Method for manufacturing ceramic article, and ceramic article

By controlling the zirconium component proportion in the porous ceramic structure through absorption and heating, the method addresses the challenge of achieving both high precision and mechanical strength in ceramic objects, improving structural integrity and reducing cracks.

JP7557264B2Active Publication Date: 2024-09-27CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2019219949
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-06
Filing Date
2019-12-04
Publication Date
2024-09-27
Estimated Expiration
2039-12-04

AI Technical Summary

Technical Problem

Existing methods for manufacturing ceramic objects with porous structures face challenges in achieving both high modeling precision and mechanical strength due to issues such as uneven melting, rapid cooling, and thermal stress, which result in cracks and insufficient mechanical strength.

Method used

A method involving the use of aluminum oxide powder layered and irradiated with an energy beam to form a porous structure, followed by absorption of a zirconium component-containing liquid and subsequent heating to control the zirconium component proportion between 0.3 mol% and 2.0 mol% in the porous portion, promoting recrystallization and strengthening the bond between crystal structures.

Benefits of technology

This approach enhances the mechanical strength of ceramic articles with porous portions while maintaining high modeling accuracy, reducing microcracks, and ensuring the structural integrity of the ceramic object.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557264000004
    Figure 0007557264000004
  • Figure 0007557264000016
    Figure 0007557264000016
  • Figure 0007557264000009
    Figure 0007557264000009
Patent Text Reader

Abstract

To provide a method for manufacturing a shaped ceramic article having a porous portion with improved mechanical strength while obtaining high modeling accuracy, as well as a ceramic article prepared by the method.SOLUTION: A method for manufacturing a ceramic article, comprising (i) a step of levelling powder of a metal oxide consisting mainly of aluminum oxide and forming a powder layer, (ii) a step of irradiating the powder layer with an energy beam based on the shaping data so as to melt, solidify or sinter the powder, (iii) a step of absorption in which a shaped article having a porous portion formed by repeating the steps (i) and (ii) is allowed to absorb a liquid that contains a zirconium component, and (iv) a step for heating the shaped article containing the zirconium component absorbed therein, wherein the step of absorbing the liquid is carried out in such a manner that the ratio of the zirconium component contained in the porous portion of the shaped article is 0.3 to 2.0 mol%, based on metallic components contained therein.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a ceramic object, and more particularly to a method for manufacturing a three-dimensional ceramic object having a porous structure. [Background technology]

[0002] In recent years, in applications such as producing prototypes in a short time or manufacturing a small number of parts, a direct printing method for producing a desired object, particularly a three-dimensional object, has become widespread. In this method, a three-dimensional object obtained by the direct printing method does not shrink significantly during subsequent heat treatment, and therefore has the advantage of being able to obtain high printing accuracy. Here, in the present invention, the printing accuracy refers to the difference (rate of change) between the dimensions of a ceramic article that has undergone a firing process after printing and the design dimensions specified using CAD or the like. In particular, in the metal field, dense and diverse objects have been obtained using the powder bed fusion method. The high density of metal objects is achieved by effectively melting and solidifying metal powder. Based on the success in the metal field, the application to ceramic materials has also been discussed, and many efforts have been reported. Aluminum oxide (Al 2 O 3 ) and zirconium oxide (ZrO, ZrO 2 Common ceramic materials such as quartz crystals (CuO) hardly absorb laser light. For this reason, in order to melt them in the same way as metals, more energy must be input, but the laser light diffuses and the melting becomes uneven, making it difficult to obtain the required modeling precision. In addition, because ceramic materials have a high melting point, when they are melted by the laser light and then solidify, they are rapidly cooled by the atmosphere and adjacent surrounding areas, and the thermal stress that occurs at this time causes many cracks in the resulting model. As a result, the mechanical strength of the resulting model is insufficient.

[0003] Porous ceramics are one of the important ceramic components used in various applications. Porous ceramics have excellent heat resistance, chemical resistance, strength, and light weight, and are used for various filters, separation columns, catalyst carriers, lightweight structural materials, heat insulation materials, vacuum chuck components, etc., taking advantage of their ability to pass fluids (liquids and gases).

[0004] Under these circumstances, Non-Patent Document 1 describes a method for manufacturing three-dimensional objects using the direct molding method, Al 2 O 3 -ZrO 2 A technology has been disclosed in which the melting point is lowered by using ceramics with a eutectic composition, thereby reducing the energy required for melting. In addition, Non-Patent Document 1 discloses a technology in which the raw ceramic material powder is heated by a heater (preheating) and irradiated with laser light to relieve thermal stress and suppress the occurrence of cracks in the resulting molded object. This manufacturing method has the advantage of being able to obtain a dense ceramic structure without shrinkage. However, due to preheating by the heater, a part of the ceramic material powder in the part not irradiated with the laser light melts, and the accuracy of the surface boundary of the structure cannot be obtained, and for example, it is difficult to mold a fine porous structure. On the other hand, if the preheating is canceled in order to prioritize molding accuracy, cracks are formed due to rapid cooling after the process as described above, and there is a problem that a porous structure with high strength cannot be obtained. For this reason, it is difficult to obtain a ceramic molded object having a porous structure that combines molding accuracy and mechanical strength with such a technology. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Physics Procedia 5 (2010) 587-594 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a method for manufacturing a ceramic article that improves the mechanical strength of a ceramic object having a porous portion, which is produced with high modeling accuracy by taking advantage of the characteristics of a direct modeling method, and a ceramic article. [Means for solving the problem]

[0007] One aspect of the present invention is a method for manufacturing a ceramic article, comprising the steps of: (i) leveling a powder of a metal oxide mainly composed of aluminum oxide to form a powder layer; (ii) irradiating the powder layer with an energy beam based on molding data to melt and solidify, or sinter, the powder; (iii) allowing a liquid containing a zirconium component to be absorbed into a shaped object having a porous portion formed by repeating steps (i) and (ii); and (iv) heating the shaped object that has absorbed the liquid containing the zirconium component, wherein in the absorption step, the liquid is absorbed so that the proportion of the zirconium component in the metal components contained in the porous portion is 0.3 mol% or more and 2.0 mol% or less.

