Positive electrode material and electrochemical and electronic devices containing the same

Optimizing cathode materials with controlled secondary particle size distributions addresses processability issues, improving cycle performance and stability in electrochemical devices by reducing particle flaws and enhancing uniformity.

JP7553353B2Active Publication Date: 2024-09-18NINGDE AMPEREX TECHNOLOGY LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2020518445
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-21
Publication Date
2024-09-18
Estimated Expiration
2040-01-21

AI Technical Summary

Technical Problem

Existing cathode materials, particularly high-nickel materials, suffer from poor processability, leading to uneven weight distribution and reduced cycle performance in electrochemical devices due to wide particle size distribution, which affects energy density and safety.

Method used

The cathode material is formulated with secondary particles having specific size distributions, including a first set larger than 1.25 times, a second set smaller than 0.75 times, and a third set between 0.75 to 1.25 times the average particle size, optimized through a two-stage stirring process to enhance uniformity and reduce particle flaws.

Benefits of technology

This approach improves the cycle performance and storage stability of electrochemical devices by minimizing particle flaws and bubbles during coating, ensuring uniform lithium and nickel content distribution, thereby enhancing kinetic and cycling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553353000004
    Figure 0007553353000004
  • Figure 0007553353000003
    Figure 0007553353000003
  • Figure 0007553353000005
    Figure 0007553353000005
Patent Text Reader

Abstract

The present application relates to a positive electrode material and an electrochemical device and an electronic device including the positive electrode material. The positive electrode material includes secondary particles formed from primary particles, and the secondary particles include a first set of secondary particles, a second set of secondary particles, and a third set of secondary particles. The particle size of the first set of secondary particles is greater than 1.25 times the average particle size of the secondary particles, the particle size of the second set of secondary particles is less than 0.75 times the average particle size of the secondary particles, and the particle size of the third set of secondary particles is 0.75 to 1.25 times the average particle size of the secondary particles. By using a positive electrode material that satisfies these particle size conditions, the electrochemical device of the present application has excellent cycle performance and storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of energy storage, and in particular to positive electrode materials and electrochemical and electronic devices including the same. [Background technology]

[0002] With the rapid development of mobile electronic technology, the frequency and experience of using mobile electronic devices such as mobile phones, tablets, laptops, drones, etc. are becoming more and more important. Therefore, electrochemical devices (e.g., lithium-ion batteries) that provide energy to electronic devices need to have higher energy density, higher rate, higher safety, and lower capacity fade after repeated charging and discharging processes.

[0003] The energy density and cycle performance of electrochemical devices are closely related to their positive electrode materials. In view of this, further research and improvement of positive electrode materials is being continued. In addition to the need for new positive electrode materials, the improvement and optimization of the material composition of positive electrode materials is also an important solution. Summary of the Invention [Problem to be solved by the invention]

[0004] SUMMARY OF THE DISCLOSURE The present application provides positive electrode materials and electrochemical and electronic devices including the positive electrode materials to at least partially address at least one problem existing in the related art. [Means for solving the problem]

[0005] According to one aspect of the present application, the present application provides a positive electrode material including secondary particles formed by primary particles, the secondary particles including a first set of secondary particles, a second set of secondary particles, and a third set of secondary particles, the particle size of the first set of secondary particles being greater than 1.25 times the average particle size of the secondary particles, the particle size of the second set of secondary particles being less than 0.75 times the average particle size of the secondary particles, and the particle size of the third set of secondary particles being 0.75 to 1.25 times the average particle size of the secondary particles.

[0006] According to another aspect of the present application, there is provided an electrochemical device including a negative electrode, a separator, and a positive electrode including the above-described positive electrode material.

[0007] According to another aspect of the present application, there is provided an electronic device including the electrochemical device described above. Effect of the Invention

[0008] The electrochemical device of the present application employs a positive electrode material that satisfies the above particle size conditions as the positive electrode, and improves the distribution of the positive electrode material during the positive electrode manufacturing process, so that the electrochemical device of the present application has excellent cycle performance and storage performance.

[0009] Additional aspects and advantages of the embodiments of the present application will be set forth in part in the following description, and / or will be illustrated by the practice of the embodiments of the present application. [Brief description of the drawings]

[0010] In order to describe the embodiments of the present application in detail, the drawings necessary for describing the embodiments of the present application or the prior art will be briefly described below. It is clear that the drawings described below are only a part of the embodiments of the present application. Those skilled in the art can obtain drawings of other embodiments based on the structures illustrated in these drawings without creative efforts.

[0011] [Figure 1] 1 is a 500x scanning electron microscope (SEM) image of a prior art positive electrode material. [Diagram 2]1 is a 500x scanning electron microscope (SEM) image of a positive electrode material according to an embodiment of the present application. [Diagram 3] FIG. 2 is a schematic diagram of the major and minor axes of a secondary particle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the present application will be described in detail. In the entire specification of the present application, the same or similar components and components having the same or similar functions are indicated by the same reference numerals. The embodiments described in this specification with reference to the drawings are exemplary and illustrative, and are used to provide a basic understanding of the present application. The embodiments of the present application should not be construed as limiting the present application.

[0013] In this specification, the terms "generally", "approximately", "substantially" and "about" are used to describe and explain small variations. When used in conjunction with an event or condition, the term can refer to an instance where the event or condition occurs exactly and an instance where the event or condition occurs very similarly. For example, when used in conjunction with a numerical value, the term can represent a variation range of ±10% or less of the numerical value, such as ±5% or less, ±4% or less, ±3% or less, ±2% or less, ±1% or less, ±0.5% or less, ±0.1% or less, or ±0.05% or less. For example, if the difference between two numerical values ​​is ±10% or less of the average value of the values ​​(e.g., ±5% or less, ±4% or less, ±3% or less, ±2% or less, ±1% or less, ±0.5% or less, ±0.1% or less, or ±0.05% or less), the two numerical values ​​are considered to be "substantially" the same.

