Double-layer fireproof pipe and its manufacturing method

By forming convex portions on the fire-resistant layer to counteract mold-induced tensile forces, the fire-resistant double-layer pipe achieves crack resistance and maintains fire resistance, simplifying manufacturing and reducing costs.

JP7553312B2Active Publication Date: 2024-09-18RESONAC CONSTR MATERIALS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020170878
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-09
Publication Date
2024-09-18
Estimated Expiration
2040-10-09

AI Technical Summary

Technical Problem

Existing fire-resistant double-layer pipes experience cracks in the fire-resistant layer due to insufficient bonding at weld portions, which are weakened by tensile forces during mold opening, leading to reduced fire resistance.

Method used

Forming convex portions on the fire-resistant layer corresponding to the mold's dividing surface, which are continuous along the pipe axis, to reduce tensile forces and maintain bonding strength, thereby preventing cracks.

Benefits of technology

The convex portions effectively suppress cracks in the fire-resistant layer, ensuring consistent fire resistance without the need for additional cushioning materials or costly automation, reducing manufacturing complexity and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553312000005
    Figure 0007553312000005
  • Figure 0007553312000002
    Figure 0007553312000002
  • Figure 0007553312000003
    Figure 0007553312000003
Patent Text Reader

Abstract

To provide a fireproof double layer pipe which can inhibit cracks of a fireproof layer of the fireproof double layer pipe, and to provide a manufacturing method of the fireproof double layer pipe.SOLUTION: In a fireproof double layer pipe 1 according to the invention, a fireproof layer 3 made of a hydraulic material is formed on an outer peripheral surface of a synthetic resin conduit. A surface of the fireproof layer 3 made of the hydraulic material has a protruding part 3A. The protruding part 3A is formed at a position corresponding to a division surface of a die which is used to form the fireproof layer made of the hydraulic material and is continuously formed in a ridge-like form along an axis of the synthetic resin conduit from one socket part 4 of the synthetic resin conduit to the other socket part 5.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a double-layered fire-resistant pipe and a manufacturing method thereof, and more particularly to a double-layered fire-resistant pipe in which cracks in the fire-resistant layer covering the outer periphery of a synthetic resin pipe are suppressed, and a manufacturing method thereof. [Background technology]

[0002] 2. Description of the Related Art Conventionally, there has been known a fire-resistant double-walled pipe in which the surface of a pipe made of a non-fire-resistant material is coated with a fire-resistant material in order to impart fire resistance to the pipe. A typical double-layer fireproof pipe is made by covering the outer periphery of a synthetic resin pipe, such as a polyvinyl chloride pipe, with a fire-resistant hydraulic material (hereinafter also referred to as "mortar").

[0003] Synthetic resin pipes such as polyvinyl chloride pipes are lighter than metal pipes and have excellent chemical resistance and impact resistance, and are therefore used for drainage pipes, ventilation pipes, and the like. However, since the synthetic resin pipe has poor fire resistance and is combustible, there is a risk of the fire spreading through the synthetic resin pipe in the event of a fire. For this reason, fire-resistant double-layer pipes, in which the outer circumference of a synthetic resin pipe is covered with mortar to impart fire resistance, are used as building materials.

[0004] However, in this double-layered fire-resistant pipe, cracks occur in the mortar coating the outer periphery of the synthetic resin pipe, and if the cracks are large, there is a risk that the pipe will not be able to exhibit the desired fire resistance. To solve this problem, a technique has been proposed in which a tape- or seal-like cushioning layer made of paper, resin, fiber, or the like is provided between the synthetic resin pipe and the mortar to prevent cracks (see Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-65768 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, as mentioned above, even when a technology such as that described in Patent Document 1 is adopted in which a tape- or seal-like cushioning layer made of paper, resin, fiber or the like is provided between the synthetic resin pipe and the mortar, cracks may occur in the mortar, particularly in the summer when temperatures are high.

[0007] Furthermore, the technique of providing a tape or seal-like cushioning layer of paper, resin, fiber, etc. between the synthetic resin pipe and the mortar as in Patent Document 1 has the problem of being labor-intensive and costly. To save this labor, automation using a tape winding machine is conceivable, but the cost of the tape winding machine is high, and even if a tape winding machine is introduced, it is difficult to automate the process. Thus, the technique of providing a tape or seal-like cushioning layer of paper, resin, fiber or the like between the synthetic resin pipe and the mortar not only increases the number of parts but also places a heavy burden on manufacturing.