[0008] Another aspect of the present invention is a method for manufacturing a ceramic article, comprising the steps of: (i) irradiating a powder of a metal oxide mainly composed of aluminum oxide with an energy beam based on molding data, and melting and solidifying or sintering the powder to form a shaped object having a porous portion; (ii) causing the shaped object formed in step (i) to absorb a liquid containing a zirconium component; and (iii) heating the shaped object having absorbed the liquid containing the zirconium component, wherein in the absorption step, the liquid is absorbed so that the proportion of the zirconium component in the metal components contained in the porous portion is 0.3 mol% or more and 2.0 mol% or less.

[0009] Another aspect of the present invention is a ceramic article having a porous portion made of a metal oxide mainly composed of aluminum oxide, wherein the ratio of zirconium components in the metal components in the porous portion is 0.3 mol% or more and 2.0 mol% or less. Another aspect of the present invention is a ceramic article made of a metal oxide containing aluminum oxide as a main component, having a dense portion and a porous portion, wherein a ratio of zirconium in the metal components contained in the porous portion is greater than a ratio of zirconium in the metal components contained in the dense portion. Effect of the Invention

[0010] According to the present invention, it is possible to provide a method for producing a ceramic article having a porous portion that realizes high mechanical strength by using a direct molding method, and a ceramic article. [Brief description of the drawings]

[0011] [Figure 1A] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 1B] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 1C] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 1D] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 1E] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 1F] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 1G] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 1H] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 2A] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 2B] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Figure 2C] FIG. 1 is a schematic cross-sectional view showing an embodiment of a method for producing a shaped article, which is a ceramic article, of the present invention. [Diagram 3] 1 is a schematic diagram of a ceramic article of the present invention as viewed from one surface. [Figure 4A] 1 is an optical microscope image of a shaped object that is a ceramic article of the present invention. [Figure 4B] 1 is an optical microscope image of a shaped object that is a ceramic article of the present invention. [Figure 5A] 1 is an SEM image of a shaped object that is a ceramic article of the present invention. [Figure 5B] 1 is a distribution image of the Zr component of a shaped product that is a ceramic article of the present invention. [Figure 6A] 1 is an SEM image of a shaped object that is a ceramic article of the present invention. [Figure 6B] 3 is a distribution image of the Zr component in a porous portion of a shaped ceramic article of the present invention. [Figure 6C] 3 is a distribution image of the Zr component in a dense portion of a shaped ceramic article of the present invention. [Figure 7] 1 is a schematic diagram showing a one-piece composite ceramic part according to the present invention, which is made up of a porous portion and a dense portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to the following specific examples.

[0013] A first aspect of the present invention is a method for producing a ceramic article having a porous portion, comprising: (i) forming a ceramic article by subjecting an aluminum oxide (Al 2 O 3 (ii) a step of irradiating the powder layer with an energy beam based on printing data to melt and solidify or sinter the powder; (iii) a step of absorbing a liquid containing a zirconium (Zr) component into a shaped object having a porous portion formed by repeating the steps (i) and (ii); and (iv) a step of heating the shaped object that has absorbed the liquid containing the zirconium component, wherein in the absorbing step, the liquid is absorbed so that the ratio of the zirconium component among the metal components contained in the porous portion is 0.3 mol% or more and 2.0 mol% or less.

[0014] [3D objects created using direct printing method] The present invention is suitable for the manufacture of articles using direct fabrication techniques, particularly powder bed fusion techniques and directed energy deposition techniques (so-called cladding techniques) that involve the deposition of build-up materials, which can significantly improve the mechanical strength of porous ceramic articles.

[0015] The basic flow of molding in the powder bed fusion method will be described with reference to Figs. 1A to 1H. First, powder 101 is placed on a base 130, and a powder layer 102 is formed using a roller 152 (Figs. 1A and 1B). When an energy beam emitted from an energy beam source 180 is irradiated onto the surface of the powder layer 102 while being scanned by a scanner unit 181 according to molding data, the powder 101 melts and then solidifies to form a solidified portion 103 (Fig. 1C). Next, the stage 151 is lowered, and a new powder layer 102 is formed on the solidified portion 103 and the unsolidified powder (Fig. 1D). This series of steps is repeated to form a solidified portion 103 of a desired shape (Figs. 1E and 1F). Finally, the unsolidified powder is removed, and unnecessary parts are removed or the molded object is separated from the base as necessary (Figs. 1G and 1H).

