Cutting edge
Laser build-up welding with vanadium, chromium, and molybdenum improves the wear resistance and reduces machining work for cutting blades in shear type crushers, addressing the limitations of arc welding.
Patent Information
- Application Number
- JP2020179796
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Existing cutting blades in shear type crushers face challenges in achieving both high hardness and toughness due to wear and tear, with conventional arc welding methods limiting material selection, causing large emissions and increased machining work.
The cutting blade employs laser build-up welding with powder materials containing vanadium, chromium, and molybdenum, allowing precise control over the build-up layer thickness and hardness, reducing the need for post-welding machining.
This approach enhances wear resistance by 1.5 to 2 times compared to arc welding, reduces machining work, and minimizes environmental impact by optimizing material selection and precision.
Smart Images

Figure 0007554464000002 
Figure 0007554464000001 
Figure 0007554464000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a cutting blade for use in a shear-type crusher or the like. [Background technology]
[0002] As shown in Figs. 3 and 4, a shear-type crusher crushes materials by the shearing force generated by opposing rotating blades C like scissors. However, the cutting blades 1 used in the rotating blades C wear down due to friction during crushing as they are used, and the blades can chip due to the impact during crushing. Therefore, the cutting blade 1 of the crusher is required to have high hardness and high toughness. However, these are contradictory functions and it has been said that it is difficult to achieve both.
[0003] In addition, the only parts of the cutting blade 1 of the crusher that wear out are the parts that come into contact with the object to be crushed, and depending on the object to be crushed, only certain parts of the cutting blade 1 may wear out.
[0004] When the cutting blade 1 wears out and its crushing performance drops significantly, it is replaced with a new one, and the used cutting blade 1 is recycled. However, refining it to regenerate it results in large amounts of CO2 emissions, which is a major environmental burden.
[0005] In order to deal with this problem, a method of repairing the worn portion by build-up welding using arc welding has been widely used in the past (see, for example, Patent Document 1). As a result, the welded portion of the cutting blade, which is built up by arc welding, ensures high hardness, and by making the base material out of a tough material, we have obtained a cutting blade that meets the requirements for performance as a crusher blade. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-196610 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the above-mentioned method of repairing the worn portion of the cutting blade by build-up welding using arc welding has the following problems. In the case of arc welding, only wire-type welding consumables can be used, so the choice of welding consumables is limited. The dilution area caused by heat input and welding materials is large, and the area with reduced hardness is widespread. - The amount of build-up increases because it is difficult to precisely control the thickness of the build-up layer, and in order to ensure the specified dimensional accuracy, 70-80% of the build-up amount needs to be machined, which increases the amount of machining work after build-up welding. In order to increase the hardness of the overlay weld, it is preferable to use welding materials with high hardness. However, if the hardness is too high (HRC60 or higher), the machinability after overlay welding deteriorates significantly, and it becomes necessary to use welding materials that are relatively easy to machine. For these reasons, the method of build-up welding by arc welding is used when repairing worn portions of cutting blades, but has the problem that it is difficult to apply to new cutting blades.
[0008] The present invention aims to provide a cutting blade that solves the problems, such as heat input and dimensional accuracy, associated with the above-mentioned conventional method of repairing worn portions of a cutting blade by build-up welding using arc welding, and that makes it possible to reinforce easily worn portions of a new cutting blade. [Means for solving the problem]
[0009] In order to achieve the above object, the cutting blade of the present invention comprises: A cutting edge portion protruding radially outward is provided, The blade tip has a tip edge portion that is sharpened in the direction of rotation, A side edge portion is provided on the outer edge of the side surface including the cutting edge portion, In the cutting blade, an upper surface of the tip edge portion and the side edge portion are formed with a build-up welded portion, The build-up weld portion is characterized in that the build-up weld portion is a laser build-up weld portion.
[0010] In this case, the laser build-up welded portion may be formed in a groove having a semicircular cross section formed in the base material of the cutting blade.
[0011] The laser build-up welded portion may contain vanadium, chromium and molybdenum. Effect of the Invention
[0012] The cutting blade of the present invention solves the problems associated with the conventional method of repairing worn portions of a cutting blade by build-up welding using arc welding, and provides the following advantageous effects. In the case of laser build-up welding, since the welding material is a powder, there are no restrictions on the choice of welding material, and the selection of welding materials is broadened. In addition to commercially available products, it is possible to create original welding powder, making it possible to achieve unique hardness and toughness. - The area of dilution caused by heat input or welding material is small, and the area of reduced hardness is limited to a narrow range, thereby minimizing the reduction in hardness. Since precise control of the thickness of the build-up layer is possible by controlling the welding material (powder) supply amount, welding speed, and other conditions, the build-up amount can be kept to a minimum, and the machining allowance required to ensure the specified dimensional accuracy can be controlled to be small (specifically, around 0.5 mm). This reduces the machining allowance required for finishing processes in areas that affect performance such as interference (for example, finish grinding of the cutting blade thickness). This, combined with the fact that machining after build-up welding is not required for areas that do not affect performance such as interference, reduces the amount of machining work required after build-up welding. - To increase the hardness of the welded overlay, it is preferable to use a welding material with high hardness, but since the process is only by polishing, it is possible to overlay with high hardness (for example, HRC60 or higher). This makes it possible to improve the wear resistance of the laser welded overlay by about 1.5 to 2 times compared to arc welding. From the above, it can be said that the build-up welding method using laser welding is an optimal method not only for repairing worn portions of cutting blades, but also for application to new cutting blades. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1(c) is a cross-sectional view taken along line AA in FIG. 1(a); FIG. 1(d) is a cross-sectional view taken along line BB in FIG. 1(b); FIG. 1(e) is a cross-sectional view taken along line CC in FIG. 1(b); and FIG. 1(f) is a view corresponding to FIG. 1(e) when build-up welding is performed by arc welding. [Diagram 2] 1(c) is a view corresponding to (d) in FIG. 1.