[0014] Additionally, amounts, ratios, and other numerical values ​​may be expressed herein in a range format. Such range formats should be understood as being for convenience and brevity and should be understood with the flexibility to include not only the numerical values ​​expressly specified as being more limited in the range, but also to include all individual numerical values ​​or subranges contained within that range as if each numerical value and subrange were expressly specified.

[0015] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may refer to any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means A only, B only, or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means A only, B only, C only, A and B (excluding C), A and C (excluding B), B and C (excluding A), or all of A, B, and C. Item A may include one or more components. Item B may include one or more components. Item C may include one or more components.

[0016] In the detailed description and claims, the terms "major axis" and "minor axis" are used as a shorthand way of describing the meaning of sieve analysis of particle size, with the "major axis" being the maximum length of the particle in an image obtained by scanning electron microscope (SEM) examination, and the "minor axis" being the maximum length of the particle perpendicular to the "major axis" in the image. Additionally, the term "average particle size" is the average major axis value of the particles in an image obtained by scanning electron microscope examination. Note that particles defined by "major axis", "minor axis" or "average particle size" include either primary particles or secondary particles.

[0017] The present application adjusts the manufacturing process of the positive electrode material to limit the particle size distribution of the secondary particles of the positive electrode material to a small range, thereby improving the processing performance of the positive electrode material in the manufacturing process of the electrochemical device (e.g., high-speed coating), and further effectively improving the cycle performance of the electrochemical device. Currently, lithium cobalt oxide is widely used as the positive electrode material of electrochemical devices (e.g., lithium ion batteries), but cobalt is an element that causes large environmental pollution and is high in cost. Therefore, high-nickel materials (nickel content accounts for more than 50% of the content of all transition metal elements) have been widely paid attention because of their low cobalt content and higher actual gram capacity than lithium cobalt oxide. However, high-nickel materials have low processability and are prone to generate particles and bubbles when coated on the positive electrode, which leads to uneven weight distribution of the positive electrode, affecting the cycle performance and rate performance of the electrochemical device.

[0018] FIG. 1 is a 500x scanning electron microscope (SEM) image of a prior art cathode material (high nickel material) with a wide particle size distribution.

[0019] According to one aspect of the present application, an embodiment of the present application provides a cathode material including secondary particles formed by primary particles, in which the secondary particles include a first set of secondary particles, a second set of secondary particles, and a third set of secondary particles, in which the particle size of the first set of secondary particles is greater than about 1.25 times the average particle size of the secondary particles, the particle size of the second set of secondary particles is less than about 0.75 times the average particle size of the secondary particles, and the particle size of the third set of secondary particles is about 0.75 to about 1.25 times the average particle size of the secondary particles.

[0020] In some embodiments, the total number of the third set of secondary particles is about 60% or more, based on the total number of the secondary particles, and the total volume of the third set of secondary particles is about 50% or more, based on the total volume of the secondary particles.

[0021] In some embodiments, based on the total number of secondary particles, the total number of the third set of secondary particles is about 80% to about 93%, and the total number of the first set of secondary particles is about 1% to about 10%.

[0022] In some embodiments, based on the total volume of the secondary particles, the total volume of the third set of secondary particles is about 80% to about 95%, and the total volume of the first set of secondary particles is about 1% to about 10%.

[0023] In some embodiments, the ratio of the total number of the first set of secondary particles to the total number of the second set of secondary particles is about 0.1 to about 10, and the ratio of the total volume of the first set of secondary particles to the total volume of the second set of secondary particles is about 0.1 to about 10.

[0024] Figure 2 is a 500x scanning electron microscope (SEM) image of a positive electrode material having a particle size distribution according to an embodiment of the present application. As shown in Figure 2, the present application adjusts the manufacturing method of the positive electrode material to make the particle size distribution of the secondary particles of the positive electrode material more concentrated. In this specification, scanning electron microscope (SEM) is used to measure the particle number, average particle size, and shape (long axis and short axis).

[0025] Figure 3 is a schematic diagram of the long and short axes of secondary particles. As shown in Figure 3, the average particle size of the secondary particles of the positive electrode material is determined by taking the average value of the long axis a of each particle measured in the microscope image as the particle size, and at the same time, recording the short axis b perpendicular to the long axis a of each particle in the microscope image.

[0026] In some embodiments, based on the total number of secondary particles of the positive electrode particles, 80% or more of the secondary particles have a ratio of the length of the major axis a to the length of the minor axis b of about 1 to about 2. In other embodiments, 80% or more of the total number of secondary particles have a ratio of the length of the major axis a to the length of the minor axis b of, for example, about 1.0, about 1.2, about 1.4, about 1.5, about 1.6, about 1.8, about 2.0, or within a range consisting of any two of these values. According to the range of the ratio of the major axis a to the minor axis b of the secondary particles of the positive electrode material in the embodiments of the present application, the particle shape is improved, the fluidity of the slurry when coating the positive electrode material is improved, and the frictional force between the secondary particles during cold rolling is reduced, thereby improving the processability of the positive electrode material.

