A kind of high thermal conductivity aramid insulation paper for electrical equipment, preparation method and application

Through the composite spinning technology of graphene, graphene oxide, boron nitride nanotubes and aramid fibers, the problem of poor thermal conductivity of the insulating system of oil-immersed transformer under high thermal loads is solved, and high thermal conductivity and mechanical strength are achieved The improvement is suitable for large capacity and high power electrical equipment.

CN118621613BActive Publication Date: 2024-11-22SICHUAN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411029864.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing oil-immersed transformer insulation system has poor thermal conductivity under high thermal loads, resulting in aging and failure, limiting its use in high thermal load applications.

Method used

Using composite spinning technology of graphene, graphene oxide, boron nitride nanotubes and aramid fibers, high thermal conductivity insulating paper is prepared by wet spinning, combining the aminoation treatment of boron nitride nanotubes and aramid short cutting The physical entanglement and hydrogen bond interaction of fibers improve thermal conductivity and mechanical strength.

Benefits of technology

It significantly improves the thermal conductivity of insulating paper while maintaining high mechanical strength, making it have wide application prospects in large capacity and high power electrical equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621613B_ABST
    Figure CN118621613B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of insulating materials, and discloses a high thermal conductivity aramid insulating paper for electrical equipment, a preparation method and an application thereof, comprising the following steps: step 1: obtaining GO / graphene fiber by wet spinning; step 2: using BNNT-NH2 spinning solution as a core layer and aramid nanofiber ANF spinning solution as a skin layer, and obtaining BNNT-NH2@ANF composite fiber by wet spinning; step 3: respectively beating GO / graphene fiber, BNNT-NH2@ANF composite fiber and AF, filtering and drying to obtain three kinds of fiber pulp; step 4: fully mixing the three kinds of fiber pulp to prepare AF / (GO / graphene) / BNNT-NH2@ANF insulating paper; the high thermal conductivity aramid insulating paper obtained by the invention can significantly improve the thermal conductivity while still maintaining very high mechanical strength, and has broad application prospects in large-capacity and high-power electrical equipment such as transformers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of insulating materials, and in particular to a high thermal conductivity aramid insulating paper for electrical equipment, a preparation method and an application thereof. Background Art

[0002] Oil-paper insulators are the main form of insulation inside power transformers and are one of the most important structures to ensure their safe and reliable operation. Among all types of oil-immersed transformer accidents, accidents caused by aging of the insulation system inside the transformer account for the vast majority. However, during the operation of oil-immersed transformers, the insulation system may gradually lose its original performance due to thermal aging, mechanical wear or chemical degradation. This aging process is often the main cause of transformer failure.

[0003] Aramid fiber is widely used in insulation materials. Its chemical stability and excellent mechanical properties make it an ideal choice for improving the reliability of transformer insulation systems. However, the poor thermal conductivity of aramid fiber limits its use in high heat load applications. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a high thermal conductivity aramid insulation paper for electrical equipment, a preparation method and an application thereof.

[0005] The technical solution adopted by the present invention is: a method for preparing high thermal conductivity aramid insulation paper for electrical equipment, comprising the following steps:

[0006] Step 1: Mix graphene and graphene oxide (GO) dispersion to obtain GO / graphene fibers by wet spinning;

[0007] Step 2: amination treatment of boron nitride nanotubes BNNT to obtain BNNT-NH2; using BNNT-NH2 spinning solution as the core layer and aramid nanofiber ANF spinning solution as the skin layer, wet spinning is performed to obtain BNNT-NH2@ANF composite fibers;

[0008] Step 3: GO / graphene fiber, BNNT-NH2@ANF composite fiber and aramid short fiber AF are pulped, filtered and dried to obtain three kinds of fiber pulp;

[0009] Step 4: Fully mix the three fiber pulps in step 3 to prepare AF / (GO / graphene) / BNNT-NH2@ANF fiber base paper, i.e. the required insulating paper.

[0010] Furthermore, in step 1, the mass ratio of GO to graphene is 1-2:40-50; the spinning rate in the wet spinning is 0.03 mL / min, and the coagulation bath is an ethyl acetate solution.

[0011] Furthermore, in the step 2, the mass ratio of ANF to BNNT-NH2 in the BNNT-NH2@ANF composite fiber is 2-10:1-3.

[0012] Furthermore, in step 2, the BNNT amination treatment is performed by plasma treatment;

[0013] The plasma treatment parameters were as follows: peak voltage of 9.5 kV, frequency of 13.56 MHz, and discharge power of 100 W.

[0014] Furthermore, in step 2, the wet-spun skin layer and core layer are extruded simultaneously at 0.03 mL / min and immersed in the first coagulation bath; after solidification and forming in the first coagulation bath, the formed fiber is pulled at a speed of 0.08 mL / min and transitioned to the second coagulation bath; wherein the first coagulation bath is a mixed solution composed of dimethyl sulfoxide, deionized water and ethanol in a volume ratio of 100:900:0.5, and the second coagulation bath is deionized water.

[0015] Furthermore, in step 3, the GO / graphene fiber, BNNT-NH2@ANF composite fiber, and aramid chopped fiber are first pretreated.

[0016] The pretreatment process of aramid chopped fiber is as follows:

[0017] Soak the aramid chopped fibers in a sodium dodecylbenzene sulfonate solution for 2 to 3 hours, wash and dry them;

[0018] The pretreatment process of GO / graphene fiber and BNNT-NH2@ANF composite fiber is as follows:

[0019] Under vacuum conditions, first treat at 60-80 °C for 1 h, and then treat at 120-150 °C for 2 h.

[0020] Furthermore, in step 4, the mass ratio of GO / graphene fiber, BNNT-NH2@ANF composite fiber and AF pulp is 1-2:1-2:10.

[0021] Furthermore, in step 4, the three types of fiber pulp are dissociated at 4000-5000 r / min for 10-15 min; a dispersant is added, and the mixed slurry is wet-coated and dried to obtain the desired insulating paper;

[0022] The net concentration of wet papermaking is 0.06-0.08 wt%, the drying temperature is 100-120 ℃, and the drying time is 2-3 h.

[0023] A high thermal conductivity aramid insulation paper for electrical equipment, wherein the thickness of the high thermal conductivity aramid insulation paper is 100-120 μm.

[0024] An application of high thermal conductivity aramid insulation paper for electrical equipment, wherein the high thermal conductivity aramid insulation paper is used for electrical equipment.

