Aluminum alloy bare material and aluminum alloy brazing sheet with excellent thermal conductivity and erosion resistance

The aluminum alloy composition with controlled Fe, Si, Cu, and Mn, and optimized compound particles addresses the challenges of thermal conductivity and corrosion in heat exchangers, enhancing electrical conductivity and structural strength for improved heat dissipation.

JP7555766B2Active Publication Date: 2024-09-25MA ALUMINUM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020151359
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-09
Publication Date
2024-09-25
Estimated Expiration
2040-09-09

AI Technical Summary

Technical Problem

Existing aluminum alloys used in automotive heat exchangers face challenges in achieving high thermal conductivity and structural strength while minimizing electrical conductivity loss and preventing wax corrosion during brazing.

Method used

An aluminum alloy composition with controlled amounts of Fe, Si, Cu, and Mn, along with optimized particle size and distribution of Al-Fe and Al-Fe-Si compounds, enhances electrical conductivity and corrosion resistance, preventing recrystallization and wax corrosion.

Benefits of technology

The alloy achieves high electrical conductivity, structural strength, and corrosion resistance, enabling further downsizing and improved heat dissipation performance in automotive heat exchangers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555766000005
    Figure 0007555766000005
  • Figure 0007555766000006
    Figure 0007555766000006
  • Figure 0007555766000007
    Figure 0007555766000007
Patent Text Reader

Abstract

To provide an aluminum alloy bare material having high electric conductivity and excellent corrosion resistance, and a brazing sheet.SOLUTION: An aluminum alloy bare material for heat exchangers contains, in mass%, Fe: 0.6% or more to 0.8% or less, Si: 0.4% or less, and Cu: more than 0.6% to 1.0% or less, with the contents of Mn and Zn controlled to 0.2% or less and 0.3% or less respectively, and the balance being Al and unavoidable impurities. The electric conductivity is 55%IACS or more. The number of Al-Fe compound particles or Al-Fe-Si compound particles with a circle equivalent diameter of 0.5-2.0 μm, distributed in a matrix, is 1.0×104-3.0×104 / mm2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum alloy bare material and an aluminum alloy brazing sheet having excellent thermal conductivity and erosion resistance. [Background technology]

[0002] In recent years, new heat exchangers such as inverter coolers are being installed in automobiles due to the trend towards electric vehicles. Inverter coolers are required to have improved heat dissipation performance in order to reduce size and weight by saving space. For example, in inverter coolers that have a structure with high component bonding density, the higher the thermal conductivity of the aluminum used in the components, the better the heat dissipation performance of the inverter cooler. Aluminum alloys used in automotive heat exchangers are generally Al-Mn alloys due to their strength and corrosion resistance. However, Mn added to Al tends to significantly reduce electrical conductivity when dissolved in the Al matrix. The thermal conductivity and electrical conductivity of Al are proportional, and a decrease in electrical conductivity leads to a decrease in thermal conductivity. Therefore, heat dissipation performance is limited in automotive heat exchangers that use Al alloys with Mn added, which has poor electrical conductivity. On the other hand, if a 1000 series alloy without Mn is used, it can have high electrical conductivity, but its strength is low as a component of an automotive heat exchanger, and the structural strength of the heat exchanger cannot be maintained. In addition, elements such as Si and Cu that improve strength by dissolving in the Al matrix can suppress the decrease in electrical conductivity and improve strength compared to Mn when compared with the same amount of addition, but the melting point of the material decreases as the amount of addition increases, so excessive addition increases the possibility of severe brazing erosion during brazing, making it difficult to maintain the shape of the heat exchanger. For this reason, in order to improve the heat dissipation performance while maintaining the structure of automotive heat exchangers, it is necessary to ensure strength and improve thermal conductivity by using aluminum alloys other than Al-Mn alloys.

