Galvanized multi-tubular beam and method for continuously forming a galvanized multi-tubular beam
The formation of protrusions in galvanized reinforcement beams to vent zinc oxide fumes during welding addresses the issue of harmful fumes and weld quality, resulting in a safe and structurally sound beam with continuous, high-quality welds.
Patent Information
- Application Number
- JP2021529270
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-01
- Filing Date
- 2019-11-26
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-11-26
AI Technical Summary
Welding galvanized metal produces zinc oxide fumes that can be harmful to operators and compromise weld quality if not properly vented, especially in enclosed areas of vehicle reinforcement beams.
A method of forming galvanized reinforcement beams with protrusions that create an evacuation gap for zinc oxide fumes, allowing them to exit the weld joint area during the welding process, using a roll forming machine with laser welding to form continuous weld joints with minimal heat affected zones.
Prevents the accumulation of zinc oxide fumes within the beam, ensuring a high-quality weld with no gas pockets or pits, thus enhancing operator safety and structural integrity.
Smart Images

Figure 0007553445000001 
Figure 0007553445000014 
Figure 0007553445000006
Abstract
Description
[Technical field]
[0001] This application claims priority to U.S. Provisional Patent Application No. 62 / 771,843, filed November 27, 2018, and U.S. Provisional Patent Application No. 62 / 812,684, filed March 1, 2019. The disclosures of these prior applications are considered part of this application and are incorporated herein by reference in their entireties.
[0002] FIELD OF THE DISCLOSURE This disclosure relates to vehicle structural and reinforcement beams and related methods of roll forming manufacturing and metal processing. [Background technology]
[0003] Vehicles undergo various tests mandated by government regulations and insurance certifications, such as tests for impact energy management and absorption. The results of these tests may depend on the design of various vehicle components and structures, including bumper assemblies and structural reinforcement beams. More specifically, the test results may depend on both the cross-sectional geometry and the quality of the welds of these beams. Summary of the Invention [Problem to be solved by the invention]
[0004] It is known to galvanize or apply a protective zinc coating to steel components of a vehicle to prevent rust or iron oxide from forming on the steel components over time. It is also commonly known that welding of galvanized metals produces zinc oxide fumes when the high heat used in some forms of welding burns or evaporates the zinc layer or coating from the steel component at or near the weld joint. Zinc oxide fumes produced during welding can be vented from the area surrounding the weld joint. However, if such fumes are not properly vented, for example if zinc oxide passes through the molten metal at the weld joint, they can be harmful to the operator and the quality of the weld can be compromised. [Means for solving the problem]
[0005] The present disclosure provides a galvanized reinforcement beam and a method for continuously forming the beam. Initially, a roll of galvanized sheet stock may be stretched in a generally horizontal plane to be processed, for example, by stretching at a generally constant speed towards and into a roll former. The roll former is configured to form the sheet into a beam with at least one longitudinally extending tubular portion. Protrusions are formed on a surface of the galvanized sheet stock either before entering the roll former or in-line with the roll former. The protrusions may be formed by a laser forming dimples with raised portions at generally consistent intervals along a generally straight line on the sheet. As the sheet is rolled, the protrusions are aligned with another section of sheet metal at a desired attachment seam surrounding the tubular portion of the beam such that the protrusions abut the opposing surface of the sheet stock to form a vent gap between the protrusions. The sheet stock is laser welded along the protrusions to continuously form a weld joint. The zinc oxide gas from the weld is allowed to exit the interior of the tubular shape through the vent gap upstream of the roll forming line from the weld joint being formed. As the weld joint is formed, the molten metal from the weld can fill the vent gap to close off the tubular shape of the beam. Thus, the protrusion can result in a weld joint that is substantially free of zinc gas pits or pockets, and can result in a thickness at the weld joint that slightly separates the planes of the sheet stock adjacent the weld joint.
[0006] According to one aspect of the disclosure, a galvanized multi-tubular beam for vehicle structure or bumper reinforcement is manufactured by roll forming a galvanized sheet metal to form two adjacent tubular sections sharing a common central wall of the beam. The outer sections of the sheet metal forming the two adjacent tubular sections extend from opposite sides of a central section of the sheet metal forming the common central wall of the beam. The galvanized multi-tubular beam includes an edge portion of one of the outer sections of the galvanized sheet metal attached to the central section of the galvanized sheet metal with a weld joint. The weld joint has a thickness separating a plane of the edge portion from a plane of the central section. The thickness of the weld joint is formed by the multiple protrusions protruding from the plane of the outer section or central section of the sheet metal such that when welding the weld joint, the longitudinal spacing between the multiple protrusions provides an exhaust opening for zinc oxide fumes resulting from welding to exit the interior of each tubular section of the beam.
[0007] The protrusions formed on the sheet stock may be spaced at a generally consistent distance. Weld joints interconnect the protrusions. The weld joints may extend continuously along the beam to surround the interior of each tubular portion of the beam. The weld joints may be formed via laser welding to form a narrow heat affected zone, e.g., approximately 1 mm to 2 mm in area.
[0008] According to another aspect of the disclosure, a method of continuously forming a galvanized reinforcement beam includes rolling a roll of galvanized sheet stock in a generally horizontal plane. Dimples are laser formed across a top surface of the sheet stock at a first laser head station as the galvanized sheet stock passes continuously through the first laser head station. The sheet stock is roll formed through a set of roll stations to form a tubular shape with an edge section of the sheet stock in contact with a middle section of the sheet stock. The edge section and / or the middle section of the sheet stock include dimples. The dimples form an exhaust gap between the edge section and the middle section of the sheet stock. The edge section is laser welded to the middle portion of the sheet stock at a second laser head station to continuously form a weld joint. Zinc oxide gas resulting from the welding is allowed to exit the interior of the tubular shape through the exhaust gap.
[0009] According to yet another aspect of the present disclosure, a galvanized multi-tubular beam is manufactured by roll forming a galvanized sheet metal to form two adjacent tubular sections sharing a common central wall of the beam. The galvanized multi-tubular beam has edge portions of outer sections of the galvanized sheet metal attached to reinforcement ribs formed in the central section of the galvanized sheet metal via weld joints. The edge portions of the galvanized sheet metal form the common central wall of the beam. The weld joints have a thickness separating a plane of the edge portions from a plane of the reinforcement ribs. The thickness of the weld joints is formed by a plurality of protrusions protruding from the plane of at least one of the edge portions or the reinforcement ribs. When welding the weld joints, the longitudinal spacing between the protrusions provides an exhaust opening for zinc oxide fumes resulting from welding to exit the interior of each tubular section of the beam.
[0010] According to yet a further aspect of the present disclosure, a method of continuously forming a galvanized reinforcement beam includes rolling a roll of galvanized sheet stock in a generally horizontal plane. The sheet stock is rolled through a first roll station to form an open cross-sectional shape with edge portions of the sheet stock spaced from a middle portion of the sheet stock. As the galvanized sheet stock continuously passes through a first laser head station, dimples are formed across a surface of the edge portions and / or middle portion of the sheet stock at the first laser head station. The sheet stock is bent through a second roll station to form a tubular shape with the edge portions of the sheet stock in contact with the middle portion of the sheet stock. The dimples form an exhaust gap between the edge portions and the middle portion of the sheet stock. The edge portions are laser welded to the middle portion of the sheet stock at the second laser head station to continuously form a weld joint along the dimples such that zinc oxide gas resulting from the welding can exit the interior of the tubular shape through the exhaust gap. Optionally, the second laser head station may not have an inner mandrel disposed within the cylindrical shape.
