CURABLE THERMALLY CONDUCTIVE POLYSILOXANE COMPOSITIONS HAVING INCREASED THIXOTROPIC INDEX - Patent application

Trialkoxy-functional polysiloxanes with specific molecular weights and concentrations are used to enhance the thixotropic index in thermally conductive polysiloxane compositions, addressing viscosity challenges and ensuring stability and application ease in two-part systems.

JP7554845B2Active Publication Date: 2024-09-20DOW SILICONES CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022560855
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-06
Publication Date
2024-09-20
Estimated Expiration
2040-05-06

AI Technical Summary

Technical Problem

Thermally conductive polysiloxane compositions face challenges in balancing viscosity to stabilize fillers against sedimentation while facilitating application, particularly in two-part curable compositions where thixotropic agents are less effective due to high filler concentrations and chemical differences.

Method used

Incorporating trialkoxy-functional polysiloxanes with specific molecular weights and concentrations to induce shear thinning properties, increasing the thixotropic index by at least 50% to 100% in both parts of the two-part curable composition, ensuring compatibility and stability.

Benefits of technology

The solution effectively stabilizes fillers against sedimentation and enhances application by preferentially increasing low shear viscosity over high shear viscosity, maintaining compatibility and facilitating mixing and distribution in the two-part composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554845000003
    Figure 0007554845000003
  • Figure 0007554845000004
    Figure 0007554845000004
  • Figure 0007554845000002
    Figure 0007554845000002
Patent Text Reader

Abstract

The composition comprises: (a) a vinyl-functional polysiloxane; (b) a silylhydride-functional polysiloxane having an average of at least two silylhydride groups per molecule; (c) 60 to 92 weight percent of a thermally conductive filler; (d) a platinum hydrosilylation catalyst; and (e) 0.05 to 2.0 weight percent of a trialkoxy-functional polysiloxane, the trialkoxy-functional polysiloxane having two or more trialkoxy functional groups per molecule and a number average molecular weight of 1200 or greater, where the weight percents are based on the weight of the composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polysiloxane compositions that can be cured by hydrosilylation.

[0002] Preface Curable thermally conductive polysiloxane compositions are useful in the electronics industry to provide thermal bridges between elements, such as between a heat source and a heat sink. Unlike thermal greases, curable thermally conductive polysiloxane compositions are curable, which means that these compositions can react to form a crosslinked polysiloxane matrix containing thermally conductive fillers. In general, the curable thermally conductive polysiloxane composition is applied to a substrate so as to be in thermal contact with the substrate and generally at least one other element, and then cured to form a cured composition that functions as a thermal bridge between the substrate and any other element that is in contact with the cured composition.

[0003] Thermally conductive silicone compositions typically contain a relatively high concentration of conductive filler in a polysiloxane matrix. The thermally conductive filler is likely to be present in a concentration of 60 weight percent (wt%) or more, and can be present in a concentration of 90 wt% or more of the polysiloxane composition. It is important that the thermally conductive polysiloxane composition is stable against settling or separation of the thermally conductive filler from the polysiloxane matrix in which it resides, so that the composition remains homogeneous during storage prior to use. One way to improve the stability against settling of the filler is to increase the viscosity of the composition as it is stored. However, increasing the viscosity of the composition also creates difficulties in applying the composition to a substrate. Typically, applying a thermally conductive polysiloxane composition requires extruding the composition through an orifice and placing it on a substrate. If the viscosity of the composition is too high, it will be difficult to extrude when applied onto a substrate. Thus, the challenge is to balance the viscosity of the conductive silicone composition between a high viscosity to stabilize the filler from settling and a low viscosity to facilitate application of the composition to a substrate.

[0004] An approach to address the viscosity challenge of thermally conductive polysiloxane compositions is to induce shear thinning behavior in the composition. Many approaches are known in the literature for adding thixotropic agents to compositions to achieve shear thinning behavior. Thermally conductive polysiloxane compositions pose unique challenges to this approach because high concentrations of thermally conductive fillers create an environment in which the viscosity is affected by solid filler-filler interactions, and possible adsorption of the thixotropic agent to the filler surface can reduce the effectiveness of the thixotropic agent in inducing shear thinning behavior throughout the composition. Furthermore, it may be particularly desirable to identify thixotropic agents that not only induce shear thinning behavior in highly filled thermally conductive polysiloxane compositions, but also induce shear thinning behavior by preferentially increasing the low shear viscosity of the composition to a high shear viscosity, thereby providing a thixotropic index that is at least 50 percent (%) higher compared to compositions without thixotropic additives.

[0005] This problem is made even more difficult in the context of two-part curable thermally conductive polysiloxane compositions. Each part of the two-part curable thermally conductive polysiloxane composition is chemically distinct from the others, but is highly filled with thermally conductive fillers. Each part of the two-part composition is desirably shear thinning, so that each is stable to filler settling when separate, but is easily mixed and dispensed. Even more desirably, each part contains the same thixotropic agent, so that the thixotropic agents are compatible when the two parts are mixed.

[0006] It would therefore be desirable, and would be an advancement in the art, to identify a thixotropic agent that induces shear thinning properties in a thermally conductive polysiloxane by preferentially increasing the low shear viscosity of the composition relative to the high shear viscosity, such that an increase in the thixotropic index is obtained of at least 50%, preferably 75% or more, and even 100% or more, relative to a composition that does not contain the thixotropic additive. Even more desirable would be for such a thixotropic agent to function in each part of a two-part curing thermally conductive polysiloxane composition. Summary of the Invention

[0007] The present invention provides a thermally conductive polysiloxane comprising a thixotropic agent that induces shear thinning properties in the thermally conductive polysiloxane by preferentially increasing the low shear viscosity of the composition relative to the high shear viscosity, resulting in a thixotropic index that is at least 50% higher, preferably at least 75% higher, and in some cases 100% higher, compared to a composition that does not contain the thixotropic additive. Additionally, the thermally conductive polysiloxane can be a two-part curing thermally conductive polysiloxane composition in which the thixotropic agent functions as such in each of the two parts.