[0003] Conventionally, an aluminum alloy material having a composition of 2.0 to 3.0 mass% Fe, 0.5 to 1.5 mass% Si, 0.05 mass% or less Ti, with the balance being Al and unavoidable impurities, has been known as an aluminum alloy material exhibiting high strength and high thermal conductivity (see Patent Document 1). In addition, an aluminum alloy fin material for heat exchangers is provided, which is composed of 0.010 to 0.4 mass% Fe, less than 0.005 mass% Cu, the balance being Al and impurities, has an Al purity of 99.30 mass% or more, has an average grain size of subgrains of 2.5 μm or less, and has an intermetallic compound content of 2000 particles / mm2 with a maximum length exceeding 3 μm. 2 The following aluminum fin material is known (see Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-256365 A [Patent Document 2] JP 2014-074198 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, with the demand for further miniaturization and high heat dissipation performance of heat exchangers, there is a demand for aluminum alloys with high electrical conductivity (= high thermal conductivity). Therefore, the inventors have been developing various Al alloys of a system different from Al-Mn alloys. In conjunction with the development of this material, the inventors have studied a composition system in which Fe, Si, and Cu are added to Al, and as a result, have found that by using an alloy containing Fe, which is hardly dissolved in the aluminum matrix, and Si, a material that has high electrical conductivity and strength sufficient to maintain the structural strength of a heat exchanger can be obtained. However, if the amount of Si added is increased, the melting point of the base material decreases when a large amount of Si is dissolved in the base material, so that the brazing material is severely eroded during brazing and the shape of the heat exchanger cannot be maintained. Furthermore, if the distribution ratio of fine Al-Fe-Si compounds relative to coarse Al-Fe compounds is low, recrystallization occurs with the coarse Al-Fe compounds as nuclei, and the recrystallized grains become fine, so that excessive brazing erosion may occur during brazing. Therefore, a process was adopted to reduce the solid solubility of Si and optimize the particle size and density of the Al-Fe compounds present in the Al matrix and the particle size and density of the Al-Fe-Si compounds. As a result, it was found that the recrystallized grains do not become fine, the erosion resistance is excellent, and the electrical conductivity is dramatically improved compared to Al-Mn alloys.

[0006] They also discovered that by adding Cu, which does not affect the distribution of these compounds, to Al within the range that does not cause brazing erosion during brazing, the material can be adapted to automotive heat exchangers, which require greater strength.

[0007] The present invention has been made in view of the above background, and aims to provide an aluminum alloy bare material and an aluminum alloy brazing sheet which have high electrical conductivity, can suppress the occurrence of brazing erosion, and have the strength and corrosion resistance required for heat exchangers. [Means for solving the problem]

[0008] (1) The aluminum alloy bare material of the present embodiment contains, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.7% or more and 1.4% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, the balance being Al and unavoidable impurities, has an electrical conductivity of 55% IACS or more, and the number of Al-Fe based compound particles or Al-Fe-Si based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in a matrix is ​​1.0 × 10 4 ~3.0×10 4 pieces / mm 2 It is characterized in that:

[0009] (2) The aluminum alloy bare material of this form is Heat to 600℃ and hold for 5 minutes, then cool to 300℃ at 60℃ / min. The material has an electrical conductivity of 44% IACS or more after heat treatment equivalent to that of heat exchanger brazing, and the number of Al-Fe compound particles or Al-Fe-Si compound particles with a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is ​​1.0 × 10 4 ~3.0×10 4 pieces / mm 2 It is preferable that:

[0010] (3) The aluminum alloy brazing sheet of this embodiment is characterized in that a core material is an aluminum alloy for heat exchangers having the composition described in (1) or (2), and an aluminum alloy layer containing, as a brazing material, 3.0 to 12.0% by mass of Si, with the remainder being Al and unavoidable impurities, is bonded to one or both surfaces of the core material.

[0011] (4) In the aluminum alloy brazing sheet of the present embodiment, the brazing filler metal preferably further contains, by mass %, Zn: 0.1 to 4.0%. (5) In the aluminum alloy brazing sheet according to (3) or (4) of the present embodiment, the aluminum alloy brazing sheet has an electrical conductivity of 53% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix of the core material is 0.1×10 4 ~3.0×10 4 pieces / mm 2It is preferable that:

[0012] (6) In the aluminum alloy brazing sheet according to any one of (3) to (5) of the present invention, Heat to 600℃ and hold for 5 minutes, then cool to 300℃ at 60℃ / min. After heat treatment equivalent to brazing a heat exchanger, the core material has an electrical conductivity of 43% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles with a circle equivalent diameter of 0.5 to 2.0 μm distributed in the core material matrix is ​​1.0 × 10 4 ~3.0×10 4 pieces / mm 2 It is preferable that:

[0013] (7) In the aluminum alloy brazing sheet according to any one of (3) to (6) of the present invention, Heat to 600℃ and hold for 5 minutes, then cool to 300℃ at 60℃ / min. It is preferable that the pitting potential difference between the surface of the core material and the surface of the brazing material after the heat treatment equivalent to that of heat exchanger brazing is 80 mV or more. Effect of the Invention

[0014] The present invention can provide an aluminum alloy bare material or an aluminum alloy brazing sheet for heat exchangers that has excellent electrical conductivity and excellent erosion resistance. The aluminum alloy bare material or brazing sheet according to the present invention has excellent electrical conductivity while suppressing braze erosion, and can therefore be applied as an aluminum alloy bare material and brazing sheet suitable for use in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of an aluminum alloy bare material according to the present invention. [Diagram 2] 1 is a partial cross-sectional view showing an example of a brazing sheet according to the present invention. [Diagram 3] FIG. 4 is a partial cross-sectional view showing another example of the brazing sheet according to the present invention. [Figure 4] FIG. 2 is a side view for explaining a joining state between the brazing sheet according to the present invention and a member to be brazed. [Diagram 5] 1 is a perspective view showing a heat exchanger configured to which a brazing sheet according to the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. Note that the drawings used in the following description may show characteristic portions in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand.

