Wet-laid nonwoven fabric manufacturing method
The use of long carbon fibers and fibrous activated carbon in a wet-laid nonwoven fabric manufacturing process addresses the corrosion issues of metal-based conductive materials, enhancing conductivity and durability for wearable devices.
Patent Information
- Application Number
- JP2020036885
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-04
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-03-04
AI Technical Summary
Existing wearable device fabrics using metal-based conductive fillers or yarns are prone to corrosion from sweat, compromising their conductive performance and durability.
A method for producing a wet-laid nonwoven fabric using carbon fibers with an average length of 10 cm or more, combined with fibrous activated carbon, to enhance conductivity and resistance to corrosion.
The method improves the conductive performance and resistance to sweat corrosion of the nonwoven fabric, making it suitable for wearable devices with enhanced flexibility and comfort.
Smart Images

Figure 0007557186000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a wetlaid nonwoven fabric, and more particularly to a method for producing a wetlaid nonwoven fabric that can contribute to improving the conductive performance of the wetlaid nonwoven fabric. [Background technology]
[0002] In recent years, wearable devices have been developed that are electronic devices with input / output, computing, and communication functions that are intended to be used in close proximity to or in close contact with the body. Known wearable devices include accessory-type wearable devices such as wristwatches, glasses, and earphones, and textile-integrated wearable devices that incorporate electronic functions into clothing. Wearable devices require conductive materials for power supply, signal transmission, etc., and various developments are currently underway.
[0003] A fabric for a wearable device is known, which includes a stretchable conductive layer having elasticity and a hot melt adhesive layer formed on one surface of the stretchable conductive layer, the stretchable conductive layer being formed by attaching a stretchable conductive film composed of a conductive composition containing an elastomer and a conductive filler filled in the elastomer to a fabric via the hot melt adhesive layer (see, for example, Patent Document 1). According to the fabric for a wearable device, the conductive film can be easily attached to a textile fabric, and is said to have electrical conductivity and elasticity.
[0004] Also, as a fabric for wearable devices, a conductive stretch knitted fabric is known in which the direction in which loops are connected and proceed in a knitted structure is defined as the course direction or course, the loops are formed of conductive yarn, and an elastic yarn is arranged in such a way that it generates a tightening force in the course direction, and when the knitted fabric is not stretched, the tightening force of the elastic yarn keeps the loops of the conductive yarn adjacent in the course direction in contact with each other, while when the knitted fabric is stretched in the course direction, the loops of the conductive yarn can be separated from each other against the tightening force of the elastic yarn (see, for example, Patent Document 2). The conductive stretch knitted fabric is a knitted fabric that is highly stretchable and flexible, and has recovery properties when repeatedly stretched, but also has a property that electrical resistance changes between stretched and non-stretched, and furthermore, it is possible to obtain breathability, moisture permeability, water absorbency, etc., and therefore it is considered to be suitable for use as a wearable material.
[0005] In response to the prior art techniques of Patent Documents 1 and 2 above, the applicant of the present application filed an invention relating to a fabric for wearable devices that contains a fibrous carbon material (see Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-1011124 A [Patent Document 2] International Publication No. 2017 / 010236 [Patent Document 3] Patent application 2019-115551 Summary of the Invention [Problem to be solved by the invention]
[0007] As a result of the inventor's investigations, it has been found that the fabric for wearable devices disclosed in Patent Document 1 uses a metal such as silver as a conductive filler, and since the conductive filler filled in the elastomer of the film is exposed to the air, there is a problem in that the conductive filler may corrode due to sweat, etc.
[0008] In addition, the conductive stretch knitted fabric disclosed in Patent Document 2 has conductive yarn in which metal components such as plated wire are exposed on the yarn surface, and there is also the problem that the exposed metal components may corrode due to sweat, etc.
[0009] As a means for solving the problems of Patent Documents 1 and 2, the present inventors have proposed in Patent Document 3 that a fabric for wearable devices contains a fibrous carbon material, which can exhibit conductive performance while also exhibiting excellent corrosion resistance against sweat, etc. Meanwhile, Patent Document 3 also proposes using carbon fibers as the fibrous carbon material, and the present inventors have investigated a method for further improving conductive performance when forming a wet-laid nonwoven fabric using carbon fibers.
