Activated carbon and its manufacturing method
By ball milling carbon aggregates and activating them with CO2, the method enhances the specific surface area and pore structure of activated carbon, addressing inefficiencies and safety concerns in existing methods.
Patent Information
- Application Number
- JP2022577680
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-25
- Filing Date
- 2021-11-22
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2041-11-22
AI Technical Summary
Existing methods for producing activated carbon, such as chemical and physical activation, face inefficiencies and safety risks, and struggle to enhance specific surface area and pore structure effectively, particularly with materials like CNTs.
A method involving ball milling of carbon aggregate precursors containing linear carbons to create cross sections, followed by activation with CO2, enhances specific surface area and pore structure without the need for additional chemicals, improving safety and efficiency.
The process increases specific surface area and porosity while minimizing electrical conductivity reduction, offering improved processability and stability of activated carbon.
Smart Images

Figure 0007556060000004 
Figure 0007556060000005 
Figure 0007556060000006
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 2020-0159437 filed on November 25, 2020, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to activated carbon and a method for producing the same. [Background technology]
[0003] In general, activated carbon is widely used in various fields from daily life to industry due to its unique adsorptive properties, and various methods for producing activated carbon have been developed.
[0004] The methods for producing activated carbon are largely divided into chemical activation and physical activation.
[0005] The chemical activation method is a process in which a carbon material is activated by reacting it with a basic substance such as KOH, NaOH, H3PO4, ZnCl2, etc. at high temperature and in an N2 or Ar atmosphere to increase the pores and specific surface area of the carbon material. However, the chemical activation method is troublesome because basic salts and impurities must be removed after the reaction, which can reduce the process efficiency. In addition, metals such as K and Na are formed during the reaction at high temperature, which can cause an explosion.
[0006] Physical activation is a process in which carbon materials are oxidized and activated at high temperatures of 700℃ to 900℃ using a CO2 / O2 mixture, O2 or H2O stream, either alone or in combination. When carbon materials are oxidized using only CO2, the activation kinetic is very slow, so a CO2 / O2 mixture, O2 or H2O stream must be used, either alone or in combination. In addition, physical activation has limitations in terms of improving the specific surface area and pore structure compared to chemical activation, and it is known that it is difficult to improve the specific surface area and pore structure of CNTs using physical activation. In addition, there is a risk of explosion due to the use of oxygen gas and steam at high temperatures.
[0007] Therefore, in order to improve the efficiency of the activation process of carbon materials, including CNTs, and make it commercially available, there is a need to develop a carbon material activation process that does not require a separate process to remove impurities and is free of the risk of explosion. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 2011-0044367 [Patent Document 2] Korean Patent Publication No. 2014-0018569 Summary of the Invention [Problem to be solved by the invention]
[0009] Therefore, the present invention aims to provide an activated carbon having an improved specific surface area and pore structure through a process with improved stability and efficiency by solving the problems of conventional methods for activating carbon materials, and a method for producing the same.
[0010] An object of the present invention is to provide an activated carbon having an improved specific surface area and pore structure.
[0011] Another object of the present invention is to provide a method for producing activated carbon with improved stability and efficiency. [Means for solving the problem]
[0012] In order to achieve the above object, the present invention provides a carbon aggregate comprising a number of linear carbons, the specific surface area of which is 350 m 2 / g or more.
[0013] The present invention also provides a method for producing activated carbon, comprising: (S1) ball milling a carbon aggregate precursor containing a plurality of linear carbons to pretreat the carbon aggregate precursor; and (S2) activating the pretreated carbon aggregate precursor by reacting it with CO2. Effect of the Invention
[0014] The activated carbon according to the present invention can increase the specific surface area and porosity through an activation process, while minimizing the decrease in electrical conductivity inherent to carbon materials.
