Biaxially oriented polyester film and its manufacturing method

A method using electrostatic adhesion and biaxial stretching with metal ion-containing resin mixtures addresses the quality issues in recycled polyester films, resulting in films with lower crystallization and improved properties.

JP7555315B2Active Publication Date: 2024-09-24NANYA PLASTICS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021135788
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-12
Filing Date
2021-08-23
Publication Date
2024-09-24
Estimated Expiration
2041-08-23

AI Technical Summary

Technical Problem

Existing biaxially oriented polyester films made from recycled materials face challenges in achieving good quality due to high crystallization rates and impurities, which affect processing conditions and film properties.

Method used

A method involving the use of a polyester resin mixture containing electrostatic adhesives with metal ions and a lubricant, applied through a casting process with controlled electrostatic adhesion and biaxial stretching, to produce a biaxially oriented polyester film with reduced crystallization and improved quality.

Benefits of technology

The method enables the production of high-quality biaxially oriented polyester films from recycled materials with lower crystallization rates, improved film uniformity, and reduced film breakage, while maintaining effective electrostatic adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555315000002
    Figure 0007555315000002
  • Figure 0007555315000003
    Figure 0007555315000003
  • Figure 0007555315000004
    Figure 0007555315000004
Patent Text Reader

Abstract

To provide a biaxially oriented polyester film having a following physical property.SOLUTION: An observed recrystallization temperature is 175°C to 200°C when cooled in a melted state at a cooling rate of 20°C / min. A biaxially oriented polyester film is formed from thick film that are melted and extruded by an extruder prior to bi-directional stretching and then cooled on a casting roll. A thick sheet before drawing has a following physical property when analyzed by differential scanning calorimetry; crystallization percentage is less than 10%.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polyester film and a method for producing the same, and more particularly to a biaxially oriented polyester film and a method for producing the same. [Background technology]

[0002] Biaxially oriented polyester films are often used in magnetic tapes, insulating tapes, photographic films, tracing films, packaging films, electrical insulating films, engineering papers, etc. Due to the increasing awareness of environmental protection, waste polyester materials are often remanufactured into polyester films. However, there is an urgent need to find a solution to the technical problem of how to achieve good quality in the remanufactured polyester films. Summary of the Invention [Problem to be solved by the invention]

[0003] Therefore, the present invention aims to provide a biaxially oriented polyester film and a manufacturing method thereof, which may be formed from recycled polyester materials and / or have better quality. [Means for solving the problem]

[0004] In one embodiment, the invention is a biaxially oriented polyester film having the following physical characteristics: an observed recrystallization temperature (Tc(A)) of 175°C to 200°C when cooled in the molten state at a cooling rate of 20°C / min, the biaxially oriented polyester film being formed from a thick sheet that is melted and extruded by an extruder and then cooled on a casting roll prior to bidirectional stretching, the thick sheet having the following physical characteristics when analyzed by differential scanning calorimetry: a percent crystallization of less than 10% prior to stretching.

[0005] According to one embodiment of the present invention, a biaxially oriented polyester film is formed from at least a polyester resin mixture, the polyester resin mixture including an electrostatic adhesion agent having metal ions and a polyester material, the weight concentration of the metal ions in the polyester resin mixture being 40 ppm to 50 ppm.

[0006] According to one embodiment of the present invention, the biaxially oriented polyester film is produced by at least an electrostatic bonding method, which includes the steps of providing a casting roll and an electrostatic bonding device configured to correspond to the casting roll, forming a molten polyester resin mixture on the casting roll, and applying an electrostatic voltage between the casting roll and the electrostatic bonding device.

[0007] According to one embodiment of the present invention, the metal ions are alkali metal ions, alkaline earth metal ions, or a combination thereof.

[0008] According to one embodiment of the present invention, the polyester material is comprised of at least recycled polyester material.

[0009] According to one embodiment of the present invention, the weight ratio of recycled polyester material to said polyester resin mixture is greater than 80% and not more than 100%.

[0010] According to one embodiment of the present invention, the polyester resin mixture further comprises a lubricant, the weight concentration of the lubricant in the polyester resin mixture being 500 ppm to 3000 ppm.