[0010] Therefore, a main object of the present invention is to provide a method for producing a wetlaid nonwoven fabric, which can contribute to improving the conductive performance of the wetlaid nonwoven fabric when a wetlaid nonwoven fabric containing carbon fibers as a fibrous carbon material is obtained. [Means for solving the problem]
[0011] As a result of investigations conducted by the present inventors to solve the above problems, it was found that by producing a wetlaid nonwoven fabric by a wet papermaking method using carbon fibers having an average fiber length of 10 cm or more, the conductive performance of the resulting wetlaid nonwoven fabric can be improved compared to when carbon fibers having an average fiber length of less than 10 cm, for example 100 mm or less, are used.
[0012] That is, the present invention provides the following aspects. Item 1. A method for producing a wetlaid nonwoven fabric, comprising: a preparation step of preparing carbon fibers having an average fiber length of 10 cm or more; a slurry preparation step of preparing a slurry using the carbon fibers; and a wetlaid papermaking step of wetlaid papermaking using the prepared slurry. Item 2. A method for producing a wetlaid nonwoven fabric, comprising: a preparation step of preparing carbon fibers having an average fiber length of 10 cm or more and fibrous activated carbon; a slurry preparation step of preparing a slurry using the carbon fibers and the fibrous activated carbon; and a wet papermaking step of wet papermaking using the prepared slurry. Effect of the Invention
[0013] According to the method for producing a wetlaid nonwoven fabric of the present invention, the method includes a preparation step of preparing carbon fibers having an average fiber length of 10 cm or more, a slurry preparation step of preparing a slurry using the carbon fibers, and a wetlaid papermaking step of wetlaid papermaking using the prepared slurry, and therefore when a wetlaid nonwoven fabric containing carbon fibers as a fibrous carbon material is obtained, the method can contribute to improving the conductive performance of the wetlaid nonwoven fabric. Therefore, the obtained wetlaid nonwoven fabric can be suitably used for, for example, a wearable device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The method for producing a wetlaid nonwoven fabric of the present invention includes a preparation step of preparing carbon fibers having an average fiber length of 10 cm or more, a slurry preparation step of preparing a slurry using the carbon fibers, and a wetlaid papermaking step of wetlaid papermaking using the prepared slurry. Each step will be described in detail below.
[0015] <Preparation process> 1. Carbon fiber In the method for producing a wetlaid nonwoven fabric of the present invention, the preparation step is a step of preparing carbon fibers having an average fiber length of 10 cm or more. This can improve the conductive performance of the resulting wetlaid nonwoven fabric compared to the case where carbon fibers having an average fiber length of less than 10 cm, for example, 100 mm or less, are used. The average fiber length is preferably 30 cm or more, more preferably 40 cm or more. The upper limit of the average fiber length is not particularly limited, but may be, for example, 1000 cm or less, preferably 100 cm or less. In the present invention, the average fiber length is measured by observing 10 arbitrarily selected carbon fibers at a magnifying glass and an image analyzer at a magnification of 1000 times, measuring the fiber length of each, and taking the average value of the fiber lengths of these 10 points as the average fiber length.
[0016] The mechanism by which the conductive performance of the wet nonwoven fabric obtained by using carbon fibers having an average fiber length of 10 cm or more can be improved compared to the case where carbon fibers having an average fiber length of less than 10 cm, for example, 100 mm or less, is not necessarily clear, but can be considered as follows. That is, when the average fiber length of the carbon fibers is longer, the wet nonwoven fabric obtained tends to be bulkier and thicker. When the conductivity in the planar direction of the wet nonwoven fabric is examined, the cross-sectional area of the wet nonwoven fabric increases by the amount of the increase in thickness, and the resistance as a conductor decreases. In addition, according to the study by the present inventors, it has been found that the volume resistivity of the wet nonwoven fabric obtained by using carbon fibers having an average fiber length of 10 cm or more is also smaller than that of the case where carbon fibers having an average fiber length of less than 10 cm, for example, 100 mm or less, are used. This is thought to be because, by using a wet papermaking method, which will be described later, tends to make the fibers relatively dense, it is possible to maintain many contact points between the carbon fibers even if the average fiber length is increased, and this, together with the increased thickness, also results in a lower volume resistivity.
