Layered manufacturing method and layered manufactured body
By forming cavities in supports within metal overhang parts during additive manufacturing, the method ensures complete removal of supports with long extensions, addressing the limitations of traditional flame-based removal methods.
Patent Information
- Application Number
- JP2021030238
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing methods for removing supports in metal overhang parts during additive manufacturing face challenges when the supports have a shape that extends long in the depth direction, as flames used for removal often fail to reach and burn the entire support due to heat absorption, leaving residues.
The method involves forming cavities in the supports that extend from the exposed surface towards the depth direction, allowing flames to penetrate and burn the support by creating passages for the flame to reach the back side, and optionally using a fuse to ensure complete removal.
This approach effectively removes supports with a long extension in the depth direction by ensuring the flame can reach and burn the entire support, even when traditional methods fail, thereby completing the manufacturing process efficiently.
Smart Images

Figure 0007554138000007 
Figure 0007554138000002 
Figure 0007554138000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an additive manufacturing method and an additive manufactured object. [Background technology]
[0002] In order to form an overhanging part having a surface facing downward in the metal lamination direction by 3D additive manufacturing, which forms a product by laminating metal, supports that support the overhanging part are also formed when the overhanging part is formed. The supports need to be removed after forming, but in narrow areas that cannot be accessed by tools, it is often difficult to remove the supports with tools. As one method other than physically removing the supports with tools, Patent Document 1 describes a method of burning and removing supports using a thermal deburring device for burning and removing burrs generated during machining. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2020 / 089303 Summary of the Invention [Problem to be solved by the invention]
[0004] However, according to the inventors' investigations into a method of burning and removing supports using a thermal deburring device, when the support has a shape that extends long in the depth direction relative to the exposed surface exposed from the overhanging portion, it was found that while the support can be burned and removed up to a certain distance in the depth direction from the exposed surface, part of the support remains at the back side in the depth direction.
[0005] In view of the above circumstances, an object of at least one embodiment of the present disclosure is to provide an additive manufacturing method and an additive manufactured body that are capable of removing a support having a shape that extends long in the depth direction. [Means for solving the problem]
[0006] In order to achieve the above-mentioned objective, the additive manufacturing method disclosed herein is an additive manufacturing method for forming a product by stacking metal, wherein a semi-finished product of the product comprises at least one overhanging portion having a surface facing downward in the stacking direction of the metal, and a support supporting the overhanging portion, the support having an exposed surface from which the support is exposed from the overhanging portion, and the additive manufacturing method includes a step of stacking the metal to form the semi-finished product, a step of forming at least one cavity in the support extending from the exposed surface toward the depth direction of the support, and a step of burning and removing the support.
[0007] Further, the present disclosure provides an additive manufacturing object of metal, the additive manufacturing object comprising at least one overhang portion having a surface facing downward in a lamination direction of the metal, and a support supporting the overhang portion, the support having an exposed surface where the support is exposed from the overhang portion, and at least one cavity portion extending from the exposed surface toward a depth direction of the support is formed in the support. A fuse is inserted into the at least one cavity. is. Effect of the Invention
[0008] According to the additive manufacturing method and additive manufactured body disclosed herein, the flame can reach the back of the cavity to combust the supports at the back in the depth direction, making it possible to remove supports having a shape that extends long in the depth direction. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a front view of a semi-finished product (laminate manufactured body) manufactured by the lamination manufacturing method according to embodiment 1 of the present disclosure. [Diagram 2]FIG. 1 is a front view of a product manufactured by the additive manufacturing method according to embodiment 1 of the present disclosure. [Diagram 3] FIG. 2 is a cross-sectional view taken along line III-III in FIG. [Figure 4] 1 is a flowchart of an additive manufacturing method according to a first embodiment of the present disclosure. [Diagram 5] 11 is a flowchart of some steps of a modified example of the additive manufacturing method according to the first embodiment of the present disclosure. [Figure 6] FIG. 11 is a cross-sectional view of a semi-finished product (laminate manufactured body) manufactured by the lamination manufacturing method according to the embodiment 2 of the present disclosure. [Figure 7] FIG. 11 is a cross-sectional view of a semi-finished product (laminate manufactured body) manufactured by the lamination manufacturing method according to the embodiment 3 of the present disclosure. [Figure 8] 13A to 13C are front views of a first lid part, a second lid part, and a third lid part used in an additive manufacturing method according to embodiment 3 of the present disclosure. [Figure 9] 11 is a flowchart of some steps of an additive manufacturing method according to embodiment 3 of the present disclosure. [Figure 10] 13A to 13C are views for explaining the process of burning and removing supports in step S3 of the additive manufacturing method according to the third embodiment of the present disclosure. [Figure 11] 13 is a cross-sectional view of a modified example of a semi-finished product manufactured by the additive manufacturing method of the present disclosure. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an additive manufacturing method and an additive manufactured body according to embodiments of the present disclosure will be described with reference to the drawings. Each embodiment described below shows one aspect of the present disclosure, and is not intended to limit the present disclosure. The embodiments can be modified as desired within the scope of the technical concept of the present disclosure.