[0025] The beneficial effects of the present invention are:

[0026] The present invention grafts amino groups on the surface of boron nitride nanotubes to further prepare BNNT-NH2@ANF composite fibers; the three types of fibers, GO / graphene fibers, BNNT-NH2@ANF composite fibers and aramid chopped fibers, are mixed, which not only retains the high thermal conductivity of graphite and BNNT, but also the composite fibers and AF chopped fibers are physically entangled and hydrogen-bonded to interact with each other, so that the prepared high thermal conductivity aramid insulation paper can significantly improve the thermal conductivity while still maintaining very high mechanical strength, and has broad application prospects in large-capacity and high-power electrical equipment such as transformers. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a SEM image of graphene used in an embodiment of the present invention.

[0028] Figure 2 This is a SEM image of the aramid fiber used in the embodiment of the present invention.

[0029] Figure 3 This is a SEM image of the BNNT used in the embodiment of the present invention.

[0030] Figure 4 This is a test diagram of the thermal conductivity of the insulating paper obtained in Comparative Example 1 and Examples 1 to 8 of the present invention.

[0031] Figure 5 This is a test diagram of the thermal conductivity of the insulating paper obtained in Comparative Examples 1 to 8 of the present invention.

[0032] Figure 6 This is a cross-sectional SEM image of the composite insulating paper obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0034] A method for preparing high thermal conductivity aramid insulation paper for electrical equipment comprises the following steps:

[0035] Step 1: Mix graphene and graphene oxide (GO) dispersion to obtain GO / graphene fibers by wet spinning;

[0036] Graphene oxide GO and graphene are mixed in a solvent to obtain a uniformly dispersed spinning solution. GO is a thin sheet with a diameter of 30 to 50 μm, and graphene is a plate-like particle with a diameter of about 3 μm. There are a large number of functional groups (such as -OH, -COOH, -O-) on the surface of GO, which can be stably dispersed in polar solvents such as water, N,N-dimethylformamide DMF and ethanol to obtain a GO dispersion. Graphene particles are added to the GO dispersion to obtain a GO / graphene spinning solution. The mass ratio of GO to graphene is 1 to 2:40 to 50. The SEM image of the graphene used in the present invention is shown as follows Figure 1 shown.

[0037] The GO / graphene spinning solution was placed in a syringe and spun into a coagulation bath containing ethyl acetate using a 27-gauge needle at a rate of 0.03 mL / min to obtain GO / graphene fibers. After the GO / graphene fibers were coagulated in the coagulation bath, they were wound with a roller at a collection rate of 1.0 mL / min and dried by irradiation with a thermal infrared lamp. The rolled GO / graphene fibers were placed in a vacuum oven at 60 °C to dry and remove residual solvent and moisture.

[0038] Step 2: amination treatment of boron nitride nanotubes BNNT to obtain BNNT-NH2, and mixing with a solvent to obtain a BNNT-NH2 spinning solution; using the BNNT-NH2 spinning solution as the core layer and the aramid nanofiber ANF spinning solution as the skin layer, a BNNT-NH2@ANF composite fiber is obtained by wet spinning;

[0039] The BNNT amination is carried out by plasma treatment:

[0040] The peak voltage of the plasma generator is 9.5 kV, the frequency is 13.65 MHz, and the discharge power is 100 W. Argon plasma is used in continuous wave mode to clean and activate the surface of BNNT. NH3 plasma is treated in P (pulse) mode for 2 min to provide etching and formation of amino functional groups on the surface of BNNT to obtain BNNT-NH2. The SEM of BNNT used in the present invention is as follows: Figure 3 shown.

[0041] The preparation process of BNNT-NH2 spinning solution is as follows:

[0042] BNNT-NH2 is mixed with dimethyl sulfoxide (DMSO) to obtain BNNT-NH2 / DMSO spinning solution.

[0043] The preparation process of aramid nanofiber ANF spinning solution is as follows:

[0044] Cut the Kevlar fiber into small pieces less than 1 cm, pour acetone into it until the fiber surface is covered, and ultrasonically treat it for 24 h at a power of 500 W. After filtering the acetone, dry it in a vacuum oven at 45 °C and store it in a sealed container; weigh the treated Kevlar fiber (1.6 g) and KOH (2.4 g) and add them to a mixed solution of DMSO (320 mL) and deionized water (10 mL), stir at 30 °C in the dark for 14 days, and obtain a dark red ANF / DMSO spinning solution (1 wt%). The SEM of the Kevlar fiber (i.e., aramid fiber) used in the present invention is as follows: Figure 2 shown.

[0045] The process of preparing BNNT-NH2@ANF composite fibers by wet spinning is as follows:

[0046] The ANF / DMSO spinning solution and the BNNT-NH2 / DMSO spinning solution are placed in the syringe connecting the cortex and core tubes. The two tubes are connected by a special coaxial spinning needle. The models of the inner and outer needles are 22 G and 17 G respectively. The outer needle is connected to the ANF / DMSO spinning solution, and the inner needle is connected to the BNNT-NH2 / DMSO spinning solution. After the device is connected, the syringes containing different spinning solutions are fixed in the card slots of the dual-channel micro-injection pump respectively, and the propeller is set to extrude the two spinning solutions at a constant speed of 0.03mL / min. At the same time, ensure that the coaxial spinning needle is vertically immersed in the first coagulation bath, the components are DMSO / H2O / CH3COOH mixed solution, and the volume ratio is 100:900:0.5 mL. The fiber was initially solidified and formed in the first coagulation bath, and the formed fiber was pulled through the first coagulation bath at a constant flow rate of 0.08 mL / min and immersed in the second coagulation bath. The second coagulation bath was deionized water, and its function was to achieve complete protonation and precipitation of ANF in the fiber cortex to promote complete solidification of the fiber.

[0047] After the BNNT-NH2@ANF fibers were completely solidified, they were curled and collected, and dried in a forced air drying oven at 50 °C for 10 min to obtain BNNT-NH2@ANF composite fibers with a core-skin structure. The mass ratio of ANF to BNNT-NH2 in the BNNT-NH2@ANF composite fibers was 2-10:1-3.

[0048] Step 3: GO / graphene fiber, BNNT-NH2@ANF composite fiber and aramid short fiber AF are pulped, filtered and dried to obtain three kinds of fiber pulp;

[0049] GO / graphene fiber, BNNT-NH2@ANF composite fiber, and aramid chopped fiber were first pretreated.

[0050] The pretreatment process of aramid chopped fiber is as follows:

[0051] The aramid short fibers were soaked in sodium dodecylbenzene sulfonate solution for 2-3 h, washed and dried; the concentration of the sodium dodecylbenzene sulfonate solution was (2-3)×10 -3 mol / L, the soaking temperature is 40-60 ℃; it is washed with deionized water, and after repeated washing three times, it is dried in a vacuum drying oven at 100-120 ℃ for 1 h.