[0027] In some embodiments, the ratio of Dv10 to Dn10 of the secondary particles is about 1 to about 3. The closer the ratio of Dv10 to Dn10 of the secondary particles is to 1, the more concentrated the particle distribution is. In other embodiments, the ratio of Dv10 to Dn10 of the secondary particles is, for example, about 1.0, about 1.2, about 1.4, about 1.5, about 2.0, about 2.5, about 3.0, or within a range consisting of any two of these values.

[0028] By adopting a positive electrode material that satisfies the secondary particle size distribution of the embodiment of the present application, the occurrence rate of particle scratches and bubbles during high-speed coating can be reduced in the positive electrode manufacturing process of the present application. In addition, the manufacturing method of the positive electrode material of the present application can effectively suppress the generation of fine powder due to sintering and reduce the uneven distribution of lithium content and nickel content caused by large differences in particle size. The positive electrode material of the present application and the electrochemical device thereof have excellent cycle stability.

[0029] In some embodiments, the average particle size of the secondary particles of the positive electrode material is about 1 μm to about 30 μm. In other embodiments, the average particle size of the secondary particles is, for example, about 1 μm, about 5 μm, about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, or within a range consisting of any two of these values. The average particle size range of the positive electrode material of the embodiments of the present application can improve the kinetic performance of the positive electrode material and reduce the risk of negative reaction with the electrolyte.

[0030] In some embodiments, the length of the major axis of the primary particles constituting the secondary particles is from about 100 nm to about 5 μm, and the length of the minor axis of the primary particles is from about 10 nm to about 1 μm. In other embodiments, the length of the major axis of the primary particles is, for example, about 100 nm, about 200 nm, about 500 nm, about 1 μm, about 3 μm, about 5 μm, or within a range consisting of any two of these values. In other embodiments, the length of the minor axis of the primary particles is, for example, about 10 nm, about 50 nm, about 100 nm, about 200 nm, about 500 nm, about 800 nm, about 1 μm, or within a range consisting of any two of these values. The ranges of the lengths of the major and minor axes of the primary particles in the embodiments of the present application can improve the kinetic performance of the cathode material and improve the high-temperature storage performance and cycle performance of the electrochemical device.

[0031] In some embodiments, the shape of the primary particles includes, but is not limited to, one or more shapes such as plate-like, needle-like, rod-like, spherical, and ellipsoidal. In some embodiments, the crystal structure of the primary particles includes one or more of a hexagonal crystal structure, a spinel structure, and a rock salt structure, and the crystal structure belongs to the R-3m space group.

[0032] In some embodiments of the present application, the cathode material contains a lithium-containing metal oxide represented by the general formula Li x M1 y M2 z O2, where: 0.95 ≦ x ≦ 1.05, 0 < y ≦ 1, 0 ≦ z ≦ 0.1, y + z = 1, M1 is selected from the group consisting of Ni, Co, Mn, Al, and combinations thereof, and M2 is selected from the group consisting of Mg, Ti, Zr, Sc, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof.

[0033] The lithium-containing metal oxide (e.g., high-nickel material) has a concentrated particle size distribution and a large particle size, which ensures high battery capacity and further ensures the cycle stability of the material. It should be noted that, without departing from the spirit of the present invention, a person skilled in the art can select any common positive electrode active material in the field according to specific needs, but is not limited thereto.

[0034] In some embodiments, the secondary particles of the positive electrode material further comprise a surface layer comprising at least one of the elements B, Al, Zr, C, and S.

[0035] In some embodiments, the specific surface area of ​​the positive electrode material is about 0.300 m 2 / g ~ approx. 1.000m 2 / g.

[0036] In some embodiments, a method for producing the cathode material of the present application includes the following steps.

[0037] 1. Precursor Preparation The batch method is used to prepare the precursor. A certain amount of transition metal salt solution is mixed with an alkali liquid and an aqueous ammonia in a stoichiometric ratio to the substrate, and then injected into a reactor filled with nitrogen gas, and the pH value of the solution in the reactor is maintained within a certain range by adjusting the content of the aqueous ammonia. Then, the reaction solution in the reactor is stirred at a high speed at a stirring speed of about 600 rpm to about 1000 rpm, and the high speed stirring time is about 6 hours to about 15 hours. After the high speed stirring, the reaction solution is stirred at a low speed at a stirring speed of about 600 rpm to about 1000 rpm, and the low speed stirring time is about 12 hours to about 30 hours, and the reaction solution is aged to generate secondary particles. The obtained solid-liquid mixture is filtered, washed with water, and dried to obtain a precursor.

[0038] 2. Manufacturing of cathode materials A certain proportion of precursors are prepared and mixed with lithium salt and doping raw materials in a stoichiometric ratio of the base, and then primary sintering is performed, with the sintering temperature being about 750°C to about 830°C and the heat treatment time being about 8 hours to about 20 hours. After the primary sintering, the primary sintered product is washed with water and dried, and then mixed with the raw material for the surface layer to perform secondary sintering, with the sintering temperature being about 350°C to about 450°C and the heat treatment time being about 2 hours to about 10 hours, followed by cooling, drying, crushing and classification to obtain the positive electrode material.

[0039] In the present invention, a two-stage stirring method of high speed and low speed is adopted in the preparation of the precursor, and the stirring speed and time are controlled to achieve the effect of controlling the particle size distribution and shape of the secondary particles of the positive electrode material. The width of the distribution is simultaneously affected by the speed of high speed stirring and the time of low speed stirring, and the sphericity is mainly affected by the speed of high speed stirring. Both the stirring time and the stirring speed need to be controlled within a reasonable range. If the stirring time is too short, the small particles cannot grow sufficiently, and the effect of concentrating the particle size distribution cannot be obtained. If the stirring time is too long, the particle size of the entire primary particles is too large, which is unfavorable to the rate performance and wastes resources. If the stirring speed is too small, the reaction is insufficient, which is unfavorable to the formation of secondary particles with a concentrated particle size distribution and a spherical shape. If the stirring intensity is too large, the grown primary particles are easily broken, which generates fine powder, which is also unfavorable to the formation of secondary particles with a concentrated particle size distribution.

