Polarizer, method for producing polarizer, and optical laminate including said polarizer

The polarizer maintains neutral hue and durability by adhering to specific transmittance and hue parameters, achieved through a manufacturing process involving aerial stretching and drying shrinkage of a laminate with iodine, addressing the issue of increased transmittance in neutral hue polarizers.

JP7555880B2Active Publication Date: 2024-09-25NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021103749
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-23
Publication Date
2024-09-25
Estimated Expiration
2037-09-14

AI Technical Summary

Technical Problem

Existing polarizers with neutral hues tend to increase transmittance, leading to durability issues, and there is a need for a polarizer that maintains neutral hue without increasing transmittance.

Method used

A polarizer with a transmittance parameter of 0.8 or more and a hue parameter of 5 or less, manufactured through a process involving aerial stretching, dyeing, and drying shrinkage of a laminate of a thermoplastic resin base material and a polyvinyl alcohol resin layer, using iodine as the dichroic substance.

Benefits of technology

The polarizer achieves a neutral hue without increasing transmittance, enhancing durability and maintaining desired optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555880000013
    Figure 0007555880000013
  • Figure 0007555880000014
    Figure 0007555880000014
  • Figure 0007555880000015
    Figure 0007555880000015
Patent Text Reader

Abstract

To provide a polarizer with neutralized hue.SOLUTION: A polarizer of the present invention is characterized in that a transmittance parameter represented by a formula (1) below is 0.8 or grater, and a hue parameter represented by a formula (2) below is 5 or less. In the formula (1), T420 and T550 respectively represent a parallel transmittance at a wavelength of 420 nm and a parallel transmittance at a wavelength of 550 nm. In the formula (2), a represents "a" parallel hue a value and "b" represents a parallel hue b value.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizer, a method for producing a polarizer, and an optical laminate including the polarizer. [Background technology]

[0002] Polarizers are used in display devices such as liquid crystal display devices. In recent years, polarizers with better characteristics are in demand. For example, in order to make the colors of a displayed image clearer, polarizers with a neutral hue are in demand. However, when the hue of a polarizer is neutralized, the transmittance of the polarizer tends to increase. A polarizer with a high transmittance may have durability problems. In addition, a method has been proposed for obtaining a hue-neutral polarizer by using a dichroic substance having an absorption maximum in a specific wavelength range (Patent Document 1). Even when the hue is neutralized by using such a dichroic substance, the transmittance of the polarizer tends to be high. Therefore, a polarizer with a neutral hue without increasing the transmittance is in demand. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-210624 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the present invention is to provide a polarizer having a neutral hue without increasing the transmittance. [Means for solving the problem]

[0005] The polarizer of the present invention has a transmittance parameter represented by formula (1) of 0.8 or more and a hue parameter represented by formula (2) of 5 or less.

number

number

[0006] According to the present invention, a polarizer with a neutralized hue can be provided. More specifically, the polarizer of the present invention has a transmittance parameter of 0.8 or more and a hue parameter of 5 or less. A polarizer that satisfies such parameters has a neutralized hue. Furthermore, the hue of the polarizer of the present invention can be neutralized by reducing the thickness of the polarizer. Therefore, the hue can be neutralized without increasing the transmittance of the polarizer. Therefore, according to the present invention, a polarizer having a desired transmittance and a neutralized hue can be provided. Furthermore, a decrease in the durability of the polarizer can be prevented. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a schematic diagram showing an example of a drying shrinkage treatment using a heating roll. [Diagram 2] 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram illustrating a method for measuring front white luminance (a) and front black luminance (b). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Preferred embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.

[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(550)" is the in-plane retardation of a film measured at 23°C with light of 550 nm wavelength. Re(550) is calculated by the formula: Re = (nx-ny) x d, where d (nm) is the thickness of the film. "Re(450)" is the in-plane retardation of a film measured at 23°C with light of 450 nm wavelength. (3) Retardation in the thickness direction (Rth) "Rth(550)" is the retardation in the thickness direction of the film measured at 23°C with light of 550 nm wavelength. Rth(550) is calculated by the formula: Rth = (nx-nz) x d, where d (nm) is the thickness of the film. "Rth(450)" is the retardation in the thickness direction of the film measured at 23°C with light of 450 nm wavelength. (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re.

[0010] A. Polarizer The polarizer of the present invention has a transmittance parameter of 0.8 or more and a hue parameter of not more than 5. When the polarizer satisfies such parameters, a polarizer with a neutral hue can be obtained.

[0011] The transmittance parameter is a value calculated from the following formula (1). In formula (1), T 420 is the parallel transmittance (H0) at a wavelength of 420 nm, and T 550 and r each represent the parallel transmittance (H0) at a wavelength of 550 nm. The transmittance parameter of the polarizer of the present invention is 0.8 or more, and preferably 0.85 or more. The transmittance parameter is preferably closer to 1 because the hue is more neutralized. The transmittance parameter is, for example, 1.0 or less. The parallel transmittance is the transmittance value of a parallel laminated polarizer produced by overlapping two identical polarizers so that their absorption axes are parallel to each other. The parallel transmittance of a polarizer is measured, for example, using a spectrophotometer (manufactured by JASCO Corporation, product name "V-7100"). These transmittances are Y values ​​corrected for luminosity using a 2-degree visual field (C light source) according to JIS Z 8701-1982.

number

[0012] The hue parameter is a value calculated from the following formula (2). In formula (2), a represents the parallel hue a value, and b represents the parallel hue b value. The hue parameter of the polarizer of the present invention is 5 or less, and preferably 4.5 or less. The hue parameter is preferably closer to 0 because the hue of the polarizer is more neutral. The hue parameter is, for example, 1.0 or more. In this specification, the parallel hue a value and the parallel hue b value refer to the hue a value and the b value measured using the parallel laminated polarizer. The hue a value and the hue b value refer to the single hue according to the National Bureau of Standards (NBS). The hue a value and the hue b value can be measured using a spectrophotometer (manufactured by JASCO Corporation, product name "V-7100").

number

[0013] The thickness of the polarizer is preferably 8 μm or less, more preferably 5 μm or less. By setting the thickness of the polarizer in this range, a polarizer with a more neutral hue can be obtained. The thickness of the polarizer is preferably 1.0 μm or more, more preferably 2.0 μm or more.

[0014] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is preferably 40.0% or more, more preferably 41% or more, even more preferably 42.0% or more, still more preferably 42.5% or more, and particularly preferably 43.0% or more. The single transmittance is, for example, 50% or less.

[0015] The parallel transmittance (H0) of the polarizer at a wavelength of 420 nm is preferably 20% to 40%, and more preferably 22% to 38%. By having such characteristics, a polarizer with a more neutral hue can be obtained. The parallel transmittance (H0) is as described above. Note that this transmittance is a Y value corrected for luminous efficiency using a 2-degree visual field (C light source) according to JIS Z 8701-1982.

[0016] The degree of polarization of the polarizer is preferably 99.8% or more, more preferably 99.9% or more, and even more preferably 99.95% or more. The degree of polarization (P) is calculated by measuring the single transmittance (Ts), parallel transmittance (Tp) and crossed transmittance (Tc) and using the following formula. Here, Ts, Tp and Tc are Y values ​​measured using a 2-degree visual field (C light source) according to JIS Z 8701 and corrected for visibility. Polarization degree (P)(%)={(Tp-Tc) / (Tp+Tc)}1 / 2×100

[0017] The single hue a of the polarizer measured by NBS is -1.2 to 0, and preferably -1.0 to 0. The single hue b of the polarizer measured by NBS is 0 to 3.0, and preferably 0 to 2.5. The closer the single hue a value and single hue b value of the polarizer are to 0, the more vivid the color of the displayed image can be obtained. Therefore, the ideal values ​​of the single hue a value and single hue b value are 0.

[0018] The polarizer of the present invention is composed of a resin film containing a polyvinyl alcohol-based resin (hereinafter referred to as a "PVA-based resin"). Examples of PVA-based resins include polyvinyl alcohol and ethylene-vinyl alcohol copolymers. Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymers are obtained by saponifying ethylene-vinyl acetate copolymers.

[0019] The saponification degree of the PVA resin is usually 85 mol% or more, preferably 95.0 mol% or more, and more preferably 99.0 mol% or more. The saponification degree is 100 mol% or less, preferably 99.95 mol% or less, and more preferably 99.93 mol% or less. When the PVA resin contained in the polarizer satisfies such a saponification degree, excellent humidification reliability can be achieved. The saponification degree can be determined in accordance with JIS K 6726-1994.