[0052] The pretreatment process of GO / graphene fiber and BNNT-NH2@ANF composite fiber is as follows:

[0053] Under vacuum conditions, first treat at 60-80 °C for 1 h, and then treat at 120-150 °C for 2 h; the negative pressure is 0.3-0.6 MPa.

[0054] The three pretreated fibers were placed in a homogenizer, deionized water was added, the speed of the homogenizer was 18000-20000 rpm / min, and the homogenization time was 10-15 min. After filtering and drying, GO / graphene fiber pulp, aramid short fiber pulp and BNNT-NH2@ANF composite fiber pulp were obtained.

[0055] Step 4: Fully mix the three fiber pulps in step 3 to prepare AF / (GO / graphene) / BNNT-NH2@ANF fiber base paper, i.e. the required insulating paper.

[0056] GO / graphene fiber pulp, BNNT-NH2@ANF composite fiber pulp and aramid short fiber pulp with a mass ratio of 1-2:1-2:10 are added to a fiber disintegrator containing deionized water and mixed evenly; the speed of the disintegrator is 4000-5000 r / min, and the disintegration time is 10-15 min. A dispersant composed of a mixture of polyethylene oxide PEO and anionic polyacrylamide APAM with a mass ratio of 6:1 is added. The amount of the dispersant added is 2-4 wt% of the dry weight of the mixed fiber. The composite dispersant is added to the dissociated GO / graphene fiber, BNNT-NH2@ANF composite fiber and aramid short fiber slurry to obtain a uniformly dispersed mixed fiber slurry.

[0057] The mixed fiber slurry is wet-papered on a paper sheet former with a web concentration of 0.06-0.08%. The paper-made mixed fiber base paper is dried in a blast oven at a temperature of 100-120 °C for 2-3 h to obtain AF / (GO / graphene) / BNNT-NH2@ANF ultrafine fiber base paper, i.e., the desired high thermal conductivity aramid insulation paper.

[0058] Example 1

[0059] A method for preparing high thermal conductivity aramid insulation paper for electrical equipment comprises the following steps:

[0060] Step 1: Mix graphene and graphene oxide (GO) dispersion to obtain GO / graphene fibers by wet spinning;

[0061] Graphene oxide GO is dispersed in N,N-dimethylformamide DMF to obtain a GO dispersion; graphene particles are added to the GO dispersion to obtain a GO / graphene spinning solution with a GO mass concentration of 1 wt% and a graphene mass concentration of 50 wt%.

[0062] The GO / graphene spinning solution was injected into a 6 ml syringe and spun into a coagulation bath containing ethyl alcohol at a rate of 0.03 mL / min using a 27-gauge needle. After the GO / graphene fiber was coagulated in the coagulation bath, it was wound with a roller at a collection rate of 1.0 mL / min and dried by irradiation with a thermal infrared lamp. The rolled GO / graphene fiber was placed in a vacuum oven at 60 °C to dry and remove the residual solvent or moisture in the fiber.

[0063] Step 2: amination treatment of boron nitride nanotubes BNNT to obtain BNNT-NH2; using BNNT-NH2 spinning solution as the core layer and aramid nanofiber ANF spinning solution as the skin layer, wet spinning is performed to obtain BNNT-NH2@ANF composite fibers;

[0064] The preparation process of BNNT-NH2 is as follows:

[0065] The peak-to-peak voltage of the plasma generator was adjusted to 9.5 kV, the frequency was 13.56 MHz, and the discharge power was 100 W. The BNNT was cleaned and surface activated with argon plasma in (continuous wave) mode. Next, NH3 plasma was treated in P (pulse) mode for 2 min to provide etching and the formation of amino functional groups on the BNNT surface to obtain BNNT-NH2.

[0066] The preparation process of aramid nanofiber ANF spinning solution is as follows:

[0067] Kevlar fiber was cut into small pieces less than 1 cm, acetone was poured into the fiber surface, and ultrasonic treatment was performed at a power of 500 W for 24 h. After filtering the acetone, it was dried in a vacuum oven at 45 °C and sealed for storage. 1.6 g of treated Kevlar fiber and 2.4 g of KOH were weighed and added to a mixed solution of 320 mL of DMSO and 10 mL of deionized water. Stirred at 30 °C in the dark for 14 d to obtain a dark red ANF / DMSO dispersion with a mass concentration of 1 wt%.

[0068] The spinning solution was prepared according to the mass ratio of ANF and BNNT-NH2 of 5:1, and the ANF / DMSO and BNNT-NH2 / DMSO spinning solutions were placed in the syringes connecting the cortex and core layer catheters. The two catheters were connected by special coaxial spinning needles, and the models of the inner and outer needles were 22 G and 17 G, respectively.

[0069] Among them, the outer needle is connected to the ANF / DMSO spinning solution, and the inner needle is connected to the BNNT-NH2 / DMSO spinning solution. After the device is connected, the syringes containing different spinning solutions are fixed in the card slots of the dual-channel microinjection pump respectively, and the propeller is set to extrude the two spinning solutions at a constant speed of 0.03 mL / min. At the same time, ensure that the coaxial spinning needle is vertically immersed in the first coagulation bath. The first coagulation bath is composed of a mixture of 100 mL of DMSO, 900 mL of H2O and 0.5 mL of CH3COOH. The fiber is initially solidified and formed in the first coagulation bath, and the fiber is pulled at a constant 0.08 mL / min to transition from the first coagulation bath and immersed in the second coagulation bath. The second coagulation bath is deionized water.

[0070] After the BNNT-NH2@ANF fiber was completely solidified, it was curled and collected, and dried in a forced air drying oven at 50 °C for 10 min to obtain a BNNT-NH2@ANF composite fiber with a skin-core structure.

[0071] Step 3: GO / graphene fiber, BNNT-NH2@ANF composite fiber and aramid short fiber AF are pulped, filtered and dried to obtain three kinds of fiber pulp;

[0072] All three types of fibers need to be pretreated first.

[0073] The pretreatment process of aramid chopped fiber is as follows:

[0074] The aramid short fibers were cut into 2 × 10 -3 The samples were immersed in a 60 ℃ sodium dodecylbenzene sulfonate solution with a temperature of 20 ℃ and 100 ℃, washed three times with deionized water, and dried in a vacuum drying oven at 100 ℃ for 1 h.