[0011] (Embodiment 1) <Configuration of product and layered object according to embodiment 1 of the present disclosure> As shown in Fig. 1, an additive manufacturing object 1 according to embodiment 1 of the present disclosure is a semi-finished product manufactured by stacking metals, and includes an overhanging portion 2 having a surface facing downward in the metal stacking direction, and a support 3 supporting the overhanging portion 2. By removing the support 3 from the semi-finished product by an operation described below, a product 10 as shown in Fig. 2 is completed. As shown in Fig. 1, the support 3 has a configuration with a larger specific surface area or a smaller apparent heat capacity than the overhanging portion 2, and has, for example, a lattice structure including many small cavities.
[0012] The support 3 has an exposed surface 3a exposed from the overhang portion 2. As shown in FIG. 3, the support 3 has a shape that extends long from the exposed surface 3a in the depth direction. The support 3 has a cavity 4 formed so as to extend from the exposed surface 3a toward the back side in the depth direction of the support 3. Although FIG. 3 shows one cavity 4 formed, two or more cavities 4 may be formed. In addition, the length of the cavity 4 is arbitrary as long as it extends from the exposed surface 3a toward the depth direction of the support 3, and may have, for example, 1 / 3, 1 / 2, or 2 / 3 of the length of the depth direction of the support 3, or may penetrate the support 3 in the depth direction. In addition, the cavity 4 is not necessarily limited to a shape that extends straight, and may have a shape that has some curves or bends. Furthermore, the inner peripheral surface that defines the cavity 4 has the same configuration as the lattice structure of the support 3. That is, in order to form the cavity 4, a surface that is denser than the lattice structure (a surface that does not include many cavities) is not formed.
[0013] <Additive manufacturing method according to embodiment 1 of the present disclosure> Next, an additive manufacturing method according to the first embodiment of the present disclosure will be described with reference to Figures 1 to 3 and the flowchart in Figure 4. In step S1 of this additive manufacturing method, metal is laminated to form an additive manufactured body 1 as a semi-finished product. For example, a powder bed type additive manufacturing device (3D printer) can be used to laminate metal by a known method used in three-dimensional additive manufacturing, such as laser melting or electron beam melting.
[0014] In step S2 following step S1, a hollow portion 4 is formed in the support 3. As in the flowchart of FIG. 3, in a form in which step S2 is performed after step S1, the hollow portion 4 is machined (e.g., drilled) in the support 3 after the layered object 1 is molded. Step S2 is not limited to this form, and may be a form in which steps S1 and S2 are performed simultaneously, that is, a form in which the hollow portion 4 is formed during the molding of the layered object 1, or in other words, a form in which the support 3 is molded so that the hollow portion 4 is included in the support 3. In the former form, the support 3 can be designed without considering the hollow portion 4, and therefore the design of the support 3 can be simplified compared to the latter form. On the other hand, in the latter form, the hollow portion 4 is formed during the molding of the layered object 1, and therefore the number of steps in the layered object molding method can be reduced compared to the former form.