[0017] Fig. 1 shows an example of an aluminum alloy bare material according to the present invention, and Fig. 2 shows a cross-sectional structure of an aluminum alloy brazing sheet for heat exchangers according to a first embodiment, which has a core material made of the same components as the aluminum alloy bare material shown in Fig. 1. The aluminum alloy brazing sheet A of this embodiment is in the form of a plate or sheet, and has a three-layer structure in which a first brazing material layer 2 is laminated on both the top and bottom surfaces of a core material 1 made of the same components as the aluminum alloy bare material shown in Fig. 1. The brazing material layer 2 may be laminated on only one side of the core material 1, as in other embodiments described later.

[0018] "Aluminum alloy bare material and core material" The bare material M and the core material 1 are made of an aluminum alloy containing, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.7% or more and 1.4% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the remainder being Al and unavoidable impurities. The aluminum alloy bare material M can be rolled into a plate shape as shown in Fig. 1 and used as a fin for a heat exchanger, or the aluminum alloy and double-sided clad material can be processed into a cup shape and used as a component to be brazed by stacking them alternately. One example of the use of the aluminum alloy bare material M of this embodiment is the brazing sheet A shown in Fig. 2, which uses an alloy of the same composition as the core material 1, but it is of course possible to use it for other purposes.

[0019] The reasons for limiting the composition of the component elements contained in the aluminum alloy constituting the bare material M and the core material 1 will be explained below. Fe: 0.6% or more and 0.8% or less Fe is added to Al to precipitate Al-Fe or Al-Fe-Si compound particles in the aluminum alloy matrix, and is added to Al to improve material strength through particle dispersion strengthening. If the Fe content is below the lower limit, the Al-Fe compound particles or Al-Fe-Si compound particles cannot be dispersed as desired (required number per unit area). If the Fe content exceeds the upper limit, the number of dispersed Al-Fe compound particles or Al-Fe-Si compound particles increases more than necessary, and when a corrosive solution adheres to the bare material or core material itself, the cathodic reaction on the surface is promoted, and the self-corrosion resistance is reduced.

[0020] Si: 0.7% or more and 1.4% or less Si improves the material strength of Al by dissolving in Al or precipitating in the aluminum alloy matrix as compound particles such as Al-Fe-Si. If the Si content exceeds the upper limit, the melting point of the aluminum alloy is lowered more than necessary, which may cause the core material to melt during brazing and lead to poor brazing. If the Si content exceeds the upper limit, the electrical conductivity after brazing may decrease. If the Si content is below the lower limit, the desired dispersion state of the compound particles is not obtained, the recrystallized grains become fine, and the bare material and the core material are excessively eroded by the brazing, which may prevent the shape of the heat exchanger from being maintained.

[0021] Cu: 0.6% or less Cu is added to dissolve in Al to improve the material strength of Al. If the Cu content is below the lower limit, the heat exchanger will not have enough strength to maintain its structure. If the Cu content is above the upper limit, the electrical conductivity after brazing will decrease. In addition, an increase in the Cu content may cause Cu to precipitate on the surface during corrosion of the Al alloy, which may reduce its self-corrosion resistance. In addition, when used as a brazing sheet, a large amount of Cu diffuses from the core material to the brazing material during brazing, making the potential of the brazing material more noble, and the potential difference between the brazing material and the core material will be small, so the sacrificial corrosion protection provided by the brazing material may not work effectively.

[0022] Mn: 0.2% or less It is difficult to completely eliminate Mn from the aluminum alloy when manufacturing it, so for manufacturing reasons, only a small amount is included. Even if only a small amount of Mn is included, it significantly reduces the electrical conductivity when dissolved in Al. However, if the Mn content is 0.2% or less, the amount of Mn dissolved in Al can be minimized by carrying out a predetermined homogenization treatment, thereby suppressing the reduction in electrical conductivity. The Mn content is more preferably 0.1% or less. Zn: 0.3% or less Zn is an element that contributes to ensuring corrosion resistance, and if the Zn content exceeds 0.3%, the self-corrosion resistance decreases. The Zn content is more preferably 0.2% or less.