[0011] These and other goals, advantages, objectives and features of the present disclosure will become apparent from a review of the following specification in conjunction with the drawings. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a top view of a bumper reinforcement beam supported by a crash can on a vehicle frame according to one or more embodiments illustrated herein. [Diagram 2] FIG. 2 is a cross-sectional view of the reinforcement beam taken along line II-II in FIG. [Figure 2A] FIG. 4 is a cross-sectional view of an additional reinforcement beam. [Diagram 3] FIG. 1 is a schematic elevational view of an apparatus configured to manufacture a reinforcement beam of the present invention. [Figure 4A]3 is a series of cross-sectional views labeled S1-S24 illustrating the shape of the sheet metal stock at various forming steps when roll forming the beam of FIG. 2. [Figure 4B] 2A-2C are a further series of cross-sectional views labeled S25-S46 illustrating the shape of the sheet metal stock at additional forming steps when roll forming the beam of FIG. [Figure 5A] FIG. 1 is a schematic perspective view of a laser station for forming dimples across a top surface of sheet metal stock. [Figure 5B] FIG. 5B is an enlarged view of the formed dimple shown in section VB of FIG. 5A. [Figure 5C] FIG. 5C is a cross-sectional view of the dimple shown along line VC-VC in FIG. 5B. [Figure 6A] FIG. 4C is a perspective view of a portion of a partially shaped beam at shaping step S25 of FIG. 4B. [Figure 6B] FIG. 6B is a cross-sectional view of the partially shaped beam of FIG. 6A. [Figure 6C] FIG. 6C is an enlarged view of the dimple shown in section VIC of FIG. 6B. [Figure 7A] FIG. 4C is a perspective view of a portion of the partially shaped beam at laser welding step S29 of FIG. 4B. [Figure 7B] FIG. 7B is another perspective view of the section of the beam shown in FIG. 7A. [Figure 7C] FIG. 7C is an enlarged view of the laser weld shown in section VIIC of FIG. 7B. [Figure 7D] FIG. 7B is a cross-sectional view of a section of the beam shown in FIG. 7A. [Figure 7E] FIG. 7E is a cross-sectional view of the beam along the seam before it is welded closed, taken along line VIIE-VIIE in FIG. 7D. [Figure 7F] FIG. 7E is an enlarged view of the weld formed at section VIIF in FIG. 7D. [Figure 7G] FIG. 7F is an enlarged view of the weld after formation of FIG. 7F, showing the narrow heat affected zone. [Figure 8A]FIG. 4C is a perspective view of a portion of a partially shaped beam at shaping step S37 of FIG. 4B. [Figure 8B] FIG. 8B is a cross-sectional view of the partially shaped beam of FIG. 8A. [Figure 9A] FIG. 4C is a perspective view of a portion of the partially shaped beam at laser welding step S46 of FIG. 4B. [Figure 9B] FIG. 9B is a cross-sectional view of a portion of the beam shown in FIG. 9A. [Figure 10] FIG. 4 is a cross-sectional view of an additional reinforcement beam. [Figure 11] FIG. 11 is a perspective view of an end section of the beam shown in FIG. [Figure 12A] 11A-11C are perspective views of the partially formed reinforcement beam shown in FIG. 10 at various stages in forming the beam. [Figure 12B] 12B is a cross-sectional view of the partially shaped beam of FIG. 12A at a laser station forming dimples across the mating surface of the sheet metal. [Figure 12C] FIG. 12C is a cross-sectional view of the partially shaped beam of FIG. 12B at a laser station welding the edges of the sheet metal to the mating surfaces and enclosing the cylindrical portion of the reinforcement beam. [Figure 13A] 12D is a perspective view of the partially shaped beam of FIG. 12C, where the sheet metal has been further shaped to the shape of the reinforcement beam shown in FIG. [Figure 13B] FIG. 13B is a cross-sectional view of the partially shaped beam of FIG. 13A at a laser station forming dimples across another mating surface of the sheet metal. [Figure 13C] 11 is a cross-sectional view of the shaped reinforcement beam of FIG. 10 at a laser station where the edge of the sheet metal is welded to the mating surface and surrounds the second cylindrical portion of the reinforcement beam. [Figure 14] FIG. 4 is a cross-sectional view of an additional reinforcement beam. [Figure 15] FIG. 15 is a perspective view of an end section of the beam shown in FIG. [Figure 16A] 15A-15C are perspective views of the partially formed reinforcement beam shown in FIG. 14 at various stages in forming the beam. [Figure 16B] 16B is a cross-sectional view of the partially shaped beam of FIG. 16A at a laser station forming dimples across the mating surface of the sheet metal. [Figure 16C] 16C is a cross-sectional view of the partially shaped beam of FIG. 16B at a laser station welding the edges of the sheet metal to the mating surfaces and enclosing the cylindrical portion of the reinforcement beam. FIG. [Figure 17A] 16D is a perspective view of the partially shaped beam of FIG. 16C where the sheet metal has been further shaped to the shape of the reinforcement beam shown in FIG. [Figure 17B] FIG. 17B is a cross-sectional view of the partially shaped beam of FIG. 17A at a laser station forming dimples across another mating surface of the sheet metal. [Figure 17C] 15 is a cross-sectional view of the shaped reinforcement beam of FIG. 14 at a laser station where the edge of the sheet metal is welded to the mating surface and surrounds the second cylindrical portion of the reinforcement beam. [Figure 18] A cross-sectional view of an additional reinforcement beam. [Figure 19A] 19A-19C are cross-sectional views of the partially shaped beam at various stages in shaping the reinforcement beam shown in FIG 18, showing the position of the laser station for encircling the cylindrical portion of the reinforcement beam. [Figure 19B] 19B is a cross-sectional view of the partially shaped beam of FIG. 19A where the sheet metal has been further shaped to the shape of the reinforcement beam shown in FIG. 18 and shows the location of another laser station to enclose a second cylindrical portion of the reinforcement beam. [Figure 20] FIG. 4 is a cross-sectional view of an additional reinforcement beam. [Figure 20A]FIG. 21 is an enlarged view of a weld formed in section XXA in FIG. 20. [Figure 21] FIG. 1 is a schematic perspective view of an example of a protrusion disposed across a top surface of sheet metal stock. [Figure 22] 1 is a schematic perspective view of another example of a protrusion disposed across a top surface of sheet metal stock; FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Referring now to the drawings and the exemplary embodiment depicted therein, a galvanized beam 10 may be generally continuously formed in a roll forming process that includes a method of continuously welding one or more seams of the closed beam 10 in a manner that vents zinc oxide fumes generated within the enclosed area of the beam 10 during welding of the galvanized sheet stock used to form the beam 10. The galvanized multi-tubular beam 10 may be used for vehicle structural reinforcement or bumper reinforcement, for example as shown in FIG. 1, where the beam 10 is bent longitudinally with varying degrees of bending to match the design of the bumper of a particular vehicle. When used as a bumper reinforcement, the beam 10 may be attached to a crash can located in front of the vehicle frame to span the width of the vehicle frame. Alternatively, the beams described herein, whether straight or curved, may be adapted for a variety of alternative structural or reinforcement applications, such as rear bumpers, door impact beams, frame members (e.g., roof bows, headers, pillars, rocker rails, seat members, etc.), and frame members for vehicle battery tray supports, among other possible vehicle and non-vehicle related members and components.
[0014] The beam 10 may be manufactured, for example, by roll forming a galvanized sheet metal 12, shown unrolled from a roll in FIG. 3, to form two adjacent tubular portions 14, 16 that share a common central wall 18 of the beam 10. The outer sections 12a, 12c of the sheet metal 12 forming the two adjacent tubular portions 14, 16 extend from opposite sides of a central section 12b of the sheet metal 12 that forms the common central wall 18 of the beam. Such sections may initially be delimited in the forming step S2 of FIG. 4A. Once the beam 10 is formed, the two adjacent tubular portions 14, 16 of the beam 10 are defined by front walls 20, 22, rear walls 24, 26, a top wall 28, and a bottom wall 30, for example, as oriented in FIGS. 1 and 2. The front walls 20, 22 of the adjacent tubular portions 14, 16 are substantially aligned with each other to form the outward or impact surface of the beam when used as a bumper reinforcement beam. Similarly, rear walls 24, 26 are generally aligned with one another and substantially parallel to front walls 20, 22. Additionally, upper and lower walls 28, 30 are substantially parallel to one another and to central wall 18, and generally perpendicular to front and rear walls 20, 22, 24, 26. It will be appreciated that additional embodiments of the beam can take on a variety of shapes and orientations from those shown in Figure 2 and can include, for example, alternative dimensional proportions for different applications of the beam.
[0015] 3, as the galvanized sheet stock 12 is unrolled from the roll, protrusions 32 may be formed on the top surface of the sheet stock 12, for example, at a laser head station 31 prior to the roll forming line. It is also envisioned that the protrusions may alternatively be formed in a processing line separate from the roll forming line, for example, by re-rolling the sheet after forming the protrusions and then moving the rolled roll to the roll forming line. Alternatively, the protrusions may be formed in-line or during the roll forming process, for example just prior to welding, to reduce the risk that the protrusions will be distorted by the roll former station.
[0016] The laser head station 31 shown in Figure 3 may form protrusions or dimples 32 at substantially consistent spacing and along a substantially straight line longitudinally along the length of the shaped beam 10. It is understood that the spacing or separation between the protrusions may vary along the beam. It is also contemplated that the protrusions may be formed by alternative devices, such as by mechanically deforming the sheet with a sawtooth disk, stamping device, or other contemplated means.
[0017] Furthermore, protrusions can be arranged on the sheet by, for example, electrospark deposition (ESD) (i.e., pulsed fusion build-up or pulsed electrode build-up) as shown in FIG. 21. In this electrospark deposition (ESD), a pulsed microwelding process provides intermittent ESD material 33 arranged in the plane of the galvanized sheet metal 12 and protruding out of the plane of the galvanized sheet metal 12. These protrusions 33 likewise create exhaust openings for the zinc oxide fumes resulting from the welding to exit the interior of each tubular portion of the formed beam. Protrusions can also be arranged on the sheet by, for example, additive manufacturing (i.e., 3D printing) as shown in FIG. 22. A solid material 35 (e.g., laser sintering or molten metal powder) is arranged in the plane of the galvanized sheet metal 12 and protrudes out of the plane of the galvanized sheet metal 12. These protrusions 35 likewise create exhaust openings for the zinc oxide fumes resulting from the welding to exit the interior of each tubular portion of the formed beam.