[0016] Next, the cladding method will be described with reference to Figures 2A to 2C. The cladding method is a technique in which powder is ejected from a plurality of powder supply holes 202 in a cladding nozzle 201, and an energy beam 203 is irradiated onto the area where the powder is focused, to additionally form solidified portions 103 at desired locations (Figure 2A), and this process is repeated to obtain a molded object 110 of a desired shape (Figures 2B and 2C). Finally, unnecessary portions are removed and the molded object 110 is separated from the base 130 as necessary.

[0017] [About porous parts] According to the direct molding method that can obtain a three-dimensional object with a dense and complicated shape, the above-mentioned molded object 110 having various porous structures can be formed by inputting appropriate (three-dimensional) molding data. By firing the above-mentioned molded object 110 by the manufacturing method of the present invention, a porous portion is formed, and a ceramic article having a porous portion can be obtained. In the present invention, the porous portion refers to a portion having a porosity of 5 vol (volume) % or more, a bridge portion having a thickness of 1 mm or less, and a plurality of openings having a pore diameter of 50 μm or more and 1000 μm or less. In contrast, in the present invention, the dense portion refers to a portion having a porosity of less than 5 vol (volume) % and a bridge portion having a thickness of 1 mm or more. Here, the porosity refers to the ratio of open pores to the volume of the ceramic article, and does not include closed pores. An open pore is a pore in which a part of the pore is connected to the outside (also called an open pore). A closed pore is a pore that is not connected to the outside. In addition, a communicating pore is a pore that is connected to the outside at both ends, and is included in open pores. Porosity can be measured by the mercury injection method. , hole The thickness of the bridge section refers to the shortest distance between a hole and its adjacent hole.

[0018] Fig. 3 is a schematic diagram showing an enlarged partial area of ​​a surface of a porous ceramic 301, which is a ceramic article having a porous portion according to the present invention, where the cross-sectional shape of the pores can be seen. Here, the cross-sectional shape refers to the shape of a surface perpendicular to the extension direction of the pores. Fig. 3 shows an example, and is not limited thereto. Fig. 3 shows a hole with a circular cross-sectional shape, but the cross-sectional shape of the hole may be any of a circle, a square, or a triangle, and holes of a plurality of shapes may be provided in combination.

[0019] In the present invention, the porosity is the open porosity measured by the mercury injection method as described above. In the case of a porous ceramic 301 having pores 302 as shown in FIG. 3, the porosity is the ratio of the volume of the pores 302 to the total volume of the porous ceramic 301 including the pores. The porous portion has a plurality of pores with a pore diameter of 50 μm or more and 1000 μm or less. In the present invention, the pore diameter 303 refers to the minor axis diameter (2b) of an elliptical shape (including a circular shape) that approximates the contour of the hole. The method of approximating the contour of the hole to an elliptical shape is as follows. First, the maximum distance (2a) between the contours of the hole and the area S of the contour of the hole are measured. The minor axis radius b of the approximated ellipse can be calculated by b=S / (πa). From the above, the major axis diameter 2a and the minor axis diameter 2b are derived. The pore diameter can be measured using an optical microscope, a scanning electron microscope (SEM), or the like in any cross section that is approximately perpendicular to the pores of the ceramic article. The period 304 of the open pores, the shape, the pore diameter 303, the porosity, etc. of the porous part can be controlled independently by changing the modeling data to be input. In addition, by reducing the irradiation energy density of the energy beam, a randomly shaped porous part can be formed. The average pore diameter is the average value of the pore diameters 303 of the multiple pores in the porous part. In calculating the average pore diameter, the open pores and the closed pores may be considered to have approximately the same diameter, and the open pores and the closed pores may be measured and calculated without distinguishing between them. In the present invention, the average pore diameter of the pores in the porous part is preferably 50 μm or more and 1000 μm or less. It is not possible to distinguish between open pores and closed pores by simply observing an arbitrary cross section of a ceramic article with an optical microscope, SEM, or the like. It is possible to determine whether a pore of interest is an open pore or a closed pore by slice and view, which is observed with an SEM while cutting with a focused ion beam (FIB), or by X-ray computed tomography (X-ray CT). The same method can be used to observe the interconnected pores.

[0020] Here, we will describe the pore diameter 303, pore period 304, and porosity of the pores 302 of the porous ceramic 301 shown in Figure 3. Consider a case where the pores 302 are circular and the pore period 304 is equidistant. If the pore period is 1, when the porosity (vol%) is 5, 10, 20, 30, 40, 50, and 60, the pore diameters are 0.25, 0.36, 0.51, 0.62, 0.71, 0.80, and 0.87, respectively, and the bridge thicknesses are 0.75, 0.64, 0.50, 0.38, 0.29, 0.20, and 0.13, respectively.

[0021] The pore diameter 303 of the porous portion of the present invention may be constant in the direction of extension of the pores, or may change along the way. Also, one pore may be divided into multiple pores along the way. Multiple openings with different cross-sectional shapes may be combined. In either case, in order to complete the porous portion, it is necessary to remove the unsolidified powder remaining in the pores after the shaping is completed. For this reason, both ends of the pores are connected to the outside.

[0022] In the above-mentioned direct modeling method for producing a three-dimensional object, the accuracy of modeling is about several tens of μm. Therefore, if the diameter of the holes formed in the porous portion is 50 μm or less, a uniform pore diameter 303 cannot be obtained, and the open pores 302 may be filled, resulting in a decrease in porosity. In addition, if the average pore diameter is larger than 1000 μm, the porous portion will not function as a pore capable of controlling the flow of gas or liquid, so it is preferable that the average pore diameter is 1000 μm or less. Therefore, it is preferable that the average pore diameter of the open pores 302 is 50 μm or more and 1000 μm or less. When the porous portion is formed for the purpose of weight reduction, etc., the preferable pore diameter is not limited to this as long as the desired mechanical strength can be obtained.

