Laminated film for speaker diaphragm and its manufacturing method
The laminated film with a thermoplastic polyolefin and thermoplastic aromatic liquid crystal polyester skin layer, supported by a core layer, addresses the limitations of conventional speaker diaphragms by enhancing sound quality and productivity.
Patent Information
- Application Number
- JP2022565365
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-27
- Filing Date
- 2021-11-24
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2041-11-24
AI Technical Summary
Conventional speaker diaphragms face challenges with insufficient strength, storage modulus, internal loss, and heat resistance, leading to poor sound quality and high production costs, especially in high-end electronic devices.
A laminated film structure with a skin layer composed of thermoplastic polyolefin and thermoplastic aromatic liquid crystal polyester, supported by a core layer, which enhances storage modulus and internal loss, improving sound quality and productivity.
The laminated film achieves high storage modulus and internal loss, ensuring wide sound reproduction bands and excellent sound pressure flatness, while being cost-effective and industrially viable.
Smart Images

Figure 0007554847000002 
Figure 0007554847000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated film for a speaker diaphragm, and a manufacturing method thereof. [Background technology]
[0002] Traditionally, small speakers (usually called "microspeakers") used in a variety of electronic devices, such as car speakers, mobile phones, portable game devices, smartphones, tablet-type mobile terminals, digital cameras, digital video cameras, laptops, LCD TVs, portable audio devices, microphones, and earphones, have used single-layer speaker diaphragms made of polyethylene terephthalate.
[0003] However, in recent years, as electronic devices have become more functional and performant, the characteristics required for speaker diaphragms have become increasingly strict, including light weight, high strength and rigidity, durability, heat resistance, and, if necessary, excellent moisture resistance and water resistance.
[0004] For this reason, single-layer speaker diaphragms made of super engineering plastics such as polyetherimide (PEI) and polyetheretherketone (PEEK), which are not only lightweight and excellent in heat resistance and moldability, but also have excellent propagation speed and a relatively good reproduction band, are also being considered. However, although these single-layer films have a good propagation speed of about 1000 to 1500 m / s, their internal loss Tan δ (also called loss tangent) is only about 0.04 to 0.05, and there are limitations in terms of sound quality, especially in terms of frequency characteristics of sound pressure, making it difficult to meet the required performance in high-end electronic devices that require high sound quality.
[0005] In order to solve these problems, a multi-layered speaker diaphragm has been studied, in which a skin layer is provided on a core layer to form a multi-layer structure. For example, Patent Documents 1 to 3 disclose a multi-layered speaker diaphragm in which a skin layer made of polyester resin, PEEK, or the like is laminated on a core layer made of thermoplastic elastomer, silicone rubber, or a resin-impregnated base material. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 03-102999 [Patent Document 2] Japanese Patent Application Publication No. 03-107300 [Patent Document 3] JP 2005-101889 A [Patent Document 4] JP 2018-064150 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the techniques of Patent Documents 1 to 3 using a polyester resin as a skin layer have insufficient strength, and also insufficient storage modulus E' (25°C, frequency 1 Hz) and internal loss Tan δ (25°C, frequency 1 Hz). Furthermore, the techniques of Patent Documents 1 to 3 have the disadvantage that the heat resistance of the skin layer is low, so that the storage modulus value fluctuates greatly with temperature changes, and the region in which sound transmission is stable is narrow.
[0008] In addition, even in the technology of Patent Document 4, in which PEEK is used as a skin layer, the storage modulus E' and internal loss Tan δ are still insufficient. Moreover, in the technology of Patent Document 4, a relatively hard PEEK film of the micron order is laminated by dry lamination on a silicone rubber layer that is the core layer. In this lamination method, the film is difficult to handle during production, resulting in poor productivity, and the obtained laminate is prone to thickness unevenness and poor thickness precision. Moreover, the PEEK film is relatively expensive, resulting in poor economic efficiency. Therefore, from the perspective of mass production of high-quality and high-quality speaker diaphragms, the technology of Patent Document 4 has poor industrial applicability.
[0009] The present invention has been made in view of the above problems. An object of the present invention is to provide a laminated film for a speaker diaphragm, which has both a high storage modulus E' and a high internal loss Tan δ, and is excellent in productivity and economy and has high industrial applicability, and a method for producing the same. [Means for solving the problem]
[0010] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have newly designed and developed a multilayer film having a laminated structure in which a thermoplastic polyolefin resin layer of a specified composition serves as a skin layer and this skin layer is supported on a core layer, and have found that the above-mentioned problems can be solved by using this laminated film, thus completing the present invention.
[0011] That is, the present invention provides various specific embodiments as shown below. (1) A laminated film for speaker diaphragms, comprising at least a skin layer containing at least 60 to 90 mass % of a thermoplastic polyolefin having a melting temperature of 230°C or higher and 10 to 40 mass % of a thermoplastic aromatic liquid crystal polyester, based on the total amount of resin solids, and a core layer containing one or more types selected from the group consisting of a thermoplastic elastomer and a thermoplastic polyolefin having a melting temperature of 230°C or higher, and having a laminated structure in which at least one of the skin layers is supported on the core layer.
[0012] (2) 7.0×10 8 The laminate film for speaker diaphragm according to (1), having a storage modulus E' (25°C, frequency 1 Hz) of at least Pa. (3) The laminate film for a speaker diaphragm according to (1) or (2), which has an internal loss Tan δ (at 25° C. and a frequency of 1 Hz) of 0.04 or more.
[0013] (4) The laminate film for speaker diaphragms according to any one of (1) to (3), wherein the thermoplastic polyolefin of the skin layer includes one or more selected from the group consisting of polypropylene-based polymers, cyclic olefin polymers, and cyclic olefin copolymers. (5) The laminate film for a speaker diaphragm according to any one of (1) to (4), wherein the thermoplastic aromatic liquid crystal polyester of the skin layer contains a thermoplastic wholly aromatic liquid crystal polyester. (6) The laminate film for a speaker diaphragm according to any one of (1) to (5), wherein the thermoplastic elastomer of the core layer includes at least one selected from the group consisting of a polyolefin-based thermoplastic elastomer, a polyester-based thermoplastic elastomer, and a polyurethane-based thermoplastic elastomer. (7) The laminate film for a speaker diaphragm according to any one of (1) to (6), wherein the skin layer has a total thickness of 15% or more and 80% or less of the total thickness of the laminate film.