[0020] The average degree of polymerization of the PVA resin can be appropriately selected depending on the purpose. The average degree of polymerization is usually 1000 to 10000, preferably 1200 to 6000, and more preferably 2000 to 5000. The average degree of polymerization can be determined in accordance with JIS K 6726-1994.

[0021] The polarizer typically contains a dichroic material. Specific examples of the dichroic material include iodine and organic dyes. These may be used alone or in combination of two or more. As the dichroic material, iodine is preferably used.

[0022] B. How to make a polarizer The polarizer can be produced by any appropriate method. The polarizer can be obtained by subjecting a resin film to various treatments, such as swelling, stretching, dyeing, insolubilization, crosslinking, washing, and drying. In one embodiment, when the resin film is subjected to various treatments, the resin film may be a resin layer formed on a substrate. A laminate of a substrate and a resin layer can be obtained by, for example, a method of applying a coating liquid containing a material for forming the resin film to the substrate, a method of laminating a resin film on the substrate, or the like.

[0023] In the method for producing a polarizer of the present invention, a laminate of a thermoplastic resin substrate and a polyvinyl alcohol-based resin is preferably subjected to an air-stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. In this laminate, the PVA-based resin layer preferably contains a halide and a PVA-based resin. The method for producing a polarizer of the present invention may also include any other appropriate steps. Examples of the other steps include an insolubilization treatment, a crosslinking treatment, and a cleaning treatment. These treatments may be performed at any appropriate stage in the method for producing a polarizer.

[0024] B-1. Preparation of laminate The laminate can be obtained by any suitable method. For example, it can be obtained by forming a PVA-based resin layer containing a halide and a PVA-based resin on one side of a thermoplastic resin substrate. The PVA-based resin layer can be formed by any suitable method. It is preferably formed by applying a coating liquid containing a halide and a PVA-based resin to one side of a long-sized thermoplastic resin substrate and drying it. By using a long-sized thermoplastic resin, the laminate can be continuously subjected to processing while being transported. In this specification, "long-sized" means an elongated shape in which the length is sufficiently long relative to the width.

[0025] B-1-1. Thermoplastic resin base material Any suitable forming material (thermoplastic resin) can be used as the forming material of the thermoplastic resin substrate. For example, ester-based resins such as polyethylene terephthalate-based resins, cycloolefin-based resins such as norbornene-based resins, olefin-based resins such as polypropylene, (meth)acrylic resins, polyamide-based resins, polycarbonate-based resins, and copolymer resins thereof can be mentioned. Among these, norbornene-based resins and amorphous polyethylene terephthalate-based resins are preferable.

[0026] In one embodiment, amorphous (uncrystallized) polyethylene terephthalate resins are preferably used. Among them, amorphous (hard to crystallize) polyethylene terephthalate resins are particularly preferably used. Specific examples of amorphous polyethylene terephthalate resins include copolymers further containing isophthalic acid and / or cyclohexanedicarboxylic acid as dicarboxylic acids, and copolymers further containing cyclohexanedimethanol and / or diethylene glycol as glycols.

[0027] In a preferred embodiment, the thermoplastic resin substrate is made of a polyethylene terephthalate resin having an isophthalic acid unit. This is because such a thermoplastic resin substrate has excellent stretchability and can suppress crystallization during stretching. This is believed to be because the introduction of the isophthalic acid unit imparts a large bend to the main chain.

[0028] The polyethylene terephthalate resin has a terephthalic acid unit and an ethylene glycol unit. The content of the isophthalic acid unit is preferably 0.1 mol% or more, more preferably 1.0 mol% or more, based on the total of all repeating units. This is because a thermoplastic resin substrate with extremely excellent stretchability can be obtained. On the other hand, the content of the isophthalic acid unit is preferably 20 mol% or less, more preferably 10 mol% or less, based on the total of all repeating units. By setting such a content ratio, the crystallinity can be satisfactorily increased in the drying shrinkage treatment described below.

[0029] The thickness of the thermoplastic resin substrate is preferably 20 μm to 300 μm, more preferably 50 μm to 200 μm. If the thickness is less than 20 μm, it may be difficult to form a PVA-based resin layer. If the thickness exceeds 300 μm, for example, in the underwater stretching treatment described below, it may take a long time for the thermoplastic resin substrate to absorb water, and an excessive load may be required for stretching. The surface of the thermoplastic resin substrate may be subjected to a surface modification treatment (for example, corona treatment, etc.), or an easy-adhesion layer may be formed. By such a treatment, a laminate having excellent adhesion between the thermoplastic resin substrate and the resin layer can be obtained.

[0030] The glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 120° C. or lower, more preferably 100° C. or lower, and even more preferably 90° C. or lower. This is because, when the laminate is stretched, the stretchability can be sufficiently ensured while suppressing the crystallization of the resin layer (PVA-based resin). As a result, a polarizer having excellent polarization properties can be produced. On the other hand, the glass transition temperature of the thermoplastic resin substrate is preferably 60° C. or higher. By using such a thermoplastic resin substrate, defects such as deformation of the thermoplastic resin substrate (e.g., generation of unevenness, sagging, wrinkles, etc.) during application and drying of the coating liquid containing the PVA-based resin can be prevented, and a laminate can be produced satisfactorily. In addition, the stretching of the PVA-based resin layer can be satisfactorily performed at a suitable temperature (e.g., about 60° C.). The glass transition temperature of the thermoplastic resin substrate can be adjusted, for example, by introducing a modifying group into the constituent material and / or by heating using a crystallizing material. The glass transition temperature (Tg) is a value determined in accordance with JIS K 7121.

[0031] The thermoplastic resin substrate preferably has a water absorption rate of 0.2% or more, more preferably 0.3% or more. The thermoplastic resin substrate absorbs water, and the water acts as a plasticizer to plasticize the substrate. As a result, the stretching stress can be significantly reduced, and the substrate can be stretched at a high ratio. On the other hand, the water absorption rate of the thermoplastic resin substrate is preferably 3.0% or less, more preferably 1.0% or less. By using such a thermoplastic resin substrate, it is possible to prevent problems such as a significant decrease in the dimensional stability of the thermoplastic resin substrate during production, which leads to a deterioration in the appearance of the obtained polarizer. In addition, it is possible to prevent the thermoplastic resin substrate from breaking during underwater stretching, and the PVA-based resin layer from peeling off from the thermoplastic resin substrate. The water absorption rate of the thermoplastic resin substrate can be adjusted, for example, by introducing a modifying group into the constituent material. The water absorption rate is a value determined in accordance with JIS K 7209.

[0032] The thermoplastic resin substrate may be stretched in advance (before forming the PVA-based resin layer described later). In one embodiment, the thermoplastic resin substrate is stretched in the lateral direction (direction perpendicular to the longitudinal direction) of the long-sized thermoplastic resin substrate. The lateral direction is preferably a direction perpendicular to the stretching direction of the laminate described later. In this specification, "perpendicular" also includes the case where the direction is substantially perpendicular. Here, "substantially perpendicular" includes the case where the direction is 90°±5.0°, and is preferably 90°±3.0°, and more preferably 90°±1.0°.

[0033] The stretching temperature of the thermoplastic resin substrate is preferably from the glass transition temperature (Tg) of Tg-10° C. to Tg+50° C. The stretching ratio of the thermoplastic resin substrate is preferably from 1.5 to 3.0 times.

[0034] Any suitable method may be adopted as the stretching method of the thermoplastic resin substrate. Specifically, it may be fixed-end stretching or free-end stretching. The stretching method may be dry stretching or wet stretching. The stretching of the thermoplastic resin substrate may be performed in one stage or multiple stages. When it is performed in multiple stages, the above-mentioned stretching ratio is the product of the stretching ratios in each stage.

[0035] B-1-2. Coating solution As described above, the coating liquid contains a halide and a PVA-based resin. The coating liquid is typically a solution in which the halide and the PVA-based resin are dissolved in a solvent. As the PVA-based resin, those disclosed in Section A can be used. The content of the PVA-based resin in the coating liquid is preferably 3 to 20 parts by weight per 100 parts by weight of the solvent. With such a content, a uniform coating film that is in close contact with the thermoplastic resin substrate can be formed.

[0036] Any suitable halide may be used as the halide. For example, iodide and sodium chloride may be used. For example, iodide may be potassium iodide, sodium iodide, and lithium iodide. Among these, potassium iodide is preferred.

