was calculated to be the half-value angle (degrees).
[0081] <Total light transmittance and haze> The total light transmittance (Tt) was measured according to a method conforming to JIS K7361-1:1997, and the haze was measured according to a method conforming to JIS K7136:2000, using a haze meter "NDH4000" (product name, manufactured by Nippon Denshoku Industries Co., Ltd.), with the light diffusion layer of each light diffusion film as the light incident surface.
[0082] [Manufacturing of light diffusion films] <Examples 1 to 7 and Comparative Example 1> The light diffusion particles, resin binder, and an appropriate amount of organic solvent shown in Table 1 were mixed and stirred to obtain a coating solution for a light diffusion layer, which was then coated by bar coating onto a substrate film made of a polycarbonate film having a thickness of 250 μm and a glass transition temperature of 150° C. so that the thickness after drying would be the value shown in Table 1, and then dried to form a light diffusion layer, thereby obtaining the light diffusion films of Examples 1 to 7 and Comparative Example 1. SEM photographs of the cross section of the light diffusion film of Example 5 are shown in Figures 5 to 7. Figure 5 is an SEM photograph of the cross section of the light diffusion film at an elongation rate of 0%. Figure 6 is an SEM photograph of the cross section of the light diffusion film at an elongation rate of 40%. Figure 7 is an SEM photograph of the cross section of the light diffusion film at an elongation rate of 80%.
[0083] <Reference example 1> After mixing and stirring the coating solution R1 for light diffusion layer having the following formulation, it was coated by bar coating method on a support made of a polyethylene terephthalate film "Lumirror T60" (product name, manufactured by Toray Industries, Inc.) having a thickness of 250 μm so as to have a thickness after drying of 5 μm, and dried to form a light diffusion layer. Next, on the side of the support opposite to the side on which the light diffusion layer was formed, a coating solution for backcoat layer having the following formulation was coated by bar coating method so as to have a thickness after drying of 5 μm, and dried to form a backcoat layer, and a light diffusion film of Reference Example 1 was obtained. (Light diffusion layer coating solution R1) Acrylic polyol resin (solid content 50%, Tg 96°C, refractive index 1.51) 6 parts by weight Acrylic polyol resin (solid content 50%, Tg 19°C, refractive index 1.49) 14 parts by weight Polyisocyanate (solid content 60%) 4 parts by weight Acrylic resin particles (average particle size 2 to 3 μm, refractive index 1.49) 11 parts by weight Dilution solvent (appropriate amount) (Coating solution for backcoat layer) Acrylic polyol resin (solid content 50%, Tg 65°C, refractive index 1.49) 10 parts by weight Polyisocyanate (solid content 60%) 2 parts by weight Acrylic resin particles (average particle size 5 μm, refractive index 1.49) 0.1 parts by weight Dilution solvent (appropriate amount)
[0084] [evaluation] <Extension test> As an evaluation of shape conformity, a tensile test was performed according to JIS K7127:1999 to measure the elongation rate of each film. A sample was prepared by cutting into a rectangular shape of 100 mm long x 25 mm wide. Next, markings were made at 50 mm intervals near the center of the sample, excluding both ends, and the sample was placed in a tensile tester "AGS-1kNX" (trade name, manufactured by Shimadzu Corporation) equipped with a temperature control mechanism so that the marked part was not pinched by the chuck. The substrate was set to 160 ° C., and a tensile test was performed with a chuck distance of 50 mm and a tensile speed of 200 mm / min. The half-value angle at elongation rates of 0%, 40%, 60%, 80%, and 120%, the total light transmittance at elongation rates of 0% and 120%, and the haze at elongation rates of 0% and 120% were measured, and are shown in Table 1.