[0008] The present invention is a result of the discovery that a trialkoxy-functional polysiloxane having two or more trialkoxy functional groups, preferably trimethoxy functional groups, per molecule and having a number average molecular weight of more than 1200, preferably more than 2000, can act as a thixotropic agent in a thermally conductive polysiloxane, and even in each component of a two-part curable thermally conductive polysiloxane composition, by preferentially increasing the low shear viscosity of the composition relative to the high shear viscosity, thereby obtaining an increase in the thixotropic index of at least 50%, 75% or more, or even 100% or more relative to the composition without a thixotropic additive. However, surprisingly, the trialkoxy-functional polysiloxane must be present in an amount of 2.0% by weight or less and at the same time approximately 0.05% by weight or more of the weight of the composition. The increase in the thixotropic index obtained by excess trialkoxy-functional polysiloxane is actually less than 50%.

[0009] In a first aspect, the invention is a composition comprising: (a) a vinyl-functional polysiloxane; (b) a silylhydride-functional polysiloxane having an average of at least two silylhydride groups per molecule; (c) 60 to 92 weight percent of a thermally conductive filler; (d) a platinum hydrosilylation catalyst; and (e) 0.05 to 2.0 weight percent of a trialkoxy-functional polysiloxane, the trialkoxy-functional polysiloxane having two or more trialkoxy functional groups per molecule and a number average molecular weight of 1200 or greater, where the weight percents are based on the weight of the composition.

[0010] In a second aspect, the invention is a process comprising the steps of: (a) combining together all of the components of the composition of the first aspect; (b) optionally heating; and (c) hydrosilylation curing a vinyl-functional polysiloxane and a silylhydride-functional polysiloxane to form a cured composition.

[0011] In a third aspect, the invention is an article comprising a cured composition in contact with a substrate prepared according to the process of the second aspect.

[0012] The compositions of the present invention are useful as curable thermally conductive polysiloxane compositions that can be used as thermally crosslinked materials in devices such as electronic devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Test methods refer to the test method most recent as of the priority date of this document unless a date is given with the test method number. Reference to a test method includes both a reference to the testing society and the test method number. The following test method abbreviations and designations apply herein: ASTM refers to the American Society for Testing and Materials, EN refers to European Norm, DIN refers to the Deutsches Institut fur Normung, ISO refers to the International Organization for Standards, and UL refers to the Underwriters Laboratory.

[0014] Products identified by trade names refer to compositions available under those trade names as of the priority date of this document.

[0015] "Plurality" means two or more. "And / or" means "and, or alternatively." All ranges include endpoints unless otherwise indicated. All weight percentage (wt%) values ​​are by weight of the composition and all volume percentage (vv%) values ​​are by volume of the composition unless otherwise indicated.

[0016] "Polysiloxane" and "siloxane" are used interchangeably and refer to molecules containing multiple Si-O-Si bonds.

[0017] The "thixotropy index" of a composition refers to the ratio of the viscosity of the composition under low shear to the viscosity of the composition under high shear. As used herein, the viscosity of polysiloxanes and compositions is measured using a cone and plate rheometer equipped with a CP52 spindle at 0.1 revolutions per minute (shear rate 0.2 (s ) for low shear viscosity). -1 ) and for the measurement of high shear viscosity, a speed of 10 revolutions per minute (shear rate 20 s -1 ) Unless otherwise stated, viscosity is in millipascal seconds (mPa s).

[0018] "Molecular weight" refers to number average molecular weight expressed in Daltons unless otherwise specified. Molecular weight is measured using triple detector gel permeation chromatography (light scattering, refractive index and viscosity detectors) and a single polystyrene standard.

[0019] The composition of the present invention comprises a vinyl-functional polysiloxane. Desirably, the vinyl-functional polysiloxane comprises, on average, two or more vinyl functional groups per molecule. The vinyl functional groups can be present on the vinyl-functional polysiloxane as pendant groups, as terminal groups, or as both pendant groups and terminal groups. Desirably, the vinyl-functional polysiloxane is a linear polysiloxane having the following molecular structure (I): R x Vi (3-x) SiO-(R2SiO) d -SiR y Vi (3-y) (I) In the formula, R is independently selected from alkyl and aryl groups having 1 to 6 carbon atoms in each case, Vi is a vinyl group (-CH=CH2), x and y indicate the average number of terminal R groups on each end of the linear polysiloxane, each independently selected from a number ranging from 0 to 2, preferably 1 to 2, and desirably x=y, (3-x) and (3-y) indicate the average number of terminal Vi groups on each end of the linear polysiloxane, and d is the average number of (R2SiO) groups in the linear polysiloxane, typically 10 or more, preferably 50 or more, and 1000 or less, preferably 500 or less. Desirably, R is methyl in each case. At the same time, it is generally desirable that x and y are each 2.

[0020] Examples of suitable vinyl-functional polysiloxanes include those available from Gelest under the designations DMS-V21 (wherein in structure (I) each R is methyl, x=y=2, and d is approximately 78, providing a molecule with a viscosity of 100 centistokes and a molecular weight of 6000) and DMS-V25 (wherein in structure (I) each R is methyl, x=y=2, and d is approximately 230, providing a molecule with a viscosity of 500 centistokes and a molecular weight of 17,200); and DOWSIL™ SFD-119 Fluid (wherein in structure (I) each R is methyl, x=y=2, and d is approximately 162, providing a molecule with a viscosity of 450 centistokes and a molecular weight of 12,000); and DOWSIL™ SFD-117 and vinyl-terminated polydimethylsiloxanes available from The Dow Chemical Company under the designation Fluid (structure (I) where each R is methyl, x=y=2, and d is approximately 324, giving the molecule a viscosity of 2000 centistokes and a molecular weight of 24000). DOWSIL is a trademark of The Dow Chemical Company.