[0011] In one embodiment, the present invention provides a method for making a biaxially oriented polyester film, the method including the steps of providing a casting roll and an electrostatic bonding device configured to correspond to the casting roll, providing an electrostatic voltage between the casting roll and the electrostatic bonding device to extrude a molten polyester resin mixture onto the casting roll to form a thick sheet, and biaxially stretching the thick film to form a biaxially oriented polyester film.

[0012] In one embodiment, the present invention provides a method for making a biaxially oriented polyester film, the method comprising the steps of forming a molten polyester resin mixture on a casting roll to form a thick sheet, the thick sheet prior to stretching having the following physical properties as analyzed by differential scanning calorimetry: percent crystallization less than 10%, and biaxially stretching the thick film to form a biaxially oriented polyester film, the biaxially oriented polyester film having an observed recrystallization temperature of 175° C. to 200° C. when cooled in the molten state at a cooling rate of 20° C. / min.

[0013] The method of making a biaxially oriented polyester film of the present disclosure includes extruding a molten polyester resin mixture onto a casting roll to form a thick sheet, and biaxially stretching the thick film to form the biaxially oriented polyester film, the polyester resin mixture including an electrostatic adhesion agent having metal ions and a polyester material, the weight concentration of the metal ions in the polyester resin mixture being 40 ppm to 50 ppm. Effect of the Invention

[0014] In view of the above, the biaxially oriented polyester film of the present invention can be made from recycled polyester materials, and the biaxially oriented polyester film of the present invention can have better quality. [Brief description of the drawings]

[0015] The accompanying drawings are included to provide a further understanding of the disclosure, and are incorporated in and constitute a part of this specification. The drawings illustrate embodiments of the disclosure and, together with the detailed description, serve to explain the principles of the disclosure.

[0016] [Figure 1] 1 is a schematic partial flowchart of a method for producing a biaxially oriented polyester film according to an embodiment of the present disclosure.

[0017] [Diagram 2] FIG. 1 is a partial perspective view of an apparatus for producing a biaxially oriented polyester film according to an embodiment of the present disclosure.

[0018] [Diagram 3] FIG. 1 is a partial schematic side view of an apparatus for producing a biaxially oriented polyester film according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Reference will now be made in detail to illustrative embodiments of the present disclosure, examples of which are illustrated in the accompanying drawings, and wherever possible, the same reference numbers are used in the drawings and the detailed description to refer to the same or like parts.

[0020] In the following detailed description, for purposes of illustration and not limitation, example embodiments that reveal specific details are provided to enable a thorough understanding of the various principles of the present disclosure. However, it will be apparent to those skilled in the art that other embodiments may be practiced that depart from the specific details disclosed herein. Also, detailed descriptions of well-known devices, methods and materials may be omitted in order to clarify the explanation of the various principles of the present disclosure.

[0021] As used herein, ranges may be expressed as from "about" a particular value to "about" another particular value, but may also be directly stated as the particular value and / or to the other particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when values ​​are expressed as approximations, by use of the antecedent "about," the particular value forms another embodiment. Moreover, the endpoints of each range are expressly related to, or independent of, the other endpoint.

[0022] As used herein, non-limiting terms (eg, may, can, for example, or other similar terms) are non-required or optional embodiments, inclusions, additions, or presences.

[0023] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by those skilled in the art. Furthermore, terms (e.g., defined in a common dictionary) are to be interpreted as having a meaning consistent with the meaning in the relevant technical context, and are not to be interpreted as idealized or overly formal unless specifically defined.

[0024] [Recycled polyester material]

[0025] The method for recycling polyester materials may, for example, include collecting various kinds of waste polyester materials, and corresponding classification may be performed according to the type, color, and / or intended use of the waste polyester materials. The classified waste polyester materials may then be compressed and packaged. The packaged waste polyester materials may then be transported to a waste disposal site. The waste polyester materials may, for example, include recycled polyester bottles, but the present disclosure is not limited thereto.

[0026] The method for recycling polyester material may further include removing objects (e.g., bottle caps, labels, and / or adhesives, etc.) on the waste polyester material. Then, physically and mechanically crushing the waste polyester material. Then, using a suitable method (e.g., flotation) to separate the crushed polyester material. Then, the crushed and separated waste polyester material may be dried to obtain a treated recycled polyester material.

[0027] In certain embodiments, the recycled polyester material may further include, for example, processed recycled polyester material purchased directly.