[0018] A line of protrusions or dimples 32 are formed on or along the sheet 12 to coincide with attachment points or weld seams when the sheet 12 is formed to close the tubular portion of the corresponding beam 10. As shown in step S1 of FIG. 4A, a laser head station 31 may form dimples 32 at two locations with two separate laser beams 34 or their equivalent. The selected locations of each line of dimples 32 coincide with later-formed weld joints 36, 38 of the beam 10. These weld joints 36, 38 are formed on or along the dimples 32 to surround the interior regions of the respective adjacent tubular portions 14, 16 of the beam 10. As further shown in FIGS. 5A and 5B, the two lines of dimples 32 are parallel to each other and have the same rough spacing or separation between each individual dimple 32 along the length of the sheet 12.
[0019] The dimples 32 may each have a recessed portion 40 and a raised portion 42. These portions may be formed from laser pulsing or otherwise intermittently contacting the sheet 12 (i.e., laser dimpling). More specifically, the sheet material, laser intensity, and the speed at which the sheet 12 moves relative to the laser beam 34 may be calibrated and configured such that the laser beam does not penetrate the sheet, but instead forms a recessed portion 40 of a desired depth, as shown, for example, in FIG. 5B, and a corresponding raised portion 42 of a desired height. To do so, a small pool of molten metal may be formed on the top surface of the sheet 12 by heat generated from the laser 34 contacting the sheet 12. When the laser 34 is stopped or no longer in contact with the sheet 12 (or is otherwise sufficiently reduced in intensity), the metal cools and hardens with the raised portion 42, as shown, for example, in FIG. 5C, protruding at a height that extends beyond the top surface around the metal sheet 12. The length of each dimple longitudinally along the length of the sheet may be approximately 2 mm to 5 mm. It is also contemplated that the dimples may also or alternatively be formed on the bottom surface of the sheet, such as in a location disposed in central section 12b of the sheet metal that contacts an edge portion of outer section 12a of sheet 12.
[0020] With further reference to FIG. 3, a roll of galvanized sheet stock may be stretched in a generally horizontal plane to be processed, for example, by being stretched at a generally constant speed toward and into a roll former or roll forming apparatus, for example, at a laser station 31 that first forms protrusions or dimples 32 on the top surface of the sheet 12. The galvanized multi-tubular beam 10 is then formed into its shape by a roll forming apparatus processing a single sheet 12 through a series of paired rolls at the roll forming station. Each station performs a forming operation illustrated by the roll forming flower diagrams of forming steps S2-S28 and S30-S45 shown in FIGS. 4A and 4B. During the roll forming process, the sheet metal 12 is shaped such that adjacent tubular portions 14, 16 are formed on either side of a single central wall 18. Again, it is envisioned that the beam formed in the exhaust welding process may have another profile or shape than that shown in FIG. 2, such as a B-shaped beam or a D-shaped beam.
[0021] As shown in FIG. 3, the roll former may include a first series of forming rolls 44 at a station that continuously bends the outer section 12a of the sheet metal 12 and the central section 12b of the sheet metal 12, for example, corresponding to forming steps S2-S28 shown in FIGS. 4A and 4B. Thus, the first series of forming rolls 44 continuously shapes the sheet metal 12 toward and into the shape of the corresponding cylindrical portion 14 of the beam 10, while orienting the central wall 18 of the beam 10 toward and into a generally perpendicular orientation relative to the other outer sections 12c of the sheet metal 12. In doing so, edge portions of the outer sections 12a of the sheet metal 12 are formed with radiused ends configured to contact the central section 12b of the sheet metal 12, such as shown in step S25 shown in more detail in FIGS. 6A and 6B. Thus, the first series of forming rolls 44 may deform slightly less than "half" the width of the sheet in a first direction (shown as a counterclockwise direction in FIGS. 4A and 4B) to form a first tube or tubular section with a radiused edge of the sheet abutting the radiused end of the central wall. It is contemplated that the first series of forming rolls may include a greater or lesser number of stations to form the sheet from the flat section to generally provide a tubular section with an vent seam as disclosed herein ready for welding of the galvanized sheet.
[0022] Prior to welding at the first laser welding station 46 (FIG. 3), the first series of forming rolls 44 may place the line of protrusions 32 of the outer section 12a of the metal sheet 12 in contact with the generally flat surface of the sheet 12, for example as shown in FIG. 7E. The line of contact of the protrusions 32 with the central section 12b of the sheet 12 may be at the end of the central wall 18, at which the central wall 18 becomes generally planar or flat. The longitudinal spacing between the protrusions 32 provides exhaust openings 48 for zinc oxide fumes resulting from welding to exit the interior of each cylindrical portion of the beam 10. The separation provided by the protrusions 32 between the edge portions of the outer section 12a and the central section 12b is approximately 50 microns to 300 microns. The line of protrusions shown in FIG. 7E is therefore an example of an exhaust seam configured for continuous laser welding of a galvanized sheet continuously roll-formed into a cylindrical beam. It is beneficial to evacuate fumes trapped in galvanized steel welds, especially in enclosed areas of the tube, to have a consistent weld without gas openings or pockets that can form with pressurized gases, such as zinc oxide gas.
[0023] As shown in Figures 7A-7F, the weld joint 36 is formed at a first welding station 46 via laser welding along the exhaust seam to form a continuously closed weld joint 36 along the length of the beam 10. Due to the protrusions 32 forming the exhaust openings 48, the weld joint 36 has a thickness (approximately 50 microns to 300 microns) that slightly separates the plane of the edge portion of the outer section 12a from the plane of the central section 12b. When the weld joint 36 is welded, the longitudinal spacing between the protrusions 32 provides the exhaust openings 48 for zinc oxide fumes 50 resulting from welding to exit the interior of the tubular portion 14 of the beam 10 upstream from the welding station 46 in the roll former (i.e., before the exhaust openings 20 being welded are closed at the welding station 46).
[0024] As shown in Figure 7D, the laser beam 52 generated by the welding station 46 to form the weld joint 36 is positioned approximately perpendicular to the orientation of the center wall 18. This substantially perpendicular orientation of the laser beam 52 further forms the weld joint 36 with a relatively narrow heat affected zone 54, as shown, for example, in Figure 7G. The heat affected zone 54 can be, for example, approximately 1 mm to 2 mm.
[0025] Thus, when the outer section 12c of the sheet 12 is generally perpendicular to the central wall section 12b, the location of the weld joint 36 is commensurate with the presence and depth of the reinforcing ribs 56 molded in the front wall 22 of the second tubular portion 16 of the beam 10. In an alternative embodiment, as shown in FIG 2A, the beam 110 is similarly shaped, but the outer section 112c of the sheet 112 does not have the reinforcing ribs to allow for a more vertical orientation of the laser welder when welding the weld joint 136 along the length of the beam 110.
[0026] Referring again to FIG. 4B, after the formation of the weld joint 36, the sheet metal 12 continues to the second series of forming rolls 58 at the station. The second series of forming rolls 58 at the station continuously bend the remaining outer section 12c of the sheet metal 12, for example, corresponding to the forming steps S30-S45. Thus, the second series of forming rolls 58 continuously shapes the sheet metal 12 to the shape of the corresponding tubular portion 16 of the beam 10, so as to substantially finish the shape of the beam 10. In doing so, the edge portion of the outer section 12c of the sheet metal 12 is configured to contact and form a lap joint with the rear wall 24 of the tubular portion 14 of the first beam 10, for example, as shown in step S37 in more detail in FIGS. 8A and 8B. The lap joint includes a thickness that separates the plane of the edge portion from the plane of the rear wall 24. The thickness of the weld joint is formed by the protrusions 32 protruding from the plane (and / or edge) of the rear wall 24 so that when welding the lap joint, zinc oxide fumes 50 exit the interior of each tubular portion 16 of the beam through the exhaust openings 48 formed by the protrusions 32. The separation between the edge portions of the outer section 12c provided by the protrusions 32 and the rear wall 24 is approximately 50 microns to 300 microns. Thus, the second series of forming rolls 58 can deform the remaining "half" of the width of the sheet in the same rotational direction as the first series of forming rolls (shown as a counterclockwise direction in Figures 4A and 4B) to form a second tube or tubular portion. Again, it is contemplated that the second series of forming rolls can include a greater or lesser number of stations to generally provide a tubular portion with an exhaust seam as disclosed herein ready for welding of the galvanized sheet.
[0027] For example, the second series of forming rolls 58 shown in FIG. 3 may place the edge of the outer section 12c of the sheet metal 12 in contact with a recessed area 60 molded along the back wall 24, as shown in FIG. 9A. The recessed area 60 in the back wall 24 may provide an area for a second line of protrusions 32. The recessed area 60 allows the back walls 24, 26 of the beam to be positioned in generally planar alignment with one another. The longitudinal spacing between the protrusions 32 again provides vent openings 48 for zinc oxide fumes resulting from welding to exit the interior of each cylindrical portion of the beam 10. Thus, the line of protrusions shown in FIG. 9A is another example of an vent seam configured for continuous laser welding of a continuously roll-formed galvanized sheet into a cylindrically shaped beam.