[0023] "Brazing material" The reasons for limiting the composition of the component elements contained in the brazing material 2 will be explained below. Si: 3.0-12.0% Silicon is added to form a molten braze during brazing and to form a fillet at the brazed joint. If the Si content is below the lower limit, the amount of molten brazing filler metal will be small, and the brazing bondability will be reduced.If the Si content is above the upper limit, the amount of molten brazing filler metal generated during brazing will be excessive, and the core material 1 or the member to be brazed will be melted intensely, making it impossible to maintain the shape of the heat exchanger, which may result in a decrease in performance or a loss of appearance. In addition, when a mass% range or a numerical range is expressed using "~", the lower and upper limits are included unless otherwise specified. For example, 3.0-12.0% means that the content is 3.0 mass% or more and 12.0 mass% or less.

[0024] Zn: 0.1-4.0% Zn is added to brazing filler metal to obtain the sacrificial corrosion protection effect of the core material. If more than 4.0% Zn is added, the corrosion rate increases, and the brazing filler metal corrodes early, so that the core material cannot be protected from corrosion, and the corrosion resistance decreases.

[0025] "Particle size of Al-Fe compound particles or Al-Fe-Si compound particles" 0.5~2.0μm (0.5μm or more and 2.0μm or less) If the particle size (circle equivalent diameter) of the compound particles is less than 0.5 μm, the compound particles are redissolved in the matrix during brazing, and the electrical conductivity of the material after brazing decreases. If the particle size exceeds 2.0 μm, effective particle dispersion strengthening cannot be achieved, and the material strength decreases, so the structural strength of the heat exchanger cannot be maintained. In addition, if there are many compound particles larger than 2.0 μm, recrystallization progresses with the compound particles as nuclei, and the recrystallized grains become fine, causing severe erosion of the aluminum alloy bare material and core material, making it impossible to maintain the shape of the heat exchanger.

[0026] Number of Al-Fe compound particles or Al-Fe-Si compound particles: 1.0×10 4 ~3.0×10 4 pieces / mm 2 (1.0×10 4 pieces / mm 2 Above 3.0×10 4 pieces / mm 2 below)" The number of compound particles is 1.0×10 4When the amount of an element added to a material is less than 1, the element is dissolved in the matrix and the electrical conductivity is greatly reduced. Conversely, when the amount of an element added is small, the electrical conductivity is high because the degree of solid solubility is low, but the material strength is low and the structural strength required for applications such as heat exchangers cannot be maintained. The number of compound particles is 3.0×10 4 When the number of particles exceeds 1, the number of compounds exposed to the surface increases. The increase in the number of compound particles increases the cathodic reaction occurring on the material surface, and the self-corrosion resistance of the Al alloy decreases. The number of Al-Fe compound particles or Al-Fe-Si compound particles is 1.0×10 4 ~3.0×10 4 pieces / mm 2 The range is more preferable.

[0027] Number of Al-Fe compound particles or Al-Fe-Si compound particles after brazing: 1.0 x 10 4 ~3.0×10 4 pieces / mm 2 (1.0×10 4 pieces / mm 2 Above 3.0×10 4 pieces / mm 2 below)"

[0028] "Potential difference between core potential and brazing material potential" When the potential difference between the core material potential and the brazing material potential is 80 mV or more, the brazing material improves the sacrificial corrosion protection (corrosion resistance) of the core material. When the potential difference is 80 mV or less, the sacrificial corrosion protection does not work effectively and the core material corrodes significantly. The fact that corrosion resistance improves when the potential difference is 80 mV or more can be confirmed, for example, by the corrosion test described below.

[0029] The corrosion test is carried out by immersing a brazed test sample, in which the brazing material and the core material are overlapped so that the core material is exposed, in OY water. The composition of OY water is 195 ppm Cl. - , 60ppmSO4 2- , 1ppmCu 2+ , 30 ppm Fe 3+ It is an aqueous solution containing The test cycle is 88°C for 8 hours, followed by 16 hours at room temperature. When heating to 88°C, the corrosive solution is stirred using a magnetic stirrer. The specific liquid volume is 16.7ml / cm 2 The sample size is adjusted so that For those with a potential difference of 80 mV or more, after four weeks of OY water testing, the core material had 0.1 pits / mm2 or less in depth. 2 The number is less than this, and the corrosion resistance is good. Therefore, if the potential difference between the core material and the brazing material is 80 mV or more, the brazing sheet is less susceptible to pitting corrosion and can be provided as a brazing sheet with excellent corrosion resistance.

[0030] "Manufacturing method" For example, aluminum alloys for bare materials and core materials, and aluminum alloys for brazing materials are cast by semi-continuous casting. An aluminum alloy for the core material can be used that contains, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.7% or more and 1.4% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, with the remainder being Al and unavoidable impurities. Bare material and core material can be manufactured from this aluminum alloy. An aluminum alloy for brazing filler metal can be used that contains, by mass%, 3.0 to 12.0% Si, and can further contain 0.1 to 4.0% Zn as necessary, with the remainder being Al and unavoidable impurities. Brazing filler metal can be produced from this aluminum alloy.

