Manufacturing method of electroplated abrasive tools

By using an acidic solution to roughen and etch aluminum-based materials, the method addresses the bonding strength issue in electrodeposited abrasive tools, enabling partial plating and enhancing bonding strength without strong alkaline treatments.

JP7553382B2Active Publication Date: 2024-09-18株式会社ジェイテクトグラインディングツール
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021028064
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-09-18
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

The bonding strength between aluminum-based materials and plating layers in electrodeposited abrasive tools is insufficient, making it difficult to apply double zincate treatment, which is strongly alkaline and complicates partial plating, thus preventing the formation of a roughened surface.

Method used

A method using an acidic solution containing copper ions to dissolve and roughen the aluminum-based base material, followed by selective etching and base plating, allowing for partial masking and increased bonding strength without strong alkaline solutions.

Benefits of technology

This method enables partial plating and enhances bonding strength between the base material and abrasive grains, reducing tool weight and improving handling properties while ensuring high bonding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553382000005
    Figure 0007553382000005
  • Figure 0007553382000006
    Figure 0007553382000006
  • Figure 0007553382000004
    Figure 0007553382000004
Patent Text Reader

Abstract

To provide a manufacturing method for an electro-deposition abrasive grain tool which adopts aluminum or an aluminum alloy for the base material and can enhance a bond strength with a plating layer for fixing the base material with abrasive grains.SOLUTION: A manufacturing method for an electro-deposition abrasive grain tool 1 includes a base material coarsening step S3 for melting the surface of a base material 10 and for substituting the surface of the base material 10 with copper serving as substitution metal by bringing the base material 10 with an acidic solution which contains copper ions and melts aluminum or an aluminum alloy, a substitution etching step S5 for exposing a coarsening surface 10a of the base material 10 by selectively etching the substitution metal in the surface of the base material 10 by means of the acidic solution, a ground plating step S10 for forming a ground plated layer 31 on the coarsening surface 10a of the base material 10, and abrasive grain fixing steps S11 - S13 for disposing abrasive grains 20 on the surface of the ground plated layer 31, and for forming a fixed plated layer 32 for fixing the abrasive grains 20.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an electroplated abrasive tool. [Background technology]

[0002] Patent Document 1 describes an electroplated abrasive tool in which abrasive grains such as diamond or CBN are fixed to the surface of a base material (also called a base metal) made of an iron-based material by nickel plating. Patent Document 2 also describes a similar electroplated abrasive tool.

[0003] In recent years, from the viewpoint of weight reduction, the use of aluminum or aluminum alloys as the substrate has been considered. However, the bonding strength between the aluminum-based substrate and the plating layer for fixing the abrasive grains is insufficient, making it difficult to use the aluminum-based substrate.

[0004] Incidentally, as a method for roughening the surface of an aluminum-based material, for example, a double zincate treatment is known as described in Patent Document 3. In addition, as a method for roughening the surface of an aluminum-based material, a method different from the zincate treatment is proposed in Patent Document 4. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-111302 A [Patent Document 2] Japanese Patent Application Publication No. 6-114739 [Patent Document 3] Japanese Unexamined Patent Publication No. 61-148900 [Patent Document 4] JP 2007-138224 A Summary of the Invention [Problem to be solved by the invention]

[0006] When double zincate treatment is applied as a roughening method for aluminum-based substrates, the strong alkaline treatment solution is not easy to handle, and the use of a strong alkaline treatment solution makes partial plating impossible. In electroplated abrasive tools, it is necessary to form a plating layer only on the part where the abrasive grains are arranged, and not to form a plating layer on the mounting surface that abuts against the mounting counterpart. However, as described above, since the double zincate treatment uses a strong alkaline treatment solution, masking is difficult, and partial plating cannot be performed. Therefore, double zincate treatment cannot be applied to form a roughened surface of an aluminum-based substrate.