[0015] In addition, the method for producing activated carbon according to the present invention does not use additional chemical substances, but activates carbon through dry ball milling and a reaction process with CO2, thereby improving the safety and efficiency of the activation process. [Brief description of the drawings]
[0016] [Figure 1A] FIG. 1A is a schematic diagram showing the morphological change that occurs when a carbon aggregate precursor is ball-milled. [Figure 1B] FIG. 1B is a schematic diagram showing the morphological change when a carbon aggregate precursor is chemically treated. [Figure 2A] 2A and 2B are scanning electron microscope (SEM) and transmission electron microscope (TEM) photographs of the activated carbons prepared in Example 1 and Comparative Example 1, respectively. [Figure 2B]2A and 2B are scanning electron microscope (SEM) and transmission electron microscope (TEM) photographs of the activated carbons prepared in Example 1 and Comparative Example 1, respectively. [Diagram 3] 1 is a graph showing the results of particle size analysis of activated carbons produced in Example 1 and Comparative Example 1. [Figure 4A] 4A and 4B are graphs showing the measurement results of the specific surface area of the activated carbons prepared in Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 4B] 4A and 4B are graphs showing the measurement results of the specific surface area of the activated carbons prepared in Examples 1 and 2 and Comparative Examples 1 and 2. [Diagram 5] 1 is a graph showing the powder resistance analysis results of the activated carbon produced in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will now be described in more detail to aid in understanding the invention.
[0018] The term "carbon aggregate precursor" used in the present specification means a carbon material used as a raw material for producing activated carbon, which has a shape like a cotton clump formed by linear carbon being entangled and aggregated with each other.
[0019] The term "carbon aggregate" used in the present specification means a carbon material contained in activated carbon, and refers to a carbon material that is activated after a carbon aggregate precursor containing linear carbon is subjected to a ball milling process to form a number of cross sections due to frictional force with linear carbon balls. The carbon aggregate precursor containing linear carbon has a shape like a lump of cotton, and when it is rubbed against a ball, it does not come apart one by one, but the linear carbon may be cut in the middle and broken, or a part of the surface of the linear carbon may be cut to form an edge.
[0020] The term "cross section" used in the present specification includes both ends formed when the carbon aggregate precursor is broken by friction with the balls during ball milling, and edges formed on the surface of the linear carbon by friction.
[0021] Activated carbon The present invention relates to activated carbon having an improved specific surface area and pore structure.
[0022] The activated carbon according to the present invention comprises carbon aggregates containing a large number of linear carbons and has a specific surface area of 350 m 2 / g or more.
[0023] When comparing single carbon and carbon aggregates having the same specific surface area, the single carbon has a problem that it is easily scattered and has poor processability because it is larger in volume and lighter than the carbon aggregates. In particular, when the single carbon and carbon aggregates are used as electrode materials, the single carbon has a problem that a large amount of solvent is consumed during slurry preparation, resulting in a low solid content of the slurry and a decrease in processability.
[0024] In the present invention, the carbon aggregate is formed by linear carbon entangled with each other to form a shape like a mass of cotton. The linear carbon includes at least one selected from the group consisting of carbon nanotubes (CNTs) and carbon fibers, but is not limited thereto as long as a large number of linear carbons can be entangled with each other to form an aggregate shape.
[0025] The linear carbon has a length of 500 nm or more and a cross-sectional diameter of 2 nm to 100 nm. Specifically, the linear carbon may have a length of 500 nm or more, 600 nm or more, or 700 nm or more, and the upper limit of the length is not particularly limited, but may be 300 μm or less, 400 μm or less, or 500 μm or less. The cross-sectional diameter of the linear carbon may be 2 nm or more, 5 nm or more, or 10 nm or more, and may be 80 nm or less, 90 nm or less, or 100 nm or less. The length and cross-sectional diameter of the linear carbon are set within an appropriate range that allows the linear carbon to be entangled with each other and form aggregates well.
[0026] If the length of the linear carbon is less than 500 nm, it may be difficult to form carbon aggregates due to the short length, and even if carbon aggregates are formed, they may be easily detached. If the length of the linear carbon exceeds 500 μm, carbon aggregates are formed even with a small number of linear carbons, so the number of cross sections of linear carbon exposed on the surface of the carbon aggregate is also reduced, and the degree of improvement in the specific surface area is negligible.
[0027] In the present invention, the cross section of the linear carbon may be exposed on the surface of the carbon aggregate.
[0028] The cross section of the linear carbon is formed by breaking the linear carbon when a carbon aggregate precursor containing the linear carbon is rubbed against a ball during a ball milling process described below.
[0029] The cross section of the linear carbon is exposed on the surface of the carbon aggregate, thereby increasing the specific surface area of the activated carbon including the carbon aggregate. As defined above, the "cross section" of the linear carbon in this specification means including all ends formed when the carbon aggregate precursor is broken by friction with the ball during ball milling, and edges formed on the surface of the linear carbon by friction.
[0030] In the present invention, the activated carbon includes amorphous carbon, which can further increase the specific surface area of the activated carbon.