[0028] In one embodiment, the recycled polyester material may also be further recycled by the below described method of forming a biaxially oriented polyester film.

[0029] The recycled polyester material obtained by the above method may be further formed into recycled polyester chips for subsequent film manufacturing processing in the following manner.

[0030] The terms "polyester," "polyester material," and the like, in this disclosure refer to any type of polyester, particularly aromatic polyesters, and more specifically, polyesters derived from purified terephthalic acid (PTA) and ethylene glycol (EG) (i.e., ethylene terephthalate (PET)).

[0031] The polyester in this specification may further be, for example, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, or a combination thereof. In this embodiment, the polyester is preferably polytrimethylene terephthalate, polypropylene terephthalate, or a combination thereof. Furthermore, a copolymer may be used, and the copolymer may be, in particular, a copolymer obtained by using two or more dicarboxylic acids and / or two or more diol components.

[0032] [Method of manufacturing chemically recycled polyester chips] (may contain electrostatic adhesion agents and / or lubricants)

[0033] Step 1-1: Chemical depolymerization of recycled polyester material, refer to Figure 1. For example, recycled polyester material and depolymerization solution may be placed in a depolymerization tank 110 for chemical depolymerization.

[0034] Generally, the chemical depolymerization solution can cut the polyester molecules in the recycled polyester material, thereby achieving the effect of depolymerization. Also, a polyester composition with short molecular chains and / or an ester monomer consisting of one dibasic acid and two diols (e.g., bis(2-hydroxyethyl) terephthalate, BHET) can be obtained. That is, the average molecular weight of the mixture after chemical depolymerization is generally smaller than the average molecular weight of the recycled polyester material.

[0035] Furthermore, the present disclosure does not limit the type of depolymerization solution. For example, hydrolysis may be carried out by water. In another example, alcohol (e.g., methanol, ethanol, ethylene glycol, diethylene glycol, or a mixture thereof) may be used for alcoholysis.

[0036] In one embodiment, the depolymerization solution is preferably an alcohol, and a more preferred alcoholysis solution may be ethylene glycol, in part because ethylene glycol can be a reactive monomer for producing virgin polyester chips.

[0037] When the chemical depolymerization reaction is carried out, a heating step may be suitably carried out. Generally, heating may accelerate the progress of the chemical reaction. For example, the recycled polyester material and ethylene glycol may be placed in the depolymerization tank 110 for the alcoholysis reaction at a temperature of 200° C. to 230° C. for about 3 hours.

[0038] Step 1-2: Progress of the esterification reaction.

[0039] The product of the above chemical depolymerization reaction is then subjected to an esterification reaction. It is worth noting that in the present disclosure, it is not necessary to completely depolymerize all polyester materials.

[0040] For example, the product after the above chemical depolymerization reaction may be transferred to the esterification tank 120 for esterification reaction. The esterification reaction is generally a reversible reaction. Therefore, in the esterification reaction, a part of the depolymerization solution and / or the product (e.g., alcohol and / or water) may be obtained by distillation. In this way, the amount or concentration of the other product (e.g., polyester product) may be increased by the balance of the chemical reaction.

[0041] In one embodiment, the product after the above chemical depolymerization reaction may first be filtered through a filter to remove at least a portion of the impurities in the recycled polyester material, thereby reducing the concentration of non-polyester impurities, before being transferred to the esterification tank 120. In one embodiment, the pore size of the filter may be between 1 μm and 10 μm.

[0042] After the esterification reaction has proceeded for a predetermined period of time, an electrostatic adhesion agent may be added to the esterification tank 120. The electrostatic adhesion agent may include a metal salt.

[0043] In some embodiments, the metal salt used in the electrostatic adhesion agent may be a non-transition metal salt, hi some embodiments, the metal salt used in the electrostatic adhesion agent may be an alkali metal salt, an alkaline earth metal salt, or a combination thereof.

[0044] In some embodiments, the alkali metal salt may include a lithium salt, a sodium salt, a potassium salt, or a combination thereof, where the lithium salt may include, for example, lithium acetate dihydrate (CH3COOLi·2H2O), the sodium salt may include, for example, sodium acetate trihydrate (CH3COONa·3H2O), and / or the potassium salt may include, for example, potassium acetate (CH3COOK), but the disclosure is not limited thereto.