[0007] An object of the present invention is to provide a method for manufacturing an electroplated abrasive tool that can apply aluminum or an aluminum alloy to a base material without applying a double zincate treatment, and can increase the bonding strength between the base material and a plating layer for fixing the abrasive grains. [Means for solving the problem]

[0008] The method for manufacturing an electroplated abrasive tool has a substrate having abrasive grains fixed to its surface, and includes a substrate roughening step of contacting the substrate made of aluminum or an aluminum alloy with an acidic liquid that contains copper ions and dissolves aluminum or an aluminum alloy, thereby dissolving the substrate surface and replacing the substrate surface with copper as a replacement metal, a replacement metal selective etching step of selectively etching the replacement metal on the substrate surface using the acidic liquid to expose the roughened surface of the substrate, a base plating step of forming a base plating layer on the roughened surface of the substrate, and an abrasive grain fixing step of arranging abrasive grains on the surface of the base plating layer and forming a fixing plating layer for fixing the abrasive grains.

[0009] An acidic solution is used in the substrate roughening step and the selective replacement metal etching step. This allows the substrate surface to be partially masked, and the substrate surface can be partially roughened. Furthermore, by roughening the surface of the aluminum or aluminum alloy substrate, the undercoat plating layer is engaged with the unevenness of the substrate surface. This increases the bonding strength between the substrate and the undercoat plating layer. Furthermore, a fixing plating layer for fixing the abrasive grains is formed on the surface of the undercoat plating layer, and sufficient bonding strength between the plating layers can be ensured. This increases the bonding strength between the substrate and the abrasive grains.

[0010] In this way, by applying aluminum or an aluminum alloy to the substrate, the weight of the electroplated abrasive tool can be reduced. Since the surface of the substrate can be roughened using an acidic liquid instead of a strong alkaline liquid, partial plating can be performed and handling is also improved. Furthermore, by roughening the surface of the substrate, the bonding strength between the substrate and the undercoat plating layer can be increased, and as a result, a high bonding strength between the substrate and the abrasive can be ensured. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a cross-sectional view of an electroplated abrasive tool. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a surface portion of an electroplated abrasive tool. [Diagram 3] 1 is a flowchart showing a method for manufacturing an electroplated abrasive tool. [Figure 4] 1 is an enlarged view showing a surface portion of a substrate in a substrate roughening step, the two-dot chain line showing the shape of the substrate before the substrate roughening step. [Diagram 5] FIG. 2 is an enlarged view showing a surface portion of a substrate in a selective replacement metal etching process. [Figure 6] FIG. 4 is an enlarged view showing a surface portion of a substrate in a base plating step. [Figure 7] FIG. 4 is an enlarged view showing a surface portion of the substrate in an abrasive grain arrangement step. [Figure 8] FIG. 4 is an enlarged view showing a surface portion of a substrate in a temporary fixing plating process. [Figure 9] 1 is a table showing the presence or absence of corrosion of the surface of a substrate when the thickness of an undercoat plating layer is changed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] (1. Types of electroplated abrasive tools) Electrodeposited abrasive tools include electrodeposited wheels and electrodeposited dressers, and are tools in which abrasive grains are fixed to the surface of a substrate by electroplating.

[0013] An electroplated wheel (also called an electroplated grinding wheel) is a tool for grinding metal workpieces, in which abrasive grains (e.g., superabrasive grains) such as diamond or CBN are fixed to the surface of a substrate. An electroplated wheel has, for example, a configuration in which a plurality of abrasive grains are fixed to the outer peripheral surface of a disk-shaped substrate, or a configuration in which a plurality of abrasive grains are fixed to an axial end surface on the outer peripheral side of a disk-shaped substrate. However, the substrate is not limited to a disk shape, and can be formed into any shape, and the position at which the abrasive grains are arranged can also be set arbitrarily. In addition, the plurality of abrasive grains are fixed to the surface of the substrate by a plating layer. The plating layer is, for example, nickel plating.

[0014] An electroplated dresser is, for example, a tool for performing dressing or truing on the surface of a grinding wheel. Like an electroplated wheel, an electroplated dresser is a tool in which a plurality of superabrasive grains such as diamond are fixed to the surface of a substrate by a plating layer. The substrate of the electroplated dresser may be disk-shaped or may be any shape other than disk-shaped. For example, an electroplated rotary dresser has a plurality of abrasive grains fixed to the outer peripheral surface of a disk-shaped substrate by a plating layer.

[0015] (2. Configuration of Electrodeposited Abrasive Tool 1) The configuration of the electrodeposited abrasive tool 1 will be described with reference to Fig. 1. The electrodeposited abrasive tool 1 includes a substrate 10, abrasive grains 20, and a plating layer 30.