[0075] The pretreatment process of GO / graphene fiber and BNNT-NH2@ANF composite fiber is as follows:

[0076] In a vacuum drying oven, the sample was treated at 60 °C for 1 h under a negative pressure of 0.3 MPa and then at 120 °C for 2 h.

[0077] Then the three pretreated fibers were placed in a homogenizer separately, and deionized water was added to each fiber. The speed of the homogenizer was 18000 rpm / min, and the homogenization time was 15 min. The fibers were pulped with water as the dispersion medium for 30 min to obtain a slurry. The slurry was filtered and dried to obtain three kinds of fiber pulp.

[0078] Step 4: Add 1 g of aramid chopped fiber pulp, 0.1 g of GO / graphene fiber pulp and 0.1 g of BNNT-NH2@ANF composite fiber pulp into a fiber dissociator containing 500 mL of deionized water and mix them evenly. The speed of the dissociator is 5000 r / min and the dissociation time is 15 min.

[0079] PEO and APAM with a mass ratio of 6:1 were used as dispersants, and the amount of dispersant added was 2% of the dry weight of the mixed fiber. The dispersant was added to the dissociated slurry to obtain a uniformly dispersed mixed fiber slurry. The mixed fiber slurry was wet-coated on a paper sheet former with a web concentration of 0.06%. The paper-coated mixed fiber base paper was dried in a blast oven at 100°C for 2 h to obtain AF / (GO / graphene) / BNNT-NH2@ANF fiber base paper, which was the required insulating paper.

[0080] The SEM image of the composite insulating paper obtained in this embodiment is as follows: Figure 6 As shown in the figure, it can be seen that the composite insulating pulp is tightly connected. Due to the interaction between the amide groups between ANF, the hydroxyl groups on the surface of GO and the amino groups on the surface of functionalized BNNT-NH2, a dense structure is formed by the fiber overlap "bridge" between the layers.

[0081] Example 2

[0082] The other steps of this embodiment are the same as those of embodiment 1, except that the amount of GO / graphene pulp added in step 4 is 0.15 g.

[0083] Example 3

[0084] The other steps of this embodiment are the same as those of embodiment 1, except that the amount of GO / graphene pulp added in step 4 is 0.2 g.

[0085] Example 4

[0086] The other steps of this embodiment are the same as those of embodiment 1, except that in step 2, the spinning solution is prepared according to the mass ratio of ANF and BNNT-NH2 of 10:3.

[0087] Example 5

[0088] The other steps of this embodiment are the same as those of embodiment 1, except that in step 2, the spinning solution is prepared according to the mass ratio of ANF to BNNT-NH2 of 5:2.

[0089] Example 6

[0090] The other steps of this embodiment are the same as those of embodiment 1, except that in step 2, the spinning solution is prepared according to the mass ratio of ANF and BNNT-NH2 of 2:1.

[0091] Example 7

[0092] The other steps of this embodiment are the same as those of embodiment 1, except that in step 4, the amount of BNNT-NH2@ANF composite fiber pulp added is 0.15 g.

[0093] Example 8

[0094] The other steps of this embodiment are the same as those of embodiment 1, except that in step 4, the amount of BNNT-NH2@ANF composite fiber pulp added is 0.2 g.

[0095] Example 9

[0096] A method for preparing high thermal conductivity aramid insulation paper for electrical equipment comprises the following steps:

[0097] Step 1: Mix graphene and graphene oxide (GO) dispersion to obtain GO / graphene fibers by wet spinning;

[0098] Graphene oxide GO is dispersed in N,N-dimethylformamide DMF to obtain a GO dispersion; graphene particles are added to the GO dispersion to obtain a GO / graphene spinning solution with a GO mass concentration of 1 wt% and a graphene mass concentration of 40 wt%.

[0099] The GO / graphene spinning solution was injected into a 6 ml syringe and spun into a coagulation bath containing ethyl alcohol at a rate of 0.03 mL / min using a 27-gauge needle. After the GO / graphene fiber was coagulated in the coagulation bath, it was wound with a roller at a collection rate of 1.0 mL / min and dried by irradiation with a thermal infrared lamp. The rolled GO / graphene fiber was placed in a vacuum oven at 60 °C to dry and remove the residual solvent or moisture in the fiber.

[0100] Step 2: amination treatment of boron nitride nanotubes BNNT to obtain BNNT-NH2; using BNNT-NH2 spinning solution as the core layer and aramid nanofiber ANF spinning solution as the skin layer, wet spinning is performed to obtain BNNT-NH2@ANF composite fibers;

[0101] The preparation process of BNNT-NH2 is as follows:

[0102] The peak-to-peak voltage of the plasma generator was adjusted to 9.5 kV, the frequency was 13.56 MHz, and the discharge power was 100 W. The BNNT was cleaned and surface activated with argon plasma in (continuous wave) mode. Next, NH3 plasma was treated in P (pulse) mode for 2 min to provide etching and the formation of amino functional groups on the BNNT surface to obtain BNNT-NH2.

[0103] The preparation process of aramid nanofiber ANF spinning solution is as follows:

[0104] Kevlar fiber was cut into small pieces less than 1 cm, acetone was poured into the fiber surface, and ultrasonic treatment was performed at a power of 500 W for 24 h. After filtering the acetone, it was dried in a vacuum oven at 45 °C and sealed for storage. 1.6 g of treated Kevlar fiber and 2.4 g of KOH were weighed and added to a mixed solution of 320 mL of DMSO and 10 mL of deionized water. Stirred at 30 °C in the dark for 14 d to obtain a dark red ANF / DMSO dispersion with a mass concentration of 1 wt%.

[0105] The spinning solution was prepared according to the mass ratio of ANF and BNNT-NH2 of 5:1, and the ANF / DMSO and BNNT-NH2 / DMSO spinning solutions were placed in the syringes connecting the cortex and core layer catheters. The two catheters were connected by special coaxial spinning needles, and the models of the inner and outer needles were 22 G and 17 G, respectively.

[0106] Among them, the outer needle is connected to the ANF / DMSO spinning solution, and the inner needle is connected to the BNNT-NH2 / DMSO spinning solution. After the device is connected, the syringes containing different spinning solutions are fixed in the card slots of the dual-channel microinjection pump respectively, and the propeller is set to extrude the two spinning solutions at a constant speed of 0.03 mL / min. At the same time, ensure that the coaxial spinning needle is vertically immersed in the first coagulation bath. The first coagulation bath is composed of a mixture of 100 mL of DMSO, 900 mL of H2O and 0.5 mL of CH3COOH. The fiber is initially solidified and formed in the first coagulation bath, and the fiber is pulled at a constant 0.08 mL / min to transition from the first coagulation bath and immersed in the second coagulation bath. The second coagulation bath is deionized water.