[0031] Generally, amorphous carbon is formed during the activation of carbon, and amorphous carbon can be observed in activated carbon. For example, carbon nanotubes are not well activated in a physical activation process, so amorphous carbon is hardly observed in carbon nanotubes even after the physical activation process.
[0032] However, if the amorphous carbon is formed excessively, the degree of disorder inside the activated carbon increases, which may result in a decrease in electrical conductivity and mechanical strength. Since the amorphous carbon is related to the degree of disorder inside the activated carbon, the appropriate amount of amorphous carbon is as described below. D / I G is related to.
[0033] In the present invention, the specific surface area of the activated carbon is 350 m 2 Specifically, the specific surface area of the carbon aggregate may be 350 m 2 / g or more, 450m 2 / g or more or 550m 2 / g or more.
[0034] The specific surface area of the activated carbon is 350m 2 If the specific surface area is less than 1000 m / g, it is not significantly different from a non-activated carbon material, and therefore the reactivity may be reduced when the material is used as an electrode material. The upper limit of the specific surface area of the activated carbon is not particularly limited, but it is set to 1000 m in consideration of the durability of the activated carbon. 2 / g or less.
[0035] The total pore volume of the activated carbon is 0.8 cm 3 / g or 3.0cm 3 / g, specifically, 0.8 cm 3 / g or more, 1.0cm 3 / g or more or 1.5cm 3 / g or more, and3 / g or less or 3.0cm 3 / g or less.
[0036] The total pore volume of the activated carbon is 0.8 cm 3 If it is less than 3.0 cm / g, it is at the same level as the carbon before activation, so when it is used as an adsorbent or electrode material, the adsorption amount or storage capacity of lithium ions may decrease. 3 If it exceeds 1 / g, the durability of the activated carbon may be reduced.
[0037] In addition, I is a parameter that quantitatively indicates the degree of disorder or defect in the activated carbon crystal structure. D / I G may be 2.0 or less, specifically, 2.0 or less, 1.5 or less, 1.3 or less, or 1.0 or less. D / I G The lower limit of I is not particularly limited, but may be 0.5 or more. D / I G If it exceeds 2.0, electrical conductivity and mechanical strength may be significantly reduced due to too many defects in the carbon structure, and if it is less than 0.5, it means that activation has not been performed properly.
[0038] Above I D and I G can be measured and calculated using Raman spectroscopy, and I D The spectrum of 1310cm by Raman spectroscopy ‐1 More than 1350cm ‐1 The maximum peak intensity is in the range of I G The spectrum of 1560 cm ‐1 More than 1600cm ‐1 The maximum peak intensity is in the following range.
[0039] In general, Raman spectroscopy is commonly used to study the structure of materials by utilizing the special arrangement of light generated by the Raman effect.
[0040] In the Raman spectrum, the wave number is 1360 cm ‐1 The peak in the area around the band is called the D band, and the D band is sp 3 A peak showing a bond, which is sp 2 The bond is broken and the atom is sp 3 It increases when it becomes a bond.
[0041] In addition, in the Raman spectrum, the wave number 1580 cm ‐1 The peak in the area around the G band is called the G band, and the G band is sp 2 The peak indicates binding and means that there is no structural defect.
[0042] The D band increases when disorder or defects are generated in the structure of the material, so the maximum peak intensity of the G band (I G ) versus the maximum peak intensity of the D band (I D ) ratio (I D / I G ) can be calculated to quantitatively evaluate the degree of disorder or defect generation.
[0043] The activated carbon according to the present invention comprises carbon aggregates containing linear carbon, and due to the characteristic of the linear carbon being in the form of entangled cotton masses, rather than defects occurring on the surface of the linear carbon due to friction with the balls during the ball milling process, the linear carbon is broken and the resulting cross section is exposed on the surface of the carbon aggregates, increasing the specific surface area, and the porosity is also increased by activation, and the electrical conductivity is also excellent due to the morphological characteristics of the linear carbon.
[0044] Since the activated carbon maintains the form of carbon aggregates, it requires less solvent when added to an electrode material or a composite material, and is easy to process because of its small volume and low scattering. In addition, since the activated carbon in the form of carbon aggregates already has a cotton-like lump form, it is possible to prevent the phenomenon of irregular re-aggregation of carbon.