[0016] The substrate 10 is made of aluminum or an aluminum alloy. The substrate 10 is formed, for example, in a disk shape with a through hole formed in the center. The inner circumferential surface of the through hole constitutes a mounting surface 11 for mounting the electrodeposited abrasive tool 1 to a mating member (not shown in the figure). The mounting surface 11 of the electrodeposited abrasive tool 1, i.e., the inner circumferential surface of the through hole, is the portion where the substrate 10 is exposed and comes into direct contact with the mating member. In other words, the mounting surface 11 is a surface that is not plated or the like.

[0017] The outer peripheral surface of the substrate 10 is formed into an arbitrary shape. In Fig. 1, the outer peripheral surface of the substrate 10 is formed into a cylindrical outer peripheral surface. Alternatively, the outer peripheral surface of the substrate 10 may be formed into a mountain shape or the like in the axial cross section.

[0018] The abrasive grains 20 are superabrasive grains such as diamond, CBN, etc. The abrasive grains 20 are fixed to the surface of a substrate 10. In the electroplated abrasive tool 1 shown in FIG.

[0019] The plating layer 30 is a layer for fixing the abrasive grains 20 to the surface of the base material 10 by electrodeposition. The plating layer 30 is bonded to the surface of the base material 10 and also to the surfaces of the abrasive grains 20. The plating layer 30 is formed by, for example, nickel plating.

[0020] (3. Detailed structure of the surface of the electroplated abrasive tool 1) The detailed configuration of the surface of the electrodeposited abrasive tool 1 will be described with reference to FIG. 2. As described above, the electrodeposited abrasive tool 1 includes the substrate 10, the abrasive grains 20, and the plating layer 30. The surface 10a of the substrate 10 is roughened to have an uneven shape as shown in FIG. 2. In particular, the roughened surface 10a of the substrate 10 has a large uneven shape, and the large uneven shape has even smaller uneven shapes on the surface. In other words, the roughened surface 10a of the substrate 10 has an undercut shape in the vertical direction of FIG. 2 due to the small uneven shapes.

[0021] The plating layer 30 includes an undercoat plating layer 31 and a fixed plating layer 32. The undercoat plating layer 31 is plated on the roughened surface 10a of the substrate 10 with a plating material. The undercoat plating layer 31 has a predetermined thickness H from the convex end (the portion corresponding to the maximum height) of the unevenness of the roughened surface 10a of the substrate 10. In other words, the undercoat plating layer 31 completely covers the convex portions of the unevenness of the roughened surface 10a of the substrate 10, and is completely embedded in the concave portions of the unevenness of the roughened surface 10a. In other words, the undercoat plating layer 31 completely covers the roughened surface 10a of the substrate 10, and there is no portion where the roughened surface 10a is exposed.

[0022] The fixed plating layer 32 is plated on the surface of the base plating layer 31, and bonds the base plating layer 31 and the abrasive grains 20. The fixed plating layer 32 includes a temporary fixed plating layer 32a and a permanent fixed plating layer 32b. The temporary fixed plating layer 32a is a plating layer for temporarily fixing the abrasive grains 20 to the surface of the base plating layer 31. The temporary fixed plating layer 32a is preferably made of the same plating material as the base plating layer 31, for example, nickel plating. This can increase the bonding strength between the base plating layer 31 and the temporary fixed plating layer 32a.

[0023] The permanent fixed plating layer 32b is a plating layer formed on the surface of the temporary fixed plating layer 32a. The permanent fixed plating layer 32b bonds the abrasive grains 20 to the temporary fixed plating layer 32a, and serves to firmly bond the abrasive grains 20 to the base plating layer 31. The permanent fixed plating layer 32b may be made of the same plating material as the temporary fixed plating layer 32a, for example, nickel plating. The thicknesses of the temporary fixed plating layer 32a and the permanent fixed plating layer 32b are appropriately changed depending on the size of the abrasive grains 20.

[0024] (4. Method for manufacturing electroplated abrasive tool 1) A method for manufacturing the electroplated abrasive tool 1 will be described with reference to Figs. 3 to 8. First, as a preliminary step, the surface of the substrate 10 is masked except for the portion on which the abrasive grains 20 are to be disposed. Next, the surface of the substrate 10 is degreased, and then washed with water (S1: degreasing step, S2: water washing step). The degreasing step uses an alkaline liquid such as caustic soda, sodium phosphate, or a mixture of other liquids. For example, the degreasing step involves contacting the substrate 10 with an aqueous solution of sodium hydroxide with a concentration of 0.25 mol / L at a temperature of 50°C. The treatment time is 60 seconds.