[0015] In step S3 following step S2, the support 3 is burned to remove it from the layered product 1. Step S3 can be performed, for example, using a known thermal deburring device. This device has a configuration in which a container having a space capable of accommodating the layered product 1 is provided with a supply path for supplying a combustible gas (e.g., methane) and oxygen to the space, and a plug for emitting a spark is provided in the space. The layered product 1 is accommodated in the space inside the device, and a flame generated by the combustion of the combustible gas in the space causes metallic combustion of the support 3, thereby embrittling the support 3 and making it easy to remove it from the layered product 1. After removing the layered product 1 from the device, the embrittled support 3 is removed from the layered product 1 to complete the product 10.
[0016] In the above-mentioned study by the inventors of the present application, when the support 3 has a shape that extends long in the depth direction relative to its exposed surface 3a as shown in Fig. 3, a phenomenon was observed in which a part of the support 3 remains on the rear side in the depth direction. The inventors of the present application considered that the cause of this was that when the flame passes through the support 3 on the front side, heat is absorbed by the support 3, causing the flame to disappear, and the flame cannot advance further to the rear side. To solve this cause, in the additive manufacturing method according to embodiment 1 of the present disclosure, a hollow portion 4 is formed in the support 3.
[0017] When a hollow portion 4 is formed in the support 3, the hollow portion 4 serves as a passageway for the flame, allowing the flame to reach the back of the hollow portion 4 and combust the supports located at the back side of the support 3 in the depth direction, so that the support 3 having a shape that extends long in the depth direction can be removed.
[0018] <Modification of the additive manufacturing method according to the first embodiment of the present disclosure> 1 shows the cross-sectional shape of cavity 4 as a square, but this is not limited to a square, and may be a rectangle, a polygon other than a square, a circle, an ellipse, or any other cross-sectional shape. However, the size of opening 4a is important so that the flame can reach the back of cavity 4 without being extinguished at opening 4a in exposed surface 3a of cavity 4. For this reason, the additive manufacturing method according to embodiment 1 preferably includes a step of determining the size of opening 4a before step S1.
[0019] Next, step S10 for determining the size of the opening 4a will be described in detail with reference to Fig. 5. Step S10 includes step S11 for acquiring a range of Peclet numbers based on the shape of the opening 4a, and step S12 for calculating the size of the opening 4a so that the Peclet number falls within the range acquired in step S11. In step S11, the cross-sectional shape of the cavity 4 formed in the support 3 is specified in advance, and then a range of Peclet numbers in which the flame does not disappear at the opening 4a of the cavity 4 having the specified cross-sectional shape in the state of the flame in the thermal deburring device to be used is acquired in advance, for example, by experiment.
[0020] The Peclet number is defined by the following formula (1): 1,u is the Peclet number, and ρ u is the density of the unburned mixture, SL is the laminar burning velocity, and C p,u is the specific heat of the unburned mixture, and δ q1 is the quenching distance, λ u is the thermal conductivity of the unburned mixture.
number
[0021] The quenching distance δ has a direct relationship with the size of the opening 4a. q1 The quenching distance means the limit value of the typical dimension of the passage where quenching occurs. In other words, if the size of the opening 4a is larger than the quenching distance determined by the operation described later, the flame can reach the depth of the cavity 4 without being extinguished at the opening 4a.
[0022] The question arises as to what length the quenching distance of the opening 4a should be, but if the shape of the opening 4a is a circle, the radius of the circle is the quenching distance, if the shape of the opening 4a is an ellipse, the minor axis of the ellipse is the quenching distance, and if the shape of the opening 4a is a rectangle, the shortest distance of the perpendicular lines extending from the intersection of the two diagonals to each side is the quenching distance. If the shape of the opening 4a is any other polygon or arbitrary shape, the shortest distance from the center of gravity of the shape to the edge that defines the opening 4a is the quenching distance.