[0028] As further shown in Figures 9A and 9B, the weld joint 38 is formed via laser welding along the exhaust seam at a second welding station 64 (Figure 3) to form a continuously closed weld joint 38 along the length of the beam 10. Due to the protrusions 32 forming the exhaust openings 48, the weld joint 38 has a thickness that slightly separates the plane of the edge portion of the outer section 12c from the plane of the sheet metal it abuts. When welding the weld joint 38, the longitudinal spacing between the protrusions 32 provides the exhaust openings 48 for the zinc oxide fumes 50 resulting from the welding to exit the interior of the tubular portion 16 of the beam 10 upstream from the welding station 64 to the roll former. As shown in Figure 9B, the laser beam 66 generated by the welding station 64 to form the weld joint 38 is positioned approximately perpendicular to the orientation of the rear wall portions 24, 26. Again, this substantially perpendicular orientation of the laser beam 66 allows the weld joint 38 to be formed with a relatively small heat affected zone.
[0029] The roll former may further be configured to form channels or reinforcing ribs 56 projecting into the interior volume of each cylindrical portion 14, 16, as shown, for example, in the front wall of the beam. The reinforcing ribs 56 (i.e., inwardly molded recesses, sometimes referred to as "power ribs") further strengthen the wall section and thus, in the beam 10 shown in FIG. 2, strengthen the front surface of the beam 10 and strengthen the corresponding tube portion 14, 16. The illustrated reinforcing ribs 56 have a width diameter that is about 10%-40% of the width of the corresponding wall section (or more preferably about 20%-30% of the width) and a depth that is approximately equal to the width diameter. The bottom of the illustrated channel ribs is semicircular in shape. Nevertheless, it is envisioned that the depth and size of the channel ribs may be shallower, deeper, wider, narrower, flat-bottomed, or otherwise modified to meet the particular functional requirements of the beam.
[0030] The beam 10 is made from a sheet 12 of steel material having a thickness of 0.8 mm to 1.4 mm or approximately 1 mm to 1.5 mm, and the sheet 12 may have a tensile strength of about 800 to 2000 MPa (i.e., about 120 to 290 ksi). The illustrated beam is about 80 mm high and 40 mm deep (in the position mounted on the vehicle), with two channel ribs molded into the front face of the beam (one on top of each tube). Each illustrated reinforcing rib is about 8 mm to 10 mm deep and 8 mm to 10 mm wide, and includes a rounded bottom. However, it is envisioned that the beams of the present invention can be made from different materials including AHSS (advanced high strength steel) and that the beams of the present invention can be made from sheet metal having a thickness of about 0.8 mm to 3.0 mm (or such as 0.8 mm to 1.4 mm thick), can be made with different beam cross-sectional sizes, for example, heights of about 80 mm to 150 mm, and depths of 30 mm to 60 mm, and have a length equal to or slightly greater than the distance between the vehicle fixture / bumper frame rail tips.
[0031] Related equipment for producing the tubular reinforcement beam 10 with a roll former includes an in-line cleaning station 68 and a cutoff 70. The first and second laser welding stations 46, 64 are configured to form welds along the beam that can withstand longitudinal bending of the beam at the in-line cleaning station 68. It is understood that the laser beams of the laser welding stations 46, 64 can be positioned at various orientations relative to the beam as needed to form the desired welds, for example, above, below, or on the side of the beam. It is further noted that the roller former can employ a roll mill with a horizontal axis supporting the forming rolls, or alternatively, can employ a roll mill with a vertical axis supporting the forming rolls.
[0032] 10-13C, an additional example of a galvanized multi-tubular beam 210 is shown having two adjacent tubular portions 214, 216 that share a common central wall 218 of the beam 210. Unlike the beam 10 shown in FIG. 2, an outer section 272 of the metal sheet 212 forms the common central wall 218 of the beam 210 opposite the central section of the sheet. The central wall 218 of the beam 210 shown in FIG. 10 is formed by an edge portion 272a of the outer section 272 of the metal sheet 212 attached to an interior contact surface 274 of the beam 210 to surround one of the tubular portions 214. The other tubular portion 216 is formed by opposing outer sections 276 of sheet metal formed in an opposite rotational direction from the first tubular portion 214 such that edge portions 276a of the outer sections 276 of the sheet metal 212 are attached to opposing ends of the central wall 218 with lap joints 238 similar to those shown in the welded joints 38 of the beam 10 shown in FIG. 2.
[0033] The shaped beam 210 shown in Figures 10 and 11 may be rotated about its longitudinal axis to be oriented similarly to the beam 10 shown in Figure 2, for example, for use as a bumper reinforcement beam. The respective walls of the beam 210 may then be referred to as front walls 220, 222, rear walls 224, 226, top wall 228, and bottom wall 230. The front walls 220, 222 of adjacent tubular portions 214, 216 are substantially aligned with each other to form the outward or impact surface of the beam when used as a bumper reinforcement beam. Similarly, the rear walls 224, 226 are generally aligned with each other and substantially parallel to the front walls 220, 222. Additionally, the top and bottom walls 228, 230 are substantially parallel to each other and to the central wall 218, and generally perpendicular to the front and rear walls 220, 222, 224, 226. It will be appreciated that additional examples of beam 210 may take various orientations from those shown in Figures 10 and 11 and may include alternative cross-sectional shapes and dimensional proportions, for example, for different uses and applications of the beam.
[0034] 12A, galvanized sheet stock 212 may be roll formed through a series of roll dies to form a cross-sectional shape such as the illustrated example. This cross-sectional shape is achieved prior to closing the seam that is welded to enclose the first tubular portion 214 (FIG. 10). In this illustrated example, the seam-formed protrusions 232 (FIG. 12B) are formed in-line with the roll former after passing through several roll forming dies on the roll forming line. By roll forming the sheet stock 212 to achieve the intermediate cross-sectional shape of the beam 210 prior to forming the protrusions 232, the protrusions may then be formed without the risk of being damaged or flattened by passing through a roll forming die prior to being used in the weld seam. Specifically, as shown in FIG. 12A, the outer edge portion 272a of the sheet 212 used to form the first cylindrical portion 214 of the beam 210 is spaced upwardly from the desired contact surface 274 of the sheet so as to allow the laser beam 234 to linearly access the contact surface 274 of the sheet 212 to form the protrusion 232 (FIG. 12B).
[0035] As further shown in FIG. 12A, a trailing corner 278 of the tubular portion 214 on the opposite side of the tubular portion 214 from the contact surface 274 used to form the desired weld joint may be used as a single articulation point on the sheet. The sheet may be bent about the trailing corner 278 to rotate the edge portion 272a of the sheet down into abutting engagement with the protrusion 232 formed on the contact surface 274, as shown in FIG. 12C. Thus, as shown in FIG. 12A, the cross-sectional shape may be formed to have essentially all of the desired shape and configuration of the first tubular portion 214 created in the outer section 272 of the sheet metal prior to forming the protrusion 232, such that only a final additional bend is required at the trailing corner 278 to close and complete the shape of the first tubular portion 214. It is also envisioned that additional or alternative articulation points may be used in other examples of the beam than those shown in FIGS. 12A-12C, such as beams with alternative cross-sectional shapes or roll forming sequences.
[0036] The protrusions 232 may be formed at a surface of the sheet 212 that coincides with the portion of the sheet metal 212 that is desired to have a weld joint, for example, at the contact surface 274 of the formed sheet metal 212 shown in FIG. 12B. The protrusions 232 may be formed as the sheet metal passes continuously between the roll forming dies through a laser head station that is located in-line on the roll former. The protrusions 232 formed in-line on the roll former may be linearly spaced at generally consistent intervals along the longitudinal extension of the sheet metal 212 and may otherwise be formed in the same or similar manner as shown in FIGS. 5A-5C and described above.
[0037] To form the protrusions 232, the laser beam 234 may be angled at a substantially perpendicular orientation relative to the contact surface 274. As shown in FIG. 12B, the contact surface 274 is disposed on a side portion of a reinforcing rib 256 molded into the front wall 220 of the beam 210. The reinforcing rib 256 protrudes into the interior volume of each cylindrical portion 214, 216 to strengthen the wall section of the beam 210. Again, it is envisioned that the depth and size of the reinforcing ribs may be varied from those shown in FIGS. 10-13C, for example, to make the ribs shallower, deeper, wider, narrower, or otherwise modify the ribs to meet the particular functional requirements of the beam. Accordingly, other reinforcing ribs 256 formed in the outer section 276 of the sheet metal 212 used to form the second tubular portion 216 of the beam 10 (FIGS. 10-11) may have a depth configured to allow for a substantially perpendicular orientation of the laser beams 234, 252 relative to the corresponding weld joints 236 when forming the protrusions 232.