[0040] It should be understood that each step in the manufacturing method of the positive electrode material in the embodiment of the present application can be selected or replaced with other conventional processing methods in the field according to specific needs without departing from the spirit of the present application, but is not limited thereto.

[0041] According to another aspect of the present application, some embodiments of the present application further provide an electrochemical device including the cathode material of the present application. In some embodiments, the electrochemical device is a lithium ion battery. The lithium ion battery includes a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a positive electrode including the cathode material of the above embodiments.

[0042] In some embodiments, the positive electrode further includes a positive electrode current collector, and the negative electrode further includes a negative electrode current collector, where the positive electrode current collector may be an aluminum foil or a nickel foil, and the negative electrode current collector may be a copper foil or a nickel foil, although other positive electrode current collectors and negative electrode current collectors commonly used in the field can be used, and are not limited thereto.

[0043] In some embodiments, the negative electrode includes a negative electrode material capable of absorbing and releasing lithium (Li) (hereinafter, may be referred to as a "negative electrode material capable of absorbing / releasing lithium Li"). Examples of the negative electrode material capable of absorbing / releasing lithium (Li) may include carbon materials, metal compounds, oxides, sulfides, lithium nitrides such as LiN3, lithium metal, metals that form alloys with lithium, and polymeric materials.

[0044] In some embodiments, the positive electrode and the negative electrode may each independently further comprise at least one of an adhesive and a conductive agent.

[0045] In some embodiments, the adhesive comprises at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethylcellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, and styrene butadiene rubber. In some embodiments, the conductive agent comprises at least one of carbon nanotubes, carbon fibers, conductive carbon black, acetylene black, graphene, and ketjen black. It should be noted that those skilled in the art can select common adhesives and conductive agents according to actual needs, but are not limited thereto.

[0046] In some embodiments, the separator includes at least one selected from, but not limited to, polyethylene, polypropylene, polyethylene terephthalate, polyimide, and aramid. For example, the polyethylene includes at least one component selected from high density polyethylene, low density polyethylene, and ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have excellent short circuit prevention properties and can improve the stability of the battery due to the shutdown effect.

[0047] The lithium ion battery of the present application further includes an electrolyte, which may be one or more of a gel electrolyte, a solid electrolyte, and an electrolyte solution, the electrolyte solution including a lithium salt and a non-aqueous solvent.

[0048] In some embodiments, the lithium salt is one or more selected from LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB, and lithium difluoroborate. For example, LiPF6 is employed as the lithium salt because LiPF6 provides high ionic conductivity and can improve cycle performance.

[0049] The non-aqueous solvent may be a carbonate compound, a carboxylic acid ester compound, an ether compound, another organic solvent, or a combination thereof.

[0050] The carbonate compound may be a chain carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound, or a combination thereof.

[0051] Examples of such other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, phosphate esters, and combinations thereof.

[0052] In some embodiments, the non-aqueous solvent is selected from the group consisting of ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate, acetic acid methyl ester, ethyl propionate, and combinations thereof.

[0053] In addition, the manufacturing method of the positive electrode, negative electrode, separator, and lithium ion battery in the examples of the present application can be selected from any suitable conventional methods in the field according to specific needs without departing from the spirit of the present application, but is not limited thereto. In one embodiment of the method for manufacturing an electrochemical device, the manufacturing method of a lithium ion battery includes winding, folding or stacking the positive electrode, separator, and negative electrode in the above examples in order to form an electrode assembly, placing the electrode assembly in, for example, an aluminum plastic film, injecting an electrolyte, and then vacuum sealing, leaving, forming, shaping, and other processes to obtain a lithium ion battery.

[0054] Although the lithium ion battery has been described as an example, those skilled in the art can understand after reading this application that the positive electrode material of the present application can be applied to other suitable electrochemical devices. Such electrochemical devices include any device that performs an electrochemical reaction, and specific examples include all kinds of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors. In particular, the electrochemical device is a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0055] Some embodiments of the present application further provide an electronic device that includes the electrochemical device of the embodiments of the present application.

[0056] The electronic device of the embodiment of the present application is not particularly limited and may be any electronic device known in the art. In some embodiments, the electronic device may include, but is not limited to, a notebook computer, a pen-input computer, a mobile computer, an electronic book player, a mobile phone, a mobile fax machine, a mobile copy machine, a mobile printer, a headphone stereo, a video movie machine, a liquid crystal television, a handy cleaner, a portable CD, a mini disk, a walkie-talkie, an electronic organizer, a calculator, a memory card, a portable tape recorder, a radio, a backup power source, a motor, an automobile, a motorcycle, a motorized bicycle, a bicycle, a lighting device, a toy, a game device, a clock, an electric tool, a flash, a camera, a large-scale household battery, and a lithium-ion capacitor. EXAMPLES

[0057] In the following, some specific examples and comparative examples are presented to better illustrate the technical solution of the present application, in which the positive electrode material is subjected to laser particle size analysis and scanning electron microscope test, and the electrochemical device (lithium ion battery) is subjected to cycle performance test, cycle expansion rate test, and storage expansion rate test.