[0023] In step S11, the range of the Peclet number at which the flame does not disappear at the opening 4a of the cavity 4 having the specified cross-sectional shape is obtained, and then in step S12, the quenching distance δ is calculated based on the above formula (1) so that the Peclet number falls within the range. q1 is calculated, and the quenching distance in the specified cross-sectional shape of the cavity 4 is calculated as δ q1 The size of the opening 4a is determined to be larger than the
[0024] According to this modified example, the risk of the flame being extinguished at the opening 4a is reduced and the flame can reach the depth of the hollow portion 4, and the supports 3 located at the rear side in the depth direction of the supports 3 can be burned, so that the supports 3 having a shape that extends long in the depth direction can be removed.
[0025] (Embodiment 2) Next, an additive manufacturing method according to embodiment 2 will be described. The additive manufacturing method according to embodiment 2 differs from embodiment 1 in that a fuse is inserted into hollow portion 4. In embodiment 2, the same components as those in embodiment 1 are given the same reference numerals, and detailed descriptions thereof will be omitted. Furthermore, unless otherwise specified, the configuration of the modified example of embodiment 1 can also be applied to embodiment 2.
[0026] <Configuration of Layered Object According to Embodiment 2 of the Present Disclosure> 6, in the layered object 1 according to the second embodiment of the present disclosure, a fuse 20 is inserted into the cavity 4, preferably all the way to the back of the cavity 4. The other configurations are the same as those in the first embodiment.
[0027] <Additive manufacturing method according to embodiment 2 of the present disclosure> The additive manufacturing method according to the second embodiment of the present disclosure includes a step of inserting the fuse 20 into the cavity 4 before step S3 (see FIG. 4) of burning and removing the support 3. Other operations are the same as those of the first embodiment. When the fuse 20 is ignited by a flame, the fuse 20 burns toward the back of the cavity 4. As a result, in the cavity 4, the combustible gas is burned by the sparks scattered from the fuse 20 and a flame is generated, so that the flame can be reliably reached to the back of the cavity 4. In particular, even if the additive manufacturing method does not include step S10 and the size of the opening 4a is inappropriate or the state of the flame of the thermal deburring device changes due to an abnormality in the device, etc., and the flame disappears at the opening 4a, the second embodiment allows the flame to be reliably reached to the back of the cavity 4.
[0028] (Embodiment 3) Next, an additive manufacturing method according to embodiment 3 will be described. The additive manufacturing method according to embodiment 3 is a modification of embodiment 1 or 2, in which a plurality of hollow portions 4 are formed in the support 3. In the following, embodiment 3 will be described by making such a modification to embodiment 1, but embodiment 3 can also be configured by making such a modification to embodiment 2. In embodiment 3, the same components as those in embodiment 1 are given the same reference symbols, and detailed description thereof will be omitted. Furthermore, unless otherwise specified, the configuration of the modified embodiment of embodiment 1 can also be applied to embodiment 3.
[0029] <Configuration of Layered Object According to Third Embodiment of the Present Disclosure> As shown in Fig. 7, in the layered product 1 according to the third embodiment of the present disclosure, a support 3 is formed with a plurality of cavities 4, i.e., one first cavity 31 and two second cavities 32, 32 that are shorter in length in the depth direction of the support 3 than the first cavity 31. The arrangement of the first cavity 31 and the second cavity 32 is not particularly limited, but for example, they can be formed in the support 3 so that the first cavity 31 is located between the two second cavities 32, 32. Both the first cavity 31 and the second cavity 32 form openings 31a and 32a in the exposed surface 3a. The other configurations are the same as those of the first embodiment.
[0030] <Additive manufacturing method according to embodiment 3 of the present disclosure> The additive manufacturing method according to the third embodiment of the present disclosure differs from the first embodiment in step S3 (see FIG. 4), but the other steps are the same as those of the first embodiment. In the third embodiment, two types of lids, i.e., a first lid 33 and a second lid 34, as shown in FIG. 8, are used in step S3. The first lid 33 has a first through hole 33a that communicates with the first cavity 31 (see FIG. 7) when the first lid 33 is attached to the additively manufactured body 1 (see FIG. 7) so as to close the exposed surface 3a (see FIG. 7). The second lid 34 has second through holes 34a, 34a that communicate with the second cavities 32, 32 (see FIG. 7) when the second lid 34 is attached to the additively manufactured body 1 so as to close the exposed surface 3a.