[0045] How activated carbon is produced The present invention also relates to a method for producing activated carbon, the method for producing activated carbon includes: (S1) a step of pretreating a carbon aggregate precursor containing a plurality of linear carbons by ball milling; and (S2) a step of activating the pretreated carbon aggregate precursor by reacting it with CO2.
[0046] Here, the carbon aggregate precursor refers to a structure in which linear carbon is entangled to form a cotton-like mass. The types of linear carbon are as described above.
[0047] In the present invention, in the step (S1), the carbon aggregate precursor may be ball milled to produce activated carbon having a uniform particle size and an improved specific surface area.
[0048] In the ball milling process, the carbon aggregate precursor is rubbed against the ball, and the linear carbon contained in the carbon aggregate precursor is broken, and a number of cross sections may be generated. Since the carbon aggregate precursor is in the form of a lump of cotton, when it is rubbed against the ball, the linear carbon is not unraveled one by one, but the part rubbing against the ball is broken, and a cross section such as an end or a surface edge may be formed. In addition, since the carbon aggregate precursor has elasticity like a spring, physical changes in shape such as being pushed by the ball milling process can be minimized, and friction with the ball occurs in all xyz directions, so there is little possibility of shape deformation in a specific direction.
[0049] FIG. 1a is a schematic diagram showing the morphological change when a carbon aggregate precursor is ball-milled, and FIG. 1b is a schematic diagram showing the morphological change when the carbon aggregate precursor is chemically treated.
[0050] As shown in FIG. 1a, when the carbon aggregate precursor is ball milled (BM), some defects are generated on the surface, but only in part, and the carbon aggregate precursor is broken by friction with the ball, generating many edges, and the specific surface area may be increased.
[0051] On the other hand, as shown in FIG. 1b, when the carbon aggregate precursor is treated with acid or O2 / steam, surface defects are generally generated. D / I G increases significantly, and sp 2 Since there is a large resistance to the movement of electrons through carbon, there is a problem in that electrical conductivity is reduced.
[0052] Here, in the ball milling process, the type of ball milling process, temperature, pressure, humidity, weight ratio of the ball to the carbon aggregate precursor, material of the ball, etc. may be specified so as to maximize the frictional force between the ball and the carbon aggregate precursor.
[0053] The ball milling may be a dry ball milling. That is, the carbon aggregate precursor itself is rubbed against the ball, and no separate solvent is used during the ball milling process. The dry ball milling may improve the friction between the ball and the carbon aggregate precursor compared to the wet ball milling, and thus the number of cross sections formed on the carbon aggregate precursor may increase, thereby further improving the specific surface area. In addition, the dry ball milling process has an advantage that there are no problems such as waste water generated by removing the solvent, or the time required to remove the solvent, and the coffee ring effect generated by removing the solvent, which are caused by the wet ball milling.
[0054] Also, the ball milling may be performed under room temperature and pressure conditions, and in this case, there is an advantage in that the frictional force between the balls and the carbon aggregate precursor can be improved. At this time, the room temperature may be 0° C. or more, 25° C. or more, and 60° C. or less, or 100° C. or less. The room pressure may be 0.5 atm or more, 0.8 atm or more, and 1.3 atm or less, or 2 atm or less. For example, the room temperature and pressure are 25° C. and 1 atm.
[0055] Also, the ball milling may be performed under a humidity of 30% to 70%, and more specifically, the humidity may be 30% or more, 40% or more, or 45% or more, or 55% or less, 60% or less, or 70% or less. If the humidity is less than 30%, the grinding force may be reduced due to the static electricity generated by friction, and if it exceeds 70%, the moisture may cause structural deformation of the carbon aggregates.
[0056] In addition, the ball milling process may be performed using milling balls having a diameter of 1 to 10 mm under milling conditions of 100 to 400 RPM for 0.5 to 50 hours.
[0057] In addition, the ball milling may be performed under the condition that the weight ratio of the carbon aggregate precursor to the milling ball is 1:1 to 100:1, and specifically, the weight ratio may be 1:1 or more, 10:1 or more, 20:1 or more, or 30:1 or more, or 70:1 or less, 80:1 or less, 90:1 or less, or 100:1 or less. If the weight ratio is less than 1:1, the carbon aggregate precursor may have excessive cross sections formed thereon, resulting in poor durability, and if it exceeds 100:1, the carbon aggregate precursor may be used in an excessive amount, resulting in a negligible effect of increasing the specific surface area.