[0008] Therefore, the inventors have intensively researched technology that can suppress the occurrence of cracks in the mortar of a double-layered fire-resistant pipe, other than the technology of providing a tape or seal-like cushioning layer of paper, resin, fiber, etc. between the synthetic resin pipe and the mortar.

[0009] Through this research, the inventors discovered that when mortar is formed on a synthetic resin pipe, the strength of the mortar joints (hereinafter also referred to as welds) is weaker than other parts due to insufficient bonding, which leads to subsequent cracks. The weld of the mortar is the part where the mortar flows join together and fuse inside the mold. Generally, the weld appears on the outer surface of the synthetic resin pipe along the parting surface of the mold, on the side opposite the injection port of the mold through which the mortar is injected.

[0010] The reason why the joining of the weld portion is insufficient is not clear, but the present inventors believe that the cause is as follows. Since the weld portion of the mortar corresponds to the position of the parting surface of the mold, when the mold is opened to remove the synthetic resin pipe covered with mortar, a tensile force acts on the mortar from the mold because the mold surface and the mortar are in close contact with each other. When a tensile force acts on the weld in the direction in which the mold opens (the direction in which the weld is separated), the bond at the weld weakens and becomes insufficient. In other words, the bond at the mortar part (fireproof layer part) corresponding to the position of the mold separation surface becomes insufficient, and cracks occur when heated thereafter. In addition, since the mortar does not harden in the mold, the synthetic resin pipe covered with the mortar is taken out of the mold in an unhardened state, which results in an insufficient bond at the welded portion of the mortar.

[0011] In this way, the inventors discovered that the bonding of the mortar welds was insufficient and that cracks occurred in such areas, and came up with the idea that by suppressing the tensile force, the occurrence of cracks in the mortar of a double-layered fire-resistant pipe can be suppressed, thereby completing the present invention.

[0012] The present invention has been made under the above circumstances, and an object of the present invention is to provide a double-layered fireproof pipe capable of suppressing cracks in the fireproof layer of the double-layered fireproof pipe, and a method for manufacturing the same. [Means for solving the problem]

[0013] The fireproof double-layered pipe according to the present invention, which has been made to achieve the above object, is a fireproof double-layered pipe in which a fireproof layer made of hydraulic material is formed on the outer peripheral surface of a synthetic resin pipe, and the fireproof layer made of hydraulic material has a convex portion on the surface thereof, the convex portion being formed at a position corresponding to a parting surface of a mold used when forming the fireproof layer made of hydraulic material, and the convex portion is formed at a position corresponding to a parting surface of a mold used when forming the fireproof layer made of hydraulic material, and the convex portion is formed at a position corresponding to a parting surface of a mold used when forming the fireproof layer made of hydraulic material, and the convex portion is formed at a position corresponding to a parting surface of a mold used when forming the fireproof layer made of hydraulic material, and the convex portion is formed at a position corresponding to a parting surface of a mold used when forming the fireproof layer made of hydraulic material, and the convex portion is formed at a position corresponding to a parting surface of a mold used when forming the fireproof layer made of hydraulic material, and the convex portion is formed at a position corresponding to a parting surface of a mold used when forming the fireproof layer made of hydraulic material, and the convex portion is formed at a position corresponding to a parting surface of a mold used for ... By The present invention is characterized in that the groove is formed continuously along the axis of the synthetic resin pipe in a ridge shape.

[0014] In the double-layered fireproof pipe according to the present invention, a convex portion is formed on the surface of the fireproof layer. This convex portion is formed at a position corresponding to the parting surface of the mold used when forming the fireproof layer of the hydraulic material. Furthermore, this convex portion is formed at a position corresponding to the parting surface of the mold used when forming the fireproof layer of the hydraulic material. By , which is formed continuously along the axis of the synthetic resin pipe in a ridge shape.