[0025] Next, a step of roughening the surface of the substrate 10 is performed, followed by rinsing with water (S3: substrate roughening step, S4: water rinsing step). The substrate roughening step is a treatment for dissolving the surface of the substrate 10 and substituting the surface of the substrate 10 with copper. In the substrate roughening step, the substrate 10 is brought into contact with an acidic solution that contains copper ions and dissolves aluminum or an aluminum alloy.

[0026] Here, the acidic solution has, for example, a hydrochloric acid concentration of 0.1 mol / L to 5.0 mol / L and a copper ion concentration of 0.004 mol / L to 1.0 mol / L. In the substrate roughening step, the substrate 10 is brought into contact with the acidic solution at a temperature of 30° C. to 80° C. The treatment time is 30 sec to 20 min.

[0027] The substrate roughening step results in the surface portion of the substrate 10 becoming as shown in Fig. 4. That is, in the substrate roughening step, the surface of the substrate 10 is dissolved and formed into an uneven shape (relatively large unevenness). Furthermore, in the substrate roughening step, the dissolved aluminum on the surface of the substrate 10 is replaced with copper as a replacement metal, and copper 40 precipitates on the surface of the substrate 10. As shown diagrammatically in Fig. 4, the surface of the substrate 10 has a large uneven shape, and copper 40, indicated by circles, precipitates on the large uneven surface.

[0028] Next, copper 40 as a replacement metal on the surface of the base material 10 is selectively etched using an acidic solution to expose the roughened surface 10a of the base material 10, which is then washed with water (S5: replacement metal selective etching step, S6: water washing step). In the replacement metal selective etching step, the base material 10 after the base material roughening step (S3) is brought into contact with an acidic solution that preferentially dissolves copper 40 as a replacement metal over the base material 10, thereby dissolving copper as a replacement metal while preventing the base material 10 from dissolving.

[0029] Here, the acid solution used in the selective etching step for the replacement metal is a strong acid such as hydrochloric acid, sulfuric acid, or nitric acid. For example, the acid solution uses sodium persulfate with a concentration of 0.2 mol / L to dissolve copper as the replacement metal. The processing time is 60 seconds.

[0030] The roughened surface 10a of the substrate 10 becomes as shown in Fig. 5 by the selective replacement metal etching step. That is, the roughened surface 10a of the substrate 10 is represented by the boundary between the substrate 10 and copper, which is the replacement metal, on the surface of the substrate 10 shown in Fig. 4. Therefore, the roughened surface 10a of the substrate 10 has a large uneven shape due to the dissolution of the substrate 10, and the large uneven shape further has a small uneven shape due to the selective replacement metal etching. That is, the roughened surface 10a of the substrate 10 has an undercut shape in the vertical direction of Fig. 5 due to the small uneven shape.

[0031] Next, it is determined whether the base material roughening step (S3) and the replacement metal selective etching step (S5) have been performed a preset number of times (S7). The preset number of times is set to, for example, once or twice, but may be three or more. If the preset number of times has not been reached (S7: No), the process returns to S3, and the base material roughening step (S3) and the replacement metal selective etching step (S5) are performed again.

[0032] Here, the roughened surface 10a of the substrate 10 after the selective replacement metal etching step after the specified number of times has an arithmetic mean roughness Ra (JIS B 0031:2003, ISO 1302:2002) of 1 μm or more, or a maximum height Rz (JIS B 0031:2003, ISO 1302:2002) of 10 μm or more. Furthermore, the roughened surface 10a of the substrate 10 after the selective replacement metal etching step after the specified number of times has an arithmetic mean roughness Ra of 1 μm or more and 6 μm or less (1 to 6 μm), or a maximum height Rz of 10 μm or more and 35 μm or less (10 to 35 μm).

[0033] After the specified number of times is reached (S7: Yes), a desmutting treatment is performed, followed by rinsing with water (S8: desmutting step, S9: rinsing step). The desmutting treatment removes smut adhering to the roughened surface 10a of the substrate 10. The desmutting step is performed, for example, using 10% Top Desmut N-20 (manufactured by Okuno Chemical Industries Co., Ltd.) at room temperature for a treatment time of 12 to 24 hours.