[0058] In addition, the milling balls may be zirconia (ZrO2) balls or alumina (Al2O3) balls, and preferably, zirconia balls may be used in consideration of the frictional force with the carbon aggregate precursor.
[0059] Through this ball milling process, the carbon aggregate precursor is atomized to have a uniform particle size, and multiple cross sections are formed on the carbon aggregate precursor, which can significantly improve the activation kinetic in step (S2) described below.
[0060] In the present invention, in the step (S2), the carbon aggregate precursor pretreated in the step (S1) may be activated by reacting with CO2.
[0061] The pretreated carbon aggregate precursor has a large number of cross sections formed on its surface due to friction with the balls during ball milling, increasing its specific surface area. Therefore, the activation kinetic can be significantly improved by activating the pretreated carbon aggregate precursor by reacting it with CO2.
[0062] The reaction of the carbon aggregate precursor with CO2 may be performed under an activated atmosphere. At this time, the activated atmosphere is formed by an activated gas, and by performing the reaction under the activated atmosphere, the reactivity of the cross-section formed on the surface of the carbon aggregate precursor with CO2 can be further promoted, thereby improving activation efficiency.
[0063] In addition, the activation may be performed under one or more reducing gases selected from the group consisting of carbon monoxide, oxygen, hydrogen, ethylene, ethane, and methane. In order to prevent excessive activation, the activation process may be performed by partially mixing an inert gas such as nitrogen or argon.
[0064] Also, the activation can be performed by heat treatment after temperature elevation.
[0065] In terms of activation efficiency, it may be preferable to gradually increase the temperature during the activation. By controlling the heating rate, the carbon aggregates can be generally uniformly activated, and if the heating rate is extremely fast, the carbon aggregates may be non-uniformly activated. In this case, the heating rate may be 1° C. / min to 10° C. / min, specifically, 1° C. / min or more, 2° C. / min or more, or 3° C. / min or more, and 8° C. / min or less, 9° C. / min or less, or 10° C. / min or less. If the heating rate is less than 1° C. / min, the heating rate is too slow and the activation is too slow in the temperature range to be activated, resulting in a decrease in mechanical and / or electrical properties, and if it exceeds 10° C. / min, the heating rate is too fast and non-uniform activation may be performed.
[0066] After the temperature rise, the heat treatment may be performed at a temperature of 900° C. to 1200° C. Specifically, the heat treatment temperature may be 900° C. or more, 1000° C. or more, or 1050° C. or more, or 1100° C. or less, 1150° C. or less, or 1200° C. or less. If the heat treatment temperature is less than 900° C., the reactivity of the carbon aggregate precursor with CO2 decreases, resulting in poor activation efficiency, and if the heat treatment temperature exceeds 1200° C., the carbon aggregates may be oxidized, resulting in a significant decrease in mechanical / electrical strength and yield.
[0067] The heat treatment time is not particularly limited, but may be 1 hour or more, 2 hours or more, or 5 hours or less, 7 hours or less, or 10 hours or less, taking into consideration activation efficiency.
[0068] The activation step may also be performed in a fluidized bed reactor for uniform reaction. For example, the fluidized bed reactor may be a tube furnace or a box furnace.
[0069] When the fluidized bed reactor is used, more uniform activation is possible, the specific surface area of the activated carbon particles can be uniformly increased, and crushing of the activated carbon particles can be prevented.
[0070] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of the present invention. It is natural that such changes and modifications fall within the scope of the accompanying claims.
[0071] Example 1 (1) Pretreatment using ball milling A carbon aggregate precursor (FT series, Canon, hereinafter referred to as CNT1) in which a number of CNTs are entangled was pretreated by a ball milling process under conditions of 25°C, 1 atm, and 50% humidity. The ball milling process was carried out for 1 hour at 300 rpm using zirconia balls with a diameter of 3 mm. The weight ratio of the carbon aggregate precursor to the balls was set to 50:1 (BM.CNT1).
[0072] The CNT1 has nine walls.
[0073] (2) Activation through reaction with CO2 The pretreated carbon aggregate precursor was activated by reacting with CO2 using a fluidized bed reactor. The activation was performed by heat treating at a temperature of 950°C, increasing the temperature at a rate of 5°C / min for 3 hours, and then activating at 950°C for 3 hours to produce activated carbon (Act.BM.CNT1).
[0074] Comparative Example 1 Activated carbon was produced in the same manner as in Example 1, except that the untreated carbon aggregate precursor (CNT1) was heat-treated at a temperature of 650° C. (Act. CNT1).