[0015] In this manner, in the two-layer fireproof pipe according to the present invention, convex portions are formed on the surface of the fireproof layer at positions corresponding to the parting surfaces of the mold. This is because the formation of recesses on the parting surfaces of the mold results in the formation of protrusions on the surface of the fireproof layer. In other words, the formation of recesses on the parting surfaces of the mold weakens the tensile force acting on the mortar from the mold, and the bonding strength of the welds in the mortar is maintained. Therefore, in the fire-resistant double-layer pipe of the present invention, a convex portion is formed on the surface of the fire-resistant layer at a position corresponding to the parting surface of the mold, and the bonding strength of the weld portion is maintained, thereby suppressing cracks in such portions.

[0016] The protrusion extends from one socket of the synthetic resin pipe to another socket. On the way, Since the ridge line is formed continuously along the axis of the synthetic resin pipe, cracks in the fireproof layer can be suppressed in the entire longitudinal region of the two-layer fireproof pipe. Moreover, since the convex portion is made of the same hydraulic material as the fire-resistant layer, it can be formed inexpensively and easily.

[0017] Here, it is preferable that the convex portions are formed in pairs at opposing positions on the outer peripheral surface of the fire-resistant layer. Also, it is preferable that the taper angle of the convex portions is 2 degrees or more and 63 degrees or less. Also, a tape cushioning material may be provided between the outer peripheral surface of the synthetic resin pipe and the fire-resistant layer.

[0018] The method for producing a double-layered fireproof pipe according to the present invention, which has been made to achieve the above object, is a method for producing a double-layered fireproof pipe in which a fireproof layer of a hydraulic material is formed on the outer peripheral surface of a synthetic resin pipe, and the method comprises the steps of: drawing a part of a mold for forming a fireproof layer of a hydraulic material on the outer peripheral surface of the synthetic resin pipe from one receiving portion of the synthetic resin pipe to another receiving portion of the synthetic resin pipe; By The present invention is characterized in that a recess for forming a convex portion made of a hydraulic material is formed along the axis of the synthetic resin pipe and in a ridge-like shape, and by placing the synthetic resin pipe in the mold and injecting a hydraulic material into the outer peripheral surface of the synthetic resin pipe, a fire-resistant layer made of a hydraulic material is formed on the outer peripheral surface of the synthetic resin pipe and the convex portion is formed on the surface of the fire-resistant layer.

[0019] In the method for manufacturing a double-layered fireproof pipe according to the present invention, a parting surface of a mold for forming a fireproof layer of a hydraulic material on the outer peripheral surface of a synthetic resin pipe is provided with a pipe from one receiving portion of the synthetic resin pipe to another receiving portion. On the way, A recess for forming a protrusion made of a hydraulic material is formed continuously along the axis of the synthetic resin pipe in a ridge shape. In this way, because a recess is formed on the parting surface of the mold, when the mold is opened to remove the mortar-coated synthetic resin pipe from the mold, the tensile force acting on the mortar from the mold can be weakened, and the bonding strength of the weld part of the mortar can be maintained. As a result, in the double-layered fireproof pipe according to the present invention, the mortar welds have sufficient bonding strength, so that cracks occurring in such portions can be suppressed.

[0020] The recess is also formed so that the synthetic resin pipe is inserted from one socket to another socket. By Since the grooves are formed continuously along the axis of the synthetic resin pipe in a ridge-like shape, cracks in the fireproof layer can be suppressed in all longitudinal regions of the double-layered fireproof pipe. Furthermore, by forming the recesses on the parting surface of the mold, it is possible to suppress cracks in the fireproof layer, so that cracks in the fireproof layer can be suppressed inexpensively and easily.

[0021] Here, it is preferable that the recesses are formed in pairs at positions opposite to each other. It is also preferable that a synthetic resin pipe is placed in the mold, a hydraulic material is injected into the outer peripheral surface of the synthetic resin pipe, a fireproof layer made of hydraulic material is formed on the outer peripheral surface of the synthetic resin pipe, and after forming the protrusions, a steam curing step is performed to promote hardening of the hydraulic material, and then a drying step is performed to harden the hydraulic material. Moreover, it is desirable that the taper angle of the convex portion is not less than 2 degrees and not more than 63 degrees.

