Stereolithography process for producing copper parts with low resistivity

The stereolithography method for copper parts using a specific paste composition and controlled atmospheres addresses the challenges of traditional 3D printing, achieving low resistivity and high mechanical strength in complex copper parts.

JP7553463B2Active Publication Date: 2024-09-18COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021559867
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-12
Filing Date
2020-04-10
Publication Date
2024-09-18
Estimated Expiration
2040-04-10

AI Technical Summary

Technical Problem

Existing 3D printing methods for copper parts face challenges such as residual stresses, poor surface quality, high material costs, and environmental health risks, particularly when producing high-density parts with complex geometries.

Method used

A stereolithography method involving a paste composition of copper particles, photopolymerizable resin, and photoinitiator, followed by debinding in an oxidizing atmosphere and sintering in a reducing atmosphere, to produce copper parts with low carbon and oxygen content, ensuring high purity and low resistivity.

Benefits of technology

The method results in copper parts with low electrical resistivity and good mechanical strength, overcoming the limitations of traditional 3D printing techniques by reducing carbon and oxygen content, and enabling the production of complex shapes without cracks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553463000006
    Figure 0007553463000006
  • Figure 0007553463000012
    Figure 0007553463000012
  • Figure 0007553463000009
    Figure 0007553463000009
Patent Text Reader

Abstract

At least the following sequential steps: a) forming a part by stereolithography, a1) forming a paste layer comprising a powder of copper particles, one or more photopolymerizable precursors of a first resin, a photoinitiator, and optionally optical additives; a2) photopolymerizing a photopolymerizable precursor of the first resin wherein steps a1) and a2) form a cycle that can be repeated multiple times, b) heating to a first temperature T d performing a first heat treatment to remove the first resin; c) heating to a first temperature T d A second higher temperature T f A step of performing a second heat treatment to sinter the copper particles and obtain a copper part. A method for manufacturing a copper part, comprising:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a 3D printing method, in particular a stereolithography method, for manufacturing copper parts.

[0002] The present invention is particularly interesting because it makes it possible to obtain high density components with complex and / or textured geometries, with very high purity and therefore low resistivity, whilst not increasing the manufacturing costs.

[0003] The invention finds applications in many industrial sectors, especially in the energy sector, because copper has high thermal (385 W / m K) and electrical properties (59.6 × 106 S m -1 ) Such methods make it possible to design new geometries for manufacturing, for example, heat exchangers or electrical converters.

[0004] The invention also relates to a paste for the production of copper parts by stereolithography, in particular the paste makes it possible to obtain crack-free parts, which is particularly advantageous when producing heavy copper parts. [Background technology]

[0005] Currently, metal parts with complex geometries are primarily produced by additive manufacturing (AM).

[0006] Metal additive manufacturing is mainly represented by the techniques of melting on a powder bed: laser melting on a powder bed (or LBM for "laser beam melting") or melting by an electron beam on a powder bed (EBM for "electron beam melting").

[0007] However, these techniques, like other 3D printing techniques by fusion, have the following drawbacks: - after manufacturing, residual stresses exist in the part and a subsequent heat treatment is required to relieve the thermomechanical stresses; - Changes in local composition due to evaporation of components, - Poor surface quality, requiring a polishing process; - the need for powders with specific particle size distributions to achieve optimal layering, which creates significant raw material purchasing costs; - There is control and handling of powders during the polishing and cleaning process, which therefore requires particular precautions in terms of health, safety and the environment.

[0008] Finally, the laser / material interaction is not effective for producing high density parts, especially for copper, which is a very good thermal conductor and reflective material, so specific machines (with laser emission at green 520 nm instead of 1064 nm) need to be developed.

[0009] To overcome these problems, the manufacture of metal parts by stereolithography (SLA) is becoming widespread. This technique consists of depositing a first layer of paste containing copper powder, a photopolymerizable resin and a photoinitiator on a support and polymerizing this layer in one or more selected areas by the action of a suitable radiation, generally UV (typically 365 nm). A second layer, processed according to the same principle, is then superimposed on top of this first layer, and these operations are repeated until a three-dimensional polymerized part with the desired geometry is formed.

[0010] The polymer gives the part sufficient mechanical strength during its manufacture. It is then thermally removed in a debinding step and the part is then consolidated by sintering. The thermal cycles of metal debinding and sintering are mainly carried out in vacuum or argon to avoid oxidation of the copper. Compared to additive manufacturing by melting on a powder bed, these techniques have the advantage that they can rely on powder metallurgical know-how for debinding / sintering and can be easily integrated by manufacturers in this field.

[0011] In Lee et al. ("Development of micro-stereolithography technology using metal powder", Microelectronic Engineering 83 (2006), pp. 1253-1256), a formulation with up to 30% volume loading of 3 μm diameter copper particles is fabricated by SLA laser. For example, the formulation may contain 1,6-hexanediol diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA) as precursors of acrylate resins, N-vinyl-2-pyrrolidone (NVP) as reactive diluent, and dimethoxyphenylacetophenone (DMPA) as photoinitiator. A first debinding heat treatment is performed in vacuum at 600° C. for 1 hour, followed by a second sintering heat treatment in vacuum at 960° C. for 3 hours. The electrical resistivity of sintered parts is 200-300 nΩ·m (i.e. more than 10 times the electrical resistivity of pure copper), which can be caused by the presence of carbon contamination and / or high porosity.