[0045] In certain embodiments, the alkaline earth metal salt may include a magnesium salt, such as, but not limited to, magnesium acetate tetrahydrate ((CHCOO)Mg·4H0).

[0046] In one embodiment, the electrostatic adhesion agent may be first dissolved in a solvent (such as ethylene glycol). Then, the solution (i.e., the solvent in which at least a portion of the electrostatic adhesion agent is dissolved) is added to the esterification tank 120. At this time, the material in the esterification tank 120 has a lower viscosity ("lower viscosity" compared to the subsequently formed polyester resin mixture and / or the initial recycled polyester material) and can therefore be easily mixed evenly. Furthermore, the electrostatic adhesion agent may be present in the esterification tank 120 in the form of ions (metal cations and corresponding anions), so that it has good dispersibility and / or correspondingly good dielectric properties. In this way, the amount of electrostatic adhesion agent added can be reduced.

[0047] In a possible embodiment, the electrostatic adhesion agent may include 500 ppm magnesium acetate tetrahydrate, 100 ppm lithium acetate dihydrate, 100 ppm sodium acetate trihydrate, and 100 ppm potassium acetate, based on the total weight of materials in the esterification tank 120.

[0048] In some embodiments, the alkali metal ions and / or alkaline earth metal ions can catalyze the thermal decomposition of the polyester. Thus, when there is a higher amount of additive, the color of the subsequently formed film (such as the biaxially oriented polyester film described below) will be correspondingly yellowish (e.g., have a high b* value as expressed by the CIE Lab 1976 color space). In general, when a film has a high b* value, the product may have a low value.

[0049] After allowing the above esterification reaction to proceed for a period of time, other additives may be added to the esterification vessel 120, although the disclosure is not limited thereto. Other additives may include lubricants, stabilizers, and / or polymerization catalysts.

[0050] The lubricant may be particulate. For example, the lubricant may include silica particles, calcium carbonate particles, barium sulfate particles, polystyrene particles, silicone particles, acrylic particles, or combinations thereof. In a possible embodiment, the lubricant may include 5000 ppm of silica particles having an average particle size of approximately 2.4 μm, based on the total weight of materials in the esterification vessel 120.

[0051] The stabilizer may include an acid. In a possible embodiment, the stabilizer may include 150 ppm phosphoric acid, based on the total weight of materials in the esterification tank 120.

[0052] The polymerization catalyst may include a metal salt. In a possible embodiment, the polymerization catalyst may include 350 ppm of antimony acetate, based on the total weight of materials in the esterification vessel 120.

[0053] Steps 1-3: Progression of the polymerization reaction.

[0054] The product after the above esterification reaction is subjected to a polymerization reaction.

[0055] For example, the product after the esterification reaction described above may be transferred into a polymerization vessel 130 for a polymerization reaction.

[0056] The above polymerization reaction may include a pre-polymerization reaction and / or a main polymerization reaction.

[0057] The prepolymerization reaction is, for example, to reduce the gas pressure in the tank for a certain period of time. For example, by pumping gas (e.g., air), the gas pressure in the tank may be reduced from normal pressure (e.g., approximately 760 torr) to 10 torr within 60 minutes, or may be further reduced to less than 10 torr (e.g., 1 torr or around 1 torr).

[0058] The main polymerization reaction is, for example, by heating the material in a vessel under low pressure (e.g., below room / atmospheric pressure). For example, the polymerization reaction may be carried out at a temperature of 280° C. with the gas pressure in the vessel being less than 1 torr.

[0059] Step 1-4: Formation of polyester chips.

[0060] The polymerization reaction is allowed to proceed until the material in the vessel has a corresponding intrinsic viscosity (IV).The gas pressure in the vessel may then be increased (e.g., by filling with nitrogen gas).The material in the vessel is then extruded and / or pelletized by conventional granulation methods for typical polymer chips to form polyester chips.

[0061] In this embodiment, the intrinsic viscosity of the polyester chips formed by the above chemical remanufacturing generally does not exceed 0.65 dL / g, preferably between 0.40 dL / g and 0.65 dL / g, more preferably between 0.50 dL / g and 0.65 dL / g, and may be, for example, approximately 0.600 dL / g.