[0014] (8) 9.0×10 8 The laminate film for a speaker diaphragm according to any one of (1) to (7), having a storage modulus E' (25°C, frequency 1 Hz) of at least Pa. (9) The laminate film for a speaker diaphragm according to any one of (1) to (8), which has an internal loss Tan δ (at 25° C. and a frequency of 1 Hz) of 0.06 or more. (10) The laminate film for a speaker diaphragm according to any one of (1) to (9), which has a tensile breaking elongation at 150° C. of 200% or more. (11) The skin layer has a thickness of 2.0×10 8The laminate film for a speaker diaphragm according to any one of (1) to (10), having a storage modulus E' (25°C, frequency 1 Hz) of Pa or more and an internal loss Tan δ (25°C, frequency 1 Hz) of 0.03 or more.
[0015] (12) A method for producing a laminated film for speaker diaphragms, comprising melt-extrusion-molding a first resin composition containing at least 60 to 90% by mass of a thermoplastic polyolefin having a melting temperature of 230° C. or higher and 10 to 40% by mass of a thermoplastic aromatic liquid crystal polyester, based on the total amount of resin solids, and a second resin composition containing one or more selected from the group consisting of a thermoplastic elastomer and a thermoplastic polyolefin having a melting temperature of 230° C. or higher. Here, the production method described in the above item (12) preferably further has the technical feature described in any one of the above items (1) to (11). Effect of the Invention
[0016] According to one aspect of the present invention, it is possible to provide a laminated film for a speaker diaphragm, which has both a high storage modulus E' and a high internal loss Tan δ, and is relatively low in cost and excellent in productivity and economy, and a method for producing the same. In addition, according to a preferred aspect of the present invention, it is possible to provide an acoustic characteristic that could not be realized by the conventional technology, i.e., 7.0×10 8 It is possible to provide a laminated film for speaker diaphragms having a storage modulus E' (25°C, frequency 1 Hz) of Pa or more and an internal loss Tan δ (25°C, frequency 1 Hz) of 0.04 or more, and as a result, a speaker with a wide playback band and excellent sound pressure flatness can be realized. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a laminated film 100 for a speaker diaphragm according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. The positional relationships such as up, down, left and right are based on the positional relationships shown in the drawings unless otherwise specified. The dimensional ratios of the drawings are not limited to the ratios shown. However, the following embodiments are examples for explaining the present invention, and the present invention is not limited to these. That is, the present invention can be practiced with any changes within the scope of the gist of the present invention. In this specification, for example, the expression of a numerical range such as "1 to 100" includes both the lower limit "1" and the upper limit "100". The same applies to the expression of other numerical ranges.
[0019] (Laminated film for speaker diaphragms) 1 is a schematic cross-sectional view showing the present embodiment of a laminated film for a speaker diaphragm 100. The laminated film for a speaker diaphragm 100 of the present embodiment has a laminated structure including at least skin layers 11 and 12 and a core layer 21, with at least one of the skin layers 11 and 12 being supported on the core layer 21.
[0020] The laminated film 100 for a speaker diaphragm of this embodiment has a laminated structure (three-layer structure) in which a skin layer 11, a core layer 21, and a skin layer 12 are arranged at least in this order. In this laminated structure, the skin layer 11 is provided on the surface 21a side of the core layer 21, and the skin layer 12 is provided on the surface 21b side of the core layer 21. Note that, although the laminated film 100 for a speaker diaphragm is exemplified in this embodiment, the present invention can also be embodied as a laminated film for a speaker diaphragm having a two-layer structure in which either the skin layer 11 or the skin layer 12 is omitted, and can also be embodied in an embodiment in which, for example, a plurality of laminated films having a three-layer structure or a two-layer structure are laminated.
[0021] In this specification, "arranged at least in this order" refers not only to an embodiment in which the skin layers 11 and 12 are directly placed on the surface (e.g., surface 21a or surface 21b) of the core layer 21 as in this embodiment, but also to an embodiment in which any layer (e.g., a primer layer, an adhesive layer, a resin layer, etc.) not shown is interposed between the surface 21a, surface 21b of the core layer 21 and the skin layers 11 and 12, and the skin layers 11 and 12 are arranged (supported) at a distance from the surfaces 21a and 21b of the core layer 21. In such a case, the laminated film 100 for a speaker diaphragm will have a four-layer structure, a five-layer structure, etc.
[0022] The skin layers 11 and 12 are formed by molding a thermoplastic resin component into a film shape. The skin layers 11 and 12 are layers supported by the surfaces 21a and 21b of the core layer 21, and in this embodiment, are located on the outermost surfaces of the laminated film 100 for a speaker diaphragm. By providing the skin layers 11 and 12, it is possible to impart a good transmission speed and internal loss to the laminated film 100 for a speaker diaphragm. As the skin layers 11 and 12, a melt-extruded film such as a T-die melt-extruded film is preferably used.
[0023] The skin layers 11 and 12 contain at least 60 to 90% by mass of a thermoplastic polyolefin having a melting temperature of 230°C or higher and 10 to 40% by mass of a thermoplastic aromatic liquid crystal polyester based on the total amount of resin solids. By providing the skin layers 11 and 12 of a polymer blend mainly composed of a thermoplastic polyolefin having a high melting temperature, in combination with the core layer described below, a balance between transmission speed, internal loss, and strength that could not be achieved by conventional techniques is realized. In this specification, "mainly composed of thermoplastic polyolefin" means that the content ratio of the thermoplastic polyolefin exceeds 50% by mass with respect to the total amount of resin components contained in the skin layers 11 and 12.