[0085] [Table 1]
[0086] (Light Diffusion Particles) A-1: Benzoguanamine particles (average particle size (D 50 )2μm, refractive index n=1.67, specific gravity 1.4g / cm 3 , melting point 225℃ or higher) A-2: Styrene particles (average particle size (D 50 ) 4μm, refractive index n=1.59, specific gravity 1.1g / cm 3 , decomposition temperature 250~270℃) A-3: Acrylic particles (average particle size (D 50 ) 5μm, refractive index n=1.49, specific gravity 1.1g / cm 3 , decomposition temperature 250~270℃) A-4: Acrylic particles (average particle size (D 50 )2μm, refractive index n=1.49, specific gravity 1.1g / cm 3 , decomposition temperature 250~270℃) (Resin binder) B-1: Acrylic resin (refractive index n = 1.49, specific gravity 1.1 g / cm 3 , glass transition temperature 100℃) B-2: Acrylic thermosetting resin (refractive index n = 1.49, specific gravity 1.1 g / cm 3 )
[0087] From the results of the Examples and Comparative Examples described above, it is evident that the light diffusing film according to this embodiment can suppress the decrease in the half-value angle even after processing at a high elongation rate.
[0088] A comparison between Example 1 and Comparative Example 1 shows that the T / t ratio being within a predetermined range makes it possible to suppress a decrease in the half-value angle even after processing at a high elongation rate. The results of Examples 1 to 5 show that the half-value angle is maintained even after elongation processing in a wide range of light diffusion particle contents. Examples 6 and 7 show that even in the case of light diffusion particles containing styrene resin or acrylic resin, the light diffusion film according to this embodiment can suppress a decrease in the half-value angle even after processing at a high elongation rate. [Industrial Applicability]
[0089] The light diffusion film of the present invention can suppress a decrease in the half-value angle even after processing at a high elongation rate, and can be disposed on the surface of a transparent resin and used in LED lighting devices such as automobile headlights.
Claims
1. A light diffusion film comprising a base film and a light diffusion layer containing light diffusion particles having an average particle diameter t (D50) of 0.4 μm or more as measured by a laser diffraction particle size distribution analyzer and a resin binder, a ratio (T / t) of an average thickness T of the light diffusion layer to an average particle diameter t of the light diffusion particles is 3.0 or more and 20.0 or less; the amount of the light-diffusing particles having an average particle diameter t of 0.4 μm or more is 30% by mass or more and 80% by mass or less based on the total amount of solids in the light-diffusing layer; The intensity of transmitted light from an incident light source G (525 nm) is measured in a measurement field of view of −75 degrees to 75 degrees from the vertical to the diffusion film, and the half-value angle is defined as the angle at which the intensity I 1 / 2 of the front light intensity I 0 is half the intensity I 1 / 2 of the front light intensity I 0 . The half-value angle H 40 is the half-value angle H before elongation 0 and the half-value angle H before elongation is 25% lower than the value 0 The range is 25% higher than the value of Light diffusion film.
2. The light diffusing layer has voids therein. The light diffusing film according to claim 1 .
3. The filling amount of the light diffusing particles is 50% by mass or more and 75% by mass or less with respect to the total amount of solids in the light diffusing layer. The light diffusing film according to claim 1 .
4. The light diffusing particles have an average particle size t of 0.5 to 10.0 μm. The light diffusing film according to any one of claims 1 to 3.
5. The light diffusing layer has an average thickness T of 1.5 to 30 μm. The light diffusing film according to any one of claims 1 to 4.
6. The light diffusion layer is exposed on the outermost surface. The light diffusing film according to any one of claims 1 to 5.
7. The light diffusing particles include thermoplastic resin particles or thermosetting resin particles. The light diffusing film according to any one of claims 1 to 6.
8. The resin binder comprises a thermoplastic resin. The light diffusing film according to any one of claims 1 to 7.
9. The half-value angle H of the light diffusion film at an elongation rate of 40% 40 is 10 degrees or more, The light diffusing film according to any one of claims 1 to 8.
Citation Information
Patent Citations
Light diffusion sheet, method for producing the same and translucent screen
JP2001311806A
Light diffusion sheet, method for producing the same and translucent screen
JP2001311807A
Light diffusion element, polarizer with light diffusion element, liquid crystal display device using the same, and light diffusion element manufacturing method
JP2012068273A
Sheet for coating optical semiconductor elements
JP2018041638A
Light diffusing element, polarizing plate with light diffusing element, liquid crystal display using both, and manufacturing method for light diffusing element
WO2010106990A1