[0022] In addition, a tape cushioning material may be formed on the surface of a synthetic resin pipe, the synthetic resin pipe with the tape cushioning material formed thereon is placed in the mold, and a hydraulic material is injected onto the outer peripheral surface of the synthetic resin pipe, thereby forming a fire-resistant layer made of a hydraulic material on the outer peripheral surface of the synthetic resin pipe and forming the convex portion on the surface of the fire-resistant layer. Effect of the Invention

[0023] According to the present invention, it is possible to obtain a double-layered fireproof pipe capable of suppressing cracks in the fireproof layer of the double-layered fireproof pipe and a method for manufacturing the same. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a side view showing one embodiment of a double-walled fire-resistant pipe according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II in FIG. [Diagram 3] FIG. 3 is a flow chart showing the steps of a method for manufacturing a double-layered fire-resistant pipe. [Figure 4] FIG. 4 is a top view showing an example of a mold used in the method for producing a double-layered fire-resistant pipe according to the present invention. [Diagram 5] FIG. 5 is a cross-sectional view taken along line II-II of FIG. [Figure 6] FIG. 6 is an enlarged view of a recess formed in the mold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. However, the present invention is not limited to the embodiment described below. In addition, in each drawing, the same or corresponding elements are appropriately assigned the same reference numerals. Furthermore, the drawings are schematic, and the dimensional relationship between each element, the ratio of each element, etc. are different from the actual ones.

[0026] First, one embodiment of a double-layered fire-resistant pipe according to the present invention will be described with reference to Fig. 1 and Fig. 2. Fig. 1 is a side view of the double-layered fire-resistant pipe, and Fig. 2 is a cross-sectional view taken along line II in Fig. 1. As shown in Figures 1 and 2, this double-layered fireproof pipe 1 has a double-layer structure in which a layer of fire-resistant hydraulic material (mortar) 3 is formed on the outer surface of a synthetic resin pipe 2 made of synthetic resin such as polyvinyl chloride. Moreover, this double-layered fireproof pipe 1 is an L-shaped pipe curved from one socket portion 4 to the other socket portion 5 (or it can be said to be a quarter-circular arc shape). The double-layered fireproof pipe 1 is not limited to this shape, and may be, for example, one in which two sockets are connected by a straight pipe, or one in which three sockets are connected by a T-shaped or Y-shaped pipe, instead of the two sockets. Also, the double-layered fireproof pipe 1 includes not only straight pipes but also joint pipes.

[0027] Convex portions 3A and 3B are formed on the surface of the fire-resistant layer 3. The convex portions 3A and 3B are made of the same hydraulic material as the fire-resistant layer 3 and are formed continuously in a ridge shape from one socket portion 4 of the synthetic resin pipe 2 to the other socket portion 5 along the axis O of the synthetic resin pipe.

[0028] The protrusions 3A, 3B are formed in pairs at opposing positions on the outer peripheral surface of the fire-resistant layer 3, as shown in FIG. This convex portion, which will be described in detail later, must be formed at least on the weld side opposite the injection port side of the mold through which the hard material is injected into the mold. More preferably, as described above, it is preferable to form a pair of convex portions on the injection port side of the mold through which the hydraulic material is injected into the mold and on the side opposite the injection port side.

[0029] 2, the protrusions 3A, 3B have the same substantially triangular cross section perpendicular to the axis O of the synthetic resin pipe 2, and are formed on the same plane F including the axis O of the synthetic resin pipe 2. In this way, the protrusions 3A, 3B are formed in pairs at positions facing each other with the same shape. The cross section of the protrusions 3A, 3B is not limited to a triangular shape, but may be a semicircular or trapezoidal shape.

[0030] The plane F on which the protrusions 3A and 3B are formed corresponds to the parting surface of the mold, that is, the protrusions 3A and 3B are formed on the parting line which is the parting surface of the mold. As described later in detail, the protrusions 3A and 3B are formed by recesses on the parting surface of the mold, and the recesses can reduce the tensile force acting on the mortar from the mold, thereby maintaining the bonding strength of the protrusions 3A and 3B. Therefore, in the fire-resistant double-layered pipe of the present invention, in which a convex portion is formed at a position corresponding to the parting surface of the mold, the bonding strength of the mortar weld portion is maintained and cracks in such portion are suppressed.