[0024] The type of thermoplastic polyolefin having a melting temperature of 230°C or more contained in the skin layers 11, 12 is not particularly limited, and can be appropriately selected from known ones. Specific examples of such thermoplastic polyolefins include polypropylene-based polymers such as propylene homopolymers, propylene-ethylene block copolymers, and propylene-ethylene random copolymers; cyclic olefin-based polymers (COP) such as polymers obtained by ring-opening polymerization and hydrogenation of norbornene, copolymers made from norbornene and olefins such as ethylene, and cyclic olefin-based copolymers (COC) such as copolymers made from tetracyclododecene and olefins such as ethylene; and modified products thereof, but are not particularly limited thereto. The thermoplastic polyolefins can be used alone or in any combination and ratio of two or more kinds.
[0025] The thermoplastic polyolefin contained in the skin layers 11 and 12 is preferably a cyclic olefin polymer (COP) or a cyclic olefin copolymer (COC), and more preferably a cyclic olefin polymer (COP). Examples of the cyclic olefin polymer (COP) include polyolefin resins described in JP-A-5-317411 and JP-A-2014-068767, the contents of which are incorporated herein by reference. Note that, as commercially available products of the cyclic olefin polymer (COP), for example, ZEONEX (registered trademark) and ZEONOR (registered trademark) manufactured by Zeon Corporation, Daikyo Resin CZ (registered trademark) manufactured by Daikyo Seiko Co., Ltd., and the like are known. In addition, as commercially available products of the cyclic olefin copolymer (COC), for example, APEL (registered trademark) manufactured by Mitsui Chemicals, Inc., TOPAS (registered trademark) manufactured by Topas Advanced Polymers, and the like are known.
[0026] The melting temperature of the thermoplastic polyolefin contained in the skin layers 11 and 12 is not particularly limited, but from the viewpoint of ensuring good dispersibility with the thermoplastic aromatic liquid crystal polyester, it is preferably 210° C. or higher, more preferably 230° C. or higher, and even more preferably 250° C. or higher, and the upper limit is preferably 320° C. or lower, more preferably 300° C. or lower. In this specification, the melting temperature means the melting peak temperature in differential scanning calorimetry (DSC) when heating at a temperature rise rate of 20° C. / min in a temperature range of 30 to 400° C. using a DSC8500 (manufactured by PerkinElmer).
[0027] The content ratio of the thermoplastic polyolefin described above can be appropriately set depending on the required performance and is not particularly limited, but from the viewpoint of controlling the orientation of the thermoplastic aromatic liquid crystal polyester and ensuring good acoustic properties, it is preferably 60 to 90 mass% in total, more preferably 65 to 90 mass% in total, and even more preferably 70 to 90 mass% in total based on the total amount of resin solids contained in the skin layers 11 and 12. The type and content ratio of the thermoplastic polyolefin contained in the skin layers 11 and 12 may be the same or different.
[0028] The type of thermoplastic aromatic liquid crystal polyester contained in the skin layers 11, 12 is not particularly limited, and can be appropriately selected from known ones. Such a thermoplastic aromatic liquid crystal polyester is a concept that includes thermoplastic wholly aromatic liquid crystal polyester. Thermoplastic aromatic liquid crystal polyester is a polymer that forms an optically anisotropic molten phase, and a representative example is a thermotropic liquid crystal compound. The properties of the anisotropic molten phase can be confirmed by a known method such as a polarization inspection method using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by using a Leitz polarizing microscope and observing a sample placed on a Leitz hot stage at a magnification of 40 times under a nitrogen atmosphere.
[0029] Specific examples of thermoplastic aromatic liquid crystal polyesters include, but are not limited to, those obtained by polycondensation of monomers such as aromatic or aliphatic dihydroxy compounds, aromatic or aliphatic dicarboxylic acids, aromatic hydroxycarboxylic acids, aromatic diamines, aromatic hydroxyamines, and aromatic aminocarboxylic acids. The thermoplastic aromatic liquid crystal polyesters can be used alone or in any combination and ratio of two or more.
[0030] Among these, thermoplastic aromatic liquid crystal polyesters that exhibit thermotropic liquid crystal-like properties and have a melting temperature (melting point) of 250° C. or more, preferably 270° C. to 380° C., are preferably used. As such thermoplastic aromatic liquid crystal polyesters, for example, thermoplastic aromatic polyester resins that are synthesized from monomers such as aromatic diols, aromatic carboxylic acids, and hydroxycarboxylic acids and exhibit liquid crystallinity when melted are known. Representative examples thereof include, but are not limited to, polycondensates of ethylene terephthalate and parahydroxybenzoic acid, polycondensates of phenol and phthalic acid and parahydroxybenzoic acid, and polycondensates of 2,6-hydroxynaphthoic acid and parahydroxybenzoic acid.
[0031] A preferred embodiment is an aromatic polyester resin having, as a basic structure, 6-hydroxy-2-naphthoic acid and its derivatives (hereinafter, sometimes simply referred to as "monomer component A") and parahydroxybenzoic acid and its derivatives (hereinafter, sometimes simply referred to as "monomer component B"). In a molten state, such aromatic polyester resins form an anisotropic molten phase in which linear chains of molecules are regularly aligned, typically exhibiting thermotropic liquid crystal-like properties, and have excellent basic performance in terms of mechanical properties, electrical properties, high frequency properties, heat resistance, moisture absorption, and the like.
[0032] In addition, the aromatic polyester resin of the above-mentioned preferred embodiment can have any structure as long as it has the monomer component A and the monomer component B as essential units. For example, it may have two or more kinds of the monomer component A, or it may have three or more kinds of the monomer component A. In addition, the aromatic polyester resin of the above-mentioned preferred embodiment may contain another monomer component (hereinafter, may be simply referred to as "monomer component C") other than the monomer component A and the monomer component B. That is, the aromatic polyester resin of the above-mentioned preferred embodiment may be a two-component or more polycondensate consisting of only the monomer component A and the monomer component B, or a three-component or more polycondensate consisting of the monomer component A, the monomer component B, and the monomer component C. Examples of the other monomer components include those other than the above-mentioned monomer component A and the monomer component B, specifically, aromatic or aliphatic dihydroxy compounds and derivatives thereof; aromatic or aliphatic dicarboxylic acids and derivatives thereof; aromatic hydroxycarboxylic acids and derivatives thereof; aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids and derivatives thereof; and the like, but are not particularly limited thereto. Specific examples of the monomer component C include, but are not limited to, terephthalic acid, isophthalic acid, 6-naphthalenedicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate, etc. The other monomer components may be used alone or in any combination and ratio of two or more.