[0012] In WO 02 / 07918 A1, paste compositions containing precursors of acrylate resins and metal powders are studied. It is pointed out that it is preferable to carry out the desintering step in a vacuum in order to limit the stresses at the origin of expansion and cracks. This step can be carried out under reducing gas scavenging to remove carbon residues. To avoid oxidation of the metal particles, which can lead to differential shrinkage and therefore stresses and distortions, it is possible to provide an additional treatment of dosing the carbonated residues in the presence of an atmosphere containing oxygen, carbon monoxide or carbon dioxide in a controlled manner. It is also shown that the sintering step can be carried out in a neutral atmosphere (argon or nitrogen), in a reducing atmosphere or in a vacuum. More specifically, in the examples, it is shown that the debinding step is carried out in a primary vacuum (10 -2 The sintering process was carried out in a vacuum of 10 MPa for 40 h, and the sintering process was carried out in the presence of argon or in a secondary vacuum (10 -6 ~10 -4However, such a method is time consuming and difficult to commercialize. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] WO 02 / 07918(A1) [Non-patent literature]

[0014] [Non-Patent Document 1] Lee et al., “Development of micro-stereolithography technology using metal powder,” Microelectronic Engineering 83 (2006), pp. 1253-1256. Summary of the Invention [Problem to be solved by the invention]

[0015] It is therefore an object of the present invention to provide a method for manufacturing copper components with low resistivity, which is easy to implement and industrializable. [Means for solving the problem]

[0016] The objective is to provide a method for the preparation of ... polymeric material comprising the following steps: a) forming a part by stereolithography, the forming comprising: a1) forming a paste layer comprising a powder of copper particles, one or more photopolymerizable precursors of a first resin, a photoinitiator and optionally optical additives; a2) photopolymerizing a photopolymerizable precursor of the first resin wherein steps a1) and a2) form a cycle that can be repeated multiple times, b) in a first atmosphere at a first temperature T d performing a first heat treatment to remove the first resin; c) in a second atmosphere at a first temperature T d A higher second temperature T f A step of performing a second heat treatment to sinter the copper particles and obtain a copper part. Including, The first atmosphere comprises an oxidizing atmosphere containing at least 10% by volume of an oxidizing agent, such as dioxygen, and the second atmosphere comprises a reducing atmosphere. This is achieved by the manufacturing method of copper parts by 3D printing, in particular stereolithography.

[0017] The present invention differs from the prior art essentially in the performance of a debinding step in an oxidizing atmosphere, which is concomitant with the performance of a sintering step in a reducing atmosphere.

[0018] The combination of these two atmospheres results in sintered parts with low carbon and oxygen content, high purity and therefore low electrical resistivity.

[0019] By low carbon content is to be understood a carbon content lower than 0.1% by weight, preferably a carbon content lower than 0.05% by weight, even more preferably a carbon content lower than 0.02% by weight.

[0020] By low oxygen content is to be understood an oxygen content below 0.1% by weight.

[0021] In the prior art methods, the amount of dioxygen in the debinding step is zero or controlled to avoid oxidation of the metal particles. Thus, carbonated residues of unburned resin remain in the part. The materials obtained in such methods are therefore not pure metals, but rather metal / ceramic or metal / carbon composites. These materials are neither characterized by low carbon content nor low oxygen content.

[0022] In the method of the invention, the debinding step is carried out in an oxidizing agent-rich atmosphere (higher than 10% by volume). Such a step seems counterintuitive, since it is known that working in an oxidizing atmosphere leads to oxidation of the metals and thus to mechanical brittleness of the resulting parts and / or parts with poorer thermal or electrical properties. However, the resulting parts have low resistivity and very good mechanical strength. Without being bound by theory, it is likely that the organic matrix (resin, photopolymerizable precursor) present in the paste is largely or completely decomposed during the first heat treatment, with the formation or degassing of CO or CO2. The oxygen content in the parts obtained at the completion of the first heat treatment is reduced thanks to the second heat treatment in a reducing atmosphere.

[0023] By reducing atmosphere is to be understood an atmosphere containing dihydrogen, which can be used alone or mixed with so-called natural gases such as argon or nitrogen.

[0024] By made of copper it is to be understood that the part is made up of copper, possibly containing impurities (which typically account for less than 0.2% by weight).

[0025] The manufacturing method for copper parts is simple to implement and does not require precise monitoring of the oxygen content. The resulting parts are more homogeneous. The stereolithography manufacturing method makes it possible to produce parts with various complex geometries. Furthermore, in contrast to the SLM process, the manufacture of copper parts by SLA does not involve the mixing of different powders.