[0031] 2, when the ratio of the height W of the top of the convex portion to the length L of half the width of the convex portion is taken as W:L, the convex portion is formed to have a taper angle of W:L=1:20 to 0.5. When W:L=1:20 to 0.5 is expressed as a normal angle, it corresponds to a taper angle of approximately 2 degrees to 63 degrees. If the taper angle exceeds 0 degrees, convex portions 3A and 3B can be formed on the outer peripheral surface of the fire-resistant layer 3. However, in order to reduce the demolding resistance when removing the two-layer fire-resistant pipe from the mold and to suppress deformation of the two-layer fire-resistant pipe (molded product), it is preferable that the taper angle be approximately 2 degrees or more.

[0032] Furthermore, if the taper angle exceeds 63 degrees, the convex portions 3A, 3B will have a sharp shape, and chipping or the like will easily occur in the convex portions 3A, 3B, and cracks or the like will easily occur from the chipped portions. Therefore, the taper angle is preferably 63 degrees or less. More preferably, the taper angle is 60 degrees or less. Particularly preferably, W:L=1:10, which is a taper angle of about 5 to 6 degrees in normal angle notation, reduces the mold release resistance when removing the double-layered fireproof pipe, suppresses deformation of the double-layered fireproof pipe (molded product), makes it difficult for chips to occur in the protruding parts 3A and 3B, and further suppresses cracks in the fireproof layer.

[0033] Next, an embodiment of the method for producing a double-layered fire-resistant pipe according to the present invention will be described below with reference to a flow chart shown in FIG. First, a typical method for manufacturing a double-layered fireproof pipe will be described with reference to Fig. 3. As shown in the figure, the method for manufacturing a double-layered fireproof pipe 1 includes a mixing and kneading step (step S1) of hydraulic materials (raw materials), a step (step S2) of setting a synthetic resin pipe, a die molding step (step S3) of molding a fireproof layer on the outer circumferential surface of the synthetic resin pipe using a die, a steam curing step (step S4), and a drying step (step S5).

[0034] The mixing and kneading step (step S1) of hydraulic materials (raw materials) is a step of adding water to raw materials such as cement, aggregate, fibers, molding aids, and other additives, and mixing and kneading the materials. As the hydraulic material (raw material), a hydraulic substance that is fire-resistant, flame-retardant or non-combustible and does not lose its strength even at high temperatures, such as cement, gypsum, clay, diatomaceous earth, etc., is used. Preferably, mortar mainly made of cement, which is usually used in double-layered fireproof pipes, or fiber mortar mixed with short fibers, etc., is used because of its excellent practicality. The thickness of the fireproof layer 3 made of the fire-resistant hydraulic material varies depending on the diameter of the synthetic resin pipe 2, and is appropriately set so as to have the required strength and fire resistance. The mixing and kneading are carried out under known general conditions.

[0035] Next, a step (step S2) is performed of setting the synthetic resin pipe 2. As the synthetic resin pipe 2, for example, a synthetic resin pipe 2 such as a polyvinyl chloride pipe is generally used. The step of setting the synthetic resin pipe 2 (step S2) is a step of setting the synthetic resin pipe 2 which serves as the inner layer of the two-layer fire-resistant pipe 1 in a mold. At this time, a gap is formed between the inner peripheral surface of the mold and the outer peripheral surface of the synthetic resin pipe, and a hydraulic material (raw material) described later is injected into this gap.

[0036] Following the step of setting the synthetic resin pipe 2 (step S2), a step of molding with a metal mold (step S3) is carried out. In the die molding process (step S3), as described above, the hydraulic material (fire-resistant layer raw material) mixed and kneaded in step S1 is pressed into the gap between the synthetic resin pipe 2 and the die. The hydraulic material (fire-resistant layer raw material) pressed into the gap between the synthetic resin pipe 2 and the die covers the synthetic resin pipe 2 as a fire-resistant layer.

[0037] By the way, when the hydraulic material (raw material of the fireproof layer) that covers the synthetic resin pipe 2 is molded using a metal mold, unlike normal resin molding, the hydraulic material (raw material of the fireproof layer) does not harden inside the metal mold. For example, mortar is a hydraulic material, and water is added before it is pressed into a mold, but it is difficult to evaporate the water inside the mold. Therefore, the hydraulic material (the raw material of the fireproof layer) is removed from the mold before hardening is complete, and the hydraulic material (the raw material of the fireproof layer) is dried.