[0017] The average fiber diameter of the carbon fibers is not particularly limited, but may be, for example, 5 to 30 μm, and preferably 5 to 20 μm. In the present invention, the average fiber diameter is measured and calculated using a reflecting microscope in accordance with JIS K 1477:2007 7.3.1.
[0018] In the method for producing a wetlaid nonwoven fabric of the present invention, the carbon fiber may be either anisotropic or isotropic. When the obtained wetlaid nonwoven fabric is used as a fabric for a wearable device, it is preferable to use isotropic carbon fiber from the viewpoint of reducing the polarizability in the thickness direction of the wetlaid nonwoven fabric. Isotropic carbon fiber can be obtained, for example, from isotropic pitch as a raw material. Here, isotropy refers to optical isotropy, in which molecules or groups of molecules are randomly oriented.
[0019] 2. Fibrous activated carbon In the manufacturing method of the wetlaid nonwoven fabric of the present invention, in addition to the carbon fibers described above, activated carbon fibers can be prepared in the preparation step. By combining activated carbon fibers as the fibrous carbon material, it is possible to improve the adsorption performance of odorous components and the like generated by a user wearing a wearable device while improving the conductive performance.
[0020] The type of fibrous activated carbon is not particularly limited, but any fibrous activated carbon produced by infusible polyacrylonitrile, rayon, phenol resin, coal pitch, petroleum pitch, or other fibers, carbonizing them, and then activating them by holding them in an atmosphere containing water vapor and carbon dioxide at a predetermined temperature for a predetermined time can be used. Among these, coal pitch, petroleum pitch, and polyacrylonitrile fibrous activated carbons are preferred from the viewpoint of further reducing the conductive performance of the wet-laid nonwoven fabric obtained by the manufacturing method of the present invention. The fibrous activated carbon may be used alone or in combination of two or more types.
[0021] The specific surface area of the fibrous carbon material used in the present invention is not particularly limited. In particular, from the viewpoint of further improving the conductive performance of the obtained wetlaid nonwoven fabric, the specific surface area of the fibrous carbon material is preferably 500 to 4000 m 2 / g, preferably 500 to 2000m 2 / g, more preferably 500 to 1000m 2In the present invention, the specific surface area is a value measured by the BET method (single point method) using nitrogen as an adsorbed substance.
[0022] In the present invention, the average fiber diameter of the fibrous activated carbon is not particularly limited, but may be, for example, 5 to 30 μm, and from the viewpoint of achieving both electrical conductivity and suppression of roughness caused by coal dust, preferably 10 to 20 μm. The average fiber diameter of the fibrous activated carbon is measured and calculated by a reflecting microscope in accordance with JIS K 1477:2007 7.3.1.
[0023] In the present invention, the average fiber length of the fibrous activated carbon is not particularly limited. For example, the average fiber length may be 1 cm or more, and is preferably 1 to 100 cm. The average fiber length of the fibrous activated carbon is measured by observing 10 arbitrarily selected fibrous activated carbons at 1000 times magnification using a magnifying glass and an image analyzer, measuring the fiber length of each, and averaging the fiber lengths of these 10 points.
[0024] 3. Other materials In the preparation step of the wetlaid nonwoven fabric manufacturing method of the present invention, materials other than carbon fibers, fibrous activated carbon, and other fibrous carbon materials, for example, materials that can contribute as binder components or aggregates of the wetlaid nonwoven fabric, can be prepared. Examples of such materials include pulp. Examples of pulp include cellulosic pulp such as wood pulp, acrylic pulp, and the like. In addition, examples of such materials include synthetic resin materials with a melting point of 200° C. or less and / or synthetic resin materials with a melting point of 200° C. or more. As materials other than the fibrous carbon materials, a combination of pulp, polyester fibers, and polyolefin fibers can be preferably used.
[0025] <Slurry preparation process> The method for producing a wetlaid nonwoven fabric of the present invention includes a slurry preparation step of preparing a slurry using the carbon fibers prepared in the preparation step, and, if necessary, the further prepared fibrous activated carbon and other materials described above.