[0023] [Effects of zirconium-containing liquid] In direct manufacturing methods such as the powder bed direct manufacturing method and cladding method mentioned above, the ceramic powder melted by energy beam irradiation is cooled by the surroundings and solidifies to form a molded object. Since the difference between the melting temperature and solidification temperature of ceramics is large, thermal stress occurs, and many microcracks occur in the molded object. The microcracks are distributed over the entire molded object (surface and interior). When the cross section of the molded object is examined with a scanning electron microscope, most of the microcracks are several nm to several μm in width. The length of the microcracks also varies from several μm to several mm.

[0024] According to the present invention, by absorbing a zirconium component-containing liquid into microcracks in a ceramic object having a porous structure and then heating the object, it is possible to reduce the number of microcracks and improve the mechanical strength of the object.

[0025] When the cross section of the shaped object obtained by absorbing the zirconium-containing liquid and then heating is observed, it is confirmed that crystals of zirconium composition are formed throughout, and the mechanical strength of the resulting ceramic article is improved. This is because the aluminum oxide and zirconium components constituting the shaped object form a eutectic relationship, so that microcracks are easily reduced during the heating process, and recrystallization progresses, strengthening the bonding force between the crystalline structures, thereby improving the mechanical strength of the ceramic article. The zirconium is absorbed through the pores of the shaped object and adheres to the surfaces of the porous structure and microcracks of the shaped object. It is presumed that the zirconium component attached to the porous surface diffuses into the solid phase over a wide area within the crystals constituting the shaped object by heating, and the crystals are recrystallized with a composition containing the zirconium component. It is believed that such a structure strengthens the bonding force between the crystalline structures of the resulting ceramic article, improving the mechanical strength.

[0026] Therefore, the present invention is characterized in that a zirconium component is introduced into a shaped product formed by melting and solidifying a powder with an energy beam. Even if the powder contains a zirconium component in advance, it is not possible to prevent cracks from occurring during shaping, so the bonding strength between the crystal structures is not sufficient and the effect of the present invention (improved mechanical strength) cannot be obtained.

[0027] [Effect of porous part on absorption of zirconium-containing liquid] The difference in the absorption effect of the zirconium component-containing liquid between the porous part and the dense part will be described. Here, in the present invention, the porous part and the dense part have different porosities, and the porosity of the porous part is 5 vol% or more, and the porosity of the dense part is less than 5 vol%. When the porosity of the porous part is 5 vol% or more, it is possible to obtain the necessary functions of a porous part, such as heat resistance, light weight, and use as a flow path. Furthermore, when the porosity of the porous part is 5 vol% or more, the zirconium component can be distributed inside the porous part of the shaped product, and sufficient strength can be obtained. The porosity of the porous part is preferably 5 vol% or more and 60 vol% or less. When the porosity of the porous part is 60 vol% or less, sufficient strength as a ceramic article can be obtained, which is preferable. The closed pores contained in the porous part do not contribute much to improving the function of the porous part. Furthermore, they do not have the function of distributing the zirconium component inside the shaped product. Therefore, from the viewpoint of obtaining sufficient strength, the ratio of closed pores contained in the porous part is preferably 1 vol% or less. More preferably, it is 0.5 vol% or less.

[0028] In order to repair microcracks that occur during molding, it is necessary to make the molded object absorb a sufficient amount of zirconium components. In a ceramic molded object having a porous portion, the zirconium component-containing liquid penetrates into the inside of the molded object through the openings. In addition, since the surface area is large, a large amount of zirconium components penetrates compared to a dense portion. In addition, since the bridge portion forming the holes in the porous portion is fine and thin, the concentration of zirconium has a large effect on the molding accuracy and mechanical strength. In other words, if the amount of zirconium components absorbed in the porous portion is not controlled, the tissue containing the zirconium components will become enlarged in the subsequent heating process, which may lead to a deterioration in molding accuracy, and it is more difficult for the porous portion, which has a finer structure than the dense portion, to achieve both molding accuracy and mechanical strength than the dense portion. Therefore, in the present invention, it has been found that molding accuracy and mechanical strength are correlated with the Zr content, and that it is preferable to set the Zr content to an appropriate value in order to achieve both molding accuracy and mechanical strength.

[0029] First, regarding mechanical strength, when the Zr content is low, the degree of improvement in mechanical strength is small, and the possibility of the porous portion being damaged during processing or in the usage environment increases. In the present invention, when the ratio of the zirconium component in the metal components constituting the metal oxide in the porous portion is 0.3 mol% or more, a mechanical strength sufficient for practical use as a ceramic article can be obtained.

[0030] Next, the molding accuracy will be described. If the content of the zirconium component added to the aluminum oxide, which is the main component, becomes excessive, the melting point of the porous part will be lowered, and when the molded object that absorbs zirconium is heated, some parts will melt the crystals. As a result, the fine bridge part of the porous body in particular will be easily deformed, losing the molding accuracy, blocking the openings, and no longer functioning as a porous body. Therefore, from the viewpoint of molding accuracy, the porous part requires more precise control of the Zr content than the dense part. In the present invention, the proportion of the zirconium component in the metal components that make up the metal oxide in the porous part is set to 2.0 mol% or less, so that the shape of the bridge part is maintained and sufficient molding accuracy is obtained.