[0026] Advantageously, the first atmosphere contains at least 15% by volume, preferably at least 20% by volume, of dioxygen.

[0027] Advantageously, the first heat treatment is carried out in air, which greatly simplifies the method.

[0028] Advantageously, the first heat treatment is carried out at a temperature between 300 and 800 ° C. The debinding temperature T d Depends on the binder being implemented.

[0029] Advantageously, the first heat treatment is carried out for a period of between 2 and 7 hours.

[0030] Advantageously, the second heat treatment is carried out at a temperature between 980 and 1080° C., advantageously between 980 and 1075° C. The sintering temperature of copper is clearly indicated and depends on the method of preparation of the powder, the particle size and on the auxiliary substances that may be added.

[0031] Advantageously, the second heat treatment is carried out for a period ranging from 1 to 7 hours, preferably from 1 to 4 hours.

[0032] Increasing the duration of sintering and / or increasing the sintering temperature not only reduces the amount of oxygen present in the part, but also results in a denser part.

[0033] Advantageously, step a2) is carried out by laser or digital light processing (DLP). The use of a DLP light source makes it possible to illuminate the entire part at once, which simplifies the process, makes the illumination and therefore the crosslinking more homogeneous and increases the production speed.

[0034] Advantageously, the paste comprises a tetrafunctional acrylate, a difunctional acrylate and 2,2-dimethoxy-2-phenylacetophenone. Surprisingly, it has been observed that with such a paste composition, no or very few cracks occur in the parts. It is therefore possible to produce heavy parts of very good quality.

[0035] Even more preferably, the tetrafunctional acrylate is di(trimethylolpropane)tetraacrylate and the difunctional acrylate is bisphenol A ethoxylate dimethacrylate.

[0036] Advantageously, the copper powder comprises at least 35% by volume of the paste, preferably 35-65% by volume. The ratio of copper particles to resin is adjusted according to the mechanical properties required in the composite material. The volume percentages are to be understood herein and hereinafter as being based on the total volume of the paste.

[0037] Advantageously, the copper particles have a maximum dimension smaller than 45 μm, preferably smaller than 25 μm.

[0038] Advantageously, the optical additive is selected from silica, polythiophene, polyvinyl alcohol, polypropylene, and a pre-crosslinked and milled second resin. By adding any of these additives to the paste, a paste is obtained with good reactivity (i.e. reactivity of less than 30 seconds, in some cases less than 2 seconds depending on the nature of the optical additive) that is comparable to SLM type processes in terms of production speed, while avoiding the disadvantages of the SLM process mentioned above.

[0039] The present invention relates to a paste intended for use in a stereolithography process to produce copper parts, comprising: - copper powder, - a plurality of photopolymerizable precursors of a first resin; - a photoinitiator, and - optionally an optical additive selected from silica, polythiophene, polyvinyl alcohol, polypropylene, and a pre-crosslinked and ground second resin, a photopolymerizable precursor consisting of a tetrafunctional acrylate and a difunctional acrylate, and a photoinitiator consisting of 2,2-dimethoxy-2-phenylacetophenone; The present invention also relates to a paste comprising:

[0040] Advantageously, the tetrafunctional acrylate is di(trimethylolpropane)tetraacrylate and the difunctional acrylate is bisphenol A ethoxylate dimethacrylate.

[0041] Such pastes are of particular interest for the production of components, especially heavy components, since the resulting components are unlikely or do not exhibit any cracks at all.

[0042] The paste is obtained by mixing, in particular, a photopolymerizable precursor of the resin, in viscous or liquid form, with copper powder ensuring perfect homogeneity of the mixture, reducing the steps of handling the powder and limiting the environmental and health risks associated with handling the powder.

[0043] Other features and advantages of the present invention will become apparent from the following supplemental description.

[0044] Needless to say, this supplemental description is provided solely for the purpose of illustrating the subject matter of the present invention, and should not be construed as limiting this subject matter.

[0045] The invention will be better understood on reading the description of embodiments given for purely indicative and non-limiting purposes with reference to the accompanying drawings, in which: [Brief description of the drawings]

[0046] [Figure 1] 1 is a graph depicting the thickness of different paste layers filled with copper particles, crosslinked at 365 nm, as a function of exposure time for different paste compositions in accordance with certain embodiments of the present invention. [Diagram 2] 1 represents a 30*30 mm2 green copper part fabricated by SLA in accordance with a specific embodiment of the present invention. [Figure 3a] 1 represents a green copper part (using a photocrosslinkable resin) prior to debinding according to another specific embodiment of the present invention. [Figure 3b] 13 depicts a green copper part (using a photocrosslinkable resin) after debinding in air and sintering in hydrogen according to another specific embodiment of the present invention. [Figure 4]13 illustrates an optical image of a section of a part after debinding under air and sintering under H2 with a density of 94.5% according to another specific embodiment of the present invention. [Figure 5a] 5A-5C are photographic images of parts obtained according to different embodiments of the method of the present invention. [Figure 5b] 5A-5C are photographic images of parts obtained according to different embodiments of the method of the present invention. [Figure 5c] 5A-5C are photographic images of parts obtained according to different embodiments of the method of the present invention. [Figure 5d] 5A-5C are photographic images of parts obtained according to different embodiments of the method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] The present invention relates to a method for producing copper parts by three-dimensional printing.