[0021] Typically, the concentration of the vinyl-functional polysiloxane in the composition is 5% by weight or more, 10% by weight or more, 15% by weight or more, or even 20% by weight or more, based on the weight of the composition, while typically being 35% by weight or less, 30% by weight or less, 25% by weight or less, 20% by weight or less, or even 15% by weight or less. The concentration of the vinyl-functional polysiloxane will usually vary within these ranges depending on the amount of thermally conductive filler in the composition, which is typically selected based on the desired thermal conductivity properties of the composition.

[0022] The compositions of the present invention comprise a silylhydride-functional polysiloxane having an average of at least two silylhydride groups per molecule. For the avoidance of doubt, a silylhydride group is a SiH group. The silylhydride-functional polysiloxane may also be referred to as the crosslinker in the composition. Desirably, the silylhydride-functional polysiloxane is a linear polysiloxane having the following general molecular structure: R 3-h H h SiO-(HRSiO)a -(R2SiO) b -SiH h’ R 3-h’ (II) [wherein R is as above, H is hydrogen, subscripts h and h' refer to the average number of terminal hydrogens at each end of the molecule and have a value of 0, 1, 2, or 3 (preferably 0, 1, or 2, more preferably 0 or 1, and most preferably 0), subscript a is the average number of (HRSiO) groups per molecule, and generally subscript b is the average number of (RSiO) groups per molecule.] Subscript a or subscript b may be 0, but subscripts a and b are not both 0. Preferably, subscript a is 1 or more, and may be 5 or more, or even 10 or more, while typically 50 or less, and may be 40 or less, 30 or less, or even 20 or less. Subscript b is desirably 0 or more, and may be 1 or more, 2 or more, 3 or more, 4 or more, or even 5 or more, while typically 150 or less, preferably 100 or less. At the same time, the subscript a is desirably 5 percent (%) or more, 6% or more, 7% or more, 8% or more, 9% or more, 10% or more, 15% or more, 20% or more, 25% or more, or even 30% or more of the sum of the subscripts a and b, while typically being 50% or less, 45% or less, 40% or less, or 35% or less, and may be 30% or less, 25% or less, 20% or less, 15% or less, or even 10% or less. The silylhydride functional polysiloxane typically has a molecular weight of 1000 or more, 1500 or more, 1900 or more, 2000 or more, while typically being 5000 or less, 4000 or less, 3000 or less, 2500 or less, or even 2000 or less.

[0023] Examples of suitable silylhydride functional polysiloxanes include trimethylsiloxy terminated hydride functional polymers available from Gelest under the designations HMS-071 (structure (II), where R is methyl, a is 6-7% of the sum of a and b, number average molecular weight of 1900-2000, viscosity of 19 mPa·s), HMS-301 (structure (II), where R is methyl, a is 25-35% of the sum of a and b, number average molecular weight of 1900-2000, viscosity of 14 mPa·s) and DMS-H11 (structure (II) with terminal hydrogen, viscosity of 7-10 mPa·s and number average molecular weight of 1000-1100).

[0024] Typically, the concentration of silylhydride functional polysiloxane in the composition is 0.2% by weight or more, 0.5% by weight or more, 1.0% by weight or more, 2.0% by weight or more, or even 3.0% by weight or more, and at the same time, typically, 8% by weight or less, and 5% by weight or less, based on the weight of the composition. The concentration of silylhydride functional polysiloxane and vinyl functional polysiloxane in the composition is preferably such that the molar ratio of total silylhydride groups to vinyl groups (SiH / Vi ratio) is 0.5 or more, or even 1.0 or more, and at the same time, typically, is 3.0 or less, or even 2.0 or less.

[0025] The composition includes a thermally conductive filler. In the broadest scope of the present invention, the composition of the thermally conductive filler can be any composition that has a higher thermal conductivity than polysiloxane. For example, the thermally conductive fillers can be particles of a material selected from the group consisting of aluminum, copper, silver, carbon nanotubes, carbon fibers, graphene, graphite, silicon nitride, boron nitride, aluminum nitride, diamond, silicon carbide, alumina, aluminum trihydrate, zinc oxide, beryllium oxide, and magnesium oxide. The thermally conductive filler desirably includes or even consists of alumina particles.

[0026] The filler particles may be of any typical particle size or combination of particle sizes commonly used in thermally conductive compositions. In general, the thermally conductive particles desirably have a median particle size of 0.2 micrometers or more, and may have a median particle size of 0.5 micrometers or more, 1.0 micrometers or more, 1.5 micrometers or more, 2.0 micrometers or more, 4.0 micrometers or more, 8.0 micrometers or more, 10.0 micrometers or more, 15 micrometers or more, 20 micrometers or more, 25 micrometers or more, or even 30 micrometers or more, while the median particle size is typically 50.0 micrometers or less, 40 micrometers or less, 30 micrometers or less, 20 micrometers or less, 15 micrometers or less, 10.0 micrometers or less, 9.0 micrometers or less, 8.0 micrometers or less, 7.0 micrometers or less, 6.0 micrometers or less, 5.0 micrometers or less, 4.0 micrometers or less, 3.0 micrometers or less, or even 2.0 micrometers or less. The median particle size of the fillers is measured by laser diffraction particle size analysis using a HELOS Instrument, Sympatec GmbH (Clausthal-Zellerfeld, Germany).

[0027] The composition may, and desirably, contain thermally conductive filler particles having two or more, or even three or more, different median particle sizes. By combining thermally conductive filler particles of different particle sizes, the composition can contain a higher loading of thermally conductive filler particles without increasing the overall viscosity, as if all the thermally conductive filler particles at the same loading were of the same particle size. For example, the composition can contain a combination of a relatively small particle size thermally conductive filler (median particle size in the range of 1.0 to 5.0 micrometers) and a larger particle size thermally conductive filler (median particle size in the range of more than 5.0 micrometers, preferably 6.0 micrometers or more, or even 8.0 micrometers or more, and at the same time 10.0 micrometers or less). Another option for the composition is to contain thermally conductive fillers with three different median particle sizes. The thermally conductive filler can include a combination of small, medium, and large particles, where the small particles have a median particle size of 0.1 micrometers or more, preferably 0.2 micrometers or more, and simultaneously 1.0 micrometers or less, preferably 0.8 micrometers or less, and can be 0.6 micrometers or less, 0.5 micrometers or less, or even 0.4 micrometers or less, the medium particles have a median particle size of 1.1 micrometers or more, preferably 2 micrometers or more, and simultaneously typically 5.0 micrometers or less, preferably 4.5 micrometers or less, and can be 4.0 micrometers or less, 3.5 micrometers or less, 2.5 micrometers or less, or even 2 micrometers or less, and the large particles have a particle size of 5.1 micrometers or more, 6.0 micrometers or more, 7.0 micrometers or more, or even 8.0 micrometers or more, while simultaneously typically 50 micrometers or less, 40 micrometers or less, 30 micrometers or less, 20 micrometers or less, or even 10 micrometers or less, 9 micrometers or less, or 8 micrometers or less.