[0038] In this drying step, the coated synthetic resin pipe 2 is removed from the mold, and the hydraulic material (fire-resistant layer raw material) coating the synthetic resin pipe 2 may be allowed to dry naturally. However, in order to quickly achieve sufficient hardening strength, a steam curing step (step S4) is carried out prior to the drying step (step S5). This steam curing is performed using high-temperature steam under normal pressure. Then, a steam curing step (step S4) is performed, and after a drying step (step S5), a normal inspection is performed, and the double-layered fireproof pipe 1 is completed.

[0039] As described above, in the method for producing a double-layered fireproof pipe, the hydraulic material (fireproof layer raw material), for example, mortar, is removed from the mold in an insufficiently hardened state. As already mentioned, when unnecessary external forces (tensile forces) are applied to the fireproof layer during manufacturing (when opening the mold and when removing the double-layered fireproof pipe from the mold), the bonding strength of the welds in the mortar (fireproof layer) is weakened, causing cracks in the fireproof layer. Here, by forming the convex parts 3A and 3B on the outer peripheral surface of the fireproof layer 3 (forming the concave parts on the mold), the mold release resistance when opening the mold or removing the double-layered fireproof pipe from the mold can be reduced, and the weakening of the bonding strength of the mortar can be suppressed. As a result, the probability of cracks occurring in the fireproof layer can be reduced.

[0040] As already mentioned, the manufacturing method of the double-layered fireproof pipe according to the embodiment of the present invention is characterized in that a ridge-like convex portion is formed in the longitudinal direction from one receiving portion to the other receiving portion, and further characterized in that the double-layered fireproof pipe can be produced without applying any unnecessary external force (tensile force) to the fireproof layer during manufacturing (when opening the mold or when removing the double-layered fireproof pipe from the mold).

[0041] Fig. 4 is a top view showing an example of a mold used in a manufacturing method of a fire-resistant double-layered pipe, Fig. 5 is a cross-sectional view taken along line II-II in Fig. 4, and Fig. 6 is an enlarged view of a recess formed in the mold. Figs. 4 and 5 each show only one of a pair of molds.

[0042] 5, a cavity 10A is formed in a mold 10, and a synthetic resin pipe 2 is set in the cavity 10A at the position indicated by the dashed line in the figure. Then, a hydraulic material (fireproof layer raw material) is injected from an injection port 11 into a gap S between the synthetic resin pipe 2 and the mold 10. By using this mold 10, a hydraulic material (fire-resistant layer raw material), such as mortar, is pressed into the gap S between the synthetic resin pipe 2 and the mold 10, covering the synthetic resin pipe 2 as the outer layer of the fire-resistant double-layer pipe 1, and is molded into a predetermined shape.

[0043] The side opposite to the injection port 11 is called the weld portion 12. The hydraulic material (fireproof layer raw material) injected from the injection port 11 flows through the gap between the synthetic resin pipe 2 and the mold 10, splitting into left and right flows, and then joins at the weld portion 12. Mold 10 is provided with weld portion 12 and recess 14 on the side where injection port 11 is located (i.e., the side opposite weld portion 12, hereinafter referred to as injection port side 13). Since recess 14 is thus formed in weld portion 12 and injection port side 13, ridge-like protrusions 3A, 3B are formed in pairs at opposing positions on the outer circumferential surface. The recess 14 is for forming ridge-like protrusions 3A, 3B in the longitudinal direction from one socket portion of the double-layered fireproof pipe 1 to the other socket portion.

[0044] As shown in FIG. 5, the recess 14 is formed at the edge portion of the joining surface of the mold 10 . Therefore, the ridge-like protrusions 3A and 3B formed by the recess 14 are formed on the same plane (on the parting surface of the mold). That is, the ridge-like protrusions 3A and 3B are formed on the parting line of the mold.