[0033] In this specification, the term "derivative" refers to a monomer component having a modification group such as a halogen atom (e.g., fluorine atom, chlorine atom, bromine atom, iodine atom), an alkyl group having 1 to 5 carbon atoms (e.g., methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, s-butyl group, t-butyl group, etc.), an aryl group such as a phenyl group, a hydroxyl group, an alkoxy group having 1 to 5 carbon atoms (e.g., methoxy group, ethoxy group, etc.), a carbonyl group, -O-, -S-, -CH2-, etc., introduced therein (hereinafter, this may be referred to as a "monomer component having a substituent"). Here, the "derivative" may be an ester-forming monomer such as an acylation product, an ester derivative, or an acid halide of the monomer components A and B which may have the above-mentioned modification group.
[0034] Particularly preferred embodiments include binary polycondensates of parahydroxybenzoic acid and its derivatives with 6-hydroxy-2-naphthoic acid and its derivatives; ternary or higher polycondensates of parahydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, and monomer component C; and polycondensates of parahydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, and terephthalic acid, isophthalic acid, 6-naphthalenedicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol. and ternary or higher polycondensates consisting of parahydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, terephthalic acid, isophthalic acid, 6-naphthalenedicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate, and their derivatives, and one or more monomer components C. These can be obtained as having a relatively low melting temperature compared to, for example, homopolymers of parahydroxybenzoic acid, and therefore, thermoplastic liquid crystal polymers using these have excellent moldability during thermocompression bonding to an adherend.
[0035] The melting temperature of the thermoplastic aromatic liquid crystal polyester contained in the skin layers 11 and 12 is not particularly limited, but from the viewpoint of ensuring good dispersibility with the thermoplastic polyolefin, it is preferably 220°C or higher, more preferably 240°C or higher, and even more preferably 260°C or higher, and the upper limit is preferably 350°C or lower, more preferably 330°C or lower.
[0036] The content ratio of the thermoplastic aromatic liquid crystal polyester described above is appropriately set according to the required performance and is not particularly limited, but from the viewpoint of controlling the orientation of the thermoplastic aromatic liquid crystal polyester and ensuring good acoustic properties, it is preferably 10 to 40 mass% in total, more preferably 10 to 35 mass% in total, and even more preferably 10 to 30 mass% in total based on the total amount of resin solids contained in the skin layers 11 and 12. The type and content ratio of the thermoplastic aromatic liquid crystal polyester contained in the skin layers 11 and 12 may be the same or different.
[0037] The skin layers 11 and 12 may further contain an inorganic filler in addition to the above-mentioned thermoplastic polyolefin and thermoplastic aromatic liquid crystal polyester. By containing an inorganic filler, a higher storage modulus E' can be achieved, which is particularly useful for improving acoustic properties, for example.
[0038] The inorganic filler used here may be any known filler in the art, and the type is not particularly limited. For example, kaolin, calcined kaolin, calcined clay, uncalcined clay, silica (e.g., natural silica, fused silica, amorphous silica, hollow silica, wet silica, synthetic silica, aerosil, etc.), aluminum compounds (e.g., boehmite, aluminum hydroxide, alumina, hydrotalcite, aluminum borate, aluminum nitride, etc.), magnesium compounds (e.g., magnesium aluminometasilicate, magnesium carbonate, magnesium oxide, magnesium hydroxide, etc.), calcium compounds (e.g., calcium carbonate, Examples of the stannate include, but are not limited to, calcium hydroxide, calcium sulfate, calcium sulfite, calcium borate, etc.), molybdenum compounds (e.g., molybdenum oxide, zinc molybdate, etc.), talc (e.g., natural talc, calcined talc, etc.), mica, titanium oxide, zinc oxide, zirconium oxide, barium sulfate, zinc borate, barium metaborate, sodium borate, boron nitride, aggregated boron nitride, silicon nitride, carbon nitride, strontium titanate, barium titanate, and zinc stannate. These can be used alone or in combination of two or more. Among these, talc and silica are preferred from the viewpoints of strength, acoustic properties, etc.
[0039] The inorganic filler used here may be surface-treated as known in the art. The surface treatment can improve moisture resistance, adhesive strength, dispersibility, etc. Examples of surface treatment agents include, but are not limited to, silane coupling agents, titanate coupling agents, sulfonic acid esters, carboxylic acid esters, and phosphoric acid esters.
[0040] The median diameter (d50) of the inorganic filler can be appropriately set according to the required performance and is not particularly limited. From the viewpoints of kneadability and handleability during preparation, and the effect of improving strength and acoustic properties, the d50 of the inorganic filler is preferably 0.01 μm or more and 50 μm or less, more preferably 0.03 μm or more and 50 μm or less, and even more preferably 0.1 μm or more and 50 μm or less.
[0041] The content of the inorganic filler is not particularly limited and can be appropriately set according to the required performance, taking into consideration the blending balance with other essential components and optional components. From the viewpoints of kneading and handling during preparation, the effect of reducing the linear expansion coefficient, etc., the content of the inorganic filler is preferably 0.5% by mass or more and 40% by mass or less in total, more preferably 1% by mass or more and 30% by mass or less in total, and even more preferably 3% by mass or more and 20% by mass or less in total, in terms of solid content relative to the total amount of the skin layers 11 and 12. The types and content ratios of the inorganic fillers that can be contained in the skin layers 11 and 12 may be the same or different.