[0048] The method comprises at least the following sequential steps: a) forming a part by stereolithography, the forming comprising: a1) forming a paste layer comprising copper powder, a photopolymerizable resin, a photoinitiator, and optionally optical additives and / or reactive diluents; a2) photopolymerizing a photopolymerizable precursor of the first resin to form the first resin. wherein steps a1) and a2) form a cycle that can be repeated multiple times, b) heating the part to a first temperature T in an oxidizing atmosphere containing at least 10% by volume of an oxidizing agent. d performing a first heat treatment to remove the first resin; c) in a reducing atmosphere at a first temperature T d A higher second temperature T f A step of performing a second heat treatment to sinter the copper particles and obtain a copper part. Includes.

[0049] Build the part: The part is built in step a) by stereolithography, i.e. obtained by the sequential polymerization of several paste layers.

[0050] The paste comprises copper powder, one or more photopolymerizable precursors of the first resin (so-called polymeric or organic binders), one or more photoinitiators, and optionally optical additives. The paste is viscous, optionally liquid, and its components are advantageously homogeneously dispersed.

[0051] The copper powder occupies at least 35% by volume in order to obtain a dense part after heat treatment. Preferably, the powder occupies 35-65% by volume of the paste, more preferably 40-65% by volume, even more preferably 45-65% by volume. This percentage is the so-called packing percentage. Such a packing percentage leads to a proper distribution of the powder in the polymer and to a sufficient amount of deposits homogeneously distributed in the copper matrix.

[0052] The particles forming the copper powder preferably have a diameter smaller than 50 μm, for example a diameter of 49 μm, even more preferably a diameter smaller than 30 μm. For example, the particles have a diameter smaller than 25 μm. Advantageously, the copper particles have a diameter larger than 5 μm, for example a diameter of 8 μm or more. For example, the diameter of the particles ranges from 5 to 25 μm or from 8 to 25 μm. For example, the particles have a diameter of 8 μm, 14 μm or 24 μm.

[0053] The size of the particles is preferably smaller than the thickness of the layer formed in step a1).

[0054] Preferably, the particles are spherical in order, on the one hand, to impart a better reactivity to the resin and, on the other hand, to obtain a final part with better compactness and higher density.

[0055] Advantageously, the copper particles are stored in a non-oxidizing atmosphere before being used. Alternatively, a chemical treatment may be carried out to remove the oxide layer that may form on the surface of the copper particles. Depending on the oxygen content present on the surface of the copper particles, it is also possible to carry out a heat treatment in a reducing atmosphere at a temperature below 500 ° C for, for example, 1 to 4 hours.

[0056] Copper oxide has a high refractive index (2.6) compared to that of acrylate-type resins (1.5). This difference in refractive index leads to a competition between the UV light absorption by the powder and the activation of the photoinitiator present in the formulation (and therefore the crosslinking of the acrylates). These phenomena therefore lead to a low reactivity of these filled resins. Non-oxidized copper has a refractive index of 1.3621, close to that of the resins.

[0057] The paste comprises one or more precursors of the first resin. By precursor it is to be understood monomers and / or oligomers and / or prepolymers that lead to the formation of a polymer. By way of example, for the SLA process, mention may be made of monomers and oligomers of the epoxide (also called "epoxy"), acrylate, urethane acrylate, polyether acrylate, polyether acrylate modified by amine, epoxy acrylate or polyester acrylate type.

[0058] Advantageously, functional acrylates are chosen, such as urethane acrylates, amine-modified polyether acrylates, epoxy acrylates or polyester acrylates, or mixtures thereof, which contribute to the wetting of the resin on the particles.

[0059] Preferably, the paste comprises a tetrafunctional acrylate, such as di(trimethylolpropane)tetraacrylate, and a difunctional acrylate, such as bisphenol A ethoxylate dimethacrylate.

[0060] Advantageously, a tetrafunctional acrylate / difunctional acrylate weight ratio of 1 to 5, preferably 2 to 4, for example 3, is selected. By adding difunctional acrylate to tetrafunctional acrylate, it is possible to extend the length of the crosslinked chains, limiting the shrinkage and thus obtaining parts without any cracks. With such a ratio, it is possible to obtain so-called solid parts, such as cylinders, whether perforated or non-perforated, typically having a thickness of more than 3 mm.

[0061] Advantageously, the paste also contains an acrylic reactive diluent for adjusting the viscosity and the degree of crosslinking. The acrylic reactive diluent may be a compound defined by the following formula:

[0062] [ka]

[0063] Where: R is a polyvalent group, such as a hydrocarbon, polyalkyl ether, or alkoxylated polyol type group; M is an integer depending on the R group.