[0037] The content of the halide in the coating solution is preferably 5 to 20 parts by weight per 100 parts by weight of the PVA-based resin, and more preferably 10 to 15 parts by weight per 100 parts by weight of the PVA-based resin. If the content of the halide exceeds 20 parts by weight per 100 parts by weight of the PVA-based resin, the halide may bleed out, causing the finally obtained polarizer to become cloudy.

[0038] Any suitable solvent can be used for the coating liquid. For example, water, dimethylsulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine are listed. Among these, water is preferable. The solvent may be used alone or in combination of two or more.

[0039] The coating liquid may contain additives other than the PVA-based resin and the halide. Any suitable additives can be used as the additives. Examples of the additives include plasticizers and surfactants. Examples of the plasticizers include polyhydric alcohols such as ethylene glycol and glycerin. Examples of the surfactants include nonionic surfactants. These can be used for the purpose of further improving the uniformity, dyeability, and stretchability of the resulting PVA-based resin layer.

[0040] B-2. Air stretching process As described above, the laminate is subjected to air-stretching, dyeing, underwater stretching, and drying shrinkage in this order. Generally, the orientation of polyvinyl alcohol molecules in the PVA-based resin increases when the PVA-based resin layer is stretched, but when the stretched PVA-based resin layer is immersed in a liquid containing water, the orientation of the polyvinyl alcohol molecules may be disturbed and the orientation may decrease. In particular, when underwater stretching is performed in boric acid water and the laminate is stretched in boric acid water at a relatively high temperature to stabilize the stretching of the thermoplastic resin, the tendency of the orientation degree to decrease is remarkable. For example, the stretching of a PVA film alone in boric acid water is generally performed at 60°C, whereas the stretching of a laminate of A-PET (thermoplastic resin substrate) and a PVA-based resin layer is performed at a high temperature of around 70°C. In this case, the orientation of PVA at the beginning of stretching may decrease before the orientation increases due to underwater stretching. In response to this, by performing high-temperature stretching (auxiliary stretching) in air before stretching a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate in boric acid water, crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules can be prevented from being disturbed and the orientation can be prevented from being reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained by immersing the laminate in a liquid through a treatment process, such as a dyeing treatment and an underwater stretching treatment.

[0041] In particular, in order to obtain high optical properties, a two-stage stretching method is selected that combines air stretching (auxiliary stretching) and stretching in boric acid water. By introducing auxiliary stretching like two-stage stretching, it is possible to stretch while suppressing crystallization of the thermoplastic resin substrate. Therefore, the problem of the thermoplastic resin substrate being excessively crystallized and reduced in stretchability in the subsequent boric acid water stretching is solved, and the laminate can be stretched at a higher magnification. Furthermore, when applying a PVA-based resin onto a thermoplastic resin substrate, it is necessary to lower the application temperature compared to when applying a PVA-based resin onto a normal metal drum in order to suppress the influence of the glass transition temperature of the thermoplastic resin substrate. As a result, the crystallization of the PVA-based resin becomes relatively low, and a problem of insufficient optical properties can be obtained. In contrast, by introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA-based resin even when applying a PVA-based resin onto a thermoplastic resin, and it is possible to achieve high optical properties. At the same time, by increasing the orientation of the PVA-based resin in advance, problems such as a decrease in the orientation or dissolution of the PVA-based resin when it is immersed in water in the subsequent dyeing process or underwater stretching process can be prevented, making it possible to achieve high optical properties.

[0042] The method of in-air stretching (hereinafter also referred to as auxiliary in-air stretching) may be fixed-end stretching (for example, a method of stretching using a tenter stretching machine) or free-end stretching (for example, a method of uniaxially stretching a laminate between rolls having different peripheral speeds). In order to obtain high optical properties, free-end stretching may be actively adopted. In one embodiment, the in-air stretching process includes a heated roll stretching process in which the laminate is stretched by the difference in peripheral speed between heated rolls while being transported in its longitudinal direction. The in-air stretching process typically includes a zone stretching process and a heated roll stretching process. The order of the zone stretching process and the heated roll stretching process is not limited, and the zone stretching process may be performed first, or the heated roll stretching process may be performed first. The zone stretching process may be omitted. In one embodiment, the zone stretching process and the heated roll stretching process are performed in this order. In another embodiment, the film is stretched in a tenter stretching machine by gripping the film ends and widening the distance between the tenters in the machine direction (the increase in the distance between the tenters is the stretching ratio). At this time, the distance between the tenters in the width direction (perpendicular to the machine direction) is set to be arbitrarily close. Preferably, it can be set to be closer to the free end stretching ratio in the machine direction. In the case of free end stretching, the shrinkage ratio in the width direction = (1 / stretching ratio) 1 / 2 It is calculated as follows.

[0043] The auxiliary air-drawing may be performed in one step or in multiple steps. When the auxiliary air-drawing is performed in multiple steps, the draw ratio is the product of the draw ratios in each step. The draw direction in the auxiliary air-drawing is preferably approximately the same as the draw direction in the underwater drawing.

[0044] The stretching ratio in the auxiliary in-air stretching is preferably 2.0 to 3.5 times. The maximum stretching ratio in the case where the auxiliary in-air stretching and the underwater stretching are combined is preferably 5.0 times or more, more preferably 5.5 times or more, and even more preferably 6.0 times or more, based on the original length of the laminate. In this specification, the "maximum stretching ratio" refers to the stretching ratio just before the laminate breaks, and refers to a value 0.2 lower than the stretching ratio at which the laminate breaks, which is determined separately.

[0045] The stretching temperature of the auxiliary in-air stretching can be set to any appropriate value depending on the material of the thermoplastic resin substrate, the stretching method, etc. The stretching temperature is preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate, more preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate + 10°C, and even more preferably equal to or higher than Tg + 15°C. Meanwhile, the stretching temperature is preferably equal to or lower than 170°C. By stretching at such a temperature, rapid crystallization of the PVA resin can be suppressed, and defects due to the crystallization (for example, the orientation of the PVA resin layer due to stretching is hindered) can be suppressed.

[0046] B-3. ​​Insolubilization treatment If necessary, after the auxiliary air stretching treatment and before the dyeing treatment and the underwater stretching treatment, the laminate is subjected to an insolubilization treatment. The insolubilization treatment is typically performed by immersing the PVA-based resin layer (laminate) in an aqueous boric acid solution. By performing the insolubilization treatment, water resistance is imparted to the PVA-based resin layer, and it is possible to prevent a decrease in the orientation of PVA when immersed in water. The concentration of the aqueous boric acid solution is preferably 1 part by weight to 4 parts by weight with respect to 100 parts by weight of water. The liquid temperature of the insolubilization bath (aqueous boric acid solution) is preferably 20°C to 50°C.

[0047] B-4. Dyeing process The dyeing treatment is preferably carried out by adsorbing the dichroic substance. Examples of the adsorption method include a method of immersing the PVA-based resin layer (laminate) in a dyeing solution containing the dichroic substance, a method of applying the dyeing solution to the PVA-based resin layer, and a method of spraying the dyeing solution onto the PVA-based resin layer. A method of immersing the PVA-based resin layer (laminate) in the dyeing solution is preferred, because the dichroic substance can be well adsorbed.

[0048] When iodine is used as the dichroic material, an iodine aqueous solution is preferably used as the dye solution. The amount of iodine is preferably 0.05 to 5.0 parts by weight relative to 100 parts by weight of water. In order to increase the solubility of iodine in water, it is preferable to add an iodide to the iodine aqueous solution. Examples of iodides include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. Potassium iodide is preferably used as the iodide. The amount of iodide is preferably 0.1 to 10 parts by weight, more preferably 0.3 to 5 parts by weight, relative to 100 parts by weight of water. When an aqueous iodine solution containing potassium iodide is used as the staining solution, the content ratio of iodine to potassium iodide in the aqueous iodine solution is preferably 1:5 to 1:20, and more preferably 1:5 to 1:10.

[0049] The temperature of the dye solution during dyeing is preferably 20° C. to 50° C. When dyeing is performed by immersion, the immersion time is preferably 5 seconds to 5 minutes, and more preferably 30 seconds to 90 seconds. The dyeing conditions (concentration, solution temperature, immersion time) can be set so that the polarization degree or single transmittance of the finally obtained polarizer falls within a desired range.