[0031] "Homogenization treatment" The obtained core material can be subjected to homogenization treatment at 400°C to 600°C for 3 to 12 hours. By selecting the appropriate temperature and time, it is possible to obtain the desired properties of high electrical conductivity and optimal dispersion of compound particles in the matrix.

[0032] For the brazing material, in order to improve machinability, a homogenization treatment may be performed under conditions selected from the ranges of 400° C. to 500° C. and a treatment time of 1 to 10 hours.

[0033] "Pasting" When used as a brazing sheet, it can be produced by combining it appropriately on one or both sides of a sheet-shaped or plate-shaped core material with a cladding ratio of brazing material:core material=5-15%:85-95%.When used on both sides, the brazing sheet can be produced by combining it with a cladding ratio of skin material:core material:skin material=5-15%:70-90%:5-15%. There are no particular limitations on the preparation of the brazing material, and it can be prepared under the conditions for preparing the brazing material when manufacturing a general brazing sheet. After homogenization, the surface is machined, rolled to the desired thickness by hot rolling, cut to a specified length, and bonded to the core material.

[0034] "Hot rolling, cold rolling, annealing" Bare aluminum alloys and materials made by combining core and skin materials can be manufactured by hot rolling (or clad rolling) using a hot rolling mill. After the hot rolling, the steel sheet can be cold-rolled to a desired thickness. In this case, annealing may be performed as many times as necessary during the cold rolling to continue the rolling. The thickness of the final material is not particularly limited, but the reduction ratio from the thickness finished by hot rolling and the thickness annealed for further rolling to the final thickness is preferably 20 to 99%. In addition, annealing may be performed after cold rolling to achieve O temper. Annealing may be performed by performing heat treatment at 200°C to 500°C for 1 to 10 hours using a batch annealing furnace, for example.

[0035] The aluminum alloy bare material M produced according to the steps described above or the aluminum alloy brazing sheet A having the configuration shown in FIG. 2 is used for the purpose of brazing by placing it for about 1 to 30 minutes in an inert gas atmosphere at a brazing temperature in the range of, for example, about 590 to 620°C when producing a heat exchanger or the like. For example, it is used in assembling heat exchangers by laminating it with brazing target components such as fins and tubes of various heat exchangers or cup-shaped bodies, and after assembling the fins, tubes, or cup-shaped bodies, the whole is heated to the brazing temperature to melt the brazing material 2 of the aluminum alloy brazing sheet A, and then cooled to room temperature to form a fillet and complete the brazing. Alternatively, components such as fins and tubes of a heat exchanger can be directly formed with the brazing sheet and used for brazing. The workpiece to be brazed may be a bare aluminum alloy material M shown in FIG.

[0036] FIG. 3 shows a brazing sheet B obtained by cladding and rolling a brazing material 2 on only one side of a core material 1, and FIG. 4 is an explanatory diagram showing the state in which this brazing sheet B is used to braze a brazing target member 3 such as a fin. Brazing is completed by brazing the brazing sheet B and the brazing target member 3 shown in FIG. 4 under the brazing conditions described above.

[0037] The bare material M and the brazing sheets A and B have high electrical conductivity, excellent erosion resistance, and the strength and corrosion resistance required for heat exchangers, and therefore can be provided as brazing sheets suitable for use in automotive heat exchangers, which have been required in recent years to be further miniaturized and have high heat dissipation performance. The brazing material 2 may have a multi-layer structure, such as a two-layer structure including a first brazing material 2A and a second brazing material 2B as shown by the two-dot chain line in FIG. 4, or another multi-layer structure.

[0038] 5 shows an aluminum heat exchanger 5 in which fins 6 are formed using the brazing sheet A or brazing sheet B, and an aluminum alloy tube 7 is used as the brazing target component. The fins 6 and tubes 7 can be combined with a reinforcing material 8 and a header plate 9, and brazed to obtain the aluminum heat exchanger 5 for automotive use, etc. The brazing sheets A and B described above have excellent electrical conductivity, excellent erosion resistance, and the strength and corrosion resistance required for heat exchangers, and therefore can be used in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years, and can provide automotive heat exchangers, which are being further miniaturized and have high heat dissipation performance.