[0042] The skin layers 11 and 12 may contain, within a range that does not excessively impair the effects of the present invention, resin components other than the above-mentioned thermoplastic polyolefin and thermoplastic aromatic liquid crystal polyester, such as thermosetting resins and thermoplastic resins, for example, acetate polymers, poly(meth)acrylic polymers, polyester polymers, polyethersulfone polymers, polysulfone polymers, polycarbonate polymers, polyamide polymers, polyimide polymers, polyolefin polymers, polyarylate polymers, polystyrene polymers, polyvinyl alcohol polymers, etc. Furthermore, the skin layers 11 and 12 may contain, within a range that does not excessively impair the effects of the present invention, additives known in the art, such as release improvers such as higher fatty acids having 10 to 25 carbon atoms, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, and fluororesins; colorants such as dyes and pigments; organic fillers; antioxidants; heat stabilizers; light stabilizers; ultraviolet absorbers; flame retardants; antistatic agents; surfactants; rust inhibitors; antifoaming agents; fluorescent agents, etc. These resin components and additives can be used alone or in combination of two or more. These additives can be included in the molten resin composition prepared during the film formation of the skin layers 11 and 12. The content of these resin components and additives is not particularly limited, but from the viewpoints of moldability, thermal stability, etc., it is preferably 0.01 to 10 mass % each, more preferably 0.1 to 7 mass %, and even more preferably 0.5 to 5 mass % each, based on the total amount of the skin layers 11 and 12.
[0043] The thickness of the skin layers 11 and 12 can be appropriately set according to requirements and is not particularly limited. In consideration of handling and productivity, the thickness is preferably 1 μm to 40 μm, more preferably 3 μm to 30 μm, and further preferably 5 μm to 30 μm.
[0044] The melting temperature of the skin layers 11, 12 can be set appropriately according to requirements and is not particularly limited, but from the viewpoint of the heat resistance and processability of the film, it is preferably 180 to 300°C, more preferably 200 to 290°C, and even more preferably 220 to 280°C.
[0045] The method for forming the skin layers 11, 12 is not particularly limited, but a melt extrusion method is preferably used. In one preferred embodiment, a first resin composition containing the above-mentioned components is extruded from a T-die into a film by a melt extrusion film forming method using a T-die (hereinafter, sometimes simply referred to as "T-die melt extrusion") to form a film, and then, if necessary, the T-die melt extruded film is pressurized and heated to obtain the desired skin layers 11, 12. In addition, during this melt extrusion, the skin layers 11, 12 can also be co-extruded together with the core layer 21.
[0046] The acoustic properties of the single layer of the skin layers 11 and 12 can be appropriately set according to the required performance. 8 It is preferable that the skin layers 11, 12 have a storage modulus E' (25°C, frequency 1 Hz) of 5.0 x 10 Pa or more and an internal loss Tan δ (25°C, frequency 1 Hz) of 0.03 or more. By using such skin layers 11, 12 in combination with the core layer 21, it becomes easy to achieve a balance between transmission speed, internal loss, and strength that could not be achieved by conventional techniques. The storage modulus E' (25°C, frequency 1 Hz) of a single layer of the skin layers 11, 12 is more preferably 5.0 x 10 8 Pa or more, more preferably 8.0×10 8 The upper limit is not particularly limited, but is preferably 1.0×10 10The internal loss Tan δ (at 25° C. and 1 Hz frequency) of a single layer of skin layers 11 and 12 is more preferably 0.04 or more, and although there is no particular upper limit, a value of 0.80 or less is used as a guideline.
[0047] In this specification, the storage modulus E' (25°C, frequency 1 Hz) and the internal loss Tan δ (25°C, frequency 1 Hz) refer to values measured at 25°C and a frequency of 1 Hz using a dynamic viscoelasticity device RSA-G2 (manufactured by TA Instruments). Other details are in accordance with the measurement conditions described in the examples below.
[0048] The core layer 21 is a layer formed by molding a thermoplastic resin component into a film shape, and supports the above-mentioned skin layers 11 and 12. By providing the core layer 21, excellent strength and internal loss are imparted to the speaker diaphragm laminate film 100. As the core layer 21, a melt-extruded film such as a T-die melt-extruded film is preferably used.
[0049] The core layer 21 contains one or more types selected from the group consisting of thermoplastic elastomers and thermoplastic polyolefins having a melting temperature of 230° C. or higher. By providing the core layer 21, which is relatively flexible, in combination with the above-mentioned skin layers 11 and 12, it is possible to achieve a balance between transmission speed, internal loss, and strength, which could not be achieved with conventional techniques.
[0050] The type of thermoplastic elastomer contained in the core layer 21 is not particularly limited, and can be appropriately selected from known ones. Specific examples of such thermoplastic elastomers include polyolefin-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, etc., but are not particularly limited thereto. The thermoplastic elastomers can be used alone or in any combination and ratio of two or more kinds. Among these, polyester-based thermoplastic elastomers and polyurethane-based thermoplastic elastomers are preferred, and polyester-based thermoplastic elastomers are more preferred, from the viewpoint of obtaining excellent acoustic characteristics due to high internal loss.
[0051] Specific examples of polyolefin-based thermoplastic elastomers include the Milastomer series (registered trademark) manufactured by Mitsui Chemicals, Inc. and the Trexplain series (registered trademark) manufactured by Mitsubishi Chemical Corporation. Specific examples of polyester-based thermoplastic elastomers include the Hytrel series (registered trademark) manufactured by DuPont-Toray Co., Ltd. and the Tefablock series (registered trademark) manufactured by Mitsubishi Chemical Corporation. Specific examples of polyurethane-based thermoplastic elastomers include the Rezamin series (registered trademark) manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd. and the Miractoran series (registered trademark) manufactured by Tosoh Corporation.
[0052] The melting temperature of the thermoplastic elastomer contained in the core layer 21 is not particularly limited, but from the viewpoint of interlayer adhesion during lamination by coextrusion, it is preferably 150°C or higher, more preferably 170°C or higher, and even more preferably 190°C or higher, and the upper limit is preferably 250°C or lower, more preferably 230°C or lower.