[0031] In view of the above, in the present invention, in order to simultaneously realize molding precision and mechanical strength in the porous portion, the ratio of the zirconium component in the metal components constituting the metal oxide in the porous portion is set to 0.3 mol% or more and 2.0 mol% or less. Also, the ratio of the zirconium component in the metal components constituting the metal oxide in the porous portion is preferably 0.3 mol% or more and 1.5 mol% or less.

[0032] Furthermore, under these conditions, it is preferable that the zirconium component becomes a metal oxide composite with other metal components, and forms a zirconia region with an average circle equivalent diameter of 5 μm or more on the surface or inside of the bridge part. As the other metal component, for example, a gadolinium component is preferable, and the gadolinium component is preferably at least the same mole as the zirconium component, and the zirconia region is preferably a metal oxide composite of zirconium and gadolinium. By adopting such a form, the high mechanical strength of the zirconium component is effectively imparted to the bridge part, contributing to improving the mechanical strength of the entire porous part.

[0033] The method for producing a ceramic article according to the present invention is characterized by comprising the following four steps (i) to (iv). (i) A metal oxide powder containing aluminum oxide as a main component is leveled to form a powder layer. (ii) Irradiating the powder layer with an energy beam based on modeling data to melt, solidify, or sinter the powder. (iii) The above steps (i) and (ii) are repeated to form a shaped article having a porous portion, which is then allowed to absorb a liquid containing a zirconium component. (iv) heating the shaped article having absorbed the liquid containing the zirconium component;

[0034] In the absorbing step, the liquid is absorbed so that the ratio of zirconium in the metal components contained in the porous portion is 0.3 mol% or more and 2.0 mol% or less. At this time, the ratio of zirconium in the metal components contained in the porous portion is preferably 0.3 mol% or more and 1.5 mol% or less.

[0035] <Process (i)> The method for producing a shaped article according to the present invention includes the step (i) of leveling a metal oxide powder containing aluminum oxide as a main component to form a powder layer.

[0036] Aluminum oxide is a versatile structural ceramic, and by appropriately sintering or melting and solidifying it, it is possible to obtain shaped objects with high mechanical strength.

[0037] The metal oxide powder in the present invention preferably has a zirconium oxide content of less than 0.1 mol%. The ratio of zirconium components in the metal components contained in the metal oxide powder is preferably less than 0.15 mol%. In a shaped object having a porous structure in which a zirconium component-containing liquid has been absorbed, there is a large difference in the concentration of zirconium components between the crystal parts of the shaped object and the microcrack parts of the shaped object, so that only the vicinity of the microcracks can be selectively melted. This makes it possible to suppress deformation of the shaped object due to the heating process.

[0038] The powder in the present invention more preferably contains at least one selected from gadolinium oxide, terbium oxide, and praseodymium oxide as a subcomponent. By containing gadolinium oxide, the powder can be made of Al. 2 O 3 -Gd 2 O 3In the vicinity of the eutectic composition, the melting point is lower than that of aluminum oxide alone. This allows the powder to melt with a small amount of heat, and the diffusion of energy within the powder is suppressed, improving the molding precision. Furthermore, by including gadolinium oxide, the molded object has a phase-separated structure consisting of two or more phases. This suppresses the propagation of cracks and improves the mechanical strength of the molded object. The same effect as gadolinium oxide can be obtained when oxides of other rare earth elements (excluding terbium and praseodymium) are used instead of gadolinium oxide. When the energy beam is a laser beam, sufficient energy absorption in the powder suppresses the spread of heat within the powder and makes it localized, reducing the impact of heat on non-printed areas, improving the molding precision. For example, when an Nd:YAG laser is used, terbium oxide (Tb 4 O 7 ) and praseodymium oxide (Pr 6 O 11 ) exhibits good energy absorption, and is therefore preferably contained in the powder as a secondary component.

[0039] Since the eutectic composition ratio of the rare earth oxide material consisting of the minor components gadolinium oxide, terbium oxide, and praseodymium oxide to aluminum oxide is 46:54 (mol%), it is preferable that the composition ratio of the rare earth oxide material to aluminum oxide is within a range of ±5 mol% from the eutectic composition ratio, that is, 41:59 to 51:49 (mol%). Within this range, the effect of lowering the melting point can be obtained by using ceramics with a eutectic composition.

[0040] From the above viewpoints, the more suitable powder is Al 2 O 3 -Gd 2 O 3 , Al 2 O 3 -Tb 4 O 7 , Al 2 O 3 -Gd 2 O 3 -Tb 4 O 7 , Al 2 O 3-Pr 6 O 11 , Al 2 O 3 -Gd 2 O 3 -Pr 6 O 11 , Al 2 O 3 -Gd 2 O 3 -Tb 4 O 7 -Pr 6 O 11 etc.

[0041] The material of the base used in the present invention can be appropriately selected and used from materials commonly used in the production of three-dimensional objects, such as ceramics, metals, glass, etc., taking into consideration the application of the object, production conditions, etc. When the object integrated with the base is heated in step (iv), it is preferable to use heat-resistant ceramics for the base.