[0064] By way of example, the reactive diluent may be selected from 1,6-hexanediol diacrylate (HDDA), trimethylolpropane triacrylate (TMPTA), tripropylglycoltriacrylate (TPGDA), glyceryl propoxylated triacrylate (GPTA).

[0065] The paste further comprises one or more polymerization initiators (also called photoinitiators). In the case of stereolithography, the initiation of the polymerization of the acrylates is obtained by the absorption of UV light. The initiators of the acrylates are of the radical type, the choice of the initiator being guided mainly by the wavelength of the light source that the initiator absorbs.

[0066] It should be recalled that the UV range extends over wavelengths from 100 nm to 450 nm. UVC is able to crosslink materials at the surface, UVB penetrates layers and UVA, comprised between 315 and 400 nm, is able to crosslink thick layers, for example having a thickness greater than 20 μm and less than 20 mm. In the context of the present invention, the light source advantageously has a wavelength set at 365 nm.

[0067] Suitable photoinitiators for acrylate-type precursors are from the group of acetophenones, alkoxyacetophenones or phenylacetophenones, such as 2,2'-dimethoxy-2-phenylacetophenone (also called DMPA) (e.g. Irgacure 651 from IGM); from the group of alkylaminoacetophenones or morpholinobutyrophenones, such as 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (e.g. Irgacure 369 from IGM) or 2-methyl-4'-(methylthio)-2-morpholinopropiophenone (e.g. Irgacure 907 from IGM); or from the group of hydroxyalkylphenones, such as 2-hydroxy-2-methyl-1-phenyl-propan-1-one (e.g. Darocure 1173 from IGM). Suitable photoinitiators for acrylate type precursors may also consist of phosphine oxide derivatives, such as phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (eg Irgacure 819 from CIBA).

[0068] Preferably, the photoinitiator is 2,2'-dimethoxy-2-phenylacetophenone. The use of this photoinitiator leads to more homogeneous crosslinking in the layer and to a lower crosslinking rate. Crosslinking is carried out homogeneously, without the formation of cracks, and at the temperature at which debinding begins.

[0069] The optical additive allows scattering and / or reflection of light inside the paste layer, thereby improving the reactivity of the resin. For example, the optical additive is selected from silica (SiO2), polysiloxane, polythiophene, pre-crosslinked milled resin, polypropylene, and polyvinyl alcohol. Preferably, the optical additive is polypropylene or a crosslinked milled resin.

[0070] The polypropylene may be selected from polypropylenes normally used in plastics techniques such as injection molding, etc. By way of example, it is possible to use the polypropylene commercialized by the company Basel under the name HP500N, the polypropylene commercialized by the company Borealis, or Propylmatte 31 by the company Micro Powders.

[0071] The polypropylene may be functionalized, for example, the polypropylene is functionalized with groups that allow for better scattering of the incident light.

[0072] Advantageously, when the optical additive is a polymer or resin, it is removed in the debinding step, which improves the compactness, density and quality of the final part. Preferably, polypropylene is chosen, which leaves only a small amount of carbonated residue after the debinding step. Advantageously, polysiloxane is the wetting agent.

[0073] Advantageously, the second resin is of the acrylate type, which is easily removed during heat treatment.

[0074] The optical additives make up 0.1-20% by weight of the copper particles in order to obtain dense parts. Above 20%, after debinding and sintering, porous parts are obtained. At such ratios, the amount of optical additives is sufficient to scatter light, and the resulting parts have low porosity.

[0075] When the additives are in the form of particles, they preferably have smaller dimensions than the particles of the powder in order to limit the porosity in the final part to obtain a dense part. For example, the additive particles have a maximum diameter at least two times smaller, preferably ten times smaller, than the maximum diameter of the particles of the copper powder. For example, the optical additives have a dimension of 10 μm or less, for example in the range of 1-2 μm to limit the porosity of the final part, for example in the range of 8 μm to obtain a slightly porous material. Preferably, the optical additives have a maximum dimension of 2 μm or less. The final part obtained has a low porosity.

[0076] Other ingredients may be added to the paste, such as wetting agents, rheological agents, etc.

[0077] The different components are mixed to obtain a homogenous filling paste, which may be homogenized with a paddle stirrer.

[0078] Advantageously the threshold behaviour of the paste is according to the Herschel Bulkley shear thinning (n<1) or Bingham fluid equation.

[0079] Viscosity higher than 5 Pa·s, preferably 100 at 25°C -1 It is possible to select a paste with a viscosity of 10 Pa·s or more in seconds. The paste is easy to spread and sufficiently viscous to form a homogeneous layer. The viscosity of the paste can be measured with a plate / plate or cone / plate type device. For example, the viscosity is measured with an MCR300 rheometer.

[0080] The viscosity may be adapted depending on the machine, for example by adding rheological agents and dispersants.