[0050] B-5. Crosslinking treatment If necessary, after the dyeing process and before the underwater stretching process, the PVA-based resin layer is subjected to a crosslinking process. The crosslinking process is typically performed by immersing the PVA-based resin layer in an aqueous boric acid solution. The crosslinking process imparts water resistance to the PVA-based resin layer, and prevents the orientation of the PVA from decreasing when the layer is immersed in high-temperature water in the subsequent underwater stretching process. The concentration of the aqueous boric acid solution is preferably 1 to 5 parts by weight per 100 parts by weight of water. In addition, when the crosslinking process is performed after the dyeing process, it is preferable that the aqueous boric acid solution contains an iodide. By blending an iodide, it is possible to suppress the elution of iodine adsorbed to the PVA-based resin layer. The blending amount of the iodide is preferably 1 to 5 parts by weight per 100 parts by weight of water. Specific examples of the iodide are as described above. The liquid temperature of the crosslinking bath (aqueous boric acid solution) is preferably 20°C to 50°C.

[0051] B-6. Underwater stretching treatment The underwater stretching treatment is carried out by immersing the laminate in a stretching bath. According to the underwater stretching treatment, the laminate can be stretched at a temperature lower than the glass transition temperature (typically about 80°C) of the thermoplastic resin substrate and / or the PVA-based resin layer, and the PVA-based resin layer can be stretched at a high magnification while suppressing crystallization. As a result, a polarizer having excellent optical properties can be produced.

[0052] The stretching method of the laminate can be any appropriate method. Specifically, it may be fixed-end stretching or free-end stretching (for example, a method of uniaxially stretching the laminate by passing it between rolls having different peripheral speeds). Preferably, free-end stretching is selected. The stretching of the laminate may be performed in one stage or multiple stages. When performing the stretching in multiple stages, the stretching ratio (maximum stretching ratio) of the laminate described below is the product of the stretching ratios in each stage.

[0053] The underwater stretching is preferably performed by immersing the laminate in an aqueous solution of boric acid (stretching in boric acid water). By using an aqueous solution of boric acid as a stretching bath, it is possible to impart to the PVA-based resin layer rigidity capable of withstanding the tension applied during stretching and water resistance that does not dissolve in water. Specifically, boric acid can generate tetrahydroxyborate anions in the aqueous solution and crosslink with the PVA-based resin through hydrogen bonds. As a result, it is possible to impart rigidity and water resistance to the PVA-based resin layer and stretch it well, and to produce a polarizer having excellent optical properties.

[0054] The boric acid aqueous solution is preferably obtained by dissolving boric acid and / or a borate in water as a solvent. The boric acid concentration of the boric acid aqueous solution is preferably 1 to 10 parts by weight, more preferably 2.5 to 6 parts by weight, and even more preferably 3 to 5 parts by weight, relative to 100 parts by weight of water. By setting the boric acid concentration to 1 part by weight or more, dissolution of the PVA-based resin layer can be effectively suppressed, and a polarizer with higher characteristics can be produced. In addition to boric acid or a borate, an aqueous solution obtained by dissolving a boron compound such as borax, glyoxal, glutaraldehyde, or the like in a solvent can also be used.

[0055] Preferably, an iodide is further added to the stretching bath (boric acid aqueous solution). By adding an iodide, it is possible to suppress the elution of iodine adsorbed in the PVA resin layer. Specific examples of the iodide are as described above. The concentration of the iodide is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 8 parts by weight, relative to 100 parts by weight of water.

[0056] The stretching temperature (liquid temperature of the stretching bath) is preferably 40°C to 85°C, more preferably 60°C to 75°C. At such a temperature, the laminate can be stretched at a high ratio while suppressing dissolution of the PVA-based resin layer. Specifically, as described above, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 60°C or higher in relation to the formation of the PVA-based resin layer. In this case, if the stretching temperature is lower than 40°C, there is a risk that the substrate cannot be stretched well even when considering the plasticization of the thermoplastic resin substrate by water. On the other hand, the higher the temperature of the stretching bath, the higher the solubility of the PVA-based resin layer, and there is a risk that excellent optical properties cannot be obtained. The immersion time of the laminate in the stretching bath is preferably 15 seconds to 5 minutes.

[0057] The stretching ratio in the underwater stretching is preferably 1.5 times or more, more preferably 3.0 times or more. The total stretching ratio of the laminate is preferably 5.0 times or more, more preferably 5.5 times or more, based on the original length of the laminate. By achieving such a high stretching ratio, a polarizer with extremely excellent optical properties can be produced. Such a high stretching ratio can be achieved by employing an underwater stretching method (stretching in boric acid water).

[0058] B-7. Cleaning process Preferably, after the underwater stretching treatment and before the drying shrinkage treatment, the resin film is subjected to a washing treatment, typically by immersing the resin film in an aqueous potassium iodide solution.

[0059] B-8. Drying shrinkage treatment The drying shrinkage treatment may be performed by zone heating in which the entire zone is heated, or by heating the transport roll (using a so-called heating roll) (heat roll drying method). Preferably, both are used. By drying using a heating roll, it is possible to efficiently suppress the heat curl of the laminate and produce a polarizer with excellent appearance. Specifically, by drying the laminate in a state where it is aligned with the heating roll, it is possible to efficiently promote the crystallization of the thermoplastic resin substrate and increase the crystallinity, and even at a relatively low drying temperature, it is possible to satisfactorily increase the crystallinity of the thermoplastic resin substrate. As a result, the rigidity of the thermoplastic resin substrate increases and it becomes in a state where it can withstand the shrinkage of the PVA-based resin layer due to drying, and curling is suppressed. In addition, by using a heating roll, it is possible to dry the laminate while maintaining it in a flat state, so that not only curling but also wrinkles can be suppressed.

[0060] The drying shrinkage treatment is preferably carried out by heating the laminate while transporting it in the longitudinal direction. At this time, the laminate may shrink in the width direction by the drying shrinkage treatment. As a result, the optical properties can be improved. This is because the orientation of the PVA and the PVA / iodine complex can be effectively increased by shrinkage. The shrinkage rate of the laminate in the width direction by the drying shrinkage treatment is preferably 1% or more, more preferably 2% or more, and even more preferably 4% or more. In addition, the shrinkage rate of the laminate in the width direction is preferably 10% or less, more preferably 8% or less, and even more preferably 6% or less.

[0061] 1 is a schematic diagram showing an example of the drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by transport rolls R1 to R6 heated to a predetermined temperature and guide rolls G1 to G4. In the illustrated example, the transport rolls R1 to R6 are arranged so as to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rolls R1 to R6 may be arranged so as to continuously heat only one surface of the laminate 200 (for example, the thermoplastic resin substrate surface).

[0062] Drying conditions can be controlled by adjusting the heating temperature of the transport rolls (temperature of the heating rolls), the number of heating rolls, contact time with the heating rolls, etc. The temperature of the heating rolls is preferably 60°C to 120°C, more preferably 65°C to 100°C, and even more preferably 70°C to 80°C. The crystallinity of the thermoplastic resin can be increased well, curling can be suppressed well, and an optical laminate with extremely excellent durability can be produced. The temperature of the heating rolls can be measured by a contact thermometer. In the illustrated example, six transport rolls are provided, but there is no particular restriction as long as there are multiple transport rolls. The number of transport rolls is usually 2 to 40, preferably 4 to 30. The contact time (total contact time) between the laminate and the heating rolls is preferably 1 to 300 seconds, more preferably 1 to 20 seconds, and even more preferably 1 to 10 seconds.

[0063] The heating roll may be provided in a heating furnace (for example, an oven) or in a normal production line (under room temperature environment). It is preferably provided in a heating furnace equipped with a blowing means. By using drying with a heating roll in combination with hot air drying, it is possible to suppress a steep temperature change between the heating rolls, and it is possible to easily control the shrinkage in the width direction. The hot air drying temperature is preferably 30°C to 100°C. In addition, the hot air drying time is preferably 1 second to 300 seconds. The hot air speed is preferably about 10 m / sec to 30 m / sec. The wind speed is the wind speed in the heating furnace, and can be measured by a mini-vane type digital anemometer.

[0064] C. Overall configuration of optical laminate The optical laminate of the present invention includes the polarizer and a light diffusing layer. The optical laminate may include any other appropriate layer depending on the application. Examples of the other layer include a retardation layer, a surface treatment layer (e.g., an anti-reflection layer, an anti-glare layer, a hard coat layer), etc.