[0033] FIG. 1(c) is a view corresponding to (d) in FIG. [Diagram 3] FIG. 2 is an explanatory diagram of a shear-type crusher to which the cutting blade of the present invention is applied. [Figure 4] FIG. 2 is an explanatory diagram of a rotary blade of the shear-type crusher. [Diagram 5] 5(a) is a front view of the base material of the cutting blade according to a third embodiment of the present invention, (b) is a side view of the same, (c) is an enlarged cross-sectional view of part A in FIG. 5(a), (d) is an enlarged cross-sectional view of part B in FIG. 5(b), and (e) is a front view of the cutting blade which has been build-up welded by laser welding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of a cutting blade according to the present invention will be described with reference to the drawings. EXAMPLES
[0015] FIG. 1 shows a first embodiment of a cutting blade according to the present invention. This cutting blade 1 is used, for example, in a rotary blade C of a shearing crusher having a structure shown in Figs.
[0016] The shearing type crusher has been widely used and has two rotating shafts 3 each having a rectangular cross section, which are arranged substantially parallel to each other with a fixed distance therebetween. The rotating shafts 3 are rotatably installed and supported within a box-shaped casing 6 via bearings (not shown), and are configured to rotate inward (in the direction of the arrow in the figure) by a motor (not shown).
[0017] On the rotating shaft 3, disk-shaped rotating blades C are alternately provided with spacers 4 interposed therebetween. These rotating blades C are attached with their side surfaces in close contact with each other. Each rotary blade C is composed of a cutting blade 1 and a main body 2, and multiple (in this embodiment, six) cutting blades 1 are arranged on the outer peripheral surface 21 of the main body 2, and both are fixed at the bolt holes 15, 22 using bolts (not shown). The cutting blade 1 of the rotary blade C has a fixed portion 11 and a cutting edge portion 12 protruding radially outward from the fixed portion 11. The cutting edge portion 12 has a tip edge portion 13 that is sharp in the direction of rotation and has the effect of drawing in the material to be processed and cutting or shearing it. As a result, the material to be treated that is fed from above the casing 6 is crushed by the above-mentioned action of the cutting blades 1 of the rotary blades C, and is discharged downward.
[0018] A scraper 5 is provided protruding from the side of the box-shaped casing 6 toward the rotary blade C and the spacer 4. The scraper 5 serves to scrape off the material caught between the rotary blades C.
[0019] Incidentally, the cutting blade 1 of the rotary blade C wears down with use due to friction during crushing, and the blade portion may chip due to the impact during crushing, so that it becomes necessary to replace it after a certain period of use. In order to extend this period, the cutting blade 1 of this embodiment is configured to form laser build-up welds 16, 17 on the upper surface of the tip edge portion 13 that is pointed toward the rotation direction of the cutting edge portion 12 and on the side edge portion 14 on the outer edge of the side surface including the cutting edge portion 12, as shown in Figure 1.
[0020] In this case, the base material of the cutting blade 1 can be suitably made of a material having toughness, such as chrome molybdenum steel (SCM440, etc.) or wear-resistant steel (HARDOX (registered trademark) 500).
[0021] Since powder welding material is used for the material of the laser build-up welds 16 and 17, there are no restrictions on the selection of welding material, and the selection of welding materials is broadened. In this embodiment, a powder welding material containing vanadium, chromium and molybdenum is used. As a result, the build-up welds 16, 17 contain vanadium, chromium and molybdenum, and can have a high hardness (for example, HRC 60 to 65).