[0081] By way of example, the viscosity of the paste can be measured with a cone / flat head instrument CP50 / 1, with the distance between the pastes being 100 μm, for 3 min to 2 min. -1 A pre-shear of 2 to 200 seconds is performed.-1 5 min rise and 5 min to 2 min shear rate -1 Executes a return for seconds.

[0082] Advantageously, the paste is prepared at room temperature (20-25° C.).

[0083] For example, the paste is - 80 to 95% by weight, preferably 90 to 95% by weight, of copper particles, - 0.1 to 5% by weight, preferably 0.1 to 1% by weight, of one or more photoinitiators, - from 2 to 15% by weight, preferably from 2 to 10% by weight, of one or more photopolymerizable precursors of the resin, for example a mixture of tetrafunctional and difunctional precursors, optionally 0.1 to 10% by weight, preferably 0.5 to 1% by weight, of optical additives, optionally 1 to 5% by weight, preferably 1 to 2% by weight, of a reactive diluent Includes.

[0084] The components are produced by applying a succession of paste layers with a thickness of 10 to 200 μm, preferably 25 to 200 μm (step a1) and photopolymerizing (step a2), for example by means of a laser or digital light processing (or DLP).

[0085] Advantageously, step a2) is carried out under UV irradiation for a time less than 30 seconds, preferably less than 10 seconds and even more preferably less than 2 seconds.

[0086] Advantageously, the paste layer has a thickness of 30 to 50 μm and the UV irradiation is carried out for a time of 0.5 to 1 s.

[0087] Parts formed by SLA can have complex geometries with voids of various sizes and shapes.

[0088] The parts can be built by stereolithography at room temperature.

[0089] Upon completion of stereolithography, the resulting part is solid and contains the first resin with copper powder dispersed within it.

[0090] Parts Heat Treatment: During the printing process (step a), the resin acts as a binder to the raw part (also called the green part) and ensures adhesion.

[0091] This binder is then removed in a debinding step (step b) to obtain a debound part (called brown part) in the form of a copper skeleton.

[0092] The part is then sintered to obtain the final part.

[0093] The first heat treatment, which is called debinding, is carried out in an oxidizing atmosphere containing at least 10% by volume, preferably at least 15% by volume, even more preferably at least 20% by volume of an oxidizing component. Preferably, the oxidizing component is in gaseous form. The oxidizing component may be dioxygen, carbon monoxide or carbon dioxide. These molecules are introduced in sufficient amounts to allow the removal of carbonate residues. For example, the oxidizing atmosphere is a gaseous mixture containing an oxidizing agent and one or more other gases, such as argon and / or nitrogen. The oxidizing atmosphere may contain multiple oxidizing agents, such as dioxygen and carbon dioxide.

[0094] Advantageously, the oxidizing atmosphere is air.

[0095] Advantageously, the first heat treatment is carried out at atmospheric pressure (approximately 1 bar).

[0096] The first heat treatment applied to the part formed by copper particles dispersed in resin is advantageously carried out with a low temperature gradient (less than 3° C. / min, for example 1° C. / min, in some cases less than 0.1° C. / min) in order to avoid alteration of the part and the appearance of cracks. Advantageously, such a temperature increase is carried out from 50° C. to the debinding temperature T dIt is possible to carry out the process over a wider range, for example 100°C, 200°C or even from room temperature (20-25°C) to the debinding temperature. By way of example, if the debinding temperature is 400°C, a slow ramp, for example 1°C / min, is carried out from 350°C to 400°C. It is also possible to carry out a very slow ramp (for example at 0.1°C / min) from room temperature (25°C) to the debinding temperature.

[0097] Advantageously, one or more temperature steps are performed at a debinding temperature T d Advantageously, T1=T d -50℃ and / or T2=T d One step may be carried out at -100°C. The duration of each step is at least 30 minutes, preferably at least 1 hour, and even more preferably at least 2 hours. Each step may have a different duration. For example, for a debinding temperature of 450°C, the first step may be carried out at 350°C for 30 minutes and the second step at 400°C for 2 hours.

[0098] The second heat treatment, called sintering, is carried out in a reducing atmosphere, such as an atmosphere containing dihydrogen, which can reduce the amount of oxygen present in the part upon completion of the debinding process.

[0099] The second heat treatment may be carried out at a partial pressure in the range of 50 to 800 mbar.

[0100] Advantageously, the temperature step is performed at a sintering temperature T for at least 30 minutes, preferably at least 1 hour, and even more preferably at least 2 hours. f It will be carried out at.

[0101] Debinding temperature T d and sintering temperature T f is defined by the skilled artisan depending on the resin.

[0102] The skilled person can also select the number of steps as well as the temperature and duration of each step, these parameters may also be determined according to the packing rate and morphology of the powder.

[0103] For example, the debinding temperature T d is in the range of 300-800° C., preferably 400-700° C. The debinding temperature is typically determined by thermogravimetric analysis (TGA), and then the process time and ramp cycle are adjusted to limit cracking due to binder off-gassing.

[0104] For example, the sintering temperature T f is comprised within the range of 980 to 1080° C., advantageously 980 to 1075° C. Usually, the sintering temperature is evaluated by means of a dilatometer.