[0062] In some embodiments, the polyester chips formed by the above-described chemical remanufacturing may be referred to as chemically recycled polyester chips.

[0063] (Method of manufacturing virgin polyester chips) (Electrostatic adhesion agent and / or lubricant as described above may be included)

[0064] The production may be carried out by the same or similar method as the above-mentioned "Method for producing chemically recycled polyester chips", except that terephthalic acid and ethylene glycol may be added directly to the esterification tank for the esterification reaction. Also, the polyester chips formed by the above-mentioned methods (but not limited thereto) may be virgin polyester chips containing an electrostatic adhesion agent and / or a lubricant.

[0065] In this embodiment, the intrinsic viscosity of the polyester chips formed by the above method typically does not exceed 0.65 dL / g, for example, between 0.40 dL / g and 0.65 dL / g, and further, for example, between 0.50 dL / g and 0.65 dL / g, and can reach, for example, 0.600 dL / g.

[0066] In one embodiment, the polyester chips formed in the above manner may be referred to as virgin polyester chips.

[0067] (Method of manufacturing physically recycled polyester chip I) (The electrostatic adhesion agent and / or lubricant described above may be included)

[0068] In this embodiment, the recycled polyester material may be melted to be in a molten state. The molten recycled polyester material may then be filtered through a filter to remove solid impurities in the recycled polyester material. Then, an extruder (commercially available single screw extruder, SSE), twin screw extruder (TSE) or other similar screw extruder (but not limited thereto) may be used to extrude and granulate the filtered recycled polyester material to form physical recycled polyester chips I.

[0069] In one embodiment, before the recycled polyester material is melted, the recycled polyester material may be physically and mechanically broken down to reduce the time and / or energy consumption required to melt the recycled polyester material.

[0070] On the other hand, the above method reforms the recycled polyester material through cutting, dissolving, filtering and extrusion steps. In other words, generally, the physical recycled polyester chip I is produced by rearrangement of polyester molecules in the recycled polyester material.

[0071] In this embodiment, since the polyester molecules of the recycled polyester material are generally only rearranged (i.e., not essentially reorganized) in the above physical remanufacturing process, the compositions originally present in the recycled polyester material (e.g., electrostatic adhesion agents, lubricants, stabilizers, and / or polymerization catalysts, etc.) may still be present in the physical recycled polyester chip I. In other words, some of the characteristics of the physical recycled polyester chip I may be the same as or similar to some of the characteristics of the recycled polyester material originally used.

[0072] In one embodiment, the average molecular weight of recycled polyester material during physical remanufacturing process generally can hardly change. In other words, the viscosity of the recycled polyester material in the dissolved state is higher (i.e., it has lower fluidity). Therefore, when using a filter with a very small pore size, the filtration efficiency can be reduced. In one embodiment, the pore size of the filter is preferably between 10 μm and 100 μm, but the present disclosure is not limited to this range.

[0073] The physically recycled polyester chip I produced by the above physical remanufacturing generally has a relatively high intrinsic viscosity. In the present embodiment, the intrinsic viscosity of the physically recycled polyester chip is generally not less than 0.60 dL / g, and may be, for example, between 0.65 dL / g and 0.90 dL / g. Furthermore, it may be, for example, between 0.65 dL / g and 0.80 dL / g. For example, it may be approximately 0.68 dL / g.

[0074] In certain embodiments, the polyester chips formed by the above-described physical remanufacturing may be referred to as physically recycled polyester chips.

[0075] In one embodiment, the intrinsic viscosity of the physically recycled polyester chips may be adjusted by solid-state polymerization. However, the intrinsic viscosity of the physically recycled polyester chips can be easily increased, but not decreased, by solid-state polymerization. Furthermore, normal film-forming processes usually have a certain limit on the range of intrinsic viscosity of polyester chips. Therefore, using only the physically recycled polyester chips I may be more suitable for foaming and spinning processes, but less suitable for film-forming processes.

[0076] (Method of manufacturing physically recycled polyester chips II) (may contain the electrostatic adhesion agent and / or lubricant)

[0077] The production may be carried out by the same or similar method as the above "Physical Recycled Polyester Chip I Production Method", except that a corresponding feeder is added to mix additives (e.g., electrostatic adhesion agents and / or lubricants).