[0045] As already mentioned for the convex portions 3A and 3B of the two-layer fireproof pipe 1, as shown in Fig. 6, if the ratio of the height W of the top of the concave portion 14 to the length L of half the width of the concave portion 14 is W:L, then W:L is set to 1:20 to 0.5. If W:L=1:20 to 0.5 is expressed as a normal angle, it corresponds to a taper angle of approximately 2 degrees to 63 degrees. If the taper angle of the recess 14 exceeds 0 degree, the protrusions 3A and 3B can be formed on the outer peripheral surface of the fireproof layer 3. However, by forming the recess 14, the mold release resistance can be reduced when opening the mold or when removing the two-layer fireproof pipe from the mold, and a taper angle of approximately 2 degrees or more is preferable to suppress deformation of the two-layer fireproof pipe (molded product).

[0046] Furthermore, if the taper angle of the recess 14 exceeds 63 degrees, the protrusions 3A, 3B will have a sharp shape, and chipping or the like will easily occur in the protrusions 3A, 3B, and cracks or the like will easily occur from the chipped parts. Therefore, the taper angle is preferably 63 degrees or less. More preferably, the taper angle is 60 degrees or less.

[0047] Here, it is particularly preferable that the taper angle be formed at W:L = 1:10, which is approximately 5 to 6 degrees in normal angle expression, thereby reducing the mold release resistance when opening the mold or removing the double-layered fireproof tube, making it difficult for chips to occur in the convex portions 3A and 3B without weakening the bonding strength of the double-layered fireproof tube (molded product), and further suppressing cracks in the fireproof layer. EXAMPLES

[0048] <Crack strength test> Next, an experiment was conducted on the crack strength of a double-layered fireproof pipe with a protrusion. In the cracking strength experiment, the temperature was raised in a heating furnace four weeks after curing to determine the temperature at which cracks occurred in the fireproof layer. The inner pipe of the double-layered fireproof pipe was a polyvinyl chloride pipe, and the fireproof layer was made of a hydraulic material consisting of cement, inorganic fine aggregate, organic fiber, and additives such as molding aids. Then, a polyvinyl chloride pipe was placed in a mold, and a hydraulic material was injected onto the outer peripheral surface of the polyvinyl chloride pipe, forming a fire-resistant layer of the hydraulic material and forming a convex portion on the outer peripheral surface of the polyvinyl chloride pipe. After that, steam curing was performed to promote the hardening of the hydraulic material, and then a drying process was performed to harden the hydraulic material.

[0049] The polyvinyl chloride pipe used in this experiment was a joint pipe with an outer diameter of 178 mm, and a fireproof layer with a thickness of 17 mm was formed. In addition, two protrusions 3A and 3B were formed as shown in Figure 1. The W:L ratio was set to 1:10. The length dimension of W was 1 mm, and the length dimension of L was 10 mm. The reason why the test was performed four weeks after curing was that the double-layered fireproof pipe is a cement product, and the test was performed when the pipe had completely hardened.

[0050] The target temperature is 60°C for 1 hour. Since 60°C is the maximum temperature at which polyvinyl chloride does not soften, if it can withstand 1 hour at this temperature, there will be no practical problems. Therefore, as shown in Table 1, we checked the occurrence of cracks at 45°C for 0.5 hours and 1 hour, 50°C for 0.5 hours and 1 hour, 55°C for 0.5 hours and 1 hour, and 60°C for 0.5 hours and 1 hour. The results are shown in Table 1. In Table 1, "◯" indicates that no cracks occurred, "×" indicates that cracks occurred, and "-" indicates that the experiment was not performed.

[0051] The following three types of samples were used in the experiment, five of each type. 1. There is a convex part and tape cushioning. 2. There is a protrusion and no tape cushioning material. 3. No protrusions and tape cushioning. The tape cushioning material is a conventional technology in which a tape cushioning material is inserted between polyvinyl chloride and mortar.

[0052] [Table 1]

[0053] As can be seen from Table 1 of the experimental results above, in the case of "3. No protrusions and with tape cushioning," which is the conventional technology, cracks occurred even at around 55°C. On the other hand, in "1. With convex portion and with tape cushioning" and "2. With convex portion and without tape cushioning", no cracks occurred even after exposure to 60°C for 1 hour. In this way, it was confirmed that by providing a convex portion (by providing a concave portion in the mold), it is not necessary to use the conventionally used tape cushioning material, and furthermore, the crack strength is improved.