[0107] After the BNNT-NH2@ANF fiber was completely solidified, it was curled and collected, and dried in a forced air drying oven at 50 °C for 10 min to obtain a BNNT-NH2@ANF composite fiber with a skin-core structure.

[0108] Step 3: GO / graphene fiber, BNNT-NH2@ANF composite fiber and aramid short fiber AF are pulped, filtered and dried to obtain three kinds of fiber pulp;

[0109] All three types of fibers need to be pretreated first.

[0110] The pretreatment process of aramid chopped fiber is as follows:

[0111] The aramid short fibers were cut into 3 × 10 -3 The samples were immersed in a 40 ℃ sodium dodecylbenzene sulfonate solution with a temperature of 100 ℃ and 30 mol / L for 3 h, washed with deionized water for 3 times, and dried in a vacuum drying oven at 120 ℃ for 1 h.

[0112] The pretreatment process of GO / graphene fiber and BNNT-NH2@ANF composite fiber is as follows:

[0113] In a vacuum drying oven, the sample was treated at 80 °C for 1 h under a negative pressure of 0.6 MPa and then at 150 °C for 2 h.

[0114] Then the three pretreated fibers were placed in a homogenizer separately, and deionized water was added to each fiber. The speed of the homogenizer was 20,000 rpm / min, and the homogenization time was 10 min. The fibers were pulped with water as the dispersion medium for 30 min to obtain a slurry. The slurry was filtered and dried to obtain three kinds of fiber pulp.

[0115] Step 4: Add 1 g of aramid chopped fiber pulp, 0.1 g of GO / graphene fiber pulp and 0.1 g of BNNT-NH2@ANF composite fiber pulp into a fiber dissociator containing 500 mL of deionized water and mix them evenly. The speed of the dissociator is 4000 r / min and the dissociation time is 10 min.

[0116] PEO and APAM with a mass ratio of 6:1 were used as dispersants, and the amount of dispersant added was 4% of the dry weight of the mixed fiber. The dispersant was added to the dissociated slurry to obtain a uniformly dispersed mixed fiber slurry. The mixed fiber slurry was wet-coated on a paper sheet former with a web concentration of 0.08%. The paper-coated mixed fiber base paper was dried in a blast oven at 120°C for 3 h to obtain AF / (GO / graphene) / BNNT-NH2@ANF fiber base paper, which was the required insulating paper.

[0117] Example 10

[0118] A method for preparing high thermal conductivity aramid insulation paper for electrical equipment comprises the following steps:

[0119] Step 1: Mix graphene and graphene oxide (GO) dispersion to obtain GO / graphene fibers by wet spinning;

[0120] Graphene oxide GO is dispersed in N,N-dimethylformamide DMF to obtain a GO dispersion; graphene particles are added to the GO dispersion to obtain a GO / graphene spinning solution with a GO mass concentration of 2 wt% and a graphene mass concentration of 40 wt%.

[0121] The GO / graphene spinning solution was injected into a 6 ml syringe and spun into a coagulation bath containing ethyl alcohol at a rate of 0.03 mL / min using a 27-gauge needle. After the GO / graphene fiber was coagulated in the coagulation bath, it was wound with a roller at a collection rate of 1.0 mL / min and dried by irradiation with a thermal infrared lamp. The rolled GO / graphene fiber was placed in a vacuum oven at 60 °C to dry and remove the residual solvent or moisture in the fiber.

[0122] Step 2: amination treatment of boron nitride nanotubes BNNT to obtain BNNT-NH2; using BNNT-NH2 spinning solution as the core layer and aramid nanofiber ANF spinning solution as the skin layer, wet spinning is performed to obtain BNNT-NH2@ANF composite fibers;

[0123] The preparation process of BNNT-NH2 is as follows:

[0124] The peak-to-peak voltage of the plasma generator was adjusted to 9.5 kV, the frequency was 13.56 MHz, and the discharge power was 100 W. The BNNT was cleaned and surface activated with argon plasma in (continuous wave) mode. Next, NH3 plasma was treated in P (pulse) mode for 2 min to provide etching and the formation of amino functional groups on the BNNT surface to obtain BNNT-NH2.

[0125] The preparation process of aramid nanofiber ANF spinning solution is as follows:

[0126] Kevlar fiber was cut into small pieces less than 1 cm, acetone was poured into the fiber surface, and ultrasonic treatment was performed at a power of 500 W for 24 h. After filtering the acetone, it was dried in a vacuum oven at 45 °C and sealed for storage. 1.6 g of treated Kevlar fiber and 2.4 g of KOH were weighed and added to a mixed solution of 320 mL of DMSO and 10 mL of deionized water. Stirred at 30 °C in the dark for 14 d to obtain a dark red ANF / DMSO dispersion with a mass concentration of 1 wt%.

[0127] The spinning solution was prepared according to the mass ratio of ANF and BNNT-NH2 of 5:1, and the ANF / DMSO and BNNT-NH2 / DMSO spinning solutions were placed in the syringes connecting the cortex and core layer catheters. The two catheters were connected by special coaxial spinning needles, and the models of the inner and outer needles were 22 G and 17 G, respectively.

[0128] Among them, the outer needle is connected to the ANF / DMSO spinning solution, and the inner needle is connected to the BNNT-NH2 / DMSO spinning solution. After the device is connected, the syringes containing different spinning solutions are fixed in the card slots of the dual-channel microinjection pump respectively, and the propeller is set to extrude the two spinning solutions at a constant speed of 0.03 mL / min. At the same time, ensure that the coaxial spinning needle is vertically immersed in the first coagulation bath. The first coagulation bath is composed of a mixture of 100 mL of DMSO, 900 mL of H2O and 0.5 mL of CH3COOH. The fiber is initially solidified and formed in the first coagulation bath, and the fiber is pulled at a constant 0.08 mL / min to transition from the first coagulation bath and immersed in the second coagulation bath. The second coagulation bath is deionized water.

[0129] After the BNNT-NH2@ANF fiber was completely solidified, it was curled and collected, and dried in a forced air drying oven at 50 °C for 10 min to obtain a BNNT-NH2@ANF composite fiber with a skin-core structure.

[0130] Step 3: GO / graphene fiber, BNNT-NH2@ANF composite fiber and aramid short fiber AF are pulped, filtered and dried to obtain three kinds of fiber pulp;

[0131] All three types of fibers need to be pretreated first.