[0078] For example, at least one feeder (e.g., a side feeder) may be added to the twin-screw extruder according to the type and / or amount of additives (e.g., but not limited to, electrostatic adhesion agents or lubricants). The feeder may be a loss-in-weight feeder equipped with a loss-in-weight meter. The feeder may also be a common commercially available device and / or an optional accessory. In this way, when extruding the recycled polyester material, the corresponding additives may be mixed by the feeder according to the designed addition amount and / or concentration ratio.

[0079] In some embodiments, depending on the type and / or amount of additive, some properties of the recycled polyester chips (e.g., but not limited to, intrinsic viscosity, electrostatic adhesion effect, slippage, etc.) may be adjusted accordingly.

[0080] In certain embodiments, the polyester chips formed by the above-described physical remanufacturing may be referred to as physically recycled polyester chips.

[0081] In one embodiment, based on the total weight of the recycled polyester chips, the chips may include 1000 ppm magnesium acetate tetrahydrate, 200 ppm lithium acetate dihydrate, 200 ppm sodium acetate trihydrate, 200 ppm potassium acetate, and 5000 ppm silica having an average chip size of approximately 2.4 μm.

[0082] (Method of manufacturing biaxially oriented polyester film)

[0083] In this embodiment, at least one of the above polyester chips (e.g., the above chemically recycled polyester chips, the above virgin polyester chips, the above physically recycled polyester chips I, or the above physically recycled polyester chips II, etc.) may be used directly or mixed in a suitable ratio according to design requirements.

[0084] In one embodiment, the polyester chips may be dried by heat and / or low pressure. For example, the polyester chips may be vacuum dried at approximately 160° C. for 4 hours.

[0085] The polyester chips (which may be, but are not limited to, dried polyester chips) are then heated for melting and extrusion. For example, the polyester chips are melted by an extruder (such as, but are not limited to, a commercially available single screw extruder) at approximately 280° C., and the molten polyester is removed from a die (such as, but are not limited to, a T-die head) 210 and squeezed or extruded.

[0086] After being squeezed or extruded from the mold 210, the molten polyester may be dropped onto the casting roll 220. And the electrostatic adhesion device 230 corresponding to the casting roll 220 is powered on so that the electrostatic adhesion device 230 has a corresponding high potential and the casting roll 220 has a corresponding low potential (e.g., ground potential). Thus, a corresponding electrostatic voltage may be provided between the electrostatic adhesion device 230 and the casting roll 220. Of course, the respective potentials of the casting roll 220 and the electrostatic adhesion device 230 may be adjusted according to design requirements (e.g., the electrostatic adhesion device 230 has a corresponding low potential and the casting roll 220 has a corresponding high potential).

[0087] In this embodiment, the potential difference between the casting roll 220 and the electrostatic adhesion device 230 is usually 1 kilovolt (kV) or more, for example, 2 kV or more, for example, 3 kV or more, and may be 5 kV or more. The casting roll 220 may be used to cool the polyester. Hereinafter, the sheet after cooling and forming may be referred to as a thick sheet.

[0088] In this embodiment, at least one polyester chip used may contain an electrostatic adhesion agent due to the electrostatic voltage between the energized electrostatic adhesion device 230 and the casting roll 220, so that the polyester (still in a molten state or partially cooled and tacky or flaked) may better adhere to the surface 220a of the casting roll 220. In other words, the polyester may be cooled faster and more uniformly. Also, the polyester molecules may have lower crystallinity and more uniform thickness. Thus, the formed thick sheet or corresponding biaxially oriented polyester film may have better properties (e.g., lower film haze, higher thickness uniformity, and / or less susceptible to breakage).

[0089] The thick sheet may then be subjected to a corresponding biaxial orientation step in the usual manner for typical biaxially oriented polyester films.

[0090] For example, an unstretched thick sheet may first be guided to a longitudinal stretcher for longitudinal stretching to form a corresponding film (i.e., a longitudinally stretched thick sheet), and then the film may be guided to a transverse stretcher for transverse stretching to form a biaxially oriented polyester film (i.e., a transversely stretched film).