[0105] Advantageously, a temperature descending gradient is also carried out, for example consisting of a temperature gradient of less than 5° C. / min or according to one variant of between 5 and 10° C. / min. EXAMPLES

[0106] Illustrative and non-limiting examples of stereolithography copper part embodiments: First, different pastes (formulations) are prepared: The copper particles used are those sold by the company Ecka and have a particle size of <45 μm.

[0107] Formulation 1: - HDDA (Sigma aldrich) 1.7% by mass - 4.9% by weight of tetrafunctional oligoacrylate (SR355 from Sartomer) - Trifunctional oligoacrylate (Sartomer CN509) 1.7% by weight - 2-methyl-4'-methylthio-2-morpholinopropiophenone (Sigma Aldrich) 0.2% by weight - phenylbis(2,4,6-trimethyl-benzoyl)phosphine oxide (Sigma Aldrich) 0.2% by weight - 90.8% by weight (i.e. 54% by volume) copper in the resin - 0.5% by weight of optical additives

[0108] Formulation 2: - HDDA (Sigma aldrich) 1.3% by mass - Tetrafunctional oligoacrylate (Sartomer SR355) 2.2% by weight - Trifunctional oligoacrylate (Sartomer CN509) 1.3% by weight - Acrylate amine (Sartomer CN371EU) 2.2% by weight - 0.2% by weight of methyl-4'-methylthio-2-morpholinopropiophenone (Sigma Aldrich) - phenylbis(2,4,6-trimethyl-benzoyl)phosphine oxide (Sigma Aldrich) 0.2% by weight - 92.2% by weight (i.e. 58.6% by volume) copper in the resin - 0.5% by weight of optical additives

[0109] Formulation 3: - HDDA (Sigma aldrich) 1.5% by mass - 4.2% by weight of tetrafunctional oligoacrylate (SR355 from Sartomer) - Difunctional oligoacrylate (Diacryl 101) 1.4% by weight - 0.2% by weight of methyl-4'-methylthio-2-morpholinopropiophenone (Sigma Aldrich) - phenylbis(2,4,6-trimethyl-benzoyl)phosphine oxide (Sigma Aldrich) 0.2% by weight - 92.5% by weight (equivalent to 60% by volume) of copper in the resin

[0110] Formulation 4: - HDDA (Sigma aldrich) 1.5% by mass - 4.2% by weight of tetrafunctional oligoacrylate (SR355 from Sartomer) - Difunctional oligoacrylate (Diacryl 101) 1.4% by weight - 0.4% by weight of 2,2-dimethoxy-2-phenylacetophenone - 92.5% by weight (equivalent to 60% by volume) of copper in the resin

[0111] The different components of the formulation are mixed with a paddle stirrer to obtain a homogeneous filling paste.

[0112] The developed formulations exhibited a 100% -1 sec. has a viscosity higher than 5 Pa·s.

[0113] The manufacture of the different copper parts was carried out by DLP ("Digital Light Processing") type stereolithography, by depositing a first thin paste layer on a support and polymerizing this layer in one or more selected areas by the action of a suitable radiation, typically UV radiation. A second layer, also partially or completely polymerized, is then deposited on top of this first layer. These paste deposition / polymerization cycles are repeated until all polymerized parts form the desired part in the green state.

[0114] As shown in FIG. 1, depending on the composition of the paste, different thicknesses can be crosslinked under UV exposure (365 nm).

[0115] As an example, FIG. 2 shows a 30*3 mm2 30x ... 2 The copper parts shown in Fig.

[0116] The parts were manufactured by carrying out a debinding heat treatment at 400°C for 4 hours in different atmospheres (vacuum, hydrogen, argon, Ar / O2 mixed atmosphere, air) followed by a sintering step at 980°C for 4 hours in hydrogen. The copper parts account for 60% by volume of the paste. The carbon and oxygen content of the different parts was determined by elemental analysis (Instrumental Gas Analysis (IGA)). The results are reported in Table I below.

[0117] [Table 1]

[0118] The debinding atmosphere plays an important role with regard to the carbon content in the final part. In air, this content is very low (0.019% by weight), but in other conditions it reaches an average of 0.385% by weight, a value that is 20 times higher. The carbon content of parts debound in air is close to that of the starting copper powder.

[0119] Table II shows the carbon and oxygen contents measured on parts obtained after the first heat treatment of debinding in air and sintering in dihydrogen at 400 mbar for different durations and at different temperatures.

[0120] [Table 2]

[0121] By increasing the sintering duration and / or temperature, the oxygen content can be reduced and the density can be increased.

[0122] Figure 3A shows a green copper part before sintering, and Figure 3B shows the same part after debinding in air and sintering in hydrogen.

[0123] When the parts are observed with an optical microscope, the high density of the parts can be confirmed (Figure 4).

[0124] Table III shows the carbon and oxygen contents measured for the parts obtained after a first heat treatment of debinding in air at 400° C. for 4 hours and sintering in dihydrogen at 980° C. for 4 hours for the four formulations.