[0034] Next, a base plating layer 31 is formed on the roughened surface 10a of the base material 10 (S10: base plating step). The base plating layer 31 is, for example, nickel plating. In the base plating step, as shown in FIG. 6, the base plating layer 31 is formed having a thickness H from the convex ends of the unevenness of the roughened surface 10a of the base material 10. Here, the thickness H of the base plating layer 31 is at least 6 μm, and preferably 8 μm or more. Therefore, the base plating layer 31 is embedded in the recesses of the roughened surface 10a of the base material 10, and further completely covers the convex ends and recesses.

[0035] Here, known electroplating is applied to form the undercoat plating layer 31 with a thickness H of 6 μm or more. Furthermore, by employing electroplating, the undercoat plating layer 31 made of nickel plating can be formed on the roughened surface 10a of the substrate 10 without replacing the roughened surface 10a of the substrate 10 with nickel. That is, the undercoat plating layer 31 is physically anchored to the roughened surface 10a of the substrate 10. Therefore, the undercoat plating layer 31 has a high bonding strength to the substrate 10 due to the anchor effect. Alternatively, electroless plating may be applied to form the undercoat plating layer 31 with a thickness H of 6 μm or more.

[0036] Next, as shown in FIG. 7, the abrasive grains 20 are arranged on the surface of the base plating layer 31 (S11: abrasive grain arrangement step, abrasive grain fixing step). Next, as shown in FIG. 8, a temporary fixing plating layer 32a for fixing the abrasive grains 20 to the base plating layer 31 is formed (S12: temporary fixing plating step, abrasive grain fixing step). The thickness of the temporary fixing plating layer 32a is set according to the size of the abrasive grains 20. The temporary fixing plating layer 32a is, for example, nickel plating. That is, by using the same type of plating material for the temporary fixing plating layer 32a as the base plating layer 31, high bonding strength with the base plating layer 31 can be ensured. In addition, the temporary fixing plating layer 32a is formed by electroplating since it needs a thickness to hold the abrasive grains 20.

[0037] 2, a permanent fixed plating layer 32b is formed on the surface of the temporary fixed plating layer 32a (S13: permanent fixed plating step, abrasive grain fixing step). The thickness of the permanent fixed plating layer 32b is set according to the size of the abrasive grains 20. The permanent fixed plating layer 32b is nickel plated, like the temporary fixed plating layer 32a. In other words, by using the same type of plating material for the permanent fixed plating layer 32b as for the temporary fixed plating layer 32a, high bonding strength with the temporary fixed plating layer 32a can be ensured. In addition, electroless plating is preferably applied to the permanent fixed plating layer 32b. In this manner, the electrodeposited abrasive grain tool 1 is manufactured.

[0038] (5. Evaluation) The thickness H of the undercoat plating layer 31 was changed, and an evaluation was performed to check the presence or absence of corrosion on the surface of the substrate 10. The thickness H (shown in FIG. 6) of the undercoat plating layer 31 was set to 2.0 μm, 4.0 μm, 6.0 μm, 8.0 μm, and 10.0 μm. The corrosion of the substrate 10 was evaluated based on the presence or absence of black stains on the surface of the substrate 10.

[0039] The results are shown in FIG. 9. That is, when the thickness H of the undercoat plating layer 31 is 2.0 μm and 4.0 μm, corrosion was confirmed. On the other hand, when the thickness H of the undercoat plating layer 31 is 6.0, 8.0, and 10.0 μm, corrosion was not confirmed. That is, by setting the thickness H of the undercoat plating layer 31 to at least 6.0 μm, corrosion can be suppressed. Preferably, by setting the thickness H of the undercoat plating layer 31 to 8.0 μm or more, corrosion can be reliably suppressed. Note that the thicker the thickness H of the undercoat plating layer 31, the longer the processing time and the processing cost. Therefore, it is preferable that the thickness H of the undercoat plating layer 31 is, for example, 10.0 μm or less.