[0039] The brazing sheet can be used for various purposes such as forming fins of heat exchangers, forming tubes, forming header pipes, and other heat exchanger components. In such cases, various laminated structures can be adopted depending on the application, such as a single-sided brazing material type, a double-sided brazing material type, a structure combined with a sacrificial material, or a multi-layer structure combined with an intermediate material. EXAMPLES

[0040] Each aluminum alloy was produced by semi-continuous casting so as to have the composition of Alloy No. A1 to A28 shown in Tables 1 and 2. The obtained aluminum alloy ingots were subjected to homogenization annealing (homogenization treatment) under the conditions (temperature (°C) x time (h)) shown in Tables 1 and 2, and then hot rolled and cold rolled to a thickness of 1.0 mm so as to give a rolling reduction of 85%. The aluminum alloy bare materials were then produced through annealing at 350°C for 5 hours. Additionally, sample brazing sheets were prepared by combining the aluminum alloys of each alloy number listed in Tables 1 and 2 as core materials with the brazing filler metals of the compositions shown in Tables 3 and 4 by clad rolling. At this time, the brazing filler metal was laminated to one side of the core material by clad rolling so that the clad ratio was 10%, and then hot-rolled and cold-rolled to a thickness of 1.0 mm so that the reduction ratio was 85%, and annealed at 350°C for 5 hours to prepare brazing sheet samples of each number.

[0041] "Heat treatment equivalent to brazing" In order to evaluate the bare materials and brazing sheets used in the brazed heat exchangers individually, each bare material and brazing sheet sample was subjected to a brazing-equivalent heat treatment in a batch furnace. The brazing-equivalent heat treatment was performed under the following conditions: heating from room temperature to 600°C, holding at 600°C for 5 minutes, and then cooling to 300°C at 60°C / min. After reaching 300°C, each sample was quickly cooled to room temperature using a fan. The obtained bare materials and brazing sheet samples were subjected to the evaluation described below.

[0042] "Evaluation Method" <Electrical conductivity> The measurement was performed by a four-terminal method. A current of 500 mA was applied to the sample in a room temperature environment of 20 to 25° C., and the resistance was calculated from the voltage value, and then the electrical conductivity was calculated. <Compound particle distribution state> The cross sections parallel to the rolling direction were observed for the manufactured aluminum alloy bare material and brazing sheet core material, and for the aluminum alloy bare material and brazing sheet core material that had been subjected to heat treatment equivalent to brazing. The observations were performed using a field emission scanning electron microscope (FE-SEM) on cross sections that had been subjected to CP processing (cross-section polishing) based on the ion milling method. The circle equivalent diameter and distribution density of the compound particles were calculated by image analysis based on the observed images.

[0043] <Electrochemical polarization measurement> A 2.67% AlCl3 aqueous solution that had been thoroughly degassed with high-purity N2 gas and an electrochemical measurement cell were used, Pt was used as the working counter electrode, and the Luggin capillary and reference electrode Ag / AgCl were bypassed. The liquid temperature during the measurement was kept at 40°C. The measurement area of ​​the brazing material surface and core material of the sample that was subjected to heat treatment equivalent to brazing was 10 mm 2 The test area was exposed to light, and the rest was masked with insulating paint. As pretreatment for the measurement area, it was immersed in 5% NaOH at 50°C for 30 seconds, washed with water, and then immersed in 30% HNO3 at room temperature for 1 minute and washed with water. After holding the specimen at the natural potential for about 5 minutes, the potential was swept from the natural potential at a rate of 0.5 mV / s. The bending point (the region where the current suddenly stops flowing (passivation region) and the region where the current suddenly starts flowing) observed after a constant sweep of the polarization curve was determined as the pitting potential. In addition, since no bending point was observed in specimens containing a large amount of Zn, a bending potential of 0.1 mA / cm was used. 2 The potential was determined as the pitting potential (brazing material potential).

[0044] <Observation of recrystallized grains and measurement of grain size> The cross section of the brazed aluminum alloy parallel to the rolling direction was mechanically polished and anodized using Barker's solution. The recrystallized grains were photographed using an optical microscope, and the grain size was calculated by the formula: "grain size = length of line drawn on photograph / number of grains cut by line x photograph magnification." <Wax erosion assessment> For aluminum alloys brazed into a heat exchanger shape, erosion depth of 1 / 100 or less of the bare plate thickness before brazing or the core thickness of the brazing sheet was rated as excellent (◎), erosion depth of more than 1 / 100 to 1 / 20 or less was rated as good (○), and erosion depth of more than 1 / 20 to 1 / 10 of the plate thickness was rated as fair (△).

[0045] The following Tables 1 and 2 show the composition of the aluminum alloy bare materials No. A1 to A28 used in the evaluation of each test, the temperature (℃) and time (h) of the homogenization treatment, the electrical conductivity (%IACS) before and after brazing, and the number of compound particles (×10 4 pieces / mm 2 ), recrystallized grain size after brazing (μm), and braze erosion evaluation results are shown. Tables 3 and 4 show the brazing sheets of alloys B1 to B31 used in the evaluation of each test, the core alloy numbers used (corresponding to the aluminum alloy numbers shown in Tables 1 and 2), the results of measuring the electrical conductivity of the brazing sheets before and after brazing, the results of measuring the number of compound particles before and after brazing, the recrystallized grain size of the core material after brazing, the results of the brazing erosion assessment, the core material potential (mV vs Ag / AgCl), the brazing material potential (mV vs Ag / AgCl), and the potential difference between the brazing material and the core material. In addition, in each column of Tables 1 and 2, the notation "-" indicates that the corresponding component is not contained (less than the measurement limit).