[0038] Prior to welding the seam of the first tubular portion 214 of the beam 210, one or more forming rolls may further shape the outer section 272 of the sheet metal 212 to bend and rotate the edge portion 272a about the rear corner 278 and place the outer edge 272a in contact with the line of protrusions 232 of the contact surface 274 of the reinforcing rib 256, as shown in FIG. 12C. The line of contact of the protrusions 232 with the edge portion 272a of the sheet metal 212 provides a longitudinal spacing between the protrusions 232 that creates an exhaust opening for zinc oxide fumes resulting from welding to exit the interior of each tubular portion 214 of the beam 210. The separation between the planar portions of the sheet created by the protrusions 232 is approximately 50 microns to 300 microns. The protrusions 232 thus form an exhaust seam configured for continuous laser welding of the galvanized sheet that is continuously roll-formed into the tubular shaped beam 210. The vent openings allow fumes that would otherwise be trapped in the enclosed area of the tube to freely exit to have a consistent weld without gas openings or pockets that can form with pressurized gas, e.g., zinc oxide gas.
[0039] With the outer portion 272a near or in engagement with the contact surface 274, the sheet metal 212 can enter a welding station that may use an external mandrel to hold the cross-sectional shape for welding. However, due to the cross-sectional shape of the first tubular portion 214, there is otherwise no internal mandrel. The external mandrel may apply force to the walls surrounding the first tubular portion 214 without disturbing the contact between the projection 232 and the contact surface 274 and the generally perpendicular orientation of the central wall 218 relative to the front and rear walls 220, 224 of the first tubular portion 214. In particular, the opposing mandrels applying force to the front and rear walls 220, 224 do not disturb the right-angled shape of the tubular portion 214 due to the end portion 272b of the edge portion 272a being positioned at the beginning of the curved formation 280 of the reinforcing rib 256 that transitions back to the front wall 220. The outer mandrel in combination with the curved former 280 thereby prevents movement of the end portion 272b which can cause shear forces at the weld joint 236. The resulting reduction or lighting of the inner mandrel in the roll former can help reduce friction on the surface of the sheet metal which can unnecessarily lead to wearing away the galvanized coating.
[0040] As shown in FIG. 12C, the weld joint 236 is formed via laser welding along the exhaust seam to provide a continuously attached and closed seam along the length of the beam 210. Due to the protrusions 232 forming the exhaust opening, the weld joint 236 may have a thickness of, for example, approximately 50 microns to 300 microns that slightly separates the plane of the edge portion 272a of the outer section 272 from the plane of the contact surface 274. When welding the weld joint 236, the longitudinal spacing between the protrusions 232 provides an exhaust opening for zinc oxide fumes 250 resulting from welding upstream from the welding station in the roll former to exit the interior of the tubular portion 214 of the beam 210. As shown in FIG. 12C, the laser beam 252 generated by the welding station to form the weld joint 236 is positioned approximately perpendicular to the orientation of the central wall 218. This substantially vertical orientation of the laser beam 252 further creates a relatively narrow heat affected zone weld joint 236, such as approximately 1 mm to 2 mm, as shown in FIG. 7G.
[0041] After forming the weld joint 236, the sheet 212 continues into a second series of forming rolls at the station which continuously bend the other outer section 276 of the sheet 212 into the shape of the second tubular portion 216 of the beam 210. As shown in FIG. 13A, the cross-sectional shape is again formed near the seam of the tubular portion of the beam 210, but before the seam of the tubular portion of the beam 210 is closed. In the intermediate cross-sectional shape shown in FIGS. 13A and 13B, the protrusion 232 is again formed at the seam in-line with the roll former to reduce the risk of damaging or flattening the protrusion. Specifically, as shown in Figure 13A, the outer edge portion 276a of the sheet 212 used to form the second tubular portion 216 of the beam 210 is spaced upwardly from the desired contact surface 282 of the sheet to allow the laser beam 284 to directly access the contact surface 282 of the sheet 212 to form the protrusion 232. The example shown in Figures 10-13C shows the contact surface 282 used to form the laser welded lap joint 238 at the recessed area 260 formed along the rear wall 224 at the corner of the first tubular portion 214 adjacent the central wall 218.
[0042] As further shown in FIG. 13A, a rear corner 286 of the second tubular portion 216 on the opposite side of the tubular portion 216 from the weld joint 236 may be used as a single articulation point on the sheet. The sheet may be bent about the rear corner 286 to rotate the edge portion 276a of the sheet down into abutting engagement with the protrusion 232 formed at the contact surface 282, as shown in FIG. 13C. Thus, as shown in FIG. 13A, the cross-sectional shape may be formed to have essentially any desired shape and configuration of the second tubular portion 216 created at the outer section 276 of the sheet metal prior to forming the protrusion 232 at the contact surface 282, such that only a final additional bend is required at the rear corner 286 to close and complete the shape of the second tubular portion 216. It is also envisioned that additional or alternative articulation points may be used in other examples of beams than those shown in FIGS. 13A-13C, such as beams with alternative cross-sectional shapes or roll forming sequences.
[0043] As shown in FIG. 13B, the protrusions 232 may be formed as the sheet metal passes continuously between the roll forming dies through a laser head station located in-line on the roll former. The protrusions 232 shown in FIG. 13B may be formed in the same or similar manner as otherwise shown in FIGS. 5A-5C and described above. To form the protrusions 232, the laser beam 284 may be angled at a substantially perpendicular orientation relative to the contact surface 282. Similarly, the laser beam 266 used in forming the corresponding weld joint 236 may be substantially perpendicular to the contact surface 282.
[0044] Prior to welding the seam of the second tubular portion 216 of the beam 210, one or more forming rolls may further shape the outer section 276 of the sheet metal 212 to bend and rotate the edge portion 276a about the rear corner 286 and place the outer edge 276a in contact with the line of protrusions 232 of the contact surface 282 at the recessed area 260, as shown in FIG. 13C. The recessed area 260 allows the rear walls 224, 226 of the beam 210 to be positioned in a generally planar alignment with one another. The line of contact of the protrusions 232 with the edge portion 276a of the sheet metal 212 provides a longitudinal spacing between the protrusions 232 that creates an exhaust opening for zinc oxide fumes resulting from welding to exit the interior of each tubular portion 216 of the beam 210. The separation between the planar portions of the sheet metal created by the protrusions 232 is approximately 50 microns to 300 microns. The protrusions 232 thus form an exhaust seam configured for continuous laser welding of the galvanized sheet that is continuously roll-formed into the cylindrically shaped beam 210. The exhaust openings allow fumes that would otherwise be trapped in the enclosed area of the tube to freely exit in order to have a consistent weld without gas openings or pockets that can form with pressurized gas, e.g., zinc oxide gas.
[0045] With the outer portion 276a near or in engagement with the contact surface 282, the sheet metal 212 can enter a welding station that may use an external mandrel to hold the cross-sectional shape for welding with the laser beam 266. However, there is no internal mandrel due to the location of the weld joint at the lap joint that is not otherwise affected by the external mandrel force applied around the beam 212. As shown in FIG. 13C, the laser welded lap joint 238 includes a thickness that separates the plane of the edge portion from the plane of the rear wall 224. The thickness of the weld joint 238 is formed by the protrusions 232 protruding from the plane (and / or edge portion) of the rear wall 224 such that when welding the lap joint, zinc oxide fumes 250 exit the interior of each tubular portion 216 of the beam through exhaust openings formed by the protrusions 232. Thus, to form the second tubular portion 216, the forming roll may deform the remaining section 276, for example, by slightly less than "half" the width of the sheet in the opposite rotational direction from the forming roll that formed the first tubular portion 214.
[0046] The beam 210 is made from a sheet 212 of steel material having a thickness of 0.8 mm to 1.4 mm or approximately 1 mm to 1.5 mm, and the sheet 212 may have a tensile strength of about 800 to 2000 MPa (i.e., about 120 to 290 ksi). However, it is envisioned that the beams of the present invention can be made from different materials including AHSS (advanced high strength steels) and that the beams of the present invention can be made from a sheet having a thickness of about 0.8 mm to 3.0 mm (or, for example, 0.8 mm to 1.4 mm), and can be made with different beam cross-sectional sizes, for example, about 80 mm to 150 mm in height, and 30 mm to 60 mm in depth, and have lengths that are variable in size for the desired application.
[0047] 14-17C, an additional example of a galvanized multi-tubular beam 310 is shown having two adjacent tubular portions 314, 316 that share a common central wall 318 of the beam 310. Unlike the beam 10 shown in FIG. 2, the welded joints 336, 338 are both formed as lap joints. The laser welded lap joints 336, 338 of the beam 310 shown in FIG. 14 are formed in recessed areas to allow the respective front walls 320, 322 and rear walls 324, 326 of the beam 310 to be positioned in generally planar alignment with one another, similar to that shown in the welded joint 38 of the beam 10 shown in FIG. 2.