[0042] The method of disposing the powder on the base is not particularly limited. In the case of the powder bed fusion method, as shown in Figures 1A to 1H, the powder is disposed in layers on the base using a roller, blade, or the like. In the case of the cladding method, as shown in Figures 2A to 2C, the powder is sprayed from a nozzle to the energy beam irradiation position, and the powder is disposed on the base or a model placed on the base in a pile-up manner, and at the same time, the powder is melted and solidified by energy beam irradiation to produce a model.

[0043] <Process (ii)> The method for manufacturing a molded object according to the present invention includes a step (ii) of irradiating the powder layer formed in the step (i) with an energy beam based on molding data to melt, solidify, or sinter the powder. This step will be described below based on a preferred embodiment.

[0044] In the case of the powder bed fusion method, as shown in FIG. 1, a predetermined area on the surface of the powder placed on the base in step (i) is irradiated with an energy beam to melt the powder and then solidify it. In the case of the cladding method, as shown in FIGS. 2A to 2C, the powder is sprayed and supplied in step (i) to place the powder on the base in a pile-up manner, and at the same time, the entire placed powder is irradiated with an energy beam to melt and solidify the powder. When the energy beam is irradiated on the powder, the powder absorbs the energy, which is converted into heat and melts the powder. When the irradiation of the energy beam is completed, the molten powder is cooled and solidified by the atmosphere and the adjacent surroundings, and a molded object is formed. The rapid cooling during the melting and solidification process generates stress in the surface layer and inside of the molded object, and countless microcracks are formed. The molded object may be formed by irradiating the powder layer with an energy beam to sinter it.

[0045] The energy beam to be used is selected from a light source with an appropriate wavelength, taking into consideration the absorption characteristics of the powder. In order to perform high-precision modeling, it is preferable to use a laser beam or electron beam with a narrow beam diameter and high directivity. General-purpose laser beams include YAG lasers and fiber lasers in the 1 μm wavelength band, and CO lasers in the 10 μm wavelength band. 2 When the powder contains terbium oxide or praseodymium oxide as a secondary component, a YAG laser in the 1 μm wavelength range is suitable.

[0046] <Step (iii)> The method for producing a shaped article according to the present invention includes a step of causing a shaped article formed by repeating the above steps (i) and (ii) to absorb a liquid containing a zirconium component (also referred to as a zirconium component-containing liquid).

[0047] New powder is placed on the object obtained in step (ii) in step (i). When the placed powder is irradiated with an energy beam, the powder in the energy beam irradiated area melts and solidifies, forming a new object integrated with the original object. By alternately repeating steps (i) and (ii), an object having a desired three-dimensional shape can be obtained.

[0048] The resulting shaped object is then allowed to absorb a liquid containing a zirconium component (sometimes referred to as a zirconium component-containing liquid).

[0049] Here, the zirconium component-containing liquid will be explained. A preferred example of the zirconium component-containing liquid is one that is composed of a raw material for the zirconium component, an organic solvent, and a stabilizer.

[0050] Various zirconium compounds can be used as the raw material of the zirconium component. When absorbing into a shaped object mainly made of alumina, a raw material that does not contain metal elements other than zirconium is preferable. As the raw material of the zirconium component, metal alkoxides of zirconium and salt compounds such as chlorides and nitrates can be used. Among them, the use of metal alkoxides is preferable because the zirconium component-containing liquid can be uniformly absorbed into the microcracks of the shaped object. Specific examples of zirconium alkoxides include zirconium tetraethoxide, zirconium tetra n-propoxide, zirconium tetraisopropoxide, zirconium tetra n-butoxide, and zirconium tetra t-butoxide.

[0051] First, the zirconium alkoxide is dissolved in an organic solvent to prepare a solution of the zirconium alkoxide. The amount of the organic solvent added to the zirconium alkoxide is preferably 5 to 30 in molar ratio to the compound. More preferably, it is 10 to 25. In the present invention, the molar ratio of A to B is 5, which means that the molar amount of A to be added is 5 times the molar amount of B. If the concentration of the zirconium alkoxide in the solution is too low, a sufficient amount of the zirconium component cannot be absorbed into the shaped object. On the other hand, if the concentration of the zirconium alkoxide in the solution is too high, the zirconium component in the solution will aggregate, and the zirconium component cannot be uniformly arranged in the microcracks of the shaped object.

[0052] As the organic solvent, alcohol, carboxylic acid, aliphatic or alicyclic hydrocarbons, aromatic hydrocarbons, esters, ketones, ethers, or a mixture of two or more of these is used. As the alcohol, for example, methanol, ethanol, 2-propanol, butanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 1-propoxy-2-propanol, 4-methyl-2-pentanol, 2-ethylbutanol, 3-methoxy-3-methylbutanol, ethylene glycol, diethylene glycol, glycerin, etc. are preferable. As the aliphatic or alicyclic hydrocarbons, n-hexane, n-octane, cyclohexane, cyclopentane, cyclooctane, etc. are preferable. As the aromatic hydrocarbons, toluene, xylene, ethylbenzene, etc. are preferable. As the esters, ethyl formate, ethyl acetate, n-butyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, etc. are preferred. As the ketones, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc. are preferred. As the ethers, dimethoxyethane, tetrahydrofuran, dioxane, diisopropyl ether, etc. are included. When preparing the zirconium component-containing liquid used in the present invention, it is preferred to use alcohols among the above-mentioned various solvents from the viewpoint of the stability of the solution.