[0058] 1. Test method 1.1 Laser particle size analysis: Laser particle size measurement uses the principle that particles of different sizes scatter the laser with different intensities to measure particle distribution. The main indices that characterize the particle size characteristics of particles are Dn10, Dv10, Dv50, Dv90, Dv99, etc., where Dv50 is called particle size and indicates the particle size of the material when the volume accumulation of the particle size distribution from the small particle size side reaches 50% of the total volume in the volume-based particle size distribution, Dv10 is called 10% cumulative particle size and indicates the particle size when the volume accumulation of the particle size distribution reaches 10% of the total volume, and Dn10 is called 10% cumulative quantity particle size and indicates the particle size of the material when the quantity accumulation of the particle size distribution from the small particle size side reaches 10% of the total quantity in the quantity-based particle size distribution. In the examples and comparative examples of this application, the particle size of the sample particles is analyzed using a Mastersizer 2000 laser particle size distribution analyzer. A sample of the positive electrode material is dispersed in 100 mL of dispersant (deionized water) and the light shielding degree is set to 8 to 12%. The sample is then sonicated for 5 minutes at an ultrasonic intensity of 40KHz and 180W. After sonication, the sample is subjected to laser particle size distribution analysis to obtain particle size distribution data.

[0059] 1.2 Scanning electron microscope test: After imaging the positive electrode materials of the present application and comparative examples with a 500x scanning electron microscope (Germany ZEISS Sigma-02-33), about 200 to about 600 secondary particles of the positive electrode material with perfect shape and no obstruction are randomly selected from the electron microscope image, and the maximum length a (long axis) in the electron microscope image of the secondary particles is taken as the particle size, and the maximum length b (short axis) perpendicular to the long axis of each particle in the microscope image is recorded, and the volume of the secondary particles and the corresponding quantity are recorded. Then, 10 different regions of the positive electrode material are randomly selected and imaged, and 10 different electron microscope images are obtained, and the above steps are repeated to calculate the average particle size of all the secondary particles, and the average particle size of the secondary particles of the positive electrode material, the distribution of the volume and quantity of the secondary particles, and the ratio of the number or volume of each of the first set of secondary particles, the second set of secondary particles, and the third set of secondary particles to the total number or volume of the secondary particles are obtained.

[0060] 1.3 Cycle Performance Test: The lithium ion batteries of the following Examples and Comparative Examples are placed in an incubator at 45°C±2°C and left to stand for 2 hours, then charged at a constant current of 1.5C to 4.25V, then charged at a constant voltage of 4.25V to 0.02C and left to stand for 15 minutes, and then discharged at a constant current of 4.0C to 2.8V. This is considered as one charge-discharge cycle process, and the discharge capacity of the first cycle of the lithium ion battery is recorded. Then, the charge-discharge cycle process is repeated 500 times using the above method, and the discharge capacity after 500 cycles is recorded.

[0061] Four lithium-ion batteries are taken out from each set, and the average capacity retention of the lithium-ion batteries is calculated. Cycle retention of lithium-ion batteries = discharge capacity after 500 cycles (mAh) / discharge capacity after 1 cycle (mAh) x 100%.

[0062] 1.4-cycle expansion rate test: The thickness of the lithium ion battery after 500 cycles is measured using a thickness measuring device, and the thickness change after 500 cycles according to the above cycle measurement is recorded. Four lithium ion batteries are taken out from each set, and the cycle expansion rate of the lithium ion battery after 500 cycles is calculated.

[0063] Cycle expansion rate = (thickness of lithium-ion battery after 500 cycles / thickness of new lithium-ion battery-1) x 100%.

[0064] 1.5 Storage expansion rate test: The lithium ion batteries of the following examples and comparative examples are placed in an incubator at 25°C ± 2°C and left for 2 hours, then charged at a constant current of 1.5C to 4.25V, and then charged at a constant voltage of 4.25V to 0.05C, and then placed in an incubator at 85°C ± 2°C and left for 12 hours. After storage at high temperature, the thickness of the lithium ion batteries stored at high temperature is measured using a thickness measuring device, and the change in thickness after storage at high temperature is recorded. Four lithium ion batteries are taken out from each set to calculate the high temperature storage expansion rate of the lithium ion batteries.

[0065] High temperature storage expansion rate = (thickness of lithium ion battery after high temperature storage / thickness of new lithium ion battery - 1) x 100%

[0066] 2. Manufacturing method 2.1 Manufacturing of positive electrode sheet The positive electrode materials of the following examples and comparative examples are dissolved in N-methylpyrrolidone (NMP) solution together with acetylene black and polyvinylidene fluoride in a weight ratio of 94:3:3 to form a positive electrode slurry. Aluminum foil is used as the positive electrode current collector, and the positive electrode slurry is coated on the positive electrode current collector, followed by drying, cold rolling and cutting processes to obtain a positive electrode sheet.

[0067] 2.2 Manufacture of negative electrode sheet Artificial graphite, acetylene black, styrene butadiene rubber, and sodium carboxymethyl cellulose are dissolved in deionized water in a weight ratio of 96:1:1.5:1.5 to form a negative electrode slurry. Copper foil is used as the negative electrode current collector, and the negative electrode slurry is coated on the negative electrode current collector, which is then dried, cold-rolled, and cut to obtain a negative electrode sheet.

[0068] 2.3 Separator manufacturing Polyvinylidene fluoride is dissolved in water and a uniform slurry is formed by mechanical stirring. The slurry is then coated on both sides of a porous substrate (polyethylene) that is also coated on both sides with a ceramic coating layer, and the substrate is dried to form a separator.