[0028] The concentration of all thermally conductive fillers combined, where the weight percent is based on the weight of the composition, is typically 60% by weight or more, and may be 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, or even 90% by weight or more, and at the same time is typically 92% by weight or less, and may be 90% by weight or less, 85% by weight or less, 80% by weight or less, 75% by weight or less, 70% by weight or less, or even 65% by weight or less. When the thermally conductive filler is comprised of a combination of two different particle size fillers (e.g., a relatively small particle size filler and a relatively large particle size filler as described above), it is desirable for the larger particle size filler to be present in a higher weight percent than the smaller particle size filler, and preferably the larger particle size filler to be present in about twice the weight percent of the smaller particle size filler.

[0029] The composition includes a platinum hydrosilylation catalyst. The platinum hydrosilylation may be a single catalyst or a combination of catalysts. Suitable hydrosilylation catalysts include platinum metal and platinum compounds and complexes such as platinum(0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane (Karstedt's catalyst), HPtCl, di-.μ.-carbonyldi-.π.-cyclopentadienyldinickel, platinum-carbonyl complexes, platinum-divinyltetramethyldisiloxane complexes, platinum cyclovinylmethylsiloxane complexes, platinum acetylacetonate (acac), platinum black, chloroplatinic acid, platinum compounds such as chloroplatinic acid hexahydrate, reaction products of chloroplatinic acid with monohydric alcohols, platinum bis(ethylacetoacetate), platinum bis(acetylacetonate), platinum dichloride, and complexes of platinum compounds with olefins or low molecular weight organopolysiloxanes or platinum compounds microencapsulated in a matrix or core-shell type structure. The hydrosilylation catalyst may be part of a solution containing complexes of platinum with low molecular weight organopolysiloxanes, including 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane complexes with platinum. These complexes may be microencapsulated in a resin matrix. The catalyst may be 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane complexes with platinum. Suitable hydrosilylation catalysts include, for example, those described in U.S. Patent Nos. 3,159,601, 3,220,972, 3,296,291, 3,419,593, 3,516,946, 3,814,730, 3,989,668, 4,784,879, 5,036,117 and 5,175,325. Microencapsulated hydrosilylation catalysts and methods for their preparation are exemplified in U.S. Patent Nos. 4,766,176 and 5,017,654.

[0030] When the composition is a one-part system in which the components are present together in a single mixture, the platinum catalyst is desirably selected from platinum compounds that are microencapsulated in a matrix or core-shell structure for storage stability. In general, heating the one-part system releases the platinum catalyst from its encapsulant and induces a reaction.

[0031] The platinum hydrosilylation catalyst is typically present in a concentration of 1 parts per million (ppm) by weight or more, preferably 5 ppm or more, 10 ppm or more, 20 ppm or more, 30 ppm or more, 50 ppm or more, 75 ppm or more, 100 ppm or more, while typically not more than 200 ppm, not more than 100 ppm, or even not more than 50 ppm, where ppm is based on parts by weight of the composition.

[0032] The composition comprises a trialkoxy-functional polysiloxane. Preferably, "alkoxy" is selected from an alkoxy group having 1 to 6 carbon atoms, more preferably selected from triethoxy-functional and trimethoxy-functional polysiloxanes. Even more preferably, the trialkoxy-functional polysiloxane is a trimethoxy-functional siloxane.

[0033] Trialkoxy-functional polysiloxanes have two or more trialkoxy functional groups per molecule. Typically, trialkoxy-functional polysiloxanes have two or more, three or more, or even four or more trialkoxy functional groups per molecule, while typically having an average of 20 or less trialkoxy functional groups per molecule, and can have 10 or less, or even 5 or less trialkoxy functional groups. Trialkoxy-functional polysiloxanes can be linear, branched, or a blend of linear and branched on the polysiloxane chain. Linear polysiloxanes have a total concentration of -R'SiO of 0 to 3 mole percent (mol%). 3 / 2 and SiO 4 / 2The branched trialkoxy-functional polysiloxanes have siloxane units, where R' is selected from hydrogen, aryl, and alkyl groups, and have more than 3 mol%, typically 10 mol% or more, 25 mol% or more, or even 50 mol% or more of R'SiO 3 / 2 and SiO 4 / 2 For example, the trialkoxy-functional polysiloxane may be selected from those having the molecular structures (III) to (V) described below.

[0034] When the trialkoxy-functional polysiloxane is linear, the trialkoxy functional group can be terminal, pendant, or both terminal and pendant. A terminal functional group is located at the end of a linear polymer, whereas a pendant functional group extends from the polymer chain between the two ends. For example, the trialkoxy-functional polysiloxane can be or include a linear polysiloxane having a molecular structure (III) with a terminal trialkoxy functional group. ( RO )3Si-(OSiR2) c - O- Si(O R) 3(III) wherein R is as defined above (and preferably methyl), and the subscript c is the average number of (OSiR2) siloxane units per molecule, having a value of about 13 or more, 20 or more, 30 or more, 40 or more, 50 or more, 75 or more, 100 or more, 150 or more, 200 or more, 300 or more, 400 or more, 500 or more, 600 or more, or even 650 or more, while at the same time being about 2000 or less, 1000 or less, 900 or less, 800 or less, 700 or less, 650 or less, or even 645 or less.