[0075] Example 2 A carbon aggregate precursor (BM.CNT2) and activated carbon (Act.BM.CNT2) pretreated using ball milling were prepared in the same manner as in Example 1, except that a carbon aggregate precursor (FT series, Canon, hereinafter referred to as CNT2) having a different number, diameter, and length of carbon nanotube walls was used compared to a carbon aggregate precursor (FT series, Canon, CNT1) in which multiple CNTs are entangled.
[0076] The CNT2 has six walls, which is smaller than the CNT1, and therefore has a smaller diameter.
[0077] Comparative Example 2 Activated carbon was produced in the same manner as in Example 2, except that the untreated carbon aggregate precursor (CNT2) was heat-treated at a temperature of 650° C. (Act. CNT2).
[0078] Experimental Example 1: Shape and Particle Size Analysis The shapes and particle sizes of the activated carbons prepared in Example 1 and Comparative Example 1 were analyzed.
[0079] The morphology of the activated carbon was analyzed using a scanning electron microscope (SEM, JSM7610F, JOEL) and a transmission electron microscope (TEM, JEM1400FLASH, JOEL).
[0080] FIG. 2a is a SEM image of the raw material carbon aggregate precursor (CNT1), the carbon aggregate precursor pretreated using ball milling (BM.CNT1), the activated carbon activated by reacting with CO2 without pretreatment in Comparative Example 1 (Ac.CNT1), and the activated carbon activated by reacting with CO2 after pretreatment in Example 1 (Ac.BM.CNT1), and FIG. 1b is a TEM image.
[0081] As shown in FIG. 2a, the activated carbon of Example 1 (Act.BM.CNT1) has a fine and uniform shape and maintains the aggregate morphology formed by entanglement of linear carbon.
[0082] Meanwhile, it can be seen that the size of the activated carbon (Act. CNT1) of Comparative Example 1 is not significantly changed compared to the carbon aggregate precursor (CNT1) used as the raw material.
[0083] Also, as shown in FIG. 2b, it can be seen that a large amount of amorphous carbon was formed in the activated carbon (Act.BM.CNT1) of Example 1. Since the amorphous carbon was observed, it can be seen that the activation was well performed. In addition, the amorphous carbon can also show the effect of increasing the specific surface area.
[0084] The particle size of the activated carbon was analyzed using a particle size analyzer (Bluewave, Microtrac) and is shown in Table 1 and FIG.
[0085] [Table 1]
[0086] As shown in Table 1 and FIG. 3, the particle size of the activated carbon of Example 1 (Act.BM.CNT1) is significantly smaller than that of the carbon aggregate precursor (CNT1) which is the raw material.
[0087] On the other hand, it can be seen that the particle size of the activated carbon of Comparative Example 1 (Act. CNT1) is not significantly changed compared to the carbon aggregate precursor (CNT1).
[0088] Experimental Example 2: Specific surface area analysis The specific surface area of the activated carbons prepared in Examples 1 and 2 and Comparative Examples 1 and 2 was analyzed.
[0089] The specific surface area of the activated carbon was analyzed using a BET (Brunauer-Emmett-Teller) analyzer (ASAP 2020, Micrometrics Inc.), and the results are shown in Table 2 and FIG. 4a and FIG. 4b.
[0090] [Table 2]
[0091] As shown in Table 2 and FIGS. 4a and 4b, the specific surface area of the activated carbon of Example 1 (Act.BM.CNT1) and Example 2 (Act.BM.CNT2) was significantly increased compared to the raw carbon aggregate precursors (CNT1 and CNT2).
[0092] In addition, CNT1 in Example 1 has a greater number of walls and a relatively larger diameter than CNT2 in Example 2. Generally, as the number of walls in a CNT increases, the mechanical strength decreases. Therefore, the effect of increasing the specific surface area by ball milling and activation is also greater, with Example 1 being about 210% compared to Comparative Example 1, compared to an increase of about 160% in Example 2.
[0093] The activated carbons of Comparative Example 1 (Act.CNT1) and Comparative Example 2 (Act.CNT2) also had an increased specific surface area compared to the carbon aggregate precursors (CNT1, CNT2), but the degree of increase in specific surface area was relatively insignificant compared to Examples 1 and 2.
[0094] Experimental Example 3: Crystallinity analysis The crystallinity of the activated carbons prepared in Example 1 and Comparative Example 1 was analyzed.