[0026] Specifically, the slurry preparation step involves disintegrating and mixing the prepared raw materials using a pulper.
[0027] In the slurry, the content of carbon fiber in the non-volatile component is 5 to 95% by mass. When fibrous activated carbon is added, the content of the carbon fiber is preferably 5 to 30% by mass, more preferably 18 to 26% by mass. When fibrous activated carbon is added, the content of the fibrous activated carbon in the non-volatile component is preferably 10 to 40% by mass, more preferably 15 to 23% by mass. When fibrous activated carbon is added, the mass ratio of fibrous activated carbon to carbon fiber (mass of fibrous activated carbon / mass of carbon fiber) is preferably 0.5 to 4, more preferably 0.8 to 1.2. The content of materials other than carbon fiber, fibrous activated carbon, and other fibrous carbon materials is preferably 45 to 70% by mass, more preferably 47 to 70% by mass, and even more preferably 49 to 70% by mass. By setting the content of materials other than fibrous carbon materials within such a range, the wet nonwoven fabric has a better texture, and the user's wearing comfort when used as a wearable device is improved.
[0028] <Wet paper making process> The method for producing a wetlaid nonwoven fabric of the present invention includes a wetlaid papermaking step in which the prepared slurry is used to make a wet paper. The wetlaid papermaking step may be performed by a conventional method. For example, the wetlaid papermaking step may include a wire part, a press part, a dryer part, and a calendar part, and it is more preferable to include the wire part, the press part, the dryer part, and the calendar part in this order. In addition, before the wire part, defibration using a refiner or beater may be performed as necessary, within a range that does not impair the effects of the present invention. In the wetlaid papermaking step, the basis weight of the obtained wetlaid nonwoven fabric is 30 to 80 g / m 2 It is preferable to adjust the thickness to 40 to 70 g / m 2In the wet papermaking process, the thickness of the resulting wetlaid nonwoven fabric is preferably adjusted to 0.1 to 0.5 mm, and more preferably adjusted to 0.2 to 0.35 mm.
[0029] <Conductive performance of the obtained wet-laid nonwoven fabric> The wetlaid nonwoven fabric obtained by the manufacturing method of the present invention exhibits electrical conductivity because it contains specific carbon fibers. A preferred example of the electrical conductivity of the wetlaid nonwoven fabric obtained by the manufacturing method of the present invention is a volume resistivity determined by the following method of preferably 20 Ω cm or less, more preferably 10 Ω cm or less.
[0030] <Method of measuring and calculating the volume resistivity of wet nonwoven fabric> A card-type multimeter MT-4050 manufactured by Mother Tools Co., Ltd. was used to measure the resistance, and a wet nonwoven fabric was cut into a rectangle measuring 5 mm in length and 150 mm in width to serve as the measurement sample. Test leads attached to the measurement device were connected to the vertical center of the measurement sample and 5 mm from one end in the horizontal direction (longitudinal direction), and to the vertical center of the measurement sample and 5 mm from the other end in the horizontal direction (longitudinal direction), and the mode knob was set to resistance measurement (Ω), and the resistance value (kΩ) at that time was measured. The volume resistivity (Ω·cm) was then calculated using the obtained resistance value according to the following formula (1). Volume resistivity (Ω cm) = resistance value (kΩ) × 50 × thickness of wet nonwoven fabric (mm) / 15 Formula (1)
[0031] <Uses of the wetlaid nonwoven fabric obtained by the production method of the present invention> The wet nonwoven fabric obtained by the manufacturing method of the present invention exhibits conductive performance because it contains specific carbon fibers. Therefore, the wet nonwoven fabric is suitable for wearable devices. The wearable device to which the wet nonwoven fabric obtained by the manufacturing method of the present invention is applied is not particularly limited, and examples thereof include wearable devices in which the wet nonwoven fabric obtained by the manufacturing method of the present invention is arranged so as to contact or adhere to the skin of the user. Specifically, examples of the wearable device include a wearable device in which the wet nonwoven fabric obtained by the manufacturing method of the present invention is used as a bioinformation sensor for the user, and a wearable device in which the wet nonwoven fabric is used as a sensor for measuring clothing pressure, sole pressure, etc. In addition, the wet nonwoven fabric obtained by the manufacturing method of the present invention can be made excellent in flexibility because the carbon material is fibrous. Therefore, for example, the wet nonwoven fabric obtained by the manufacturing method of the present invention can be used as a wiring part of a wearable device having flexibility. Furthermore, the wearable device can be one other than one in which the wet nonwoven fabric obtained by the manufacturing method of the present invention is used as a capacitor electrode. EXAMPLES
[0032] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the examples.