[0022] The thickness of the laser build-up welded parts 16, 17 can be controlled to the minimum necessary thickness, about 1 to 3 mm, preferably about 2 mm. This makes it possible to control the cutting allowance of the laser buildup welded parts 16, 17 to be small (specifically, around 0.5 mm) in order to ensure a specified dimensional accuracy, and reduces the cutting allowance for finishing processing of parts that affect performance such as interference (for example, finish polishing of the thickness of the cutting blade 1). Combined with the fact that parts that do not affect performance such as interference do not require machining after buildup welding, the amount of machining work after buildup welding can be reduced. In this embodiment, the laser build-up welded portion 16 is provided with a cutting allowance 18 for forming the tip edge portion 13 that is sharpened toward the direction of rotation of the cutting edge portion 12. EXAMPLES
[0023] FIG. 2 shows a second embodiment of the cutting blade of the present invention. This cutting blade 1 has laser build-up welds 16, 17 formed on the upper surface of the tip edge portion 13, which is pointed in the direction of rotation of the cutting edge portion 12, and on the side edge portion 14 on the outer edge of the side surface including the cutting edge portion 12, formed within a groove with a semicircular cross section formed in the base material of the cutting blade 1. The semicircular grooves have a diameter of about 2 to 6 mm, preferably about 4 mm, and are formed in multiple rows, specifically, four rows on the upper surface of the tip edge portion 13 and two rows on the side edge portion 14. As a result, in addition to the effects of the first embodiment, the following effects are achieved. The number of welding passes can be reduced, reducing construction time and costs. By forming the laser build-up welds 16, 17 in a groove having a semicircular cross section formed in the base material of the cutting blade 1, the laser build-up welds 16, 17 are integrated with the base material of the cutting blade 1 and will not peel off. Other configurations and operations of this embodiment are similar to those of the first embodiment. EXAMPLES
[0024] FIG. 5 shows a third embodiment of the cutting blade of the present invention. The cutting blade 1 in the first and second embodiments described above is configured by dividing the cutting blade 1 into multiple pieces, but the form of the cutting blade of the present invention is not limited to this, and the configuration of the cutting blade 1 in the first and second embodiments can also be applied to an integral cutting blade 1 (rotary blade C) that is directly attached to a rotating shaft (not shown) with a rectangular cross section, as shown in Figure 3.
[0025] Specifically, this cutting blade 1 (rotary blade C) has laser build-up welds 16, 17 formed on the upper surface of the tip edge portion 13 that is pointed toward the rotation direction of the cutting edge portion 12 and on the side edge portion 14 on the outer edge of the side surface including the cutting edge portion 12, formed within grooves 17a, 17b that have a semicircular cross section and are formed in the base material of the cutting blade 1. The semicircular grooves have a diameter of about 2 to 6 mm, preferably about 4 mm, and are formed in multiple rows, specifically, four rows (not shown) on the upper surface of the tip edge portion 13 and two rows on the side edge portion 14. This provides the same advantageous effects as those provided by the second embodiment.
[0026] The cutting blade of the present invention has been described above based on several embodiments, but the present invention is not limited to the configurations described in the above embodiments, and the configuration can be changed as appropriate within the scope of the spirit of the present invention, such as by appropriately combining the configurations described in each embodiment. [Industrial Applicability]
[0027] The cutting blade of the present invention has the characteristics of being able to solve the problems of heat input, dimensional accuracy, etc., which are associated with the conventional method of repairing worn parts of cutting blades by build-up welding using arc welding, and being able to reinforce parts of new cutting blades that are prone to wear. Therefore, the cutting blade of the present invention can be suitably used for the cutting blades used in the rotary blades of the twin-shaft shear crusher described in the examples, and can also be widely applied to various cutting blades used in the rotary blades of single-shaft or multi-shaft shear crushers other than twin-shaft shear crushers, and can be used not only to reinforce parts of new cutting blades that are prone to wear, but also to repair worn parts of cutting blades. [Explanation of symbols]
[0028] 1 cutting blade 11 Fixed part 12 Cutting edge 13 Tip edge 14 Side edge part 16 Laser cladding weld 17 Laser cladding weld 18 Cutting allowance C Rotary blade
Claims
1. A cutting edge portion protruding radially outward is provided, The blade tip has a tip edge portion that is sharpened in the direction of rotation, A side edge portion is provided on the outer edge of the side surface including the cutting edge portion, A method for reinforcing a wear-prone portion of a new cutting blade by forming a build-up weld on an upper surface of the tip edge portion and on the side edge portion, The build-up weld is formed by laser build-up to a thickness of 1 to 3 mm, The build-up welded portion of the side edge portion is recessed from the side surface of the cutting blade to form a stepped recessed surface along the side edge portion, so that the recessed surface remains at a predetermined width. A method for reinforcing a portion of a new cutting blade that is easily worn, comprising:
2. A method for reinforcing a wear-prone portion of a new cutting blade as described in claim 1, characterized in that a cutting allowance is provided on the underside of the tip edge portion having a laser build-up weld formed on the upper surface of the tip edge portion, thereby forming a tip edge portion that is pointed in the rotation direction of the cutting edge portion.
3. 3. The method for reinforcing a portion of a new cutting blade that is easily worn out as set forth in claim 1 or 2, wherein the laser build-up welded portion contains vanadium, chromium and molybdenum.
Citation Information
Patent Citations
Repairing method for cutter
JP2001170849A
Valve seat manufacturing method
JP2005509522A
Blade and method for manufacturing the same
JP2011098314A
Repairing method of gas turbine moving blade and gas turbine moving blade
JP2011106431A
Regenerated cutting blade and shearing type crusher
JP2012196610A