[0053] Specific examples and preferred examples of the thermoplastic polyolefin having a melting temperature of 230°C or higher contained in the core layer 21 are the same as those described for the thermoplastic polyolefin having a melting temperature of 230°C or higher contained in the skin layers 11 and 12 described above, and duplicate explanations will be omitted here.
[0054] The core layer 21 may further contain an inorganic filler in addition to the above-mentioned thermoplastic elastomer or thermoplastic polyolefin. By containing an inorganic filler, it is possible to improve the internal loss, which is particularly useful for improving the vibration damping of a speaker diaphragm, for example. Specific examples and suitable examples of the inorganic filler used here are the same as those described for the inorganic filler that may be contained in the above-mentioned skin layers 11 and 12, and therefore repeated description here will be omitted.
[0055] The core layer 21 may further contain resin components other than the above-mentioned thermoplastic elastomers and thermoplastic polyolefins, and additives known in the art, within the scope of not excessively impairing the effects of the present invention. Specific examples and preferred examples of the resin components and additives used here are the same as those explained for the resin components and additives that may be included in the above-mentioned skin layers 11 and 12, and therefore repeated explanations will be omitted here.
[0056] The thickness of the core layer 21 can be appropriately set according to requirements and is not particularly limited. In consideration of handleability, productivity, etc., the thickness is preferably 3 μm to 70 μm, more preferably 5 μm to 60 μm, and further preferably 7 μm to 50 μm.
[0057] The melting temperature of the core layer 21 can be set appropriately according to requirements and is not particularly limited, but from the viewpoint of the heat resistance and processability of the film, it is preferably 150 to 250°C, more preferably 170 to 230°C, and even more preferably 190 to 220°C.
[0058] The method for forming the core layer 21 is not particularly limited, but a melt extrusion method is preferably used. One preferred embodiment is a method in which the second resin composition containing the above-mentioned components is extruded from a T-die into a film shape by a melt extrusion film forming method using a T-die (hereinafter, sometimes simply referred to as "T-die melt extrusion") to form a film, and then the T-die melt extruded film is pressurized and heated as necessary to obtain a predetermined core layer 21. In addition, during this melt extrusion, the core layer 21 can also be co-extruded together with the above-mentioned skin layers 11 and 12.
[0059] The laminated film 100 for speaker diaphragms is formed by laminating the above-mentioned skin layers 11, 12 and the core layer 21. The lamination method is not particularly limited, and any method known in the art can be applied. For example, the laminated film 100 for speaker diaphragms can be obtained by preparing the skin layers 11, 12 and the core layer 21 which are individually melt-extruded, disposing a primer layer, an adhesive layer, a resin layer, etc. between the skin layers 11, 12 and the core layer 21 as necessary, and dry laminating the skin layers 11, 12 and the core layer 21.
[0060] A preferred embodiment of the method for producing the laminated film 100 for speaker diaphragms includes a method in which a first resin composition for the skin layers 11 and 12, which contains the above-mentioned thermoplastic polyolefin, thermoplastic aromatic liquid crystal polyester, and resin components and additives blended as necessary, and a second resin composition for the core layer 21, which contains the above-mentioned thermoplastic elastomer and / or thermoplastic polyolefin, and resin components and additives blended as necessary, are prepared in advance, and these resin compositions are separately supplied from a melt extruder to melt-extrude the laminated films of the skin layers 11 and 12 and the core layer 21 to obtain the laminated film 100 for speaker diaphragms. Such melt-extrusion molding is superior to dry lamination in terms of handleability and handling during production, and can reduce thickness unevenness (thickness dimensional accuracy) of the resulting laminated film, thereby realizing a laminated film 100 for speaker diaphragms that is high quality, highly productive, and economical.
[0061] At this time, the preparation of each resin composition may be performed according to a conventional method, and is not particularly limited. Each of the above-mentioned components may be manufactured and processed by a known method, such as kneading, melt kneading, granulation, extrusion molding, pressing, or injection molding. When melt kneading, a kneading device such as a commonly used single-screw or twin-screw extruder or various kneaders may be used. When supplying each component to these melt kneading devices, each component may be dry-blended in advance using a mixing device such as a tumbler or Henschel mixer. When melt kneading, the cylinder setting temperature of the kneading device may be appropriately set, and is not particularly limited, but is preferably in the range of the melting temperature of the thermoplastic resin component to 360°C or less, and more preferably the melting temperature of the thermoplastic resin component +10°C to 360°C.
[0062] The conditions for melt co-extrusion may be appropriately set according to the type and composition of the resin composition used, the desired performance of the intended melt co-extruded film, etc., and are not particularly limited. In general, the set temperature of the cylinder of the extruder is preferably 230 to 360°C, more preferably 280 to 350°C. Similarly, the slit gap of the T-die may be appropriately set according to the type and composition of the resin composition used, the desired performance of the intended melt co-extruded film, etc., and is not particularly limited. In general, it is preferably 0.1 to 1.5 mm, more preferably 0.2 to 0.8 mm.
[0063] The obtained melt coextrusion film can be used as it is as a laminated film 100 for speaker diaphragms, but may be subjected to post-heat treatment (annealing) as necessary to reduce the film orientation degree. The post-heat treatment may be performed using a method known in the art, such as contact heat treatment or non-contact heat treatment, and the type is not particularly limited. For example, heat setting can be performed using known equipment such as a non-contact heater, oven, blower, heat roll, cooling roll, heat press, double belt heat press, etc. At this time, a release film or a porous film known in the art can be arranged on the surface of the melt coextrusion film as necessary, and heat and pressure treatment can be performed.