[0069] 2.4 Preparation of electrolyte In an environment where the water content is less than 10 ppm, lithium hexafluorophosphate and a nonaqueous organic solvent (ethylene carbonate (EC): diethyl carbonate (DEC): propylene carbonate (PC): propyl propionate (PP): vinylene carbonate (VC) = 20:30:20:28:2 (weight ratio)) are prepared in a weight ratio of 8:92 to form an electrolyte solution.

[0070] 2.5 Lithium-ion battery production The positive electrode sheet, the separator, and the negative electrode sheet are laminated in this order, and a separator is placed between the positive electrode sheet and the negative electrode sheet to provide a separating function, and then the electrode assembly is wound up. The electrode assembly is then placed in an aluminum plastic film packaging bag, and moisture is removed at 80°C to obtain a dry electrode assembly. The electrolyte is then injected into the dry electrode assembly, and the process of vacuum sealing, standing, chemical conversion, shaping, etc. is carried out to complete the manufacture of the lithium ion battery in each of the following examples and comparative examples.

[0071] [Example 1] Batch method: Nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O) and manganese sulfate (MnSO4·H2O) are added to Ni 0.8 Co 0.1 Mn 0.1 The three solutions are mixed in a stoichiometric ratio of (OH)2 to prepare a mixed salt solution, and 1M sodium hydroxide solution (NaOH) and 1M ammonia solution (NH3·H2O) are prepared as alkaline solutions. After filling the reactor with water and nitrogen gas, the above three solutions are added and the pH value in the reactor is maintained at approximately 11.0±0.1. After that, the mixture is stirred at high speed for 12 hours at a rotation speed of 800 rpm. After high-speed stirring, the mixture is stirred at low speed for 24 hours at a rotation speed of 300 rpm. The resulting solid-liquid mixture is filtered, washed with water, and dried to obtain the precursor.

[0072] The obtained precursor, LiOH, and Al2O3 were mixed with LiNi 0.8 Co 0.08 Mn 0.1 Al 0.02 The primary sintering is carried out at 780℃ in an oxygen atmosphere for 12 hours, and the primary sintering is carried out after washing and drying to obtain the primary sintered material. The primary sintered material is uniformly mixed with boric acid (H3BO3) and the secondary sintering is carried out at 400℃ in an oxygen atmosphere for 5 hours, and the positive electrode material is obtained after screening.

[0073] [Example 2] The manufacturing method is the same as that of Example 1, but the difference is that in Example 2, high-speed stirring is performed at a rotation speed of 600 rpm.

[0074] [Example 3] The manufacturing method is the same as that of Example 1, but the difference is that in Example 3, high-speed stirring is performed at a rotation speed of 700 rpm.

[0075] [Example 4] The manufacturing method is the same as that of Example 1, but the difference is that in Example 4, high-speed stirring is performed at a rotation speed of 900 rpm.

[0076] [Example 5] The manufacturing method is the same as that of Example 1, but the difference is that in Example 5, high-speed stirring is performed at a rotation speed of 1000 rpm.

[0077] [Example 6] The manufacturing method is the same as that of Example 1, but the difference in Example 6 is that the high-speed stirring time is 6 hours.

[0078] [Example 7] The manufacturing method is the same as that of Example 1, but the difference in Example 7 is that the high-speed stirring time is 9 hours.

[0079] [Example 8] The manufacturing method is the same as that of Example 1, but the difference in Example 8 is that the high-speed stirring time is 15 hours.

[0080] [Example 9] The manufacturing method is the same as that of Example 1, except that in Example 9, low-speed stirring is performed at a rotation speed of 200 rpm.

[0081] [Example 10] The manufacturing method is the same as that of Example 1, except that in Example 10, low-speed stirring is performed at a rotation speed of 400 rpm.

[0082] [Example 11] The manufacturing method is the same as that of Example 1, but the difference in Example 11 is that the low speed stirring time is 12 hours.

[0083] [Example 12] The manufacturing method is the same as that of Example 1, but the difference in Example 12 is that the low speed stirring time is 18 hours.

[0084] [Example 13] The manufacturing method is the same as that of Example 1, but the difference in Example 13 is that the low speed stirring time is 30 hours.

[0085] [Example 14] The manufacturing method is the same as in Example 1, but in Example 14, nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and manganese sulfate (MnSO4·H2O) were used instead of Ni 0.6 Co 0.2 Mn 0.2 The precursor, LiOH, and Al2O3 were mixed in a stoichiometric ratio to form a mixed salt solution, and the resulting precursor was mixed with LiNi 0.6 Co 0.18 Mn 0.2 Al 0.02 The difference is that O2 is mixed in a stoichiometric ratio.

[0086] [Example 15] The manufacturing method is the same as in Example 1, but in Example 15, nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and manganese sulfate (MnSO4·H2O) were used instead of Ni 0.5 Co 0.2 Mn 0.3 The precursor, LiOH, and Al2O3 were mixed in a stoichiometric ratio to form a mixed salt solution, and the resulting precursor was mixed with LiNi 0.5 Co 0.18 Mn 0.3 Al 0.02 The difference is that O2 is mixed in a stoichiometric ratio. Comparative Example 1

[0087] [Comparative Example 1] Continuous method: Nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O) and manganese sulfate (MnSO4·H2O) were 0.8 Co 0.1 Mn 0.1The three solutions are mixed in a stoichiometric ratio of (OH)2 to prepare a mixed salt solution, and 1M sodium hydroxide solution (NaOH) and 1M ammonia solution (NH3·H2O) are prepared as alkaline solutions. After filling the reactor with water and nitrogen gas, the above three solutions are added and the pH value in the reactor is maintained at approximately 11.0±0.1. Then, the mixture is continuously stirred for 48 hours at a rotation speed of 600 rpm. After continuous stirring, the resulting solid-liquid mixture is filtered, washed with water, and dried to obtain the precursor.