[0035] Alternatively, the trialkoxy-functional polysiloxane may have the related molecular structure (IIIb): ( RO )3Si-R”-SiR2-(OSiR2) c -R”-Si(O R) 3(IIIb) wherein R, subscript c are as defined above for molecular structure (III), and R″ is a divalent hydrocarbon having 1 to 6 carbons, preferably —CH2CH2—.

[0036] The trialkoxy-functional polysiloxane can be or include a linear polysiloxane having the molecular structure (IV) having pendant trialkoxy functional groups. R3SiO-(SiR2O) m -(SiRAO) n -SiR3(IV) wherein each R is independently as defined above (and preferably methyl), subscript m is the average number of (SiRO) units per molecule and typically has the value set forth in subscript c of molecular structure (III), subscript n is the average number of (SiRAO) units per molecule and is 2 or greater, and preferably has about the value set forth in subscript c of molecular structure (III), and A has the structure: -R”Si(O R) 3 wherein R is as described above (and is preferably methyl) and R″ is as defined above for molecular structure (IIIb).

[0037] The trialkoxy-functional polysiloxane can be or include a branched polysiloxane having the molecular structure (V). Si[-(OSiR2) p -R”-Si(O R) 3]4(V) wherein R and R″ are as defined above, R is preferably methyl, R″ is preferably —CH2CH2—, and the subscript p is the average number of (OSiR2) siloxane units per molecule, which is typically 20 or more, 25 or more, 30 or more, 35 or more, 40 or more, 45 or more, or even 50 or more, while also typically 100 or less, 75 or less, 60 or less, 50 or less, or even 40 or less.

[0038] The trialkoxy-functional polysiloxanes may have a number average molecular weight of 1200 or more, 1400 or more, 1500 or more, 1600 or more, 1700 or more, 1800 or more, 1900 or more, 2000 or more, 3000 or more, 4000 or more, 5000 or more, 6000 or more, 7000 or more, 8000 or more, 9000 or more, 10000 or more, 11000 or more, or even 12000 or more, while typically having a number average molecular weight of 100000 or less, 90000 or less, 80000 or less, 70000 or less, 60000 or less, 50000 or less, 40000 or less, 30000 or less, 20000 or less, or even 15000 or less.

[0039] Desirably, the trialkoxy-functional polysiloxane has one or less silylhydride (-SH) groups, and preferably has no silylhydride (-SH) groups.

[0040] The trialkoxy-functional polysiloxane is preferably present in a concentration of 0.025% by weight or more, 0.05% by weight or more, preferably 0.10% by weight or more, 0.15% by weight or more, 0.20% by weight or more, 0.25% by weight or more, and may be present in a concentration of 0.30% by weight or more, 0.40% by weight or more, 0.50% by weight or more, 0.60% by weight or more, or even 0.70% by weight or more, and at the same time, it can be present in a concentration of 2.0% by weight or less, preferably 1.5% by weight or less, 1.0% by weight or less, 0.75% by weight or less, 0.60% by weight or less, 0.55% by weight or less, 0.50% by weight or less, where the weight percentage is relative to the weight of the composition. Surprisingly, it has been found that when the trialkoxy-functional polysiloxane is present in a concentration of more than 2.0% by weight, the thixotropic index of the composition increases by less than 50%. Surprisingly, it is found that at lower concentrations, the thixotropy index of the composition increases more dramatically.For example, when the trialkoxy-functional polysiloxane is present at a concentration of 0.05% by weight or more and at the same time 0.75% by weight or less, even 0.60% by weight or less, or 0.55% by weight or less, the thixotropy index unexpectedly increases by 100% or more.The trialkoxy-functional polysiloxane induces the increase in the thixotropy index by preferentially increasing the low shear viscosity of the composition relative to the high shear viscosity.

[0041] The composition may further comprise, and preferably does comprise, a treating agent or a combination of treating agents. The treating agent functions to improve the dispersibility of the filler in other ingredients by reducing filler agglomeration and filler-filler interactions, improve wet-out of the filler surface, reduce the viscosity of the composition, and cap reactive groups on the filler surface to prevent reactions with the filler that may impair the shelf life of the composition. The treating agent comprises or consists of one or both of an alkyltrialkoxysilane and a monotrialkoxysiloxy-terminated diorganopolysiloxane.

[0042] Alkyltrialkoxysilanes are represented by the general formula: 1 )(R 2 O) 3Si, wherein R 1is alkyl desirably having an average of 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, 12 or more, 13 or more, 14 or more, 15 or more, or even 16 or more carbon atoms per molecule, and typically has 18 or fewer carbon atoms, and may have 17 or fewer, 16 or fewer, 15 or fewer, 14 or fewer, 13 or fewer, 12 or fewer, 11 or fewer, or even 10 or fewer carbon atoms; R 2 is preferably an alkyl having 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, or even 6 or more carbon atoms, and at the same time typically having 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less carbon atoms. Desirably, the alkyltrialkoxysilane is an alkyltrimethoxysilane having the above alkyl group. One example of a preferred alkyltrialkoxysilane is n-decyltrimethoxysilane. The concentration of the alkyltrialkoxysilane is about 0% by weight or more, 0.05% by weight or more, 0.10% by weight or more, 0.20% by weight or more, 0.22% by weight or more, 0.24% by weight or more, and at the same time about 0.30% by weight or less, preferably 0.28% by weight or less, 0.26% by weight or less, or 0.24% by weight or less, and may be 0.22% by weight or less, based on the weight of the composition.