[0091] More specifically, for example, the unstretched thick sheet may be guided to a longitudinal stretcher. In the longitudinal stretcher, the unstretched thick sheet may be preheated to 80° C. through a number of rollers that may be used for heating, and then heated by infrared rays at the longitudinal stretching point. During infrared heating, the thick sheet may be stretched to approximately 3.5 times its length in the length direction parallel to the conveying direction (may also be referred to as the machine direction MD) due to the speed difference between the two rollers. The longitudinally stretched thick sheet (may also be referred to as a film) may be cooled (e.g., cooled to approximately 30° C.) by rollers (without any number of rollers). Next, the two ends of the film may be clamped in the width direction of the film (i.e., the other direction perpendicular to the machine direction, which may also be referred to as the transverse direction TD). The film held by the clamps may be further guided to a transverse stretcher. In the transverse stretcher, the clamped film may first be preheated to approximately 90° C. in a preheating zone. The film is then further heated to approximately 100° C. and stretched approximately 4.0 times in the width direction. The transversely stretched film may then be heated to approximately 230° C. for heat setting.

[0092] Through the above steps, the production of the biaxially oriented polyester film according to the present embodiment is substantially completed.

[0093] In some embodiments, depending on design requirements, portions of the film may be removed after lateral stretching (eg, edge trim may be removed).

[0094] The biaxially oriented polyester film may be rolled and stored and may be further sold and / or used.

[0095] Examples and Comparative Examples

[0096] Examples and comparative examples are presented below to explain the present disclosure in detail, but the present disclosure is in no way limited to the following examples.

[0097] Each Example and Comparative Example shows a corresponding biaxially oriented polyester film formed by the above method, with the difference that the percentage of polyester chips used was adjusted so that the formed biaxially oriented polyester film had a corresponding metal ion concentration and lubricant concentration (shown as SiO2 concentration).

[0098] The biaxially oriented polyester films of Examples 1 to 4 and Comparative Examples 1 to 4 in Table 1 are evaluated. The evaluation targets include the color of the 10 laminated biaxially oriented polyester films (shown in Table 1 as "10 film color b*"), the haze of the biaxially oriented polyester films (shown in Table 1 as "film haze (%)"), the recrystallization temperature of the biaxially oriented polyester films (shown in Table 1 as "recrystallization temperature Tc(20)(°C)"), the film break rate of the biaxially oriented polyester films (shown in Table 1 as "film break rate (number of times / 24 hours)"), and the crystallization rate of the thick sheet used to form the biaxially oriented polyester films (shown in Table 1 as "crystallization rate of thick sheet after cooling and forming").

[0099] For color testing, the CIE 1976 color space b* value may be analyzed by Tokyo Denshoku's color difference meter ND300A (Hunter method).

[0100] Regarding the haze test, the haze of the polyester film in the following embodiments may be tested by a Tokyo Denshoku haze meter (model TC-HHIII). The method follows the JIS K770 specification.

[0101] The recrystallization temperature or crystallization rate may be analyzed by differential scanning calorimetry (DSC) according to the ISO11358-3:2013 (discrimination of temperatures and enthalpies of melting and crystallization) standard.

[0102] The film break rate may be the number of film breaks per unit time under the same stretching conditions (including longitudinal stretching or transverse stretching as described above).

[0103] [Table 1]

[0104] In the above examples or comparative examples, the method for evaluating the electrostatic adhesion effect may include: heating 10 milligrams (mg) of thick sheet at a heating rate of 20°C / min until it melts after being cooled and formed by differential scanning calorimetry (DSC), and then calculating the crystallization rate by the following formula: C=(A1-A2) / B. C is the crystallinity of the thick sheet sample after being cooled and formed. A1 is the endothermic peak area of ​​the melting point (Tm). A2 is the exothermic peak area of ​​the crystallization temperature (Tch). B is the theoretical value of complete crystallization (i.e., 100% crystallization) (approximately 140 J / g).

[0105] Generally, the lower the crystallization rate, the better the electrostatic adhesion effect.

[0106] In some possible embodiments, there are often many impurities that cannot be removed due to the high percentage of recycled material added. Thus, the films formed (e.g., thicker sheets) have more crystals (e.g., higher crystallization percentage) and / or higher recrystallization temperatures (Tc), which often result in a narrower range of processing conditions, higher crystallinity after cooling and forming, slower production rates, lower stretchability (e.g., better longitudinal or transverse stretching is more difficult), and / or higher film breakage.