[0088] The obtained precursor, LiOH, and Al2O3 were mixed with LiNi 0.8 Co 0.08 Mn 0.1 Al 0.02 The primary sintering is carried out at 780℃ in an oxygen atmosphere for 12 hours, and the primary sintering is carried out after washing and drying to obtain the primary sintered material. The primary sintered material is uniformly mixed with boric acid (H3BO3) and the secondary sintering is carried out at 400℃ in an oxygen atmosphere for 5 hours, and the positive electrode material is obtained after screening.

[0089] [Comparative Example 2] The production method is the same as that of Comparative Example 1, but in Comparative Example 2, the solution in the reactor is continuously stirred at a rotation speed of 800 rpm for 24 hours.

[0090] The positive electrode materials of the above examples and comparative examples were subjected to laser particle size measurement and scanning electron microscope test, and the test results were recorded. Then, a new positive electrode sheet was manufactured, and the thickness, width, length and weight of the new positive electrode sheet were measured using a thickness measuring device. Then, the lithium ion battery was subjected to limit compression density measurement, cycle performance test and storage expansion rate test, and the test results were recorded.

[0091] The statistical values ​​of the positive electrode materials of Examples 1 to 15 and Comparative Examples 1 and 2, as well as the results of the laser particle size measurement and the scanning electron microscope test, are shown in Table 1 below.

[0092] [Table 1]

[0093] The test results of the cycle performance test, cycle expansion rate test, and high-temperature storage expansion rate test for the lithium ion batteries of Examples 1 to 15 and Comparative Examples 1 and 2 are shown in Table 2 below.

[0094] [Table 2]

[0095] As shown in Table 1, in Examples 1 to 15 of the present application, the batch method is adopted: the precursor formed by high-speed stirring and low-speed stirring can effectively control the particle size range of the secondary particles of the positive electrode material. Specifically, as can be seen by comparing the quantity ratio and volume ratio of the third group of secondary particles among the secondary particles of the examples and comparative examples, the particle size distribution of the positive electrode material of the examples of the present application is relatively concentrated, and in Example 1, the quantity ratio of the third group of secondary particles can be achieved at 93% and the volume ratio at 95%. It should be noted that the Dv10 / Dn10 value of the positive electrode material in the examples of the present application is close to 1, indicating that the particle size distribution of the positive electrode material of the examples is relatively concentrated or uniform, that is, indicating that the content of fine particles in the positive electrode material of the examples of the present application is low. In contrast, the Dv10 / Dn10 values ​​of the positive electrode materials of Comparative Examples 1 and 2 are all greater than 10, indicating that a large amount of fine particles exists in the positive electrode materials of Comparative Examples 1 and 2. Furthermore, as can be seen by comparing Comparative Examples 1 to 5 with Comparative Examples 1 to 2, the ratio of the long axis a to the short axis b of the secondary particles of the positive electrode material is affected by the stirring speed of the high-speed stirring of the positive electrode material, and the higher the stirring speed, the higher the sphericity of the secondary particles.

[0096] As can be seen from Tables 1 and 2, compared with Comparative Examples 1 and 2, the lithium ion batteries having the positive electrode material of the present application in Examples 1 to 15 of the present application have significantly improved cycle performance and storage performance. As can be seen by comparing Comparative Examples 1 and 2 with Examples 1 to 15, the lithium ion batteries using the positive electrode material having the particle size distribution of the Examples of the present application can effectively maintain a cycle retention rate of 70% or more in the cycle test, and in the cycle expansion rate test and storage expansion rate test, compared with Comparative Examples 1 and 2, the lithium ion batteries of Examples 1 to 15 of the present application have significantly reduced cycle expansion rate and high temperature storage expansion rate. This indicates that the positive electrode material of the present application can make the weight distribution of the positive electrode material of the positive electrode more uniform through a specific particle size distribution, and further obtain optimal dynamic performance. In addition, the positive electrode material of the present application can reduce the content of large particles and fine particles in the positive electrode material and avoid uneven reaction or excessive reaction between the positive electrode material and the electrolyte, thereby improving the cycle performance of the lithium ion battery and reducing gas generation during high temperature storage of the positive electrode material.

[0097] Comparison of the above examples and comparative examples reveals that the positive electrode material of the present application can effectively obtain a lithium ion battery having good cycle performance and stable storage performance by controlling the total quantity ratio and total volume ratio of the secondary particles of the third group in the positive electrode material.

[0098] References throughout the specification to "some embodiments," "some embodiments," "one embodiment," "another example," "an example," "particular example," or "partial example" mean that at least one embodiment or example of the application includes the particular feature, structure, material, or characteristic described in that embodiment or example. Thus, descriptions appearing in various portions throughout the specification, such as "in some embodiments," "in an embodiment," "in one embodiment," "in another example," "in one example," "in a particular example," or "in an example," do not necessarily refer to the same embodiment or example of the application. Furthermore, particular features, structures, materials, or characteristics herein may be combined in any suitable manner in one or more embodiments or examples.