[0053] Next, the stabilizer will be described. Zirconium alkoxide is highly reactive to water, so it is rapidly hydrolyzed by the addition of moisture in the air or water, causing the solution to become cloudy and precipitate. In order to prevent this, it is preferable to add a stabilizer to stabilize the solution. Examples of the stabilizer include β-diketone compounds such as acetylacetone, 3-methyl-2,4-pentanedione, 3-ethyl-2,4-pentanedione, and trifluoroacetylacetone; β-ketoester compounds such as methyl acetoacetate, ethyl acetoacetate, butyl acetoacetate, allyl acetoacetate, benzyl acetoacetate, isopropyl acetoacetate, tert-butyl acetoacetate, isobutyl acetoacetate, ethyl 3-oxohexanoate, 2-methyl ethyl acetoacetate, 2-fluoro ethyl acetoacetate, and 2-methoxyethyl acetoacetate; and alkanolamines such as monoethanolamine, diethanolamine, and triethanolamine. The amount of the stabilizer added is preferably 0.1 or more and 3 or less in molar ratio to the zirconium alkoxide. More preferably, it is 0.5 or more and 2 or less.

[0054] Another preferred example is a zirconium component-containing liquid that is composed of particles of a zirconium component, a dispersant, and a solvent.

[0055] As the particles of the zirconium component, zirconium particles or zirconia particles, which is an oxide, can be used. The zirconium particles or zirconia particles can be produced by crushing the respective materials using a top-down method, or can be synthesized by a bottom-up method using a technique such as a hydrothermal reaction from metal salts, hydrates, hydroxides, carbonates, etc., or can be commercially available products. The size of the particles is preferably 300 nm or less, more preferably 50 nm or less, in order to allow the particles to penetrate into microcracks. The shape of the particles is not particularly limited, and may be spherical, granular, cylindrical, elliptical, cubic, rectangular, needle-like, columnar, plate-like, scaly, or pyramidal.

[0056] The dispersant preferably contains at least one of an organic acid, a silane coupling agent, and a surfactant. As the organic acid, for example, acrylic acid, 2-hydroxyethyl acrylate, 2-acryloxyethyl succinic acid, 2-acryloxyethyl hexahydrophthalic acid, 2-acryloxyethyl phthalic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, 3-methylhexanoic acid, 3-ethylhexanoic acid, etc. are preferable. As the silane coupling agent, for example, 3-acryloxypropyl trimethoxysilane, 3-methacryloxypropyl trimethoxysilane, hexyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, etc. are preferable. As the surfactant, for example, ionic surfactants such as sodium oleate, potassium fatty acid, sodium alkyl phosphate, alkylmethylammonium chloride, and alkylamino carboxylate, and nonionic surfactants such as polyoxyethylene laurin fatty acid ester and polyoxyethylene alkylphenyl ether are preferable.

[0057] As the solvent, alcohols, ketones, esters, ethers, ester-modified ethers, hydrocarbons, halogenated hydrocarbons, amides, water, oils, or a mixture of two or more of these solvents is used. As the alcohols, for example, methanol, ethanol, 2-propanol, isopropanol, 1-butanol, ethylene glycol, etc. are preferable. As the ketones, for example, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc. are preferable. As the esters, for example, ethyl acetate, propyl acetate, butyl acetate, 4-butyrolactone, propylene glycol monomethyl ether acetate, methyl 3-methoxypropionate, etc. are preferable. As the ethers, for example, ethylene glycol monomethyl ether, diethylene glycol monobutyl ether, butyl carbitol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-butoxyethanol, etc. are preferable. As the modified ethers, for example, propylene glycol monomethyl ether acetate is preferable. Preferred examples of the hydrocarbons include benzene, toluene, xylene, ethylbenzene, trimethylbenzene, hexane, cyclohexane, and methylcyclohexane. Preferred examples of the halogenated hydrocarbons include dichloromethane, dichloroethane, and chloroform. Preferred examples of the amides include dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone. Preferred examples of the oils include mineral oil, vegetable oil, wax oil, and silicone oil.

[0058] The zirconium component-containing liquid may be prepared by simultaneously mixing zirconium particles or zirconia particles, a dispersant, and a solvent, or by mixing zirconium particles or zirconia particles with a dispersant and then mixing a solvent, or by mixing the zirconium or zirconia fine particles with the solvent and then mixing the dispersant, or by mixing the dispersant with the solvent and then mixing the zirconium or zirconia fine particles. The solution may be prepared by reacting at room temperature or at reflux.

[0059] The solid concentration of the zirconia component is determined by the molar ratio of the zirconium alkoxide, organic solvent, and stabilizer. The weight percent of the zirconia solids is preferably in the range of 3% to 20%, more preferably 8% to 15%. If the concentration is low, it is difficult to obtain the effect of filling the microcracks, and if the weight percent is 3% or more, a certain effect is obtained, and if it is 8% or more, the effect is even greater. If the weight percent is high, the viscosity becomes too high, making it difficult for the liquid to be absorbed into the microcracks, and the effect is difficult to obtain, and if the weight percent is 20% or less, a certain effect is obtained, and if it is 15% or less, the effect is even greater.

[0060] In the above step (ii), the powder melted by the energy beam irradiation is cooled by the surroundings and solidifies to form an intermediate object. In the case of ceramics, the temperature difference between melting and solidifying is large, so many microcracks occur in the intermediate object.