[0132] The pretreatment process of aramid chopped fiber is as follows:

[0133] The aramid short fibers were cut into 2.5 × 10 -3 The samples were immersed in a 50 ℃ sodium dodecylbenzene sulfonate solution with a temperature of 2.5 h, washed three times with deionized water, and dried in a vacuum drying oven at 110 ℃ for 1 h.

[0134] The pretreatment process of GO / graphene fiber and BNNT-NH2@ANF composite fiber is as follows:

[0135] In a vacuum drying oven, the sample was treated at 70 °C for 1 h under a negative pressure of 0.5 MPa and then at 130 °C for 2 h.

[0136] Then the three pretreated fibers were placed in a homogenizer separately, and deionized water was added to each fiber. The speed of the homogenizer was 19000 rpm / min, and the homogenization time was 13 min. The fibers were pulped with water as the dispersion medium for 30 min to obtain a slurry. The slurry was filtered and dried to obtain three kinds of fiber pulp.

[0137] Step 4: Add 1 g of aramid chopped fiber pulp, 0.1 g of GO / graphene fiber pulp and 0.1 g of BNNT-NH2@ANF composite fiber pulp into a fiber dissociator containing 500 mL of deionized water and mix them evenly. The speed of the dissociator is 4500 r / min and the dissociation time is 13 min.

[0138] PEO and APAM with a mass ratio of 6:1 were used as dispersants, and the amount of dispersant added was 3% of the dry weight of the mixed fiber. The dispersant was added to the dissociated slurry to obtain a uniformly dispersed mixed fiber slurry. The mixed fiber slurry was wet-coated on a paper sheet former with a web concentration of 0.07%. The paper-coated mixed fiber base paper was dried in a blast oven at 110°C for 2.5 h to obtain AF / (GO / graphene) / BNNT-NH2@ANF fiber base paper, which was the required insulating paper.

[0139] Comparative Example 1

[0140] The insulating paper was prepared by the following method:

[0141] Step 1: Cut the aramid short fibers into 2×10 -3 The samples were immersed in a 60 ℃ sodium dodecylbenzene sulfonate solution with a temperature of 20 ℃ and 100 ℃, and then washed three times with deionized water. Finally, they were dried in a vacuum drying oven at 100 ℃ for 1 h until they were absolutely dry.

[0142] Step 2, weighing 1 g of aramid short fiber pulp, adding it into a fiber disintegrator containing 500 ml of deionized water and mixing it evenly, the disintegrator speed is 5000 r / min, and the disintegration time is 15 min; PEO and APAM are used as dispersants, and the addition amount is 2% of the total dry weight of the mixed fiber, and the ratio of PEO to APAM is 6:1; the composite dispersant is added into the dissociated AF ultrafine fiber slurry to prepare a uniformly dispersed mixed fiber slurry; the above slurry is directly wet-coated on a paper sheet former with a web concentration of 0.06%; the mixed fiber base paper is dried in a blast oven at a temperature of 100°C for 2 h to obtain the AF ultrafine fiber base paper.

[0143] Comparative Example 2

[0144] The insulating paper was prepared by the following method:

[0145] Step 1: Amination treatment of boron nitride nanotubes (BNNT) was performed to obtain BNNT-NH2; BNNT-NH2 spinning solution was used as the core layer, and aramid nanofiber (ANF) spinning solution was used as the skin layer to obtain BNNT-NH2@ANF composite fibers by wet spinning;

[0146] The specific process is the same as that of Example 1.

[0147] Step 2:

[0148] The aramid short fibers were cut into 2 × 10 -3 The samples were immersed in a 60 ℃ sodium dodecylbenzene sulfonate solution with a temperature of 20 ℃ and 100 ℃, washed three times with deionized water, and dried in a vacuum drying oven at 100 ℃ for 1 h.

[0149] The preprocessing process is as follows:

[0150] The BNNT-NH2@ANF composite fibers were placed in a vacuum drying oven and treated at 60 °C for 1 h under a negative pressure of 0.3 MPa, and then heated to 120 °C for 2 h.

[0151] The two pretreated fibers were placed in a homogenizer separately, and deionized water was added to each fiber. The speed of the homogenizer was 19000 rpm / min, and the homogenization time was 13 min. The fibers were pulped with water as the dispersion medium for 30 min to obtain a slurry. The slurry was filtered and dried to obtain two types of fiber pulp.

[0152] Step 3: Add 1 g of aramid chopped fiber pulp, 0.1 g of graphene, 0.002 g of GO and 0.1 g of BNNT-NH2@ANF composite fiber pulp into a fiber dissociator containing 500 mL of deionized water and mix them evenly. The speed of the dissociator is 5000 r / min and the dissociation time is 15 min.

[0153] PEO and APAM with a mass ratio of 6:1 were used as dispersants, and the amount of dispersant added was 2% of the dry weight of the mixed fiber. The dispersant was added to the dissociated slurry to obtain a uniformly dispersed mixed fiber slurry. The mixed fiber slurry was wet-coated on a paper sheet former with a web concentration of 0.06%. The paper-coated mixed fiber base paper was dried in a blast oven at a temperature of 100°C for 2 h to obtain insulating paper.

[0154] Comparative Example 3

[0155] The other steps of Comparative Example 3 are the same as those of Comparative Example 2, except that the amount of graphene added in step 3 is 0.15 g.

[0156] Comparative Example 4

[0157] The other steps of Comparative Example 4 are the same as those of Comparative Example 2, except that the amount of graphene added in step 3 is 0.2 g.

[0158] Comparative Example 5

[0159] Prepare the insulating paper as follows:

[0160] Step 1: Mix graphene and graphene oxide (GO) dispersion to obtain GO / graphene fibers by wet spinning;

[0161] The specific steps are the same as those in Example 1.

[0162] Step 2: preparing ANF fibers by wet spinning;

[0163] The preparation process of aramid nanofiber ANF spinning solution is as follows:

[0164] Kevlar fiber was cut into small pieces less than 1 cm, acetone was poured into the fiber surface, and ultrasonic treatment was performed at a power of 500 W for 24 h. After filtering the acetone, it was dried in a vacuum oven at 45 °C and sealed for storage. 1.6 g of treated Kevlar fiber and 2.4 g of KOH were weighed and added to a mixed solution of 320 mL of DMSO and 10 mL of deionized water. Stirred at 30 °C in the dark for 14 d to obtain a dark red ANF / DMSO dispersion with a mass concentration of 1 wt%.

[0165] The ANF / DMSO spinning solution was placed in a syringe with a needle of 22 G.