[0064] The treatment temperature of the post-heat treatment is preferably higher than the melting temperature of the thermoplastic resin component and lower than 70°C higher than the melting temperature, more preferably higher than +5°C higher than the melting temperature and lower than 60°C higher than the melting temperature, and even more preferably higher than +10°C higher than the melting temperature and lower than 50°C higher than the melting temperature. The thermocompression bonding conditions can be appropriately set according to the desired performance and are not particularly limited, but are preferably performed under conditions of a surface pressure of 0.5 to 10 MPa and a heating and pressing time of 250 to 430°C, more preferably under conditions of a surface pressure of 0.6 to 8 MPa and a heating and pressing time of 260 to 400°C, and even more preferably under conditions of a surface pressure of 0.7 to 6 MPa and a heating and pressing time of 270 to 370°C. On the other hand, when a non-contact heater or oven is used, it is preferable to perform the bonding under conditions of, for example, 200 to 320°C for 1 to 20 hours.
[0065] The total thickness of the laminated film 100 for speaker diaphragm can be appropriately set according to the required performance and is not particularly limited. From the viewpoints of lamination property, processability, acoustic properties, mechanical strength, etc., it is preferably 5 to 200 μm, more preferably 7 to 150 μm, and further preferably 10 to 100 μm.
[0066] The ratio of the total thickness of the skin layers 11, 12 to the total thickness of the laminated film 100 for speaker diaphragms can be set appropriately depending on the required performance and is not particularly limited. From the standpoints of lamination, processability, acoustic properties, mechanical strength, etc., the ratio is preferably 15% or more and 80% or less, and more preferably 20% or more and 70% or less.
[0067] The storage modulus E' (25°C, frequency 1 Hz) of the laminated film for speaker diaphragms 100 can be appropriately set according to the required performance and is not particularly limited. From the viewpoint of realizing a wide reproduction band, for example, it is set to 7.0 × 10 8 Pa or more, more preferably 7.0×10 8 Pa or more, more preferably 9.0×10 8 The upper limit is not particularly limited, but is preferably 9.0×10 Pa or more. 10 Pa or less is considered a guideline.
[0068] The internal loss Tan δ (at 25° C. and a frequency of 1 Hz) of the laminated film 100 for a speaker diaphragm can be appropriately set depending on the required performance and is not particularly limited. From the viewpoint of improving the flatness of the sound pressure, for example, the internal loss Tan δ is preferably 0.04 or more, more preferably 0.05 or more, and even more preferably 0.06 or more. The upper limit of the internal loss Tan δ is not particularly limited, but is approximately 1.0 or less.
[0069] The tensile breaking elongation of the laminated film 100 for speaker diaphragms at 150°C can be appropriately set according to the required performance, and is not particularly limited, but is preferably 200% or more, more preferably 240% or more, and the upper limit is not particularly limited, but is approximately 1200% or less. In this specification, the tensile breaking elongation is measured in accordance with JIS K7127 (Type 2) using a tensile tester Strograph VE1D (manufactured by Toyo Seiki Seisakusho Co., Ltd.) at 150°C in the longitudinal direction (MD direction: Machine Direction) and the transverse direction (TD direction: Transverse Direction) of the film, and the smaller value of the measured tensile breaking elongation in the longitudinal direction and the transverse direction is used. Other details are in accordance with the measurement conditions described in the examples described later.
[0070] By adopting the above-mentioned configuration, the laminated film 100 for a speaker diaphragm of this embodiment has both a high storage modulus E' and an internal loss Tan δ, and is excellent not only in acoustic characteristics but also in productivity and economy. In a particularly preferred embodiment, it has an acoustic characteristic that could not be realized by the conventional technology, that is, 8.0×10 8 It is possible to realize a storage modulus E' (25°C, frequency 1 Hz) of 0.001 Pa or more and an internal loss Tan δ (25°C, frequency 1 Hz) of 0.05 or more, thereby realizing a speaker with a wide playback frequency range and excellent sound pressure flatness. EXAMPLES
[0071] The features of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. That is, the materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. In addition, the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limits in the embodiment of the present invention, and the preferred numerical range may be a range defined by a combination of the above-mentioned upper or lower limit and the values of the following examples or the values of the examples.
[0072] The materials used in the examples and comparative examples are as follows. (Resin A) (A-1) Thermoplastic cycloolefin polymer resin, "ZEONEX (registered trademark) C2420" manufactured by Zeon Corporation, melting temperature: 263°C (A-2) Thermoplastic polypropylene resin, "SunAllomer (registered trademark) PM600M" manufactured by SunAllomer Co., Ltd., melting temperature: 163°C (Resin B) (B-1) Thermoplastic liquid crystal polymer resin, Ueno Pharmaceutical Co., Ltd. "UENO LCP (registered trademark) A-5000", melting temperature: 280°C (B-2) Polybutylene terephthalate resin, "NOVADURAN (registered trademark) 5010R8" manufactured by Mitsubishi Engineering Plastics Corporation, melting temperature: 222°C (Resin C) (C-1) Polyester elastomer resin, Toray DuPont "Hytrel (registered trademark) 7277", melting temperature: 219℃
[0073] The storage modulus E' (tensile viscoelasticity) and the internal loss Tan δ were measured under the following conditions. Apparatus: Dynamic viscoelasticity apparatus RSA-G2 (manufactured by TA Instruments) Measurement conditions: Tensile mode Vibration frequency: 1Hz Measurement temperature: A constant temperature of 25°C. Measurement direction: Longitudinal direction of film (film transport direction) Evaluation items: Storage modulus E' and internal loss Tan δ at 25℃ and 1Hz
[0074] The tensile elongation at break was measured under the following conditions. Equipment: Tensile testing machine Strograph VE1D (manufactured by Toyo Seiki Seisakusho) Sample size: 150mm x 10mm (JIS K7127: Type 2) Nominal distortion: 50mm Chuck distance: 50mm Tensile speed: 50 mm Measurement environment: 23℃×50%RH Measurement direction: Machine direction (MD) and transverse direction (TD) of the film Evaluation item: Tensile elongation at break at 150℃ in MD and TD directions
[0075] [Examples 1 to 6] Resin A and resin B, which had been dried at 80°C for 8 hours or more, were dry blended in the composition and compounding ratios shown in Table 1, the resulting blend was melt-kneaded in a co-rotating, vented twin-screw kneading extruder heated to 300°C, and the resulting strands were cut with a pelletizer to prepare a first resin composition (blend chips) for the front and back skin layers, each containing a predetermined ratio of resin A and resin B. In addition, pellets of resin C were used as they were as the second resin composition for the core layer.