[0125] [Table 3]

[0126] The parts made from the different formulations have a lower content of the light components. The carbon content is similar to that of the starting copper powder.

[0127] Parts produced in this manner using formulations 1, 2, 3 and 4 are shown in Figures 5a, 5b, 5c and 5d, respectively. The parts have good mechanical strength. More specifically, formulation 4 leads to parts with good mechanical strength and no cracks. Furthermore, formulation 4 does not introduce phosphorus and leads to parts with good thermal and electrical properties. In particular, the thermal conductivity of the parts is identical to that of the pressed and sintered starting powders.

Claims

1. At least the following sequential steps: a) forming a part by stereolithography, said forming comprising: a1) forming a paste layer comprising a powder of copper particles, one or more photopolymerizable precursors of a first resin, a photoinitiator, and optionally optical additives; a2) photopolymerizing the photopolymerizable precursor of the first resin; wherein steps a1) and a2) form a cycle which may be repeated multiple times; b) in a first atmosphere at a first temperature T d performing a first heat treatment to remove the first resin; c) in a second atmosphere at the first temperature T d A higher second temperature T f A step of performing a second heat treatment to sinter the copper particles and obtain a copper part.

1. A method for manufacturing a copper part comprising: the first atmosphere comprises an oxidizing atmosphere containing at least 10 volume percent of an oxidizing agent, the second atmosphere comprises a reducing atmosphere, the photopolymerizable precursor comprises a tetrafunctional acrylate and a difunctional acrylate, and the photoinitiator comprises 2,2-dimethoxy-2-phenylacetophenone.

2. The method of claim 1, wherein the oxidizing agent is dioxygen.

3. 3. The method of claim 2, wherein the first atmosphere contains at least 15% by volume of dioxygen.

4. 4. The method according to claim 1, wherein the first atmosphere consists of air.

5. 5. A method according to any one of claims 1 to 4, characterized in that the second atmosphere consists of dihydrogen or a mixture of dihydrogen and argon.

6. Method according to any one of the preceding claims, characterized in that the first heat treatment is carried out at a temperature between 300 and 800°C.

7. 7. Method according to any one of claims 1 to 6, characterized in that the first heat treatment is carried out for a period of between 2 and 7 hours.

8. Method according to any one of the preceding claims, characterized in that the second heat treatment is carried out at a temperature between 980 and 1080°C.

9. 9. Method according to any one of claims 1 to 8, characterized in that the second heat treatment is carried out for a period of 1 to 7 hours.

10. The method according to claim 1, wherein the mass ratio of the tetrafunctional acrylate to the difunctional acrylate is in the range of 1 to 5.

11. The method according to claim 10, characterized in that the weight ratio of said tetrafunctional acrylate / said difunctional acrylate is in the range of 2-4.

12. 12. The method according to claim 1, wherein the tetrafunctional acrylate is di(trimethylolpropane)tetraacrylate and the difunctional acrylate is bisphenol A ethoxylate dimethacrylate.

13. 13. The method according to claim 1, wherein the copper powder comprises at least 35% by volume of the paste layer.

14. The method of claim 13, wherein the copper powder comprises 35 to 65 volume percent of the paste layer.

15. 15. The method according to any one of claims 1 to 14, characterized in that the optical additive is selected from silica, polythiophene, polyvinyl alcohol, polypropylene, and a pre-crosslinked and milled second resin.

16. It is intended for use in a stereolithography process to produce copper parts, - copper powder, a photopolymerizable precursor of the first resin, - photoinitiators, as well as optionally optical additives, A paste comprising: A paste, characterized in that the photopolymerizable precursor comprises a tetrafunctional acrylate and a difunctional acrylate, and the photoinitiator comprises 2,2-dimethoxy-2-phenylacetophenone.

17. The paste of claim 16, wherein the optical additive is selected from silica, polythiophene, polyvinyl alcohol, polypropylene, and a pre-crosslinked and milled second resin.

18. 18. Paste according to claim 16 or 17, characterized in that the mass ratio of the tetrafunctional acrylate to the difunctional acrylate is in the range of 1 to 5.

19. The paste of claim 18, wherein the mass ratio of the tetrafunctional acrylate to the difunctional acrylate is in the range of 2 to 4.

20. 20. A paste according to any one of claims 16 to 19, characterized in that the tetrafunctional acrylate is di(trimethylolpropane)tetraacrylate and the difunctional acrylate is bisphenol A ethoxylate dimethacrylate.

Citation Information

Patent Citations

  • Photosensitive resin for DLP 3D printing

    CN109535330A

  • Paste composition filled with metal powder, method for obtaining metal product from the composition, and metal product obtained by the method

    JP2004504490A

  • Photosensitive electroconductive paste

    JP2009075307A

  • Photocurable composition for photo-shaping, metal shaped article, and method for producing the same

    JP2009084388A

  • Economical manufacturing method for metal parts

    JP2019502028A