[0099] Although exemplary embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limiting the present application, and that changes, substitutions and modifications can be made to the embodiments without departing from the spirit, principles and scope of the present application. <Additional Notes> The present invention includes the following aspects. <Section 1> The secondary particles are formed by the primary particles, the secondary particles being a first set of secondary particles having a particle size greater than 1.25 times the average particle size of the secondary particles; a second set of secondary particles having a particle size less than 0.75 times the average particle size of the secondary particles; A third set of secondary particles having a particle size of 0.75 to 1.25 times the average particle size of the secondary particles; A positive electrode material comprising: <Section 2> Item 2. The positive electrode material according to item 1, wherein the total number of the secondary particles of the third group is 60% or more, calculated based on the total number of the secondary particles. <Section 3> Item 2. The positive electrode material according to item 1, wherein the total volume of the third set of secondary particles is 50% or more, calculated based on the total volume of the secondary particles. <Section 4> The secondary particles are (a) the ratio of Dv10 to Dn10 of the secondary particles is 1 to 3; (b) 80% or more of the secondary particles, calculated based on the total number of the secondary particles, have a ratio of the length of their major axis to their minor axis of 1 to 2; (c) the average particle size of the secondary particles is 1 μm to 30 μm The positive electrode material according to item 1, which satisfies at least one of the following characteristics. <Section 5> Item 2. The positive electrode material according to item 1, wherein the crystal structure of the primary particles includes one or more of a hexagonal structure, a spinel structure, and a rock salt structure, and the crystal structure belongs to an R-3 space group. <Section 6> (a) the total number of the secondary particles of the third set is 80% to 93% and the total number of the secondary particles of the first set is 1% to 10%, calculated based on the total number of the secondary particles; (b) the total volume of the third set of secondary particles is 80% to 95% and the total volume of the first set of secondary particles is 1% to 10%, calculated based on the total volume of the secondary particles; (c) the ratio of the total number of the first set of secondary particles to the total number of the second set of secondary particles is 0.1 to 10, and the ratio of the total volume of the first set of secondary particles to the total volume of the second set of secondary particles is 0.1 to 10. The positive electrode material according to item 1, which satisfies at least one of the following characteristics. <Section 7> General formula Li x M1 y M2 z O 2 represented by the formula: 0.95 ≦ x ≦ 1.05, 0 < y ≦ 1, 0 ≦ z ≦ 0.1, y + z = 1, M1 is selected from the group consisting of Ni, Co, Mn, Al, and combinations thereof, and M2 is selected from the group consisting of Mg, Ti, Zr, Sc, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof, the cathode material according to item 1, comprising a lithium-containing metal oxide. <Item 8> The secondary particles further comprise a surface layer containing at least one element of B, Al, Zr, C, and S, the cathode material according to item 1. <Item 9> Specific surface area is 0.300 m 2 / g to 1.000 m 2 / g, the cathode material according to item 1. <Item 10> An anode, A separator, An electrochemical device comprising a cathode containing the cathode material according to any one of items 1 to 9. <Item 11> An electronic device comprising the electrochemical device according to item 10.

Claims

1. The secondary particles are formed by the primary particles, the secondary particles being a first set of secondary particles having a particle size greater than 1.25 times the average particle size of the secondary particles; a second set of secondary particles having a particle size less than 0.75 times the average particle size of the secondary particles; a third set of secondary particles having a particle size between 0.75 and 1.25 times the average particle size of the secondary particles; Including, Calculated based on the total number of the secondary particles, the total number of the third group of secondary particles is 80% to 93%, and the total number of the first group of secondary particles is 1% to 10%; Calculated based on the total number of the secondary particles, 80% or more of the secondary particles have a ratio of the length of their major axis to their minor axis of 1 to 1.5; The ratio of Dv10 to Dn10 of the secondary particles is 1.0 to 1.9; The positive electrode material comprises a lithium-containing metal oxide in which the nickel content is 50% or more of the content of all transition metal elements; The positive electrode material, wherein the secondary particles have an average particle size of 5 μm to 30 μm.

2. 2. The cathode material of claim 1, wherein a total volume of the third set of secondary particles is 50% or more, calculated based on the total volume of the secondary particles.

3. 2. The cathode material of claim 1, wherein the crystal structure of the primary particles comprises one or more of a hexagonal structure and a rock salt structure, and the crystal structure belongs to an R-3 space group. (a) a total volume of the third set of secondary particles is 80% to 95% and a total volume of the first set of secondary particles is 1% to 10%, calculated based on the total volume of the secondary particles; (b) the ratio of the total number of the first set of secondary particles to the total number of the second set of secondary particles is 0.1 to 10, and the ratio of the total volume of the first set of secondary particles to the total volume of the second set of secondary particles is 0.1 to 10. The positive electrode material according to claim 1 , which satisfies at least one of the following characteristics:

5. The lithium-containing metal oxide has the general formula Li x M1 y M2 z O 2 wherein: 0.95≦x≦1.05, 0<y≦1, 0≦z≦0.1, y+z=1; M1 is selected from the group consisting of Ni, Co, Mn, Al, and combinations thereof; and M2 is selected from the group consisting of Mg, Ti, Zr, Sc, V, Cr, Fe, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof, and the nickel content accounts for 50% or more of the content of all transition metal elements.

6. 2. The cathode material of claim 1, wherein the secondary particles further comprise a surface layer comprising at least one element of B, Al, Zr, C, and S.

7. Specific surface area is 0.300m 2 / g to 1.000m 2 / g.

8. A negative electrode; A separator; and a positive electrode comprising the positive electrode material according to any one of claims 1 to 7.

9. An electronic device comprising the electrochemical device of claim 8 .

Citation Information

Patent Citations

  • Transition metal composite hydroxide particles, production method thereof, positive electrode active material for lithium ion secondary battery, production method thereof, and lithium ion secondary battery

    JP2019077577A