[0048] The shaped beam 310 shown in Figures 14 and 15 may be rotated about its longitudinal axis to be oriented similarly to the beam 10 shown in Figure 2, for example, for use as a bumper reinforcement beam. The respective walls of the beam 310 may thereby be referred to as front wall 320, 322, rear wall 324, 326, top wall 328, and bottom wall 330. The front walls 320, 322 of adjacent tubular portions 314, 316 are substantially aligned with one another to form the outward or impact surface of the beam when used as a bumper reinforcement beam. Similarly, the rear walls 324, 326 are generally aligned with one another and substantially parallel to the front walls 320, 322. Additionally, the top and bottom walls 328, 330 are substantially parallel to one another and to the central wall 318, and generally perpendicular to the front and rear walls 320, 322, 324, 326. It will be appreciated that additional examples of beam 310 may take various orientations from those shown in Figures 14 and 15 and may include alternative cross-sectional shapes and dimensional proportions, for example, for different uses and applications of the beam.
[0049] 16A, galvanized sheet stock 312 may be roll formed through a series of roll dies to form a cross-sectional shape such as the example shown. This cross-sectional shape is achieved prior to closing the seam that is welded to enclose the first tubular portion 314 (FIG. 14). In this illustrated example, the seam-formed protrusions 332 (FIG. 16B) are formed in-line with the roll former after passing through several roll forming dies on the roll forming line. By roll forming the sheet stock 312 to achieve the intermediate cross-sectional shape of the beam 310 prior to forming the protrusions 332, the protrusions may then be formed without the risk of being damaged or flattened by passing through a roll forming die prior to being used in the weld seam. Specifically, as shown in FIG. 16A, an outer edge portion 372a of the sheet 312 used to form the first cylindrical portion 314 of the beam 310 is spaced downwardly from a desired contact surface 374 of the sheet to allow the laser beam 334 to have linear access to the contact surface 374 of the sheet 312 to form the protrusion 332 (FIG. 16B).
[0050] As further shown in FIG. 16A, after the projection 332 is formed, the front corner 388 of the tubular portion 314 may be used as a single articulation point on the sheet. The sheet may be bent about the front corner 388 to rotate the edge portion 372a of the sheet up into abutting engagement with the projection 332 formed at the contact surface 374, as shown in FIG. 16C. Thus, the cross-sectional shape may be formed to have essentially any desired shape and configuration of the first tubular portion 314 created in the outer section 372 of the sheet metal prior to forming the projection 332, such that only a final additional bend is required at the front corner 388 to close and complete the shape of the first tubular portion 314, as shown in FIG. 16A. It is also envisioned that additional or alternative articulation points may be used in other examples of the beam than those shown in FIGS. 16A-16C, such as beams with alternative cross-sectional shapes or roll forming sequences.
[0051] The protrusions 332 may be formed on a surface of the sheet 312 that corresponds to a portion of the sheet 312 that is desired to have a weld joint, such as the contact surface 374 of the formed sheet metal 312 shown in FIG. 16B. The contact surface 374 used to form the laser welded lap joint 336 is located in a recessed area 390 formed along the front wall 322 at the corner of the second tubular portion 316 adjacent the central wall 318. The protrusions 332 may be formed as the sheet metal passes continuously between the roll forming dies through a laser head station that is located in-line on the roll former. To form the protrusions 332, the laser beam 334 may be angled to a substantially perpendicular orientation relative to the contact surface 374. The protrusions 332 formed in-line on the roll former may be linearly spaced at substantially consistent intervals along the longitudinal extension of the sheet 312 and may otherwise be formed in the same or similar manner as shown in FIGS. 5A-5C and described above.
[0052] Prior to welding the seam of the first tubular portion 314 of the beam 310, one or more forming rolls may bend and rotate the edge portion 372a about the front corner 388 and further shape the outer section 372 of the sheet metal 312 to place the outer edge 372a into a line of protrusions 332 of the contact surface 374, as shown in FIG. 16C. The line of contact of the protrusions 332 against the edge portion 372a of the sheet metal 312 provides a longitudinal spacing between the protrusions 332 that creates an exhaust opening for the zinc oxide fumes 350 resulting from the welding to exit the interior of each tubular portion 314 of the beam 310 (FIG. 16C). The separation between the planar portions of the sheet metal created by the protrusions 332 is approximately 50 microns to 300 microns.
[0053] With the outer portion 372a near or in engagement with the contact surface 374, the sheet metal 312 can enter a welding station that may use an external mandrel to hold the cross-sectional shape for welding. However, due to the cross-sectional shape of the first tubular portion 314, there is otherwise no internal mandrel. As shown in FIG. 16C, a weld joint 336 is formed via laser welding along the exhaust seam to provide a continuously attached and closed seam along the length of the beam 310. Due to the protrusions 332 forming the exhaust opening, the weld joint 336 may have a thickness of, for example, approximately 50 microns to 300 microns. This slightly separates the plane of the edge portion 372a of the outer section 372 from the plane of the contact surface 374. When welding the weld joint 336, the longitudinal spacing between the protrusions 332 provides an exhaust opening for zinc oxide fumes 350 resulting from welding upstream from the welding station in the roll former to exit the interior of the tubular portion 314 of the beam 310. As shown in Figure 16C, the laser beam 352 generated by the welding station to form the weld joint 336 is positioned approximately perpendicular to the orientation of the central wall 318. This substantially perpendicular orientation of the laser beam 352 further forms the weld joint 336 with a relatively narrow heat affected zone, e.g., approximately 1 mm to 2 mm, as shown in Figure 7G.
[0054] After forming the weld joint 336, the sheet 312 continues into a second series of forming rolls at the station which continuously bend the other outer section 376 of the sheet 312 into the shape of the second tubular portion 316 of the beam 310. As shown in FIG. 17A, the cross-sectional shape is again formed near the seam of the tubular portion of the beam 310, but before closing the seam of the tubular portion of the beam 310. In the intermediate cross-sectional shape shown in FIGS. 17A and 17B, the protrusion 332 is again formed in-line at the seam in the roll former to reduce the risk of damaging or flattening the protrusion. Specifically, as shown in FIGURE 17A, the outer edge portion 376a of the sheet 312 used to form the second tubular portion 316 of the beam 310 is spaced upwardly from the desired contact surface 382 of the sheet to allow the laser beam 384 to directly access the contact surface 382 of the sheet 312 to form the protrusion 332. The example shown in FIGURES 14-17C illustrates the contact surface 382 that is used to form the laser welded lap joint 338 at the recessed area 360 formed along the rear wall 24 at the corner of the first tubular portion 314 adjacent the central wall 318.
[0055] As further shown in FIG. 17A, a rear corner 386 of the second tubular portion 316 on the opposite side of the tubular portion 316 from the weld joint 336 may be used as a single articulation point on the sheet. The sheet may be bent about the rear corner 386 to rotate the edge portion 376a of the sheet downward into abutting engagement with the protrusion 332 formed at the contact surface 382 as shown in FIG. 17C. Thus, as shown in FIG. 17A, the cross-sectional shape may be formed to have essentially any desired shape and configuration of the second tubular portion 316 created at the outer section 376 of the sheet metal prior to forming the protrusion 332 at the contact surface 382 such that only a final additional bend is required at the rear corner 386 to close and complete the shape of the second tubular portion 316. It is also envisioned that additional or alternative articulation points may be used in other examples of beams than those shown in FIGS. 17A-17C, such as beams with alternative cross-sectional shapes or roll forming sequences.
[0056] As shown in FIG. 17B, protrusions 332 may be formed as the sheet metal passes continuously between the roll forming dies through a laser head station located in-line on the roll former. The protrusions 332 shown in FIG. 17B may be formed in the same or similar manner as in FIGS. 5A-5C and described above. To form the protrusions 332, the laser beam 384 may be angled at a substantially perpendicular orientation relative to the contact surface 382. Similarly, the laser beam 366 used in forming the corresponding weld joint 336 may be substantially perpendicular to the contact surface 382.
[0057] Prior to welding the seam of the second tubular portion 316 of the beam 310, one or more forming rolls may further shape the outer section 376 of the sheet metal 312 to bend and rotate the edge portion 376a about the rear corner 386 and place the outer edge 376a in contact with the line of protrusions 332 of the contact surface 382 at the recessed area 360, as shown in FIG. 17C. The recessed area 360 allows the rear walls 324, 326 of the beam 310 to be positioned in a generally planar alignment with one another. The line of contact of the protrusions 332 with the edge portion 376a of the sheet metal 312 provides a longitudinal spacing between the protrusions 332 that creates an exhaust opening for zinc oxide fumes resulting from welding to exit the interior of each tubular portion 316 of the beam 310. The separation between the planar portions of the sheet metal created by the protrusions 332 is approximately 50 microns to 300 microns. The protrusions 332 thus form an exhaust seam configured for continuous laser welding of the galvanized sheet that is continuously roll-formed into the cylindrically shaped beam 310. The exhaust openings allow fumes that would otherwise be trapped in the enclosed area of the tube to freely exit in order to have a consistent weld without gas openings or pockets that can form with pressurized gas, e.g., zinc oxide gas.