[0095] The crystallinity of the activated carbon was measured by Raman spectroscopy [using a DXR Raman Microscope (Thermo Electron Scientific Instruments LLC)] at 1580 ± 20 cm ‐1 Maximum peak intensity of G band at (I G ) for 1360±50cm ‐1Maximum peak intensity of the D band at D ) ratio (I D / I G , R value) were measured and are shown in Table 3 below.
[0096] Above I D / I G The larger the value, the more disordered or defective the crystals are.
[0097] [Table 3]
[0098] As shown in Table 3, the I D / I G Since the increase in the carbon aggregate precursor (CNT1) is not large compared to the raw material, it can be seen that the internal disorder or defects are not significantly increased by the activation process including ball milling and reaction with CO2.
[0099] Experimental Example 4: Powder Resistance Analysis The activated carbon prepared in Example 1 was analyzed for powder resistance.
[0100] Using a powder resistance device (Loresta-GX, MCP-PD51), 0.5 g of sample was filled into a target holder and pressed with 400 kgf, 800 kgf, 1200 kgf, 1600 kgf, and 2000 kgf, and the conductivity was measured at 60 MPa.
[0101] As shown in FIG. 5, the activated carbon (Act.BM.CNT1) produced in Example 1 has a conductivity that is not significantly different from that of the raw material carbon aggregate precursor (CNT1).
[0102] From this, it was confirmed that the present invention can produce activated carbon with little decrease in electrical conductivity while significantly increasing the specific surface area of the raw material, the carbon aggregate precursor itself, and uniformly reducing the particle size.
[0103] Although the present invention has been described above with reference to limited embodiments and drawings, the present invention is not limited thereto, and it is of course possible for a person having ordinary skill in the art to which the present invention pertains to make various modifications and variations within the technical spirit of the present invention and the equivalent scope of the following claims.
Claims
1. It contains carbon aggregates containing many linear carbons and amorphous carbons, and has a specific surface area of 350 m 2 / g or more, The cross-sectional diameter of the linear carbon is between 2 nm and 100 nm.
2. The activated carbon according to claim 1 , wherein the linear carbon comprises at least one selected from the group consisting of carbon nanotubes (CNTs) and carbon fibers.
3. 3. The activated carbon according to claim 1 or 2, wherein a cross section of the linear carbon is exposed on a surface of the carbon aggregate.
4. I of the activated carbon D / I G is below 2.0, I D and I G and I are the maximum peak intensities of activated carbon measured by Raman spectroscopy. G is a vibration frequency of 1560 cm ‐1 or 1600 cm ‐1 The maximum peak intensity in the range is I D The vibration frequency is 1310 cm ‐1 or 1,350 cm ‐1 The activated carbon according to any one of claims 1 to 3, wherein the activated carbon has a maximum peak intensity in a range.
5. The pore volume of the activated carbon is 0.8 cm 3 / g to 3.0 cm 3 The activated carbon according to any one of claims 1 to 4, wherein the activated carbon has a molecular weight of 1000 to 20000.
6. (S1) pretreating a carbon aggregate precursor containing a plurality of linear carbons by ball milling; and (S2) The pretreated carbon aggregate precursor is subjected to CO 2 Activating the compound by reacting it with The cross-sectional diameter of the linear carbon is 2 nm to 100 nm.
7. 7. The method of claim 6, wherein the ball milling in step (S1) is performed under conditions of room temperature, normal pressure, and humidity of 30% to 70%.
8. 8. The method for producing activated carbon according to claim 6 or 7, wherein the ball milling in step (S1) is performed under a weight ratio of carbon aggregate precursor:milling balls of 1:1 to 100:
1.
9. The balls used in the ball milling are made of zirconia (ZrO 2 ) ball or alumina (Al 2 O 3 9. The method for producing activated carbon according to claim 6, wherein the activated carbon is a ball.
10. The method of claim 6, wherein the activation in step (S2) is performed by increasing the temperature at a rate of 1° C. / min to 10° C. / min and then performing a heat treatment to activate the activated carbon.
11. The method of claim 10, wherein the heat treatment is performed at a temperature of 900°C to 1200°C.
Citation Information
Patent Citations
Carbon electrode
JP2011049067A
Activated carbon fiber
JP2011105545A
Gas adsorbent and method of producing the same
JP2015167941A
Adsorption material
JP2016059856A
Porous nanocarbon manufacturing method using ball milling
KR1020090074360A