[0065] In one embodiment, the optical laminate of the present invention includes the polarizer, a retardation layer that substantially functions as a λ / 4 plate, and a light diffusion layer. FIG. 2 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. This optical laminate 100 includes a polarizer 10, a retardation layer 20 that substantially functions as a λ / 4 plate, and a light diffusion layer 30. As described above, the polarizer 10 has a transmittance parameter of 0.8 or more and a hue parameter of 5 or less. By including such a polarizer, an optical laminate that can provide a liquid crystal display device having excellent display characteristics (for example, vivid colors, excellent reflection hue, viewing angle characteristics, etc.) can be obtained.

[0066] In the illustrated example, the optical laminate 100 includes only one light diffusion layer 30, but may include two or more light diffusion layers. For example, a light diffusion layer may be further provided between the polarizer 10 and the retardation layer 20. The retardation layer 20 may be a single layer or may have a laminated structure. Although not illustrated, each of the above layers may be laminated via an adhesive layer (adhesive layer or pressure-sensitive adhesive layer). In one embodiment, the light diffusion layer 30 is a light diffusion pressure-sensitive adhesive layer. In this embodiment, the light diffusion layer also functions as an adhesive layer. The optical laminate 100 may further include any other appropriate layer. Examples of the other layers include those described above.

[0067] The thickness of the optical laminate can be set to any appropriate value, typically about 40 μm to 300 μm.

[0068] C-1. Light diffusion layer The light diffusion layer 30 may be composed of a light diffusion element, or may be composed of a light diffusion adhesive or a light diffusion adhesive. The light diffusion element includes a matrix and light diffusion fine particles dispersed in the matrix. The light diffusion element may be a light diffusion cured layer (for example, formed by applying a dispersion liquid (light diffusion layer forming coating liquid) containing a matrix resin, light diffusion fine particles, and additives as necessary, onto any appropriate substrate, and curing and / or drying it), or may be a light diffusion film (for example, a commercially available film). The light diffusion adhesive has a matrix composed of an adhesive, and the light diffusion adhesive has a matrix composed of an adhesive.

[0069] The light diffusion performance of the light diffusion layer can be expressed by, for example, a haze value. The haze value can be set to any appropriate value depending on the application in which the optical laminate is used. For example, when used in a reflective liquid crystal display device, the haze value of the light diffusion layer is preferably 80% or more, more preferably 80% to 98%, and even more preferably 85% to 98%. When used in a transmissive liquid crystal display device, the haze value of the light diffusion layer is preferably 20% or more, more preferably 20% to 80%, and even more preferably 20% to 60%. By setting the haze value in the above range, a display device with excellent viewing angle characteristics can be provided. The haze value of the light diffusion layer can be controlled by adjusting the constituent material of the matrix (adhesive), and the constituent material, volume average particle diameter, and blending amount of the light diffusing fine particles.

[0070] The total light transmittance of the light diffusing layer is preferably 75% or more, more preferably 80% or more, and further preferably 85% or more.

[0071] The thickness of the light diffusion layer can be appropriately adjusted depending on the configuration, the desired light diffusion performance, etc. Specifically, the thickness of the light diffusion layer is preferably 5 μm to 100 μm, and more preferably 10 μm to 30 μm.

[0072] In one embodiment, the light diffusion layer 30 is made of a light diffusion adhesive. The light diffusion adhesive typically contains an adhesive as a matrix and light diffusing fine particles dispersed in the adhesive. By making the light diffusion layer out of a light diffusion adhesive, it is possible to omit an adhesive layer (adhesive layer or adhesive layer) used when bonding other components such as a polarizer and / or a retardation layer, which can contribute to making the display device thinner.

[0073] Any suitable adhesive (matrix) can be used. Specific examples of the adhesive include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, epoxy-based adhesives, and cellulose-based adhesives, and preferably acrylic-based adhesives. By using an acrylic-based adhesive, a light diffusion layer having excellent heat resistance and transparency can be obtained. The adhesive may be used alone or in combination of two or more kinds.

[0074] Any appropriate acrylic adhesive can be used. The glass transition temperature of the acrylic adhesive is preferably from -60°C to -10°C, more preferably from -55°C to -15°C. The weight average molecular weight of the acrylic adhesive is preferably from 200,000 to 3,000,000, more preferably from 250,000 to 2,800,000. By using an acrylic adhesive having such properties, appropriate adhesion can be obtained.

[0075] The refractive index of the acrylic pressure-sensitive adhesive is preferably 1.40 to 1.65, and more preferably 1.45 to 1.60.

[0076] The acrylic adhesive is usually obtained by polymerizing a main monomer that provides adhesion, a comonomer that provides cohesiveness, and a functional group-containing monomer that provides adhesion and serves as a crosslinking point. The acrylic adhesive having the above characteristics can be synthesized by any suitable method, for example, by referring to "Chemistry and Applications of Adhesion and Adhesion" by Katsuhiko Nakamae, published by Dai Nippon Tosho Co., Ltd. In addition, an adhesive that is applied to a light-diffusing adhesive layer disclosed in JP 2014-224964 A may be used. The description of this document is incorporated herein by reference.

[0077] The content of the pressure-sensitive adhesive in the light diffusion layer is preferably 50% by weight to 99.7% by weight, and more preferably 52% by weight to 97% by weight.

[0078] As the light diffusing fine particles, any suitable ones can be used as long as the effect of the present invention can be obtained. Specific examples include inorganic fine particles and polymer fine particles. The light diffusing fine particles are preferably polymer fine particles. Examples of the material of the polymer fine particles include silicone resin, acrylic resin such as methacrylic resin (e.g., polymethyl methacrylate), polystyrene resin, polyurethane resin, and melamine resin. These resins have excellent dispersibility in the adhesive and an appropriate refractive index difference with the adhesive, so that a light diffusing adhesive layer with excellent diffusion performance can be obtained. Preferably, at least one selected from the group consisting of silicone resin, polystyrene resin, and acrylic resin. The shape of the light diffusing fine particles can be, for example, spherical, flat, or irregular. The light diffusing fine particles may be used alone or in combination of two or more kinds.

[0079] In one embodiment, the refractive index of the light diffusing fine particles is lower than that of the adhesive. The refractive index of the light diffusing fine particles is preferably 1.30 to 1.70, more preferably 1.40 to 1.65. When the refractive index of the light diffusing fine particles is within this range, the difference in refractive index from the adhesive can be set to a desired range. As a result, a light diffusing layer having a desired haze value can be obtained.

[0080] The absolute value of the difference in refractive index between the light diffusing fine particles and the pressure-sensitive adhesive is preferably more than 0 and not more than 0.2, more preferably more than 0 and not more than 0.15, and further preferably 0.01 to 0.13.

[0081] The volume average particle diameter of the light diffusing fine particles is preferably 1 μm to 5 μm, more preferably 2 μm to 5 μm, and further preferably 3 μm to 5 μm. When the volume average particle diameter of the light diffusing fine particles is in such a range, a light diffusing pressure-sensitive adhesive layer having a desired haze value and a neutral hue can be obtained. For example, when the optical laminate is used in a reflective liquid crystal display device, the volume average particle diameter of the light diffusing fine particles is preferably in the above range. In addition, when the optical laminate is used in a transmissive liquid crystal display device, the volume average particle diameter is preferably 2.5 μm to 5 μm. The volume average particle diameter can be measured, for example, using an ultracentrifugal automatic particle size distribution measuring device.

[0082] The content of the light diffusing fine particles in the light diffusing adhesive is preferably 0.3% by weight to 50% by weight, more preferably 3% by weight to 48% by weight. By setting the blending amount of the light diffusing fine particles within the above range, a light diffusing adhesive layer having excellent light diffusing performance can be obtained.

[0083] The light diffusing layer may contain any suitable additive, such as an antistatic agent and an antioxidant.

[0084] In another embodiment, the light diffusion layer is composed of a light diffusion element. In this case, the light diffusion layer typically includes a matrix and light diffusing fine particles dispersed in the matrix. The matrix is ​​composed of, for example, an ionizing radiation curable resin. Examples of the ionizing radiation include ultraviolet light, visible light, infrared light, and electron beams. Preferred is ultraviolet light, and therefore the matrix is ​​preferably composed of an ultraviolet curable resin. Examples of the ultraviolet curable resin include acrylic resins, aliphatic (e.g., polyolefin) resins, and urethane resins. As for the light diffusing fine particles, fine particles similar to the light diffusing fine particles that can be used in the light diffusing adhesive can be used.