[0046] [Table 1]

[0047] [Table 2]

[0048] [Table 3]

[0049] [Table 4]

[0050] The aluminum alloy bare materials of alloy Nos. A1 to A19 shown in Table 1 contain, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.7% or more and 1.4% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance being Al and unavoidable impurities. They have an electrical conductivity of 55% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is ​​1.0 × 10 4 ~3.0×10 4 pieces / mm 2 The aluminum alloy is characterized in that

[0051] The aluminum alloy bare materials of Alloy Nos. A1 to A19 showed excellent electrical conductivity of 55% IACS or more (55 to 63% IACS) before brazing and 44% IACS or more (44 to 64% IACS) after brazing. The bare aluminum alloys of alloy No. A1 to A19 had a compound particle count of 1.2×10 4 ~3.0×10 4 pieces / mm2 The range of compound particles after brazing is 1.1×10 4 ~2.9×10 4 pieces / mm 2 The range was shown. The aluminum alloy bare materials of Alloy Nos. A1 to A19 had recrystallized grain sizes in the range of 37 to 65 μm, which was sufficiently large, and therefore these alloys were capable of providing excellent evaluation results for brazing corrosion evaluation when brazed.

[0052] The aluminum alloy bare material of alloy No. A20 shown in Table 2 has a small Fe content, so the number of compound particles before and after brazing is small, the recrystallized grain size is fine, and excessive erosion occurs. The aluminum alloy bare material of alloy No. A21 had too much Fe content, so the number of compounds after brazing was too large, which promoted the cathodic reaction and reduced the self-corrosion resistance.

[0053] In the bare aluminum alloy No. A22, the Si content was low, so the ratio of Al-Fe compounds to Al-Fe-Si compounds increased, and the recrystallized grain size after brazing became too small, resulting in excessive erosion. The aluminum alloy bare material of alloy No. A23 had a high Si content, which lowered the melting point of the base material. As a result, it was excessively corroded by brazing during brazing, and the shape of the heat exchanger could not be maintained, so it could not be evaluated. The aluminum alloy bare material of alloy No. A24 had a low electrical conductivity after brazing because of the excessive Cu content.

[0054] The aluminum alloy bare material of alloy No. A25 had too much Mn and Zn content, so its electrical conductivity was low both before and after brazing. In the case of the bare aluminum alloy No. A26, the homogenization temperature was too low, so the number of compound particles was reduced both before and after brazing, and the electrical conductivity after brazing was reduced. In the case of the bare aluminum alloy material of alloy No. A27, the homogenization treatment time was too short, so the number of compound particles was reduced both before and after brazing, and the electrical conductivity after brazing was reduced. In the case of the bare aluminum alloy material of Alloy No. A28, the homogenization temperature was too high, so the number of compound particles decreased both before and after brazing, and the electrical conductivity decreased after brazing.

[0055] The brazing sheets of alloys B1 to A25 shown in Table 3 contain, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.7% or more and 1.4% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance being Al and unavoidable impurities. They have an electrical conductivity of 53% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is ​​1.0 × 10 4 ~3.0×10 4 pieces / mm 2 These brazing sheets are brazing sheets having a core material of Si. These brazing sheets are brazing sheets laminated with an aluminum alloy layer containing 3.0 to 12.0% by mass of Si as a brazing material, with the remainder being Al and unavoidable impurities.

[0056] The brazing sheets Nos. B1 to B25 have high electrical conductivity before and after brazing, the number of compound particles before and after brazing is in a suitable range, and the recrystallized grain size is also in a good range (37 to 65 μm). The brazing sheets Nos. B1 to B25 exhibited excellent electrical conductivity of 53% IACS or more (54 to 62% IACS) before brazing and 43% IACS or more (43 to 59% IACS) after brazing.

[0057] The brazing sheets No. B1 to B25 had a compound particle count of 1.0×10 4 ~3.0×10 4 pieces / mm 2 Range (1.2×10 4 ~3.0×10 4 pieces / mm 2 ), and the number of compound particles after brazing was 1.0×10 4 ~3.0×10 4 pieces / mm 2(1.1×10 4 ~2.9×10 4 pieces / mm 2 ) range is shown. Brazing sheets No. B1 to B25 have a potential difference between the core material potential after brazing and the brazing filler metal potential after brazing of 80 mV or more (81 to 268 mV), and the core material also has excellent corrosion resistance due to the sacrificial anode effect of the brazing filler metal.