[0031] As shown in Figure 9, step S3 in the additive manufacturing method according to embodiment 3 of the present disclosure includes a preparation step S21 of preparing the first lid portion 33 and the second lid portion 34, a first burn-removal step S22 of burning-removing the support 3 with the first lid portion 33 attached to the additive manufacturing body 1, a second burn-removal step S23 of burning-removing the support 3 with the second lid portion 34 attached to the additive manufacturing body 1 after the first burn-removal step S22, and a third burn-removal step S24 of burning-removing the support 3 with neither the first lid portion 33 nor the second lid portion 34 attached to the additive manufacturing body 1 after the second burn-removal step S23.
[0032] As shown in Fig. 10, in the first burning removal step S22, since the exposed surface 3a is closed by the first lid portion 33, only the inside of the thermal deburring device and the first cavity portion 31 are in communication through the first through hole 33a formed in the first lid portion 33. When a flame is generated inside the thermal deburring device in this state, the flame enters the first cavity portion 31 through the first through hole 33a and propagates to the back of the first cavity portion 31, so that the support 3 further inside than the end portion on the back side of the first cavity portion 31 is burned, or a pressure wave or detonation is generated in the first cavity portion 31, and the support 3 further inside than the end portion on the back side of the first cavity portion 31 is destroyed by the pressure wave. The layered product 1 can be removed from inside the thermal deburring device, and the embrittled or destroyed support 3 can be removed.
[0033] In the next second burning removal step S23, since the exposed surface 3a is closed by the second lid portion 34, only the inside of the thermal deburring device and the second cavity portion 32 are in communication through the second through hole 34a formed in the second lid portion 34. When a flame is generated inside the thermal deburring device in this state, the flame enters the second cavity portion 32 through the second through hole 34a and propagates to the back of the second cavity portion 32, causing the support 3 further inside than the end portion on the back side of the second cavity portion 32 to burn, or detonation occurs in the second cavity portion 32 and the support 3 further inside than the end portion on the back side of the second cavity portion 32 is destroyed by a pressure wave. The layered product 1 can be removed from inside the thermal deburring device, and the embrittled or destroyed support 3 can be removed.
[0034] The first burn-off step S22 and the second burn-off step S23 result in the support 3 on the rear side relative to the exposed surface 3a being removed. In the next third burn-off step S24, a flame is generated inside the thermal deburring device with neither the first lid part 33 nor the second lid part 34 attached to the layered object 1, and the remaining support 3 is embrittled by metal combustion caused by the flame. The layered object 1 is taken out from inside the thermal deburring device and the embrittled support 3 is removed, whereby all of the supports 3 are removed from the layered object 1, and the product 10 (see FIG. 2) is produced.
[0035] According to the third embodiment, even a support 3 having a shape that extends long in the depth direction and has a large cross-sectional area in the depth direction can be removed.
[0036] In the third embodiment, there is one first cavity 31 and two second cavity 32, but this is not limiting, and the numbers of the first cavity 31 and the second cavity 32 can be appropriately changed according to the size of the support 3. Furthermore, instead of forming two types of cavities with different lengths, three or more types of cavities with different lengths (i.e., a third cavity, etc.) may be formed according to the length of the support 3 in the depth direction.
[0037] In each of the first to third embodiments, as shown in Fig. 3, for example, the exposed surface 3a and the end surface of the layered object 1 where the exposed surface 3a is exposed are flush with each other, but this is not limited to the embodiment. As shown in Fig. 11, the exposed surface 3a may be recessed in the depth direction with respect to the end surface of the layered object 1. In the third embodiment, when the layered object 1 includes an exposed surface 3a of such a form, the first lid part 33 and the second lid part 34 are preferably structured to have a surface in contact with the exposed surface 3a, and may be configured to have a protruding part that fits into the recess of the layered object 1, and the protruding part is in contact with the exposed surface 3a.