[0043] Monotrialkoxysiloxy-terminated diorganopolysiloxanes generally have the following molecular structure (VI): R3SiO-(R2SiO) h -[(CH2) e ((CH3)2SiO) f ] g -(CH2) e -Si(OR 2 )3(VI) wherein R and R 2are each independently, in each occurrence, as defined above; the subscript h is the average number of (RSiO) units per molecule and typically has a value of 10 or more, 15 or more, 20 or more, 25 or more, or even 30 or more, and at the same time is about 150 or less, 140 or less, 130 or less, 120 or less, 110 or less, 100 or less, 90 or less, 80 or less, 70 or less, 60 or less, 50 or less, 45 or less, 40 or less, 35 or less, or even 30 or less; and the subscript e is independently the subscript f typically has a value of 0 or more, 1 or more, 2 or more, 3 or more, and at the same time is usually 4 or less, 3 or less, or even 2 or less; the subscript g typically has a value of 0 or more, 1 or more, 2 or more, 3 or more, and at the same time is about 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less; and the subscript g typically has a value of 0 or more, 1 or more, 2 or more, 3 or more, 4 or more, and at the same time is about 6 or less, 5 or less, 4 or less, or even 3 or less.

[0044] Desirably, the monotrialkoxysiloxy-terminated diorganopolysiloxane has the general molecular structure (VII): (CH3)3SiO-((CH3)2SiO) t -Si(OR 2 )3(VII) has.

[0045] One particularly preferred trialkoxysiloxy-terminated diorganopolysiloxane is R 2 is equal to methyl, and the subscript t is equal to a value of 130 or less, preferably 120 or less, preferably 110 or less, more preferably 110 or less or 100 or less, 90 or less, 80 or less, 70 or less, 60 or less, 50 or less, 40 or less, or 30 or less, and at the same time greater than 20, preferably greater than 30, to form a terminal trimethoxy-functionalized silicon atom.

[0046] The concentration of monotrialkoxysiloxy-terminated diorganosiloxane is typically 0 wt% or more, 0.10 wt% or more, 0.20 wt% or more, 0.30 wt% or more, 0.40 wt% or more, 0.50 wt% or more, 0.75 wt% or more, or even 1.0 wt% or more or 2.0 wt% or more, and at the same time about 3.0 wt% or less, 2.0 wt% or less, 1.20 wt% or less, 1.15 wt% or less, or even 1.10 wt% or less, based on the weight of the composition.

[0047] The composition may further comprise any one or any combination of a number of additional components (or may not). Examples of such additional components include cure inhibitors, antioxidant stabilizers, pigments, viscosity modifiers, silica fillers, and spacer additives. For the avoidance of doubt, the composition may not comprise any one or any combination or a number of such additional components. For example, the composition may not comprise a silica filler. "Silica filler" refers to solid particulates containing silica, including natural silica (such as crystalline quartz, ground quartz, and diatomaceous silica), and synthetic silica (fumed silica, fused silica, silica gel, and precipitated silica). Additionally or alternatively, the composition of the present invention may not comprise polyether and / or silanol-functional polydimethylsiloxane.

[0048] An example of a cure inhibitor is methyl(tris(1,1-dimethyl-2-propynyloxy))silane. When present, the inhibitor is typically present at a concentration of 0.0001% by weight or more, or 0.001% by weight or more, based on the weight of the composition, while generally being present at a concentration of 5% by weight or less, or even 1% by weight or less, or even 0.5% by weight or less.

[0049] When present, antioxidants may be included at a concentration typically between 0.001 and 1% by weight of the composition. Antioxidants may be present alone or in combination with stabilizers. Antioxidants include phenolic antioxidants and stabilizers include organophosphorus derivatives.

[0050] Examples of pigments include carbon black, graphite, titanium dioxide, and copper phthalocyanine. When present, pigments are likely to be present in a concentration of from 0.0001 to 1% by weight based on the weight of the composition.

[0051] The spacer additive is a non-thermally conductive filler having an average particle size in the range of 50 to 250 micrometers. Examples of spacers include glass and polymer beads.

[0052] The compositions of the present invention can be one- or two-component hydrosilylation curable compositions.

[0053] One-component hydrosilylation curable compositions include a vinyl-functional polysiloxane and a silylhydride-functional polysiloxane together in a single mixture. To provide storage stability against premature curing for one-component hydrosilylation curable compositions, the platinum catalyst is generally encapsulated or otherwise inhibited from activating the hydrosilylation reaction. Heating or otherwise releasing the platinum catalyst triggers its activation and hydrosilylation curing of the composition.

[0054] The two-part hydrosilylation curable composition comprises two separate parts, a first part comprising a vinyl-functional polysiloxane and a second part comprising a silylhydride-functional polysiloxane. The platinum hydrosilylation catalyst is typically included in the first part comprising the vinyl-functional polysiloxane. In one beneficial aspect of the invention, the trialkoxy-functional polysiloxane may be present in both parts of the two-part hydrosilylation curable composition, and the low shear viscosity of each part may be preferentially increased relative to the high shear viscosity to achieve a 50% or greater increase in the thixotropic index of each part, and even a 100% or greater increase. The thermally conductive filler may be present in both parts, in which case the trialkoxy-functional polysiloxane may affect each part to increase the stability of the filler in each part due to the preferential increase in low shear viscosity, while maintaining the ability to pump and mix each part under high shear due to the relatively low high shear viscosity reflected in the increase in the thixotropic index of each part. Even more beneficially, because the same additives are used in each part to achieve the increased thixotropy index and preferentially increased low shear viscosity, this property is maintained when the composition cures when the two parts are mixed since the additives are the same and therefore compatible. Two-part compositions are generally cured by mixing the first and second parts together to combine the vinyl-functional polysiloxane and the silylhydride-functional polysiloxane in the presence of a platinum catalyst. Curing typically occurs without any heating, although heating usually speeds up the curing reaction.

[0055] An example of the two-part composition of the present invention includes the following separate (meaning separated) first and second parts: (1) the first part includes (a) 7 to 35 weight percent of a vinyl-functional polysiloxane, (b) 60 to 92 weight percent of a thermally conductive filler, (c) 0.05 to 2.0 weight percent of a trialkoxy-functional polysiloxane, (d) 1 to 100 parts by weight of a platinum hydrosilylation catalyst per 1 million parts by weight of the first part, and (e) 0.1 to 2.0 weight percent of a treating agent; and (2) the second part includes (a) 10 to 15 weight percent of a vinyl-functional polysiloxane, (b) 60 to 92 weight percent of a thermally conductive filler, (c) 0.05 to 2.0 weight percent of a trialkoxy-functional polysiloxane, (d) 1 to 100 parts by weight of a platinum hydrosilylation catalyst per 1 million parts by weight of the first part, and (e) 0.1 to 2.0 weight percent of a treating agent. (b) from 2 to 5 weight percent of a silylhydride functional polysiloxane having an average of at least two silylhydride groups per molecule; (c) from 60 to 92 weight percent of a thermally conductive filler; (d) from 0.05 to 2.0 weight percent of a trialkoxy-functional polysiloxane; (e) from 0 to 1 weight percent of a pigment additive; and (f) from 0 to 0.01 weight percent of a platinum cure inhibitor, where the weight percent values ​​are based on the weight of the liquid in which the components are present.