[0058] With the outer portion 376a near or in engagement with the contact surface 382, the sheet metal 312 can enter a welding station that may use an external mandrel to hold the cross-sectional shape for welding with the laser beam 366. However, there is no internal mandrel due to the location of the weld joint at the lap joint that is not otherwise affected by the external mandrel force applied around the beam 312. As shown in FIG. 17C, the laser welded lap joint 338 includes a thickness that separates the plane of the edge portion from the plane of the rear wall 324. The thickness of the weld joint 338 is formed by the protrusions 332 protruding from the plane (and / or edge portion) of the rear wall 324 such that when welding the lap joint, zinc oxide fumes 350 exit the interior of each tubular portion 316 of the beam through exhaust openings formed by the protrusions 332. Thus, to form the second tubular portion 316, the forming roll may deform the remaining section 376, for example, by slightly less than "half" the width of the sheet in the opposite rotational direction from the forming roll that formed the first tubular portion 314.
[0059] The beam 310 is formed from a sheet 312 of steel material having a thickness of 0.8 mm to 1.4 mm or approximately 1 mm to 1.5 mm. The sheet 312 may also have a tensile strength of about 800 to 2000 MPa (i.e., about 120 to 290 ksi). However, it is envisioned that the beams of the present invention may be made from different materials including AHSS (advanced high strength steels) and that the beams of the present invention may be made from a sheet having a thickness of about 0.8 mm to 3.0 mm (or, for example, 0.8 mm to 1.4 mm), and may be made with different beam cross-sectional sizes, for example, heights of about 80 mm to 150 mm, and depths of 30 mm to 60 mm, and have lengths that are variable in size for the desired application.
[0060] 18-19B, an additional example of a galvanized multi-tubular beam 410 is shown having two adjacent tubular portions 414, 416 that share a common central wall 418 of the beam 410. The beam 410 has a laser welded lap joint 436 formed in the recessed area to allow the rear walls 424, 426 of the beam 410 to be positioned in generally planar alignment with respect to one another. The beam 410 also has a weld joint 438 formed in the seam between the central wall 418 and the front wall 422 to enclose the second tubular portion 416.
[0061] The shaped beam 410 shown in FIG. 18 can be rotated about its longitudinal axis to be oriented similarly to the beam 10 shown in FIG. 2, for example, for use as a bumper reinforcement beam. The respective walls of the beam 410 can then be referred to as a front wall 420, 422, a rear wall 424, 426, an upper wall 428, and a lower wall 430. The front walls 420, 422 of adjacent cylindrical portions 414, 416 are substantially aligned with each other to form the outward or impact surface of the beam when used as a bumper reinforcement beam. Similarly, the rear walls 424, 426 are generally aligned with each other and substantially parallel to the front walls 420, 422. Additionally, the upper and lower walls 428, 430 are substantially parallel to each other and to the central wall 318, and generally perpendicular to the front and rear walls 420, 422, 424, 426. It will be appreciated that additional examples of beam 410 may take various orientations from those shown in FIG. 18 and may include, for example, alternative cross-sectional shapes and dimensional proportions for different uses and applications of the beam.
[0062] 19A, the galvanized sheet stock 412 may be roll formed through a series of roll dies to form a cross-sectional shape as shown in solid lines that is achieved prior to closing the seam that is welded to encircle the first tubular portion 414 (FIG. 18). In this illustrated example, the seam-formed protrusions 432 are formed in-line with the roll former after passing through several roll forming dies on the roll forming line. By roll forming the sheet stock 412 to achieve the intermediate cross-sectional shape of the beam 410 prior to forming the protrusions 432, the protrusions may then be formed without the risk of being damaged or flattened by passing through a roll forming die prior to being used in the weld seam. Specifically, as shown in FIG. 19A , an outer edge portion 472a of the sheet 412 used to form the first cylindrical portion 414 of the beam 410 is spaced upwardly from a desired contact surface 474 of the sheet so as to allow the laser beam 434 to directly access the contact surface 474 of the sheet 412 to form the protrusion 432.
[0063] 19A, a rear corner 488 of the tubular portion 414 may be used as a single articulation point on the sheet after the projection 432 is formed. As shown by the dashed lines, the sheet may be bent about the rear corner 488 to rotate the edge portion 472a of the sheet downward into abutting engagement with the projection 432 at the contact surface 474. Thus, the cross-sectional shape may be formed to have essentially all of the desired shape and configuration of the first tubular portion 414 created in the outer section 472 of the sheet metal prior to forming the projection 432, such that only a final additional bend is required at the rear corner 488 to close and complete the shape of the first tubular portion 414.
[0064] The protrusions 432 may be formed at a surface of the sheet 412 that corresponds to a portion of the sheet 412 that is desired to have a welded joint, such as at a contact surface 474 of the formed sheet metal 412 shown in FIG. 19A. The contact surface 474 used to form the laser welded lap joint 436 is located in a recessed area molded along the rear wall 426 at the corner of the second tubular portion 416 adjacent the central wall 418. The protrusions 432 may be formed as the sheet metal passes continuously between the roll forming dies through a laser head station that is located in-line on the roll former. To form the protrusions 432, the laser beam 434 may be angled to a substantially perpendicular orientation relative to the contact surface 474. The protrusions 432 formed in-line on the roll former may be linearly spaced at substantially consistent intervals along the longitudinal extension of the sheet 412 and may otherwise be formed in the same or similar manner as shown in FIGS. 5A-5C and described above.
[0065] Prior to welding the seam of the first tubular portion 414 of the beam 410, one or more forming rolls may further shape the outer section 472 of the sheet metal 412 to bend and rotate edge portion 472a about rear corner 488 and place the outer edge 472a in contact with the line of protrusions 432 of the contact surface 474, as shown in FIG. 19A by a dashed line. The line of contact of the protrusions 432 against the edge portion 472a of the sheet metal 412 provides longitudinal spacing between the protrusions 432 that creates exhaust openings for zinc oxide fumes resulting from welding to exit the interior of each tubular portion 414 of the beam 410.
[0066] With the outer portion 472a near or in engagement with the contact surface 474, the sheet metal 412 can enter a welding station that may use an external mandrel to hold the cross-sectional shape for welding. However, due to the cross-sectional shape of the first tubular portion 414, there is otherwise no internal mandrel. As shown by the dashed line in FIG. 19A, the weld joint 436 is formed via laser welding with the laser beam 452 along the exhaust seam to provide a continuously attached and closed seam along the length of the beam 410. During welding, the laser beam 452 may be positioned in the same or similar orientation relative to the laser beam 434 used to form the protrusion 432. Due to the protrusion 432 forming the exhaust opening, the weld joint 436 may have a thickness of, for example, approximately 50 microns to 300 microns, slightly separating the plane of the edge portion 472a of the outer section 472 from the plane of the contact surface 474. The substantially vertical orientation of laser beam 452 further forms a weld joint 436 with a relatively narrow heat affected zone, for example, approximately 1 mm to 2 mm, as shown in FIG. 7G.
[0067] Referring to FIG. 19B, after the formation of the weld joint 436, the sheet 412 continues into a second series of forming rolls in a station. The second series of forming rolls in a station further continuously bends the other outer section 476 of the sheet 312 (FIG. 19A) to the shape of the second tubular portion 416 of the beam 410. The cross-sectional shape can be formed near the seam of the tubular portion 416 of the beam 410, but before closing the seam of the tubular portion 416 of the beam 410. In the intermediate cross-sectional shape shown in solid lines in FIG. 19B, the protrusion 432 can be formed in the formed tip region of the outer edge portion 476a. Thereby, the protrusion 432 is formed after the shape of the edge portion 476a is formed, to reduce the risk of damaging or flattening the protrusion. 19B, the outer edge portion 476a of the sheet 412 used to form the second tubular portion 416 of the beam 410 is spaced downwardly from the desired contact surface 482 of the sheet to allow the laser beam 484 to contact linearly and generally perpendicularly the surface of the tip region of the outer edge portion 476a of the sheet 412 to form the protrusion 432. Alternatively, it is contemplated that the protrusion may be formed in a lower region of the central wall of the opposing contact surfaces of the resulting weld joint.
[0068] As further shown in FIG. 19B, a rear corner 486 of the second tubular portion 416 may be used as a single articulation point on the sheet. The sheet may be bent about the rear corner 486 to rotate the formed edge portion 476a of the sheet down into abutting engagement with the protrusion 432 formed on the contact surface 482, as shown in dashed lines in FIG. 19B. Thus, the cross-sectional shape may be formed to have essentially any desired shape and configuration of the second tubular portion 416 created in the outer section 476 of the sheet metal prior to forming the protrusion 432, such that only a final additional bend is required at the rear corner 486 to close and complete the shape of the second tubular portion 416. It is also envisioned that additional or alternative articulation points may be used in other examples of the beam than those shown in FIGS. 19A and 19B, such as beams with alternative cross-sectional shapes or roll forming sequences.