[0085] The light diffusion layer can be formed, for example, by applying a dispersion (light diffusion layer forming coating liquid) containing a pressure sensitive adhesive (or adhesive or matrix resin), light diffusing fine particles, and additives as necessary, onto any suitable substrate, and curing and / or drying the resulting coating. The substrate may be, for example, a separator, or the above polarizer or retardation film. Since the light diffusion layer can be formed by coating in this way, if a long retardation film and a long polarizer are used, an optical laminate can be produced by roll-to-roll processing, and as a result, the production efficiency of liquid crystal display devices can be improved.

[0086] C-2. Retardation layer The retardation layer is a retardation layer that essentially functions as a λ / 4 plate. The retardation layer 20 may be any layer that essentially functions as a λ / 4 plate. For example, it may be a single layer (a so-called λ / 4 plate), or may be a layer having a laminated structure in which a plurality of retardation plates are combined to exhibit the optical compensation function of a λ / 4 plate.

[0087] The Nz coefficient of the retardation layer is preferably 1 to 3, more preferably 1 to 2.5, and further preferably 1 to 2. By satisfying such a relationship, a more excellent reflected hue can be achieved.

[0088] The thickness of the retardation layer can be set so as to obtain a desired in-plane retardation. The thickness of the retardation layer is preferably 10 μm to 80 μm, and more preferably 20 μm to 60 μm.

[0089] In one embodiment, the retardation layer preferably exhibits a refractive index characteristic of nx>ny≧nz. The in-plane retardation Re(550) of the retardation layer is preferably 80 nm to 200 nm, more preferably 100 nm to 180 nm, and further preferably 110 nm to 170 nm.

[0090] The retardation layer preferably has a so-called inverse dispersion wavelength dependence in which its in-plane retardation satisfies the relationship Re(450) < Re(550). By satisfying such a relationship, an excellent reflection hue can be achieved. Re(450) / Re(550) is preferably 0.8 or more and less than 1, more preferably 0.8 or more and 0.95 or less.

[0091] The retardation layer has a slow axis. The angle formed by the slow axis of the retardation layer and the absorption axis of the polarizer is preferably 38° to 52°, more preferably 42° to 48°, and even more preferably about 45°. With such an angle, very excellent antireflection characteristics can be realized.

[0092] The retardation layer is typically a retardation film formed of any suitable resin. As the resin for forming this retardation film, a polycarbonate-based resin is preferably used. Details and specific examples of the polycarbonate-based resin are described, for example, in JP-A-2014-026266. The description of this publication is incorporated herein by reference.

[0093] The retardation layer can be obtained, for example, by stretching a film formed from the above polycarbonate-based resin. As a method for forming a film from a polycarbonate-based resin, any suitable molding process can be employed. Specific examples include compression molding, transfer molding, injection molding, extrusion molding, blow molding, powder molding, FRP molding, cast coating (e.g., casting method), calendar molding, hot press method, etc. Extrusion molding or cast coating is preferred because it can enhance the smoothness of the resulting film and obtain good optical uniformity. The molding conditions can be appropriately set according to the composition and type of the resin used, the properties desired for the retardation layer, etc. Since many film products of polycarbonate-based resins are commercially available, the commercially available film may be directly subjected to the stretching treatment.

[0094] The thickness of the resin film (unstretched film) can be set to any appropriate value depending on the desired thickness of the retardation layer, the desired optical properties, the stretching conditions described below, etc. It is preferably 50 μm to 300 μm.

[0095] The stretching may be performed using any suitable stretching method and conditions (e.g., stretching temperature, stretching ratio, stretching direction). Specifically, various stretching methods such as free end stretching, fixed end stretching, free end shrinkage, and fixed end shrinkage may be used alone, simultaneously, or sequentially. Stretching may be performed in various directions or dimensions such as the length direction, width direction, thickness direction, and oblique direction. The stretching temperature is preferably Tg-30°C to Tg+60°C relative to the glass transition temperature (Tg) of the resin film, and more preferably Tg-10°C to Tg+50°C.

[0096] By appropriately selecting the above-mentioned stretching method and stretching conditions, a retardation film having the above-mentioned desired optical properties (for example, refractive index properties, in-plane retardation, Nz coefficient) can be obtained.

[0097] In one embodiment, the retardation film is produced by uniaxially stretching or fixed-end uniaxially stretching a resin film. A specific example of fixed-end uniaxial stretching is a method of stretching a resin film in the width direction (lateral direction) while running the resin film in the longitudinal direction. The stretching ratio is preferably 1.1 to 3.5 times.

[0098] In another embodiment, the retardation film can be produced by continuously obliquely stretching a long resin film in a direction at a predetermined angle θ with respect to the longitudinal direction. By adopting oblique stretching, a long stretched film having an orientation angle θ with respect to the longitudinal direction of the film (slow axis in the direction of angle θ) can be obtained, and for example, roll-to-roll lamination with a polarizer is possible, simplifying the manufacturing process. The angle θ can be the angle between the absorption axis of the polarizer and the slow axis of the retardation layer.

[0099] An example of a stretching machine used for oblique stretching is a tenter type stretching machine capable of applying a feeding force, a pulling force, or a take-up force at different speeds in the transverse and / or longitudinal directions. Tenter type stretching machines include a transverse uniaxial stretching machine and a simultaneous biaxial stretching machine, and any appropriate stretching machine can be used as long as it can continuously obliquely stretch a long resin film.

[0100] By appropriately controlling the left and right speeds in the stretching machine, respectively, a retardation layer (essentially, a long retardation film) having the desired in-plane retardation and a slow axis in the desired direction can be obtained.

[0101] The stretching temperature of the film may vary depending on the in-plane retardation value and thickness desired for the retardation layer, the type of resin used, the thickness of the film used, the stretching ratio, etc. Specifically, the stretching temperature is preferably Tg-30°C to Tg+30°C, more preferably Tg-15°C to Tg+15°C, and even more preferably Tg-10°C to Tg+10°C. By stretching at such a temperature, a retardation layer having appropriate properties can be obtained. Note that Tg is the glass transition temperature of the constituent material of the film.

[0102] In another embodiment, the retardation layer exhibits flat wavelength dispersion characteristics. In this case, Re(450) / Re(550) of the retardation layer is preferably 0.99 to 1.03, and Re(650) / Re(550) is preferably 0.98 to 1.02. In this case, the retardation layer may have a laminated structure. Specifically, by arranging a retardation film functioning as a λ / 2 plate and a retardation film functioning as a λ / 4 plate at a predetermined axial angle (for example, 50° to 70°, preferably about 60°), it is possible to obtain characteristics close to ideal reverse wavelength dispersion characteristics, and as a result, it is possible to realize very excellent antireflection characteristics.

[0103] In this embodiment, the angle between the slow axis of the retardation layer and the absorption axis of the polarizer can be set to any suitable angle. For example, the angle between the slow axis of the film functioning as a λ / 2 plate and the absorption axis of the polarizer can be 5° to 30°, preferably about 15°, and the angle between the slow axis of the film functioning as a λ / 4 plate and the absorption axis of the polarizer can be 60° to 90°, preferably about 75°. If the angle is such, very excellent antireflection properties can be realized.

[0104] In this embodiment, the retardation layer can be made of any suitable resin film that can satisfy the above-mentioned characteristics.Typical examples of such resins include cyclic olefin resins, polycarbonate resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, and acrylic resins.Among them, cyclic olefin resins or polycarbonate resins can be preferably used.

[0105] Cyclic olefin resin is a general term for resins polymerized with cyclic olefins as polymerization units, and examples thereof include resins described in JP-A-1-240517, JP-A-3-14882, JP-A-3-122137, etc. Specific examples include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers (typically random copolymers) of cyclic olefins and α-olefins such as ethylene and propylene, and graft modified products of these modified with unsaturated carboxylic acids or derivatives thereof, as well as hydrogenated products thereof. Specific examples of cyclic olefins include norbornene monomers.

[0106] In the present invention, other cycloolefins capable of ring-opening polymerization can be used in combination within the scope of the present invention. Specific examples of such cycloolefins include compounds having one reactive double bond, such as cyclopentene, cyclooctene, and 5,6-dihydrodicyclopentadiene.

[0107] The cyclic olefin resin film may be a commercially available film, specific examples of which include Zeonex and Zeonor manufactured by Zeon Corporation, Arton manufactured by JSR Corporation, Topas manufactured by TICONA, and APEL manufactured by Mitsui Chemicals.