[0076] Next, the first resin composition for the front skin layer, the second resin composition for the core layer, and the first resin composition for the back skin layer were dried at 80°C for more than 8 hours using a hopper dryer or the like, and then each was charged into three independent hoppers heated to 300°C equipped on an extruder, melt-kneaded, co-extruded into a film from the T-die polymer at the tip of the extruder, and cooled to obtain laminate films for speaker diaphragms of Examples 1 to 6 having a laminate structure of front skin layer / core layer / back skin layer and a total thickness of 50 μm.
[0077] [Comparative Examples 1 to 3] Except for changing the compounding ratio of resin A and resin B as shown in Table 1, the same procedure as in Example 1 was performed to obtain laminated films for speaker diaphragms of Comparative Examples 1 to 3 having a laminated structure of a front skin layer / core layer / back skin layer and a total thickness of 50 μm.
[0078] [Comparative Example 4] Without using the second resin composition for the core layer, the first resin composition for the front skin layer and the first resin composition for the back skin layer were each fed into two independent hoppers heated to 300°C equipped on an extruder, melt-kneaded, co-extruded into a film from the T-die polymer at the tip of the extruder, and cooled to obtain a laminated film for speaker diaphragms of Comparison Example 4 having a front skin layer / back skin layer laminate structure and a total thickness of 50 μm.
[0079] [Comparative Example 5] The same procedure was followed as in Example 1, except for using Resin A-2 instead of Resin A-1, to obtain a laminated film for speaker diaphragms of Comparative Example 5 having a laminated structure of a front skin layer / core layer / back skin layer and a total thickness of 50 μm.
[0080] [Comparative Example 6] The same procedure was followed as in Example 1, except for using resin B-2 instead of resin B-1, to obtain a laminated film for speaker diaphragms of Comparative Example 6 having a laminated structure of a front skin layer / core layer / back skin layer and a total thickness of 50 μm.
[0081] The performance of each laminated film for speaker diaphragms was evaluated, and the results are shown in Table 1. [Table 1] [Industrial Applicability]
[0082] The laminated film for speaker diaphragms of the present invention has both a high storage modulus E' and a high internal loss Tan δ, and can realize acoustic properties that could not be realized by conventional techniques. Therefore, the laminated film for speaker diaphragms of the present invention can be widely and effectively used in speaker diaphragm applications that require high sound quality. [Explanation of symbols]
[0083] 11. Skin layer 12 Skin layer 21 Core layer 21a...plane 21b...plane 100 ···Laminated film for speaker diaphragms
Claims
1. One or more skin layers containing at least 60 to 90% by mass of a thermoplastic polyolefin having a melting temperature of 230° C. or higher and 10 to 40% by mass of a thermoplastic aromatic liquid crystal polyester based on the total amount of resin solids; and a core layer containing one or more selected from the group consisting of a thermoplastic elastomer and a thermoplastic polyolefin having a melting temperature of 230° C. or higher; The skin layer has a laminate structure in which one or more of the skin layers are supported on the core layer. Laminated film for speaker diaphragms.
2. 7.0 x 10 8 Has a storage modulus E' (25°C, frequency 1 Hz) of 1 Pa or more The laminated film for a speaker diaphragm according to claim 1 .
3. Has an internal loss Tan δ of 0.04 or more (at 25°C and 1 Hz) The laminated film for a speaker diaphragm according to claim 1 or 2.
4. The thermoplastic polyolefin of the skin layer comprises at least one selected from the group consisting of polypropylene-based polymers, cyclic olefin polymers, and cyclic olefin copolymers. The laminated film for a speaker diaphragm according to any one of claims 1 to 3.
5. The thermoplastic aromatic liquid crystal polyester of the skin layer comprises a thermoplastic wholly aromatic liquid crystal polyester. The laminated film for a speaker diaphragm according to any one of claims 1 to 4.
6. The thermoplastic elastomer of the core layer includes at least one selected from the group consisting of a polyolefin-based thermoplastic elastomer, a polyester-based thermoplastic elastomer, and a polyurethane-based thermoplastic elastomer. The laminated film for a speaker diaphragm according to any one of claims 1 to 5.
7. The skin layer has a total thickness of 15% to 80% of the total thickness of the laminate film. The laminated film for a speaker diaphragm according to any one of claims 1 to 6.
8. 9.0 x 10 8 Has a storage modulus E' of 1 Pa or more (25°C, frequency 1 Hz) The laminated film for a speaker diaphragm according to any one of claims 1 to 7.
9. Has an internal loss Tan δ of 0.06 or more (at 25°C and 1 Hz) The laminated film for a speaker diaphragm according to any one of claims 1 to 8.
10. Tensile elongation at break at 150°C is 200% or more The laminated film for a speaker diaphragm according to any one of claims 1 to 9.
11. The skin layer is 2.0×10 8 Storage modulus E' (25°C, frequency 1Hz) and has an internal loss Tan δ (at 25° C. and a frequency of 1 Hz) of 0.03 or more. The laminated film for a speaker diaphragm according to any one of claims 1 to 10.
12. A first resin composition containing at least 60 to 90% by mass of a thermoplastic polyolefin having a melting temperature of 230° C. or higher and 10 to 40% by mass of a thermoplastic aromatic liquid crystal polyester based on the total amount of resin solids, and a second resin composition containing one or more selected from the group consisting of a thermoplastic elastomer and a thermoplastic polyolefin having a melting temperature of 230° C. or higher, are melt-extruded. A manufacturing method for laminated film for speaker diaphragms.
Citation Information
Patent Citations
Multilayer diaphragm for speaker
JP1991102999A
Multilayer speaker diaphragm
JP1991107300A
Diaphragm for speaker and its manufacturing method
JP2005101889A
Method for manufacturing vibration plate of speaker
JP2018064150A
Method for producing diaphragm film
JP2018183914A