[0166] After the device is connected, fix the syringes in the slots of the injection pump respectively, and set the propeller to extrude the spinning solution at a constant speed of 0.03 mL / min. At the same time, ensure that the coaxial spinning needle is vertically immersed in the first coagulation bath. The first coagulation bath is composed of a mixture of 100 mL of DMSO, 900 mL of H2O and 0.5 mL of CH3COOH. The fiber is initially solidified and formed in the first coagulation bath, and the fiber is pulled at a constant speed of 0.08 mL / min to transition from the first coagulation bath and immerse in the second coagulation bath, which is deionized water.

[0167] After the ANF fiber is completely solidified, it is curled and collected, and then dried in a forced air drying oven at 50 °C for 10 min to obtain the ANF fiber.

[0168] Step 3: pulping, filtering and drying the GO / graphene fiber, ANF fiber and aramid short fiber AF respectively to obtain three kinds of fiber pulp;

[0169] All three types of fibers need to be pretreated first.

[0170] The pretreatment process of aramid chopped fiber is as follows:

[0171] The aramid short fibers were cut into 2 × 10 -3 The samples were immersed in a 60 ℃ sodium dodecylbenzene sulfonate solution with a temperature of 20 ℃ and 100 ℃, washed three times with deionized water, and dried in a vacuum drying oven at 100 ℃ for 1 h.

[0172] The pretreatment process of GO / graphene fiber and ANF fiber is as follows:

[0173] In a vacuum drying oven, the sample was treated at 60 °C for 1 h under a negative pressure of 0.3 MPa and then at 120 °C for 2 h.

[0174] Then the three pretreated fibers were placed in a homogenizer separately, and deionized water was added to each fiber. The speed of the homogenizer was 18000 rpm / min, and the homogenization time was 15 min. The fibers were pulped with water as the dispersion medium for 30 min to obtain a slurry. The slurry was filtered and dried to obtain three kinds of fiber pulp.

[0175] Step 4: Add 1 g of aramid chopped fiber pulp, 0.1 g of GO / graphene fiber pulp and 0.1 g of ANF fiber pulp into a fiber disintegrator containing 500 mL of deionized water and mix them evenly. The speed of the disintegrator is 5000 r / min and the disintegration time is 15 min.

[0176] PEO and APAM with a mass ratio of 6:1 were used as dispersants, and the amount of dispersant added was 2% of the dry weight of the mixed fiber. The dispersant was added to the dissociated slurry to obtain a uniformly dispersed mixed fiber slurry. The mixed fiber slurry was wet-coated on a paper sheet former with a web concentration of 0.06%. The paper-coated mixed fiber base paper was dried in a blast oven at a temperature of 100°C for 2 h to obtain the desired insulating paper.

[0177] Comparative Example 6

[0178] The other steps of this comparative example are the same as those of comparative example 5, except that the amount of ANF fiber pulp added in step 4 is 0.15 g.

[0179] Comparative Example 7

[0180] The other steps of this comparative example are the same as those of comparative example 5, except that the amount of ANF fiber pulp added in step 4 is 0.2 g.

[0181] Comparative Example 8

[0182] Prepare the insulating paper as follows:

[0183] Step 1: Preparation of BNNT-NH2;

[0184] The preparation process of BNNT-NH2 is as follows:

[0185] The peak-to-peak voltage of the plasma generator was adjusted to 9.5 kV, the frequency was 13.56 MHz, and the discharge power was 100 W. The BNNT was cleaned and surface activated with argon plasma in (continuous wave) mode. Next, NH3 plasma was treated in P (pulse) mode for 2 min to provide etching and the formation of amino functional groups on the BNNT surface to obtain BNNT-NH2.

[0186] Step 2: preparing aramid nanofiber spinning solution;

[0187] The preparation process of aramid nanofiber ANF spinning solution is as follows:

[0188] Kevlar fiber was cut into small pieces less than 1 cm, acetone was poured into the fiber surface, and ultrasonic treatment was performed at a power of 500 W for 24 h. After filtering the acetone, it was dried in a vacuum oven at 45 °C and sealed for storage. 1.6 g of treated Kevlar fiber and 2.4 g of KOH were weighed and added to a mixed solution of 320 mL of DMSO and 10 mL of deionized water. Stirred at 30 °C in the dark for 14 d to obtain a dark red ANF / DMSO dispersion with a mass concentration of 1 wt%.

[0189] Step 3: The pretreatment process of aramid chopped fibers is as follows:

[0190] The aramid short fibers were cut into 2 × 10 -3 The samples were immersed in a 60 ℃ sodium dodecylbenzene sulfonate solution with a temperature of 20 ℃ and 100 ℃, washed three times with deionized water, and dried in a vacuum drying oven at 100 ℃ for 1 h.

[0191] Step 4: Add 1 g of aramid chopped fiber pulp, 0.1 g of graphene, 0.002 g of GO, 0.017 g of BNNT-NH2 and 0.083 g of ANF into a fiber disintegrator containing 500 mL of deionized water and mix them evenly. The speed of the disintegrator is 5000 r / min and the disintegration time is 15 min.

[0192] PEO and APAM with a mass ratio of 6:1 were used as dispersants, and the amount of dispersant added was 2% of the dry weight of the mixed fiber. The dispersant was added to the dissociated slurry to obtain a uniformly dispersed mixed fiber slurry. The mixed fiber slurry was wet-coated on a paper sheet former with a web concentration of 0.06%. The paper-coated mixed fiber base paper was dried in a blast oven at a temperature of 100°C for 2 h to obtain the desired insulating paper.

[0193] The thermal conductivity and mechanical properties of the above embodiments and comparative examples were tested, and the results are shown in Table 1. Figure 4 and Figure 5 shown.

[0194] Table 1. Performance test results of insulating paper obtained in Examples and Comparative Examples

[0195]

[0196] From Table 1, Figure 4 and Figure 5 It can be seen from Examples 1 to 3 that with the increase of GO / graphene fiber content, the thermal conductivity of the composite insulation paper increases significantly, and the maximum thermal conductivity reaches 0.332 W·m -1 ·K -1 . The tensile strength increases with the increase of GO / graphene fiber content. In Comparative Examples 2 to 4, graphene is directly added as a filler to the composite insulating paper. As the graphene content increases, the thermal conductivity improvement efficiency is significantly lower than that of Examples 1 to 3, and the mechanical strength deteriorates. This is because the GO sheets in the GO / graphene fibers prepared by wet spinning are spread along the fiber axis. While increasing the orientation of the sheets, the porosity in the fibers is also reduced, thereby increasing the packing density of the fibers. This not only constructs a continuous and effective phonon transmission path, provides an efficient heat conduction path, and reduces interfacial thermal resistance, but also the increase in orientation and the decrease in porosity make the internal structure of the fiber more compact, thereby enhancing the mechanical properties. The thermal conductivity of the insulating paper obtained in Comparative Example 1 is 0.131 W·m -1 ·K -1 The thermal conductivity of the composite insulating paper obtained in Example 3 is increased by 153.44% compared with the former.