[0058] The brazing sheet No. B26 shown in Table 4 has a core material of aluminum alloy No. A20 with a low Fe content, so the number of compound particles before and after brazing is small, and the desired recrystallized grain size is not obtained, resulting in a poor brazing erosion evaluation result. The brazing sheet No. B27 shown in Table 4 has a core material of the aluminum alloy No. A21 with too much Fe content, so the number of compound particles after brazing was increased and the self-corrosion resistance was reduced.

[0059] The brazing sheet No. B28 shown in Table 4 has a core material of the aluminum alloy No. A22, which has a low Si content, and therefore the recrystallized grain size was small, resulting in excessive erosion and a poor brazing corrosion evaluation result.

[0060] Brazing sheet No. B29 shown in Table 4 has a core of aluminum alloy No. A23, which has a high Si content, so the base material was excessively eroded by the brazing process and the shape of the heat exchanger could not be maintained, so it could not be evaluated. The brazing sheet No. B30 shown in Table 4 has a core material of the aluminum alloy No. A24, which has a high Cu content, and therefore the electrical conductivity before brazing was reduced. The brazing sheet No. B31 shown in Table 4 had a core material of the aluminum alloy No. A25, which had too much Mn and Zn, and therefore did not obtain the desired electrical conductivity and compound distribution, and the characteristics were not achieved.

[0061] Therefore, according to the present invention, it is possible to provide an aluminum alloy or an aluminum alloy brazing sheet for heat exchangers which has excellent electrical conductivity, the number of compounds before and after brazing is in an appropriate range, and has excellent brazing erosion evaluation properties. Furthermore, the aluminum alloy or brazing sheet according to the present invention has excellent electrical conductivity and excellent corrosion resistance, and therefore can be used as an aluminum alloy and brazing sheet suitable for use in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years. [Explanation of symbols]

[0062] A, B...aluminum alloy brazing sheet, M...aluminum alloy bare material, 1...core material, 2...filler material, 3...part to be brazed (fin), 5...heat exchanger, 6...fin, 7...tube.

Claims

1. The composition contains, by mass%, Fe: 0.6% or more and 0.8% or less, Si: more than 0.7% and 1.4% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance being Al and unavoidable impurities. The composition has an electrical conductivity of 55% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is ​​1.0×10 4 ~3.0 x 10 4 pieces / mm 2 1. An aluminum alloy bare material for a heat exchanger, comprising:

2. After subjecting a heat treatment equivalent to that for brazing a heat exchanger, which involves heating to 600°C, holding for 5 minutes, and then cooling to 300°C at 60°C / min, the material has an electrical conductivity of 44% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is ​​1.0 x 10 4 ~3.0 x 10 4 pieces / mm 2 2. The aluminum alloy bare material for heat exchangers according to claim 1,

3. 3. An aluminum alloy brazing sheet for heat exchangers, comprising the aluminum alloy for heat exchangers according to claim 1 or 2 as a core material, and an aluminum alloy layer containing, as a brazing material, 3.0 to 12.0% by mass of Si, the remainder being Al and unavoidable impurities, laminated on one or both surfaces of the core material.

4. 4. The aluminum alloy brazing sheet for heat exchangers according to claim 3, characterized in that the brazing material further contains, in mass %, Zn: 0.1 to 4.0%.

5. The core material has an electrical conductivity of 53% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the core material matrix is ​​1.0 × 10 4 ~3.0 x 10 4 pieces / mm 2 5. The aluminum alloy brazing sheet for heat exchangers according to claim 3 or 4,

6. After subjecting a heat treatment equivalent to brazing a heat exchanger, which involves heating to 600°C, holding for 5 minutes, and then cooling to 300°C at 60°C / min, the core material has an electrical conductivity of 43% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the core material matrix is ​​1.0 x 10 4 ~3.0 x 10 4 pieces / mm 2 The aluminum alloy brazing sheet for heat exchangers according to any one of claims 3 to 5, characterized in that

7. An aluminum alloy brazing sheet for heat exchangers as described in any one of claims 3 to 6, characterized in that after undergoing a heat treatment equivalent to heat exchanger brazing, which involves heating to 600°C, holding for 5 minutes, and then cooling to 300°C at 60°C / min, the pitting potential difference between the core material and the brazing material surface is 80 mV or more.

Citation Information

Patent Citations

  • Aluminum brazing sheet

    JP1992178291A

  • Aluminium fin material for brazing

    JP1993057460A

  • Manufacture of aluminum alloy brazing filler metal and heat exchanger made of aluminum alloy

    JP1995088682A

  • High strength and high thermal conduction aluminum alloy material, material fin for heat exchanger and method for producing the aluminum alloy material

    JP2002256365A

  • Aluminum alloy plate for plate fin

    JP2009161832A