[0108] D. Applications of optical laminates The optical laminate of the present invention can be used in various display devices. Examples of such display devices include liquid crystal display devices, organic electroluminescence (EL) display devices, inorganic electroluminescence (EL) display devices, electron emission display devices (e.g., field emission display devices (FEDs) and surface field emission displays (SEDs)), electronic paper (display devices using electronic ink or electrophoretic elements, plasma display devices, projection display devices (e.g., grating light valve (GLV) display devices, display devices having digital micromirror devices (DMDs)), and piezoelectric ceramic displays. These display devices may be display devices that display two-dimensional images, or stereoscopic display devices that display three-dimensional images.

[0109] E.Liquid crystal display device The liquid crystal display device of the present invention includes the optical laminate. Examples of the liquid crystal display device include a transmission type liquid crystal display device, a semi-transmission type liquid crystal display device, a reflection type liquid crystal display device, a direct-view type liquid crystal display device, and a projection type liquid crystal display device.

[0110] The liquid crystal display device of the present invention is preferably a reflective liquid crystal display device. When the reflective liquid crystal display device contains the optical laminate, a liquid crystal display device with a clearer display image can be obtained. In addition, the reflection hue and viewing angle characteristics of the liquid crystal display device can be improved. In one embodiment, the reflective liquid crystal display device of the present invention can efficiently use external light, and therefore can be suitably used as a liquid crystal display device used outdoors. In addition, as described above, the liquid crystal display device of the present invention is excellent in reflection hue and viewing angle characteristics. Therefore, even when it is made into a large liquid crystal display device, good visibility can be ensured. When it is used as a large liquid crystal display device, it may be used as one large display device, or a plurality of liquid crystal display devices may be arranged (for example, 3 vertical × 4 horizontal) to make a large liquid crystal display device. As described above, the optical laminate used in the reflective liquid crystal display device of the present invention tends to have small depolarization and light leakage at the periphery. Therefore, it can be suitably used in a large liquid crystal display device. Furthermore, it can be suitably used in a liquid crystal display device with a small or no bezel.

[0111] As described above, the liquid crystal display device of the present invention can be used as a large liquid crystal display device. When used as a single large liquid crystal display device, it can be used as a liquid crystal display device with a display screen size of, for example, 20 inches or more. EXAMPLES

[0112] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.

[0113] (1) Thickness Measurements were made using a dial gauge (PEACOCK, product name "DG-205 type pds-2"). (2) Transmittance The transmittance of the polarizers obtained in Examples 1 and 2 and Comparative Example 1 was measured using a spectrophotometer (manufactured by JASCO Corporation, product name "V-7100"). These transmittances are Y values ​​corrected for visibility using a 2-degree visual field (C light source) according to JIS Z 8701-1982. The refractive index of the protective film was 1.50, and the refractive index of the surface of the polarizer not in contact with the protective film was 1.53. (3) Transmittance parameters The parallel transmittance was measured at wavelengths of 420 nm and 520 nm in the same manner as in (2) above. The measured parallel transmittance values ​​were used to calculate the transmittance parameter according to the following formula.

number

number

number

[0114] [Example 1] Preparation of polarizer 1 The thermoplastic resin substrate was a long, amorphous, isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) with a water absorption rate of 0.75% and a Tg of approximately 75°C. One side of the resin substrate was subjected to corona treatment (treatment conditions: 55 W min / m 2 ) was applied. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER Z410") in a ratio of 9:1. The above PVA aqueous solution was applied to the corona-treated surface of a thermoplastic resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched at its free end to 2.4 times its original size in the machine direction (longitudinal direction) between rolls with different peripheral speeds in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds after adjusting the iodine concentration of the dye bath so that the single transmittance (Ts) of the finally obtained polarizer would be an arbitrary value (dyeing treatment). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution at 70°C (boric acid concentration: 4.0 parts by weight of boric acid per 100 parts by weight of water) and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, while drying in an oven maintained at 70°C, the laminate was brought into contact with a SUS heated roll whose surface temperature was maintained at 75°C for about 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 2.5%. An acrylic film (surface refractive index 1.50, 40 μm) was attached as a protective film to the surface (side opposite to the resin substrate) of each polarizer obtained above via an ultraviolet-curable adhesive. Specifically, the curable adhesive was applied so that the total thickness was 1.0 μm, and the films were attached using a rolling machine. Thereafter, the adhesive was cured by irradiating it with UV light from the protective film side. Next, the resin substrate was peeled off to obtain 10 polarizing plates having a protective film / polarizer configuration. Table 1 shows the thickness, transmittance parameter, hue parameter, transmittance, parallel hue a, and parallel hue b of the obtained polarizer.

[0115] [Table 1]

[0116] [Example 2] Preparation of polarizer 2 A polarizing plate 8 was obtained in the same manner as in Example 1, except that the PVA aqueous solution (coating solution) was coated so that the thickness of the obtained polarizer was 3 μm. The thickness, transmittance parameter, hue parameter, transmittance, parallel hue a, and parallel hue b of the obtained polarizer are shown in Table 2.

[0117] [Table 2]

[0118] (Comparative Example 1) Preparation of Polarizer 3 A 75 μm-thick polyvinyl alcohol film (PVA film) (manufactured by Kuraray Co., Ltd., product name: VF-PS-N#7500) was immersed in warm water (swelling bath) at a liquid temperature of 25°C to cause it to swell, and was stretched in the machine direction to a stretching ratio of 2.4 times the original length. Next, the film was immersed in a dye bath (iodine aqueous solution to which iodide was added at a weight ratio of iodine:potassium iodide of 1:7) at a liquid temperature of 30° C. for 60 seconds, and stretched in the machine direction to a stretching ratio of 3.3 times the original length while being dyed. The iodine content of the dye bath was changed from 0.03 parts by weight to 0.1 parts by weight per 100 parts by weight of water to adjust the transmittance of the resulting polarizer. Next, the film was immersed in an aqueous solution at a liquid temperature of 30° C. (an aqueous solution obtained by mixing 4 parts by weight of boric acid and 3 parts by weight of potassium iodide with respect to 100 parts by weight of water) for 30 seconds. Next, the film was immersed in a stretching bath (an aqueous solution obtained by blending 4 parts by weight of boric acid and 5 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 60°C for 40 seconds, and stretched in the machine direction to a stretch ratio of 6 times the original length. Next, the film was washed by immersing it in a cleaning bath (an aqueous solution obtained by mixing 3 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 30°C for 10 seconds, and then dried at 50°C for 4 minutes to obtain a polarizer. Next, a PVA resin aqueous solution (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER (registered trademark) Z-200", resin concentration: 3 wt%) was applied to the surface of the obtained polarizer, a protective film (thickness 25 μm) was attached, and this was heated for 5 minutes in an oven maintained at 60° C. to obtain a polarizing plate (polarizer (transmittance 42.3%, thickness 30 μm) / protective film). The thickness, transmittance parameter, hue parameter, transmittance, parallel hue a, and parallel hue b of the obtained polarizer are shown in Table 3.

[0119] [Table 3]

[0120] [evaluation] The polarizers obtained in Examples 1 and 2 had a transmittance parameter of 0.8 or more and a hue parameter of 5 or less, and all of them were polarizers with neutral hues. Furthermore, the hues were neutralized without being affected by the transmittance. In addition, the polarizers were thin, and thus it was possible to reduce the thickness of displays using the polarizers.

[0121] [Reference Example 1] Preparation of light-diffusing adhesive A coating solution of the light-diffusing adhesive (solid content 13.2%) was prepared by blending 100 parts of the solid content of the acrylic polymer solution with 0.6 parts of an isocyanate crosslinker (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L") and 29 parts of silicone resin microparticles as light-diffusing microparticles (manufactured by Momentive Corporation, product name: Tospearl 145, volume average particle diameter 4 μm).

[0122] [Reference Example 2] Preparation of Retardation Film 1 Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with an agitator and a reflux condenser controlled at 100°C. 9,9-[4-(2-hydroxyethoxy)phenyl]fluorene (BHEPF), isosorbide (ISB), diethylene glycol (DEG), diphenyl carbonate (DPC), and magnesium acetate tetrahydrate were mixed in a molar ratio of BHEPF / ISB / DEG / DPC / magnesium acetate = 0.348 / 0.490 / 0.162 / 1.005 / 1.00 × 10 -5After thoroughly replacing the inside of the reactor with nitrogen (oxygen concentration 0.0005 to 0.001 vol%), heating was performed with a heat medium, and stirring was started when the inside temperature reached 100°C. 40 minutes after the start of the temperature increase, the inside temperature was allowed to reach 220°C, and while controlling to maintain this temperature, pressure reduction was started, and the pressure was reduced to 13.3 kPa in 90 minutes after reaching 220°C. Phenol vapor by-produced during the polymerization reaction was led to a reflux condenser at 100°C, and a small amount of monomer components contained in the phenol vapor were returned to the reactor, and uncondensed phenol vapor was led to a condenser at 45°C and collected.