[0038] The contents described in each of the above embodiments can be understood, for example, as follows.
[0039] [1] An additive manufacturing method according to one aspect includes: An additive manufacturing method for forming a product (10) by layering metal, comprising the steps of: The semi-finished product (layered manufactured body 1) of the product (10) is At least one overhang portion (2) having a surface facing downward in the lamination direction of the metal; a support (3) for supporting the overhang portion (2), the support (3) having an exposed surface (3a) where the support (3) is exposed from the overhang portion (2); Equipped with The additive manufacturing method includes: A step (S1) of stacking the metal to form the semi-finished product (1); A step (S2) of forming at least one cavity portion (4) in the support (3) extending from the exposed surface (3a) toward a depth direction of the support (3); A step (S3) of burning off the support (3); Includes.
[0040] According to the additive manufacturing method disclosed herein, by making the flame reach the back of the hollow portion, the supports at the back side in the depth direction can be burned, making it possible to remove supports having a shape that extends long in the depth direction.
[0041] [2] An additive manufacturing method according to another aspect is the additive manufacturing method according to [1], The cavity (4) is formed during the shaping of the semi-finished product (1).
[0042] According to this configuration, the cavity is formed during the molding of the semi-finished product, so the number of steps in the additive manufacturing method can be reduced compared to when the cavity is formed in the support after the semi-finished product is molded.
[0043] [3] A further aspect of the additive manufacturing method is the additive manufacturing method of [1], The cavity (4) is formed in the support (3) after shaping of the semi-finished product (1).
[0044] According to this configuration, the support can be designed without taking into consideration the cavity, and therefore the support design can be simplified.
[0045] [4] A further aspect of the additive manufacturing method is the additive manufacturing method according to any one of [1] to [3], The method further includes a step (S10) of determining a size of an opening (4a) of the cavity portion (4) on the exposed surface (3a) before the step (S1) of shaping the semi-finished product (1), This step (S10) is A step (S11) of obtaining a range of Peclet numbers based on the shape of the opening (4a); A step (S12) of determining the size of the opening (4a) so that the Peclet number falls within the range; Includes.
[0046] With this configuration, the risk of the flame being lost at the opening is reduced and the flame can reach the back of the hollow portion, and since the supports at the back in the depth direction of the supports can be burned, supports having a shape that extends long in the depth direction can be removed.
[0047] [5] A further aspect of the additive manufacturing method is the additive manufacturing method according to any one of [1] to [4], The method further includes a step of inserting a squib (20) into the cavity (4) prior to the step (S3) of burning off the support (3).
[0048] With this configuration, the flame can reliably reach the back of the hollow portion, thereby reliably burning the supports at the back of the supports in the depth direction, making it possible to remove supports that have a shape that extends longer in the depth direction.
[0049] [6] A further aspect of the additive manufacturing method is the additive manufacturing method according to any one of [1] to [5], The hollow portion (4) includes at least one first hollow portion (31) and at least one second hollow portion (32) having a length in the depth direction shorter than that of the first hollow portion (31), The step (S3) of burning and removing the support (3) comprises: a preparation step (S21) of preparing a first lid portion (33) having a first through hole (33a) formed therein and communicating with the first cavity portion (31) when the first lid portion (33) is attached to the semi-finished product (1) so as to close the exposed surface (3a), and a second lid portion (34) having a second through hole (34a) formed therein and communicating with the second cavity portion (32) when the first lid portion (33) is attached to the semi-finished product (1) so as to close the exposed surface (3a); a first burning and removing step (S22) of burning and removing the support (3) in a state where the first cover portion (33) is attached to the semi-finished product (1); a second burn-off step (S23) of burning off the support (3) in a state in which the second lid portion (34) is attached to the semi-finished product (1) after the first burn-off step (S22); a third burn-off step (S24) of burning off the support (3) in a state in which neither the first lid portion (33) nor the second lid portion (34) is attached to the semi-finished product (1) after the second burn-off step (S23); Includes.