[0033] Example 1 <Preparation process> As fibrous carbon materials, carbon fiber with an average fiber length of 50 cm (manufactured by Osaka Gas Chemicals Co., Ltd., product name: DonaCarbo S-210, isotropic pitch carbon fiber with an average fiber diameter of 13 μm) and fibrous activated carbon (manufactured by Unitika Ltd., product name: Ador A-7, specific surface area 850 m) were used. 2 / g, average fiber diameter 17 μm, average fiber length 50 cm). As materials other than the fibrous carbon material, wood pulp, polyethylene terephthalate fiber, and polyolefin fiber were prepared.
[0034] <Slurry preparation process> The above prepared materials were pulverized and mixed using a pulper so that the mass ratio of the non-volatile components was carbon fiber / fibrous activated carbon / (wood pulp + polyethylene terephthalate fiber + polyolefin fiber) = 10 / 30 / 60, and a uniformly dispersed slurry was prepared.
[0035] <Wet paper making process> The prepared slurry was passed through a refiner, then poured onto a wire and dehydrated to adjust the basis weight.Then, the sheet was passed through a press part, dried in a dryer part, smoothed in a calendar part, and wound on a reel to produce a wet-laid nonwoven fabric by a wet papermaking method.
[0036] Comparative Example 1 A wetlaid nonwoven fabric of Comparative Example 1 was produced under the same conditions as in Example 1, except that the carbon fiber used was a carbon fiber having an average fiber length of 5.5 mm (manufactured by Osaka Gas Chemicals Co., Ltd., product name: DonaCarbo S-232, isotropic pitch carbon fiber having an average fiber diameter of 13 μm).
[0037] Example 2 <Preparation process> As fibrous carbon materials, carbon fiber with an average fiber length of 50 cm (manufactured by Osaka Gas Chemicals Co., Ltd., product name: DonaCarbo S-210, isotropic pitch carbon fiber with an average fiber diameter of 13 μm) and fibrous activated carbon (manufactured by Unitika Ltd., product name: Ador A-7, specific surface area 850 m) were used. 2 / g, average fiber diameter 17 μm, average fiber length 50 cm). As materials other than the fibrous carbon material, wood pulp, polyethylene terephthalate fiber, and polyolefin fiber were prepared.
[0038] <Slurry preparation process> The above prepared materials were pulverized and mixed using a pulper so that the mass ratio of the non-volatile components was carbon fiber / fibrous activated carbon / (wood pulp + polyethylene terephthalate fiber + polyolefin fiber) = 20 / 20 / 60, and a uniformly dispersed slurry was prepared.
[0039] <Wet paper making process> The prepared slurry was passed through a refiner, then poured onto a wire and dehydrated to adjust the basis weight.Then, the sheet was passed through a press part, dried in a dryer part, smoothed in a calendar part, and wound on a reel to produce a wet-laid nonwoven fabric by a wet papermaking method.
[0040] Comparative Example 2 A wetlaid nonwoven fabric of Comparative Example 2 was produced under the same conditions as in Example 2, except that the carbon fiber used was a carbon fiber having an average fiber length of 5.5 mm (manufactured by Osaka Gas Chemicals Co., Ltd., product name: DonaCarbo S-232, isotropic pitch carbon fiber having an average fiber diameter of 13 μm).
[0041] Evaluation method Each of the Examples and Comparative Examples was evaluated by the following methods.
[0042] <1m of wet nonwoven fabric 2 Mass per> According to JIS L 1913:2010 6.2, the mass per unit area of wet nonwoven fabric (g / m 2 ) was weighed.