[0123] Nitrogen was introduced into the first reactor and the pressure was restored to atmospheric pressure, and then the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature increase and pressure reduction in the second reactor were started, and the internal temperature was 240°C and the pressure was 0.2 kPa in 50 minutes. Thereafter, polymerization was allowed to proceed until a predetermined stirring power was reached. When the predetermined power was reached, nitrogen was introduced into the reactor to restore the pressure, and the reaction liquid was extracted in the form of strands and pelletized with a rotary cutter to obtain polycarbonate resin A with a copolymerization composition of BHEPF / ISB / DEG=34.8 / 49.0 / 16.2 [mol%]. The reduced viscosity of this polycarbonate resin was 0.430 dL / g and the glass transition temperature was 128°C.

[0124] The obtained polycarbonate resin was vacuum-dried at 80°C for 5 hours, and then a polycarbonate resin film with a thickness of 130 μm was produced using a film-making device equipped with a single-screw extruder (Isuzu Chemical Engineering Co., Ltd., screw diameter 25 mm, cylinder set temperature: 220°C), a T-die (width 900 mm, set temperature: 220°C), a chill roll (set temperature: 125°C) and a winder.

[0125] (diagonal stretching) The polycarbonate resin film obtained as described above was obliquely stretched according to Example 1 of JP 2014-194483 A to obtain a retardation film. For the detailed configuration of the apparatus, the description of JP 2014-194483 A is incorporated herein by reference. The specific preparation procedure of the retardation film is as follows: A polycarbonate resin film (thickness 130 μm, width 765 mm) was preheated to 142° C. in the preheating zone of the stretching apparatus. In the preheating zone, the clip pitch of the left and right clips was 125 mm. Next, as soon as the film entered the first oblique stretching zone C1, the clip pitch of the right clip was increased, and was increased from 125 mm to 177.5 mm in the first oblique stretching zone C1. The clip pitch change rate was 1.42. In the first diagonal stretching zone C1, the clip pitch of the left clip started to decrease, and was decreased from 125 mm to 90 mm in the first diagonal stretching zone C1. The clip pitch change rate was 0.72. Furthermore, as the film entered the second diagonal stretching zone C2, the clip pitch of the left clip started to increase, and was increased from 90 mm to 177.5 mm in the second diagonal stretching zone C2. Meanwhile, the clip pitch of the right clip was maintained at 177.5 mm in the second diagonal stretching zone C2. Simultaneously with the above diagonal stretching, the film was also stretched 1.9 times in the width direction. The above diagonal stretching was performed at 135°C.

[0126] (MD shrinkage processing) Next, in the shrink zone, MD shrinkage treatment was performed. Specifically, the clip pitch of both the left clip and the right clip was reduced from 177.5 mm to 165 mm. The shrinkage rate in the MD shrinkage treatment was 7.0%.

[0127] In this manner, a retardation film 1 (thickness: 50 μm) was obtained. The obtained retardation film had Re(550) of 141 nm and showed reverse dispersion characteristics.

[0128] [Reference Example 3] Preparation of Retardation Film 2 Cycloolefin-based retardation film A (Kaneka Corporation, product name "KUZ-Film #270", thickness 33 μm, Re(550) = 270 nm, Re(450) / Re(550) = 1.00, Nz coefficient = 1.00) and cycloolefin-based retardation film B (Kaneka Corporation, product name "KUZ-Film #140", thickness 28 μm, Re(550) = 140 nm, Re(450) / Re(550) = 1.00, Nz coefficient = 1.00) were laminated together via a 23 μm-thick light diffusion adhesive layer (light diffusion adhesive composition obtained in Reference Example 3) so that the angle between the slow axes of the films was 60 ° to produce a retardation film 2.

[0129] [Example 3] Preparation of optical laminate 1 The light diffusing adhesive composition obtained in Reference Example 1 was applied to the polarizer side of the polarizing plate including the polarizer (polarizer of Example 1-7) having a transmittance of 43.4% obtained in Example 1 so as to have a thickness of 23 μm after drying to form a light diffusing adhesive layer, and the retardation film obtained in Reference Example 2 was arranged and laminated so that the angle between the slow axis of the retardation film and the absorption axis of the polarizer was 45°. Next, the light diffusing adhesive composition was applied to the surface of the retardation film to which the polarizer was not laminated so as to have a thickness of 23 μm after drying to form a light diffusing adhesive layer, and then dried and cured to obtain an optical laminate 1. The obtained optical layered body had a Δab of 2.2 and a contrast ratio of 263. In addition, the haze of the light diffusing layer was 95.1%.

[0130] [Example 4] Preparation of optical laminate 2 The light-diffusing adhesive composition obtained in Reference Example 1 was applied to the polarizer side of a polarizing plate including a polarizer (polarizer of Example 2-2) having a transmittance of 43.4% obtained in Example 2 to a thickness of 23 μm after drying to form a light-diffusing adhesive layer, and the retardation film obtained in Reference Example 3 was bonded thereto to obtain optical laminate 2. The obtained optical layered body had a Δab of 2.1 and a contrast ratio of 260. In addition, the haze of the light diffusing layer was 95.1%.

[0131] (Comparative Example 2) Preparation of optical laminate C1 An optical laminate C1 was obtained in the same manner as in Example 3, except that a polarizing plate including the polarizer having a transmittance of 43.4% obtained in Comparative Example 1 (the polarizer of Comparative Example 1-2) was used as the polarizer. The obtained optical laminate had a Δab of 4.6 and a contrast ratio of 259. In addition, the haze of the light diffusing layer was 95.1%.

[0132] [evaluation] The optical laminates obtained in Examples 3 and 4 had a high contrast ratio and were excellent in reflected hue. The optical laminate of Comparative Example 2 had a high contrast but had room for improvement in reflected hue. [Industrial Applicability]

[0133] The polarizer of the present invention can be suitably used in displays such as liquid crystal displays, organic electroluminescence (EL) displays, inorganic electroluminescence (EL) displays, electron emission displays (e.g., field emission displays (FEDs) and surface field emission displays (SEDs)), electronic paper (displays using electronic ink or electrophoretic elements, plasma display devices, projection display devices (e.g., grating light valve (GLV) display devices and displays having a digital micromirror device (DMD)) and piezoelectric ceramic displays. [Explanation of symbols]

[0134] 10 Polarizer 20 Retardation layer 30 Light diffusing layer 100 Optical laminate

Claims

1. A polarizer having a transmittance parameter represented by formula (1) of 0.8 or more and 1.0 or less, a hue parameter represented by formula (2) of 5 or less, a thickness of 8 μm or less, and containing iodine as a dichroic material: [0010] (In formula (1), T 420 is the parallel transmittance at a wavelength of 420 nm, T 550 represents the parallel transmittance at a wavelength of 550 nm) [0025] (In formula (2), a represents the parallel hue a value, and b represents the parallel hue b value).

2. A method for producing the polarizer according to claim 1, comprising: subjecting a laminate of a thermoplastic resin substrate and a polyvinyl alcohol-based resin layer to an air-stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order; The polyvinyl alcohol-based resin layer contains a halide and a polyvinyl alcohol-based resin.

3. An optical laminate comprising the polarizer according to claim 1 , a retardation layer that substantially functions as a λ / 4 plate, and a light diffusing layer.

4. The optical laminate according to claim 3 , wherein the light diffusing layer comprises an adhesive and light diffusing fine particles.

5. 5. The optical laminate according to claim 4, wherein the light-diffusing fine particles have an average particle size of 2 μm to 5 μm.

6. A liquid crystal display device comprising the optical laminate according to claim 3 .

7. 7. The liquid crystal display device according to claim 6, which is a reflective liquid crystal display device.

Citation Information

Patent Citations

  • Polarizing film

    JP1999281817A

  • Method for manufacturing polarizing plate

    JP2013011847A

  • Polarization film, circular polarization plate and method for manufacturing the same

    JP2013210624A

  • Polarizing plate and circularly polarizing plate

    JP2016170369A

  • One-side protection polarizing film, polarizing film with adhesive layer and image display apparatus

    JP2017044882A