[0050] According to this configuration, even a support having a shape that extends long in the depth direction and has a large cross-sectional area in the depth direction can be removed.
[0051] [7] A layered object according to one aspect of the present invention includes: A metal additive manufacturing body (1), At least one overhang portion (2) having a surface facing downward in the lamination direction of the metal; a support (3) for supporting the overhang portion (2), the support (3) having an exposed surface (3a) where the support (3) is exposed from the overhang portion (2); Equipped with At least one cavity (4) extending from the exposed surface (3a) toward the depth direction of the support (3) is formed in the support (3).
[0052] According to the layered manufactured body of the present disclosure, the flame can reach the back of the hollow portion and burn the supports at the back side in the depth direction of the support, making it possible to remove supports having a shape that extends long in the depth direction. [Explanation of symbols]
[0053] 1. Laminated object (semi-finished product) 2 Overhang 3. Support 3a Exposed surface 4 Cavity 4a aperture 10 Products 20 Fuse 31 First cavity 32 Second cavity 33 1st lid part 33a 1st through hole 34 2nd lid part 34a 2nd through hole
Claims
1. An additive manufacturing method for forming a product by layering metal, comprising the steps of: The semi-finished products of the above-mentioned products are At least one overhang portion having a surface facing downward in a lamination direction of the metal; a support for supporting the overhang portion, the support having an exposed surface where the support is exposed from the overhang portion; Equipped with The additive manufacturing method includes: building up the metal to form the blank; forming at least one cavity in the support, the cavity extending from the exposed surface toward a depth direction of the support; burning off the support; An additive manufacturing method comprising:
2. The additive manufacturing method according to claim 1 , wherein the cavity is formed during the manufacturing of the semi-finished product.
3. The additive manufacturing method according to claim 1 , wherein the cavity is formed in the support after the semi-finished product is manufactured.
4. prior to the step of shaping the workpiece, determining a size of an opening of the cavity at the exposed surface; This step is obtaining a range of Peclet numbers based on the shape of the aperture; determining the size of the aperture so that the Peclet number is within the range; The additive manufacturing method according to any one of claims 1 to 3, comprising:
5. The additive manufacturing method according to any one of claims 1 to 4, further comprising the step of inserting a fuse into the cavity before the step of burning away the support.
6. The cavity includes at least one first cavity and at least one second cavity having a length in the depth direction shorter than that of the first cavity, The step of burning off the support comprises: a preparation step of preparing a first lid portion having a first through hole formed therein and communicating with the first cavity portion when the first lid portion is attached to the semi-finished product so as to close the exposed surface, and a second lid portion having a second through hole formed therein and communicating with the second cavity portion when the second lid portion is attached to the semi-finished product so as to close the exposed surface; a first burn-off step of burning off the support while the first lid portion is attached to the semi-finished product; a second burn-off step of burning off the support while the second lid portion is attached to the semi-finished product after the first burn-off step; a third burn-off step of burning off the support in a state where neither the first lid portion nor the second lid portion is attached to the semi-finished product after the second burn-off step; The additive manufacturing method according to any one of claims 1 to 5, comprising:
7. A metal additive manufacturing body, At least one overhang portion having a surface facing downward in a lamination direction of the metal; a support for supporting the overhang portion, the support having an exposed surface where the support is exposed from the overhang portion; Equipped with An additive manufacturing body, wherein at least one cavity extending from the exposed surface toward the depth direction of the support is formed in the support, and a fuse is inserted into the at least one cavity.
Citation Information
Patent Citations
Casting method for product having hollow passage
JP1995227645A
Support member for laminate molding, manufacturing method and manufacturing device of solid article by laminate molding, molding model generation device, control device and molding method of molded article
JP2017193776A
Support ink for 3D printing
JP2017500222A
Supporting member, molding model generator, controller, and method for molding molded article
JP2018135548A
Method for manufacturing three-dimensional molded article
JP2020196218A