[0107] In the above embodiments (such as, but not limited to, the first to fourth embodiments), the production may be carried out by the above method that is the same as or similar to the "chemically recycled polyester chip manufacturing method". In addition, an appropriate amount of electrostatic adhesion agent is added during the manufacturing process of the chemically recycled polyester chip. Also, since the electrostatic adhesion agent is dissolved in the solution and added / exists in the form of ions (metal cations and corresponding anions) in the reaction tank (e.g., esterification tank), the method is similar to homogeneous mixing, easy to mix and / or easy to uniformly mix, its dispersibility is good and / or the corresponding dielectric property is good. Therefore, the addition amount of the electrostatic adhesion agent can be reduced and / or a good electrostatic adhesion effect can be exerted in the subsequent manufacturing process. In this way, when the polyester resin mixture containing the chemically recycled polyester chip is molded with a cooling molding roll, the dissolved polyester polymer has a better cooling effect and the occurrence of crystallization can be reduced (e.g., the crystallization ratio is reduced).

[0108] Similarly, when the electrostatic adhesion agent is added via extrusion mixing, it is similar to the addition via heterogeneous mixing. Therefore, compared with homogeneous mixing, the electrostatic adhesion agent has lower dispersibility and / or is more difficult to form an ionic state. Therefore, it is often necessary to increase the amount of electrostatic adhesion agent added to achieve the expected electrostatic adhesion effect.

[0109] Also, alkali metal salts or alkaline earth metal salts can be good electrostatic adhesion agents. However, alkali metal ions and / or alkaline earth metal ions can catalyze the thermal decomposition of polyester. Thus, when a larger amount of alkali metal salt or alkaline earth metal salt is added, the subsequently formed film may become correspondingly yellowish, reducing the value of the product.

[0110] In summary, the biaxially oriented polyester film of the present disclosure may be made from recycled polyester materials, and the biaxially oriented polyester film of the present disclosure has better quality.

[0111] It will be apparent to one skilled in the art that various modifications and variations can be made to the structure of the present disclosure without departing from the scope of the present disclosure. In view of the above, it is intended that the present disclosure cover modifications and variations of the present disclosure provided they come within the scope of the appended claims and their equivalents. [Industrial Applicability]

[0112] The biaxially oriented polyester film and method of making the same of the present invention may be applied to any commercially available article, such as magnetic tape, insulating tape, photographic film, tracing film, packaging film, electrical insulating film, engineering paper, and the like. [Explanation of symbols]

[0113] 110 Depolymerization tank 120 Esterification tank 130 Polymerization tank 210 type (die head) 220 Casting Roll 230 Electrostatic adhesion device 220a Surface

Claims

1. 1. A biaxially oriented polyester film, comprising: a polyester resin mixture including a polyester material, an electrostatic adhesion agent having a metal ion, and a lubricant; the polyester material is composed of at least a recycled polyester material, the recycled polyester material including 80% or less of physical recycled polyester chips and 20% or more of chemical recycled polyester chips based on the total amount of the polyester material; a weight ratio of the recycled polyester material to the polyester resin mixture is greater than 80% and less than 100%; a weight concentration of the metal ions in the polyester resin mixture is 40 ppm to 50 ppm; and the biaxially oriented polyester film has the following physical characteristics: a recrystallization temperature (Tc(A)) observed when cooled in a molten state at a cooling rate of 20°C / min is greater than 175°C to 200°C; and the biaxially oriented polyester film is formed from a thick sheet that is melted and extruded by an extruder and then cooled on a casting roll prior to bidirectional stretching.

2. 2. The biaxially oriented polyester film of claim 1, wherein the metal ions are alkali metal ions, alkaline earth metal ions, or a combination thereof.

3. 2. The biaxially oriented polyester film according to claim 1, wherein the weight concentration of the lubricant in the polyester resin mixture is from 500 ppm to 3000 ppm.

Citation Information

Patent Citations

  • Polyester film and production thereof

    JP1996230032A

  • Biaxially oriented polyester film and its manufacture

    JP2000309052A

  • Recycled polyester-containing polyester structure and method for manufacturing the same

    JP2011256328A

  • Biaxially oriented polyester film

    JP2016117178A

  • Polyester film

    JP2018168381A