[0040] Next, the peel strength of the undercoat plating layer 31 relative to the surface roughness of the roughened surface 10a of the substrate 10 was evaluated. Specifically, the copper ion concentration of the acidic solution in the substrate roughening step, the concentration of hydrochloric acid, etc. were adjusted to change the surface roughness of the roughened surface 10a of the substrate 10. The arithmetic mean roughness Ra was set to 0.5, 1, 3, 6, and 9 μm. When the arithmetic mean roughness Ra was 0.5 μm and 9 μm, the anchor effect was weak and the peel strength of the undercoat plating layer 31 was small. When the arithmetic mean roughness Ra was 1 to 6 μm, a predetermined peel strength could be ensured.

[0041] As another index, the maximum height Rz was set to 5, 10, 15, 20, 25, 30, 35, 40, 45, and 50 μm. When the maximum height Rz was 5 μm or more and 40 μm or more, the anchor effect was weak and the peel strength of the undercoat plating layer 31 was small. When the maximum height Rz was 10 to 35 μm, a predetermined peel strength could be ensured.

[0042] (6. Effects) In the substrate roughening step S3 and the selective replacement metal etching step S5, an acidic solution is used. Therefore, it is possible to partially mask the surface of the substrate 10, and the surface of the substrate 10 can be partially roughened. Furthermore, by roughening the surface of the aluminum or aluminum alloy substrate 10, the undercoat plating layer 31 is engaged with the unevenness of the surface of the substrate 10. Therefore, the bonding strength between the substrate 10 and the undercoat plating layer 31 is increased. In addition, a fixing plating layer 32 for fixing the abrasive grains 20 is formed on the surface of the undercoat plating layer 31, and the bonding strength between the plating layers can be sufficiently secured. Therefore, the bonding strength between the substrate 10 and the abrasive grains 20 can be increased.

[0043] In this way, by using aluminum or an aluminum alloy for the substrate 10, the weight of the electroplated abrasive tool 1 can be reduced. Since the surface of the substrate 10 can be roughened using an acidic liquid instead of a strong alkaline liquid, partial plating can be performed and handling is also improved. Furthermore, by roughening the surface of the substrate 10, the bonding strength between the substrate 10 and the undercoat plating layer 31 can be increased, and as a result, a high bonding strength between the substrate 10 and the abrasive grains 20 can be ensured. [Explanation of symbols]

[0044] 1: electroplated abrasive tool, 10: substrate, 10a: roughened surface, 11: mounting surface, 20: abrasive, 30: plating layer, 31: undercoat plating layer, 32: fixed plating layer, 32a: temporary fixed plating layer, 32b: permanent fixed plating layer, 40: copper (replacement metal) S3: substrate roughening step, S5: replacement metal selective etching step, S11-S13: abrasive fixing step

Claims

1. A method for manufacturing an electroplated abrasive tool having abrasive grains fixed to a surface of a substrate, comprising the steps of: A substrate roughening step in which the substrate made of aluminum or an aluminum alloy is contacted with an acidic solution containing copper ions and dissolving aluminum or an aluminum alloy, thereby dissolving the surface of the substrate and replacing the surface of the substrate with copper as a replacement metal; a selective etching step of selectively etching the replacement metal on the surface of the base material using an acidic solution to expose a roughened surface of the base material; a base plating step of forming a base plating layer on the roughened surface of the base material; an abrasive grain fixing step of disposing abrasive grains on a surface of the undercoat plating layer and forming a fixing plating layer for fixing the abrasive grains; A method for manufacturing an electroplated abrasive tool comprising the steps of:

2. 2. The method for producing an electroplated abrasive tool according to claim 1, wherein the underplating step forms the underplating layer having a thickness of at least 6 μm from the convex ends of the irregularities on the roughened surface of the base material by electroplating or electroless plating.

3. 3. The method for producing an electroplated abrasive tool according to claim 1 or 2, wherein the roughened surface of the substrate has an arithmetic mean roughness Ra (JIS B 0031:2003, ISO 1302:2002) of 1 μm or more, or a maximum height Rz (JIS B 0031:2003, ISO 1302:2002) of 10 μm or more.

4. 4. The method for producing an electroplated abrasive tool according to claim 1, wherein the undercoat plating layer and the fixing plating layer are nickel platings.

Citation Information

Patent Citations

  • Aluminum with electrodeposited layer

    JP1986148900A

  • Electrodeposited grindstone

    JP1988221978A

  • Electrodeposition grinding wheel

    JP1994114739A

  • Cylindrical surface polishing grinding wheel

    JP2001054872A

  • Electrodepositted wheel and manufacturing process

    JP2001342596A