[0056] The present invention includes a process for curing the compositions of the present invention, comprising the steps of (a) combining together all of the components of the compositions described in any one of the above, (b) optionally heating, and (c) hydrosilylation curing the vinyl-functional polysiloxane and the silylhydride-functional polysiloxane to form the cured composition. Heating is generally not necessary, especially for two-component compositions, but typically accelerates the cure of the composition.

[0057] The process for curing the composition desirably includes applying the composition to a substrate after combining the components in step (a) and before step (b) to form an article on the substrate comprising the cured composition if the process includes heating. The process may further include contacting the composition with a second element after applying the composition to the substrate and before step (b) to form an article comprising the cured composition in thermal contact between the substrate and the second element if the process includes heating.

[0058] The present invention also includes articles prepared by the process of the present invention. Examples of such articles include electronic components. The cured composition of the present invention can thermally connect a heat source and a heat sink within the article and act as a thermal bridge between them. EXAMPLES

[0059] Table 1 lists the materials used in the following examples. "VP" refers to "vinyl functional polysiloxane." "SH-P" refers to "silylhydride functional polysiloxane." "TM-PS" refers to "trimethoxy functional polysiloxane." "TCF" refers to "thermally conductive filler." "TA" refers to "treating agent." [Table 1] SYL-OFF is a trademark of The Dow Chemical Company. SILASTIC is a trademark of Dow Corning Corporation. SILMER is a trademark of The Siltech Corporation.

[0060] Synthesis of TM-PS1 90.82 wt% hydroxy-terminated dimethylsiloxane (Aldrich), 9.1 wt% methyl orthosilicate (Aldrich), and 0.08 wt% glacial acetic acid (Aldrich) are charged into a reactor (e.g., round-bottom flask), mixed, and then heated to 120-130°C and continued mixing for 4 hours. Acetic acid, methanol, and excess methyl orthosilicate are removed under vacuum at 150°C for 5 hours. The resulting product is TM-PS1.

[0061] Synthesis of TM-PS3 Charge 100 g of dimethyl cyclics into a round bottom flask with tetrakis(vinyldimethylsiloxy)silane (0.9 wt% vinyl content, CAS 316374-82-0 available from Skyran Industrial Co., Ltd.) and 9.42 g of 1(-2-(trimethoxysilyl)ethyl)-1,1,3,3-tetramethyldisiloxane (available from Gleader Advanced Material Co., Ltd). Add 0.06 g of platinum catalyst II. Mix at 90° C. for 3 hours. Remove platinum residue by filtration to obtain TM-PS3.

[0062] Sample Composition A sample composition is prepared as a two-liquid curing type composition containing a first liquid (liquid A) and a second liquid (liquid B).

[0063] Composition of Solution A The formulations for each Part A sample are shown in Table 2. The VF-P component is charged to a 10 L Turello mixer vessel and mixed for 5 minutes at 20 revolutions per minute (RPM) under a nitrogen flow of 0.4 cubic meters per hour. The TCF component is added and mixing is continued for 15 minutes. The mixture is heated to 120° C. under vacuum (approximately 0.1 megapascals) for 1 hour. Cool to 22° C. and the Platinum Catalyst I component is added and mixed for 15 minutes at 750 RPM under a nitrogen purge.

[0064] Composition of Solution B The formulations for each B part sample are shown in Table 3. The VF-P, carbon black, and TA components are charged to a 10 L Turello mixer vessel and mixed for 5 minutes at 20 RPM under a nitrogen flow of 0.4 cubic meters per hour. The TCF component is added and mixing is continued for 15 minutes. The mixture is heated to 120° C. under vacuum (approximately 0.1 megapascals) for 1 hour. Cool to 22° C. and add the set inhibitor, SHF-P, and TM-PS components and mix for 15 minutes at 750 RPM under a nitrogen purge.

[0065] Table 4 shows the low shear viscosity, high shear viscosity, and thixotropy index for each sample of Part A and Part B. The low shear and high shear viscosities and thixotropy index are measured as described herein above. [Table 2] [Table 3] [Table 4]

[0066] The data in Table 4 reveal that the compositions of the claimed invention exhibit a preferential increase in low shear viscosity and an increase in thixotropy index of 50% or more, 75% or more, and in many cases even 100% or more when a trimethoxy-functional polysiloxane having a molecular weight of 1200 or more is added at a concentration of 0.05 to 2.0 weight percent based on the weight of the composition.

[0067] The reference (Ref) sample represents a composition that does not contain trimethoxy-functional polysiloxane and serves as a reference composition.

[0068] The composition of Sample 5 has greater than 2.00 wt.% trimethoxy-functional polysiloxane, and the data show that the increase in thixotropy index over the reference composition is less than a 50% increase, whereas Samples 1-4 show that the same compositions containing less than 2.00 wt.% of the same trimethoxy-functional polysiloxane all exhibit an increase in thixotropy index of greater than 50%.

[0069] Samples 12 and 13 show trimethoxy-functional linear molecules similar to TM-PS1 but which are not polysiloxanes. These samples also do not show an increase in thixotropy index of 50% or more, even at loadings where TM-PS1 shows an increase in thixotropy index of over 100%.

[0070] Samples 14 and 15 contain a linear trimethoxy-functional polysiloxane similar to TM-PS1 except that it has a molecular weight of about 1100. These samples also fail to increase the thixotropic index of the composition by more than 50% at the dosage levels at which TM-PS1 causes an increase in the thixotropic index of more than 100%.