[0069] As shown in FIG. 19B, the protrusions 432 may be formed as the sheet metal passes continuously between roll forming dies through a laser head station that is located in-line on the roll former. The protrusions 432 shown in FIG. 19B may again be formed in the same or similar manner as otherwise shown in FIGS. 5A-5C. Prior to welding the seam of the second tubular portion 416 of the beam 410, one or more forming rolls may further shape the outer section 476 of the sheet metal 412 to bend and rotate about the rear corner 486 and place the outer edge 476a in contact with a contact surface 482 located on the central wall 418, as shown in dashed lines in FIG. 19B. Again, the lines of contact of the protrusions 432 at the edge portion 476a of the sheet metal 412 to the central wall 418 provide longitudinal spacing between the protrusions 432 that creates vent openings for zinc oxide fumes resulting from welding of the seam 438, such as by laser beam 466, to exit the interior of the tubular portion 416 of each beam 410. The vent openings allow fumes that would otherwise be trapped in the enclosed area of the tube to freely exit due to having a consistent weld without gas openings or pockets that may form with pressurized gas, e.g., zinc oxide gas.
[0070] The beam 410 may be made from a sheet 412 of steel material having a thickness of 0.8 mm to 1.4 mm or approximately 1 mm to 1.5 mm, and the sheet 412 may have a tensile strength of about 800 to 2000 MPa (i.e., about 120 to 290 ksi). However, it is envisioned that the beams of the present invention may be made from different materials, including AHSS (advanced high strength steel), and that the beams of the present invention may be made from sheets having a thickness of 0.8 mm to 3.0 mm (or, for example, 0.8 mm to 1.4 mm), and may be made with different beam cross-sectional sizes, for example, about 80 mm to 150 mm in height, and 30 mm to 60 mm in depth, and may have lengths that are variable in size for the desired application.
[0071] 20 and 20A, another example of a galvanized multi-tubular beam 510 is shown having two adjacent tubular portions 514, 516 sharing a common central wall 518 of the beam 510. The beam 510 has a laser welded split joint 537 formed at the seam between the central wall 518 and the front and rear walls 520, 522 and 524, 526 to enclose the tubular portions 514, 516. The weld joint 537 is formed via laser welding along the vent seam with a laser beam 566 by directing the laser into each split seam approximately perpendicular to the orientation of the front and rear walls 520, 522, 524, 526. Also, a protrusion can be provided at the split seam to form a vent opening for zinc oxide fumes resulting from welding to exit the interior of the tubular portion of the beam 510 from the welding station upstream in the roll former.
[0072] For purposes of this disclosure, the terms "top," "bottom," "right," "left," "rear," "front," "vertical," "horizontal," and derivatives thereof, refer to the orientation depicted in FIG. 1. However, it should be understood that various alternative orientations may be provided, unless expressly specified otherwise. It should also be understood that the specific devices and processes illustrated in the accompanying drawings and described in this specification are merely exemplary embodiments of the inventive concepts defined in the appended claims. Hence, specific dimensions and other physical characteristics relating to the embodiments disclosed herein are not to be considered limiting, unless the claims expressly state otherwise.
[0073] Variations and modifications of the specifically described embodiments may be made without departing from the principles of the invention. It is intended that the invention be limited only by the scope of the appended claims as interpreted in accordance with the principles of patent law. It is to be understood that the disclosure has been described in an illustrative manner, and that the terminology used is in the nature of words of description rather than of limitation. Many modifications and variations of the disclosure are possible in light of the above teachings, and the disclosure may be practiced in ways other than as specifically described.
Claims
1. A galvanized multi-tubular beam for vehicle structure or bumper reinforcement, comprising: the galvanized multi-tubular beam having two adjacent tubular portions sharing a common central wall of the beam; outer sections of the galvanized sheet metal forming the two adjacent tubular portions extend from opposite sides of a central section of the galvanized sheet metal forming the common central wall of the beam; the galvanized multi-tubular beam includes an edge portion of one of the outer sections of the galvanized sheet metal attached to the central section of the galvanized sheet metal by a welded joint; the weld joint has a thickness separating a plane of the edge portion from a plane of the central section; the thickness of the weld joint is formed by a plurality of protrusions protruding from the plane of the outer section or the central section of the sheet metal; an exhaust opening is provided by the plurality of protrusions between a plane of the edge portion and a plane of the central section, the exhaust opening being configured to allow zinc oxide fumes resulting from welding of the weld joint to exit the weld joint; Galvanized multi-tubular beam.
2. 2. The galvanized multi-tubular beam of claim 1, wherein said weld joint extends continuously along said beam to surround said interior of said respective tubular portions of said beam.
3. The galvanized multi-tube beam of claim 1 , wherein said plurality of protrusions are consistently spaced apart.
4. The galvanized multi-tubular beam of claim 3 , wherein said welded joints interconnect said plurality of projections.
5. The galvanized multi-tubular beam of claim 1, wherein the weld joint has a narrow heat affected zone of approximately 1 mm to 2 mm.
6. 2. The galvanized multi-tubular beam of claim 1, wherein a second edge portion of the galvanized sheet metal is attached to a side wall of the tubular portion of the beam that is generally perpendicular to the central wall of the beam.
7. 7. The galvanized multi-barrel beam of claim 6, wherein said second edge portion and said side wall portion are attached together with a laser welded lap joint.
8. the laser welded lap joint includes a second thickness separating a plane of the second edge portion from a plane of the sidewall; 8. The galvanized multi-tubular beam of claim 7, wherein the thickness of the weld joint is formed by the second plurality of protrusions protruding from the plane of the second edge portion or side wall, and configured such that zinc oxide fumes resulting from welding of the lap joint exit the laser welded lap joint.
9. 2. The galvanized multi-tubular beam of claim 1, wherein a separation between said edge portions and said central section formed by said weld joint is approximately 50 microns to 300 microns.
10. The galvanized multi-tubular beam of claim 1, wherein each of said plurality of protrusions has a length of approximately 2 mm to 5 mm.
11. 2. The galvanized multi-tubular beam according to claim 1, wherein the thickness of said metal sheet is approximately 1 mm to 1.5 mm.
12. 1. A method for continuously forming a galvanized reinforcement beam, comprising: The method further comprising: unrolling a roll of galvanized sheet stock in a generally horizontal plane; forming a protrusion over a top surface of the sheet metal stock; roll forming the sheet stock through a set of a plurality of roll stations to form a tubular shape with edge sections of the sheet stock in contact with a middle section of the sheet stock; roll forming, wherein at least one of the edge section or the middle section of the sheet stock includes the protrusion, the protrusion forming a vent gap between the edge section and the middle section of the sheet stock; laser welding the edge sections of the sheet stock to the middle section at a laser head station to continuously form a weld joint, wherein zinc oxide gas resulting from the welding is allowed to exit the weld joint; The method includes:
13. The method of claim 12 , wherein the protrusions are generally consistently spaced and linearly disposed across the top surface of the sheet metal stock.
14. The method of claim 12 , wherein each of the protrusions includes a raised portion that protrudes from the upper surface a height approximately equal to a width of the vent gap.
15. The method of claim 12 , wherein the protrusions are formed by at least one of laser dimpling, mechanical deformation, electrical discharge deposition, or added material.
16. The method of claim 12 , wherein the sheet stock is longitudinally stretched at a substantially constant rate, roll formed, and welded.
17. The method of claim 12 , wherein the protrusions are formed successively at interleaved stations in the set of multiple roll stations.
18. 20. The method of claim 17, wherein the protrusions are formed with a laser head station disposed between a first station and a last station of the set of multiple roll stations to form the protrusions during the roll forming process.
19. 1. A galvanized multi-tubular beam, the galvanized multi-tubular beam having two adjacent tubular portions sharing a common central wall of the beam; The galvanized multi-tubular beam is edge portions of the outer sections of the galvanized sheet metal attached via welded joints to reinforcement ribs formed in the central section of the galvanized sheet metal, the edge portions of the galvanized sheet metal forming the common central wall of the beam; the weld joint has a thickness that separates a plane of the edge portion from a plane of the reinforcement rib; The thickness of the weld joint is formed by a plurality of protrusions protruding from the plane of at least one of the edge portion or the reinforcement rib; an exhaust opening is provided by the plurality of protrusions between a plane of the edge portion and a plane of the central section, the exhaust opening being configured to allow zinc oxide fumes resulting from welding of the weld joint to exit the weld joint; Galvanized multi-tubular beam.
20. the sheet stock is roll-formed to include a second tubular portion sharing a common central wall with the tubular portion of the beam; The method of claim 12 , wherein the outer sections of sheet metal stock extend from opposite sides of a central section of the sheet metal that forms the common central wall of the beam.
21. 21. The method of claim 20, wherein the protrusion is formed continuously on an edge portion of one of the outer sections and contacts the common center wall of the galvanized sheet stock to form the weld joint along the common center wall.
22. The method of claim 21 , wherein the protrusions are formed during the roll forming process at a laser head station disposed in the set of multiple roll stations.
Citation Information
Patent Citations
Laser welding method
JP2013530048A
Forming method of bumper beam for vehicles
KR101334621B1
Roll forming system and method thereof, and bumper beam prepared by using the same
KR1020110011082A
Profile for an automobile structural element and corresponding chassis
US20040130166A1
Bumper beam having ribs on several walls of the bumper beam
WO2018092058A1