[0054] Although the present invention has been described above based on the embodiments, the present invention is not limited to the above-mentioned embodiments. For example, even if a tape cushioning material is used, the effect of the present invention can be obtained as long as the tape cushioning material has the protrusion of the present invention, and the effect of the present invention is within the scope of the present invention. Furthermore, within the framework of the entire disclosure of the present invention, various combinations or selections (including partial deletions) of various disclosed elements (including each element of each claim, each element of each embodiment or example, each element of each drawing, etc.) are possible. In other words, the present invention includes various modifications and alterations that a person skilled in the art can make in accordance with the entire disclosure including the scope of the claims and the technical ideas. [Explanation of symbols]

[0055] 1 Fireproof double layer pipe 2. Synthetic resin pipes 3 Fireproof layer (water-hardening material: mortar) 3A Convex 3B Convex part 4,5 Socket part 10. Mold 11 Inlet 12 Weld side 13 Inlet side 14 Recess F plane O axis

Claims

1. A fire-resistant double-layer pipe in which a fire-resistant layer made of a hydraulic material is formed on the outer peripheral surface of a synthetic resin pipe, The fireproof layer of the hydraulic material has a protrusion on its surface, The convex portion is The hydraulic material is used for forming the fireproof layer, and the hydraulic material is formed at a position corresponding to the parting surface of the mold. The synthetic resin pipe is formed continuously from one socket portion to another socket portion along the axis of the synthetic resin pipe in a ridge shape. A fire-resistant double-layer pipe characterized by:

2. 2. The fire-resistant double-layer pipe according to claim 1, wherein the protrusions are formed in pairs at opposing positions on the outer peripheral surface of the fire-resistant layer.

3. 3. The fire-resistant double-walled pipe according to claim 1, wherein the convex portion has a taper angle of 2 degrees or more and 63 degrees or less.

4. 4. The fire-resistant double-layer pipe according to claim 1, wherein a tape cushioning material is provided between the outer peripheral surface of the synthetic resin pipe and the fire-resistant layer.

5. A method for manufacturing a double-layered fireproof pipe, comprising forming a fireproof layer made of a hydraulic material on the outer peripheral surface of a synthetic resin pipe, On the parting surface of the mold for forming a fireproof layer of hydraulic material on the outer surface of the synthetic resin pipe, A recess for forming a protrusion made of a hydraulic material is formed continuously along an axis of the synthetic resin pipe from one receiving portion to another receiving portion of the synthetic resin pipe in a ridge shape, A synthetic resin pipe is placed in the mold, and a hydraulic material is injected onto the outer peripheral surface of the synthetic resin pipe, A method for manufacturing a double-layered fireproof pipe, comprising forming a fireproof layer made of a hydraulic material on the outer peripheral surface of a synthetic resin pipe, and forming the convex portion on the surface of the fireproof layer.

6. 6. The method for producing a double-layered fire-resistant pipe according to claim 5, wherein the recesses are formed in pairs at positions opposite to each other.

7. A synthetic resin pipe is placed in the mold, and a hydraulic material is injected onto the outer peripheral surface of the synthetic resin pipe to form a fireproof layer made of a hydraulic material on the outer peripheral surface of the synthetic resin pipe and to form a convex portion. A steam curing step is carried out to accelerate the hardening of the hydraulic material; Then, a drying step is carried out to harden the hydraulic material.

7. The method for producing a double-layered fire-resistant pipe according to claim 5 or 6.

8. 8. The method for manufacturing a double-layered fireproof pipe according to claim 5, wherein the convex portion has a taper angle of 2 degrees or more and 63 degrees or less.

9. A tape cushioning material is formed on the surface of the synthetic resin pipe, The synthetic resin pipe on which the tape cushioning material is formed is placed in the mold, and a hydraulic material is injected onto the outer peripheral surface of the synthetic resin pipe, 9. The method for manufacturing a double-layered fireproof pipe according to claim 5, wherein a fireproof layer made of a hydraulic material is formed on the outer peripheral surface of the synthetic resin pipe, and the convex portion is formed on the surface of the fireproof layer.

Citation Information

Patent Citations

  • JP1991093692U

  • Synthetic resin pipe

    JP1996178136A

  • Fire resisting material covered pipe joint and method of making it

    JP2001235091A

  • Drain pipe or drain pipe joint of fireproof and sound insulation

    JP2005344925A

  • Method of manufacturing fire resistant double-layer pipe

    JP2008249028A