[0071] Samples 1-15 are two-part curing compositions. When the A-part and B-part compositions of each sample are mixed together, the blended compositions undergo a hydrosilylation curing reaction to produce a cured composition. The compositions of each part are modified with the same trimethoxy-functionalized polysiloxane, achieving a 50% or greater increase in thixotropic index due to the preferential increase in low shear viscosity caused by the presence of the trimethoxy-functionalized polysiloxane. Similar results are expected if these compositions are one-part curing compositions in which the cure is inhibited by using an inhibited catalyst (e.g., blocked or encapsulated catalyst) that is released by unblocking (e.g., UV-irradiation or thermal release of a blocking agent) or melting of an encapsulating material around the catalyst.

Claims

1. (a) a vinyl-functional polysiloxane; (b) a silylhydride-functional polysiloxane having an average of at least two silylhydride groups per molecule; (c) 60 to 92 weight percent of a thermally conductive filler; (d) a platinum hydrosilylation catalyst; and (e) 0.05 to 2.0 weight percent of a trialkoxy-functional polysiloxane, the trialkoxy-functional polysiloxane has 2 or more trialkoxy functional groups per molecule and a number average molecular weight of 1200 or greater, the weight percentages being based on the weight of the composition; the composition is a two-part composition comprising separate first and second parts, (a) the first liquid is (i) 7 to 35 weight percent of a vinyl-functional polysiloxane; (ii) 60 to 92 weight percent of a thermally conductive filler; and (iii) 0.05 to 2.0 weight percent of a trialkoxy-functional polysiloxane; (iv) 1 to 1,000 parts by weight of a platinum hydrosilylation catalyst per 1,000,000 parts by weight of the first liquid; and (v) 0.1 to 2.0 weight percent of a treating agent; (b) the second liquid is (i) 10 to 15 weight percent of a vinyl-functional polysiloxane; (ii) 2 to 5 weight percent of a silylhydride-functional polysiloxane having an average of at least two silylhydride groups per molecule; (iii) 60 to 92 weight percent of a thermally conductive filler; and (iv) 0.025 to 2.0 weight percent of a trialkoxy-functional polysiloxane; (v) 0 to 1 weight percent of a pigment additive; and (vi) 0 to 0.01 weight percent of a platinum cure inhibitor; provided that the weight percent values ​​are based on the weight of the liquid in which the component is present; The silylhydride functional polysiloxane has the following general molecular structure: R 3-h H h SiO-(HRSiO) a -(R 2 SiO) b -SiH h' R 3-h' (II) where R is independently selected at each occurrence from alkyl and aryl groups having 1 to 6 carbon atoms, H is hydrogen, subscripts h and h' refer to the average number of terminal hydrogens at each end of the molecule and are 0, subscript a is the average number of (HRSiO) groups per molecule, subscript b is the average number of (R 2 SiO) groups per molecule, subscript a is 5% to 50% of the sum of subscripts a and b, and the silylhydride functional polysiloxane has a molecular weight of 1000 to 5000. having The trialkoxy-functional polysiloxanes have the following molecular structures (III), (IIIb), (IV), and (V): (RO) 3 Si-(OSiR 2 ) c -O-Si(OR) 3 (III) where R is independently selected at each occurrence from alkyl and aryl groups having 1 to 6 carbon atoms, and the subscript c is the average number of (OSiR 2 ) siloxane units per molecule, which is 13 to 2000; (RO) 3 Si-R"-SiR 2 -(OSiR 2 ) c-R"-Si(OR) 3 (IIIb) wherein R, subscript c are as defined above for molecular structure (III), and R″ is a divalent hydrocarbon having 1 to 6 carbon atoms; R 3 SiO-(SiR 2 O) m -(SiRAO) n -SiR 3 (IV) wherein each R is independently selected at each occurrence from alkyl and aryl groups having 1 to 6 carbon atoms; subscript m is the average number of (SiR 2 O) units per molecule and is 13 to 2000; subscript n is the average number of (SiRAO) units per molecule and is 2 or greater; and A is a compound having the structure: -R"Si(OR) 3 ( wherein R is selected from alkyl and aryl groups having 1 to 6 carbon atoms, and R″ is a divalent hydrocarbon having 1 to 6 carbon atoms; and Si[-(OSiR 2 ) p-R"-Si(OR) 3 ] 4 (V) where R is selected from alkyl and aryl groups having 1 to 6 carbon atoms, R″ is a divalent hydrocarbon having 1 to 6 carbon atoms, and the subscript p is the average number of (OSiR 2 ) siloxane units per molecule which is 20 to 100. The composition of matter is selected from those having the formula:

2. The composition of claim 1, wherein the concentration of the trialkoxy-functional polysiloxane ranges from 0.05 to 0.75 weight percent by weight of the composition.

3. 3. The composition of claim 1 or 2, which is free of polyethers, silica fillers, and silanol-functional polydimethylsiloxanes.

4. 4. A process comprising the steps of: (a) combining together all of the components of the composition of any one of claims 1 to 3; (b) optionally heating; and (c) hydrosilylation curing the vinyl-functional polysiloxane and the silylhydride-functional polysiloxane to form a cured composition.

5. 5. The process of claim 4, further comprising applying the composition to a substrate after step (a) to produce an article comprising the cured composition on the substrate.

6. 5. The process of claim 4, further comprising contacting the composition with both a substrate and a second component after step (a) and before step (b) to form an article comprising the cured composition in thermal contact between the substrate and the second component, if the process includes heating.

7. 7. An article comprising a cured composition in contact with a substrate prepared according to claim 5 or 6.

8. The article of claim 7 which is an electronic component.

Citation Information

Patent Citations

  • Heat-conductive silicone rubber composition and molded article

    JP2005325211A

  • Thermally conductive silicone rubber composition

    JP2006274155A

  • Thermo-conductive silicone potting composition

    JP2016084378A

  • Thermally conductive silicone potting composition

    JP2019077845A