[0043] <Thickness of wet nonwoven fabric> The wet nonwoven fabric was cut into a rectangle measuring 10 cm x 15 cm to prepare a measurement sample. The thickness of the nonwoven fabric was measured at the four corners of the sample using a thickness measuring device (a dial thickness gauge manufactured by Mitutoyo Corporation), and the average value of the four thickness measurements at the four corners was recorded as the sheet thickness (mm).
[0044] <Resistance and volume resistivity of wet nonwoven fabric> The resistance was measured using a card-type multimeter MT-4050 manufactured by Mother Tools Co., Ltd. The wet nonwoven fabric was cut into a rectangle measuring 5 mm in length and 150 mm in width to serve as the measurement sample, and test leads attached to the measurement device were connected to the vertical center of the measurement sample and 5 mm from one end in the horizontal direction (longitudinal direction), and to the vertical center of the measurement sample and 5 mm from the other end in the horizontal direction (longitudinal direction), and the mode knob was set to resistance measurement (Ω) to measure the resistance value (kΩ). The volume resistivity (Ω·cm) was calculated using the obtained resistance value according to the following formula. Volume resistivity (Ω cm) = Resistance value (kΩ) × 50 × wet nonwoven fabric thickness (mm) / 15
[0045] The physical properties of each of the examples and comparative examples are shown in Table 1.
[0046] [Table 1]
[0047] Comparing Example 1 with Comparative Example 1, and Example 2 with Comparative Example 2, it was found that Examples 1 and 2 were produced by a wetlaid nonwoven fabric production method including a preparation step of preparing carbon fibers having an average fiber length of 10 cm or more, a slurry preparation step of preparing a slurry using the carbon fibers, and a wetlaid papermaking step of wetlaid papermaking using the prepared slurry. As a result, it became clear that the resistance value and volume resistivity were both low, and that this contributes to improving the conductive performance of the wetlaid nonwoven fabric when a wetlaid nonwoven fabric containing carbon fibers as a fibrous carbon material is obtained.
Claims
1. A preparation step of preparing carbon fibers having an average fiber length of 40 cm or more and fibrous activated carbon; a slurry preparation step of preparing a slurry using the carbon fiber and the fibrous activated carbon; And a wet papermaking process of wet papermaking using the prepared slurry; A method for producing a wetlaid nonwoven fabric, comprising: The fibrous activated carbon is produced by activating an infusible fibrous material, The method for producing a wetlaid nonwoven fabric, wherein the carbon fiber is other than the fibrous activated carbon.
2. A method for producing a wet nonwoven fabric according to claim 1, wherein a mass ratio of the fibrous activated carbon to the carbon fibers in the slurry in the slurry preparation step (mass of fibrous activated carbon / mass of carbon fibers) is 0.8 to 1.2 (excluding 0.8); The wetlaid nonwoven fabric has a volume resistivity of 10 Ω cm or less, as determined by the following method: <Method of measuring and calculating the volume resistivity of wet-laid nonwoven fabric> A card-type multimeter MT-4050 manufactured by Mother Tools Co., Ltd. is used as a resistance measurement device, and a measurement sample is prepared by cutting a wet nonwoven fabric into a rectangle of 5 mm length and 150 mm width. Test leads attached to the measurement device are connected to a portion of the measurement sample that is 5 mm from the center of the length and one end of the width (longitudinal direction) and a portion of the measurement sample that is 5 mm from the center of the length and the other end of the width (longitudinal direction), and the mode knob is set to resistance measurement (Ω), and the resistance value (kΩ) at that time is measured. The volume resistivity (Ω cm) is calculated using the obtained resistance value according to the following formula (1). Volume resistivity (Ω・cm) = resistance value (kΩ) × 50 × wet nonwoven fabric thickness (mm) / 15 ... formula (1)
Citation Information
Patent Citations
Carbon fiber sheet and its manufacturing method
JP2004214072A
Dispersion device and dispersion method, and dispersion treating liquid, and wet type nonwoven fabric
JP2016117030A
JP2017-1011124A
Fabric for wearable device and wearable device including same
JP7526978B2
Conductive elastic knitted fabric and conductive parts having electrical resistance variable characteristic
WO2017010236A1