[0197] Examples 4 to 6 are insulating papers with different BNNT-NH2@ANF composite fiber contents. The thermal conductivity increases with the increase of the BNNT-NH2 ratio in the composite fiber, and the tensile strength decreases slightly, but the mechanical strength is still relatively high. Examples 7 to 8 show a synergistic improvement in tensile strength and thermal conductivity as the BNNT-NH2@ANF composite fiber content increases, and the thermal conductivity improvement efficiency is lower than that of Examples 2 to 3.

[0198] It can be seen from Comparative Examples 5 to 7 that with the increase of ANF fiber pulp content, the thermal conductivity increases from 0.139 W·m -1 ·K -1 Increased to 0.153 W·m -1 ·K -1 The highly arranged molecular chains and high crystallinity in ANF also contribute to the transmission of phonons. Due to the low filling content of ANF and the low intrinsic thermal conductivity of ANF, the heat transfer network formed by the overlap between ANFs is small, and the change in the growth rate of thermal conductivity is not very obvious. It can be seen from Comparative Example 8 that the thermal conductivity improvement effect of pure physical blending of inorganic fillers is very low, so the composite insulating paper obtained by the present invention can effectively improve the thermal conductivity.

[0199] The present invention grafts amino groups on the surface of boron nitride nanotubes to further prepare BNNT-NH2@ANF composite fibers; the three types of fibers, GO / graphene fibers, BNNT-NH2@ANF composite fibers and aramid chopped fibers, are mixed, which not only retains the high thermal conductivity of graphite and BNNT, but also the composite fibers and AF chopped fibers are physically entangled and hydrogen-bonded to interact with each other, so that the prepared composite insulating paper can significantly improve the thermal conductivity while still maintaining very high mechanical strength, and has broad application prospects in large-capacity and high-power electrical equipment such as transformers.

Claims

1. A method for preparing high thermal conductivity aramid insulation paper for electrical equipment, characterized in that: The following steps are involved: Step 1: Mix graphene and graphene oxide (GO) dispersion to obtain GO / graphene fibers by wet spinning; Step 2: amination treatment of boron nitride nanotubes BNNT to obtain BNNT-NH2; using BNNT-NH2 spinning solution as the core layer and aramid nanofiber ANF spinning solution as the skin layer, wet spinning is performed to obtain BNNT-NH2@ANF composite fibers; Step 3: GO / graphene fiber, BNNT-NH2@ANF composite fiber and aramid short fiber AF are pulped, filtered and dried to obtain three kinds of fiber pulp; Step 4: Fully mix the three fiber pulps in step 3 to prepare AF / (GO / graphene) / BNNT-NH2@ANF fiber base paper, i.e. the required insulating paper.

2. The method for preparing high thermal conductivity aramid insulation paper for electrical equipment according to claim 1, characterized in that: In the step 1, the mass ratio of GO to graphene is 1-2:40-50; the spinning rate in the wet spinning is 0.03 mL / min, and the coagulation bath is an ethyl acetate solution.

3. The method for preparing high thermal conductivity aramid insulation paper for electrical equipment according to claim 1, characterized in that: The mass ratio of ANF to BNNT-NH2 in the BNNT-NH2@ANF composite fiber is 2-10:1-3.

4. The method for preparing high thermal conductivity aramid insulation paper for electrical equipment according to claim 1, characterized in that: In step 2, the BNNT amination treatment is performed by plasma treatment; The plasma treatment parameters were as follows: peak voltage of 9.5 kV, frequency of 13.56 MHz, and discharge power of 100 W.

5. The method for preparing high thermal conductivity aramid insulation paper for electrical equipment according to claim 1, characterized in that: In the step 2, the wet spinning skin layer and the core layer are extruded simultaneously at 0.03 mL / min and immersed in the first coagulation bath; after solidification and forming in the first coagulation bath, the formed fiber is pulled at a speed of 0.08 mL / min to transition to the second coagulation bath; wherein the first coagulation bath is a mixed solution composed of dimethyl sulfoxide, deionized water and ethanol in a volume ratio of 100:900:0.5, and the second coagulation bath is deionized water.

6. The method for preparing high thermal conductivity aramid insulation paper for electrical equipment according to claim 1, characterized in that: In step 3, the GO / graphene fiber, BNNT-NH2@ANF composite fiber, and aramid chopped fiber are first pretreated. The pretreatment process of aramid chopped fiber is as follows: Soak the aramid chopped fibers in a sodium dodecylbenzene sulfonate solution for 2 to 3 hours, wash and dry them; The pretreatment process of GO / graphene fiber and BNNT-NH2@ANF composite fiber is as follows: Under vacuum conditions, first treat at 60-80 °C for 1 h, and then treat at 120-150 °C for 2 h.

7. The method for preparing high thermal conductivity aramid insulation paper for electrical equipment according to claim 1, characterized in that: In the step 4, the mass ratio of GO / graphene fiber, BNNT-NH2@ANF composite fiber and AF pulp is 1-2:1-2:

10.

8. The method for preparing high thermal conductivity aramid insulation paper for electrical equipment according to claim 1, characterized in that: In step 4, the three types of fiber pulp are dissociated at 4000-5000 r / min for 10-15 min; a dispersant is added, and the mixed slurry is wet-coated and dried to obtain the desired insulating paper; The concentration of wet papermaking is 0.06-0.08 wt%, the drying temperature is 100-120 ℃, and the drying time is 2-3 hours.

9. The high thermal conductivity aramid insulation paper for electrical equipment obtained by any one of the preparation methods of claims 1 to 8, characterized in that: The thickness of the high thermal conductivity aramid insulation paper is 100-120 μm.

10. The use of high thermal conductivity aramid insulation paper for electrical equipment as claimed in claim 9, characterized in that: The high thermal conductivity aramid insulation paper is used for electrical equipment.

Citation Information

Cited By

  • Composite aramid insulation paper with low dielectric loss and high thermal conductivity and preparation method thereof

    CN121381437A

  • Low dielectric loss and high thermal conductivity composite aramid insulation paper and preparation method thereof

    CN121381437B