[0061] The zirconium component-containing liquid is distributed not only in the surface layer of the shaped object but also inside the shaped object through the microcracks. There is no particular limitation on the method of absorbing the zirconium component-containing liquid into the shaped object, so long as a sufficient amount of the zirconia component can be present in a sufficient range of the microcracks of the shaped object. The shaped object may be impregnated in the zirconium component-containing liquid, the zirconium component-containing liquid may be sprayed onto the intermediate shaped object in a mist form, or the zirconium component-containing liquid may be applied with a brush or the like. In addition, a combination of these methods may be used, or the same method may be repeated multiple times. When spraying the zirconium component-containing liquid or applying the zirconium component-containing liquid, it is preferable to spray or apply 5% by volume or more and 20% by volume or less of the zirconium component-containing liquid onto the shaped object that has not absorbed the zirconium component-containing liquid. If the amount is less than 5% by volume, the amount of the zirconium component disposed in the microcrack portion of the shaped object is insufficient, and the microcrack portion may not melt. If the content is more than 20% by volume, when step (i) is performed after step (iii), it may be difficult to uniformly distribute the powder on the shaped object due to the influence of the zirconium component-containing liquid. In the case of a large-volume shaped object obtained by repeating steps (i) and (ii) to form a shaped object having a porous portion, a method of immersing the shaped object in the zirconium component-containing liquid, degassing under reduced pressure, and impregnating the shaped object is preferable. Alternatively, it is preferable to spray the zirconium component-containing liquid in a mist form and have the liquid absorbed by the shaped object at each stage during the process of repeating steps (i) and (ii) to form a shaped object having a porous portion.

[0062] <Process (iv)> In the step (iv) of the method for producing a shaped article according to the present invention, the shaped article having absorbed the zirconium component-containing liquid is heated.

[0063] In the above step (iii), the zirconium component-containing liquid is distributed in the microcracks on the surface of the shaped object and inside the shaped object.

[0064] As mentioned above, zirconium and aluminum oxide form a eutectic, so in areas where these components exist, melting begins at the eutectic point. For example, the eutectic point of aluminum oxide and zirconium oxide is about 1900°C, and the melting points of each component alone (Al 2 O 3 is 2070℃, ZrO 2 The melting point is lower than 2715°C). In other words, melting begins at a temperature lower than the melting point of the molded object whose main component is aluminum oxide. In other words, the melting point of the area where zirconium is present can be significantly lowered locally, and this difference in melting point can be used to heat the molded object at a temperature above the eutectic point and below the melting point of the molded object, thereby selectively melting only the areas near the microcracks. Specifically, the molded object that has undergone step (iv) is heated so that the maximum temperature is between 1600°C and 1710°C.

[0065] When the microcracked area reaches a maximum temperature of 1600°C to 1710°C, the microcracked area where the zirconium component is present will melt. Therefore, the heating time is not an issue. In the molten state, atomic diffusion proceeds in the direction that reduces the surface energy, and the microcracks eventually decrease and disappear. By controlling the heating temperature, it is possible to melt only the area near the zirconium component, so the shape of the molded object does not collapse and the advantages of the direct molding method are guaranteed. Therefore, the shape of the molded object is maintained even if it is heated for a long time. After melting, the molded object solidifies and recrystallizes, and the mechanical strength is greatly improved due to the reduction and disappearance of microcracks.

[0066] If a sufficient amount of zirconia is present in the microcrack portion, the vicinity of the microcrack will melt as described above, which has the effect of reducing or eliminating the microcracks. In particular, when the vicinity of the microcrack approaches a eutectic composition in which the shaped object is mainly composed of aluminum oxide (78 mol%) and zirconium oxide (approximately 22 mol%), the vicinity of the microcrack will melt more easily. In order to reduce or eliminate the microcracks by melting the vicinity of the microcracks, it is preferable to heat at a temperature of 1650°C or higher and 1710°C or lower. More preferably, it is 1662°C to 1670°C.

[0067] The method of heating the molded object is not particularly limited. The molded object that has absorbed the zirconium component-containing liquid may be heated by irradiating it with an energy beam again, or may be heated in an electric furnace. When heating with an energy beam, it is necessary to grasp in advance the relationship between the amount of heat input by the energy beam and the temperature of the molded object using a thermocouple or the like so that the molded object is heated to the above-mentioned preferred temperature.

[0068] In the heating process, the surface layer of the molded object or the vicinity of the microcracks may melt, causing the molded object to adhere to a setter (a baking shelf, a shelf board, a base board, etc.). Therefore, when placing the molded object on a setter in the heating process, it is preferable that the setter is inactive. As an inactive setter, for example, platinum or the like can be used in an air atmosphere, and iridium or the like can be used in a low-oxygen atmosphere.

[0069] <Flow of each process> The order of each step and examples of repetition patterns will be described below.

[0070] The basic flow is to execute each step in the order of step (i), step (ii), step (iii), and step (iv), but steps (iii) and (iv) may be executed repeatedly.

[0071] By repeatedly carrying out steps (iii) and (iv), it is preferable to bring the vicinity of the microcracks of the molded object closer to a eutectic composition in which the aluminum oxide-based object is 78 mol% and the zirconium oxide is about 22 mol%. This makes it easier to melt the vicinity of the microcracks, improving the effect of reducing and eliminating the microcracks. At this time, the liquid is absorbed in the absorption step so that the ratio of the zirconium component to the metal component contained in the porous portion is 0.3 mol% or more and 2.0 mol% or less.

[0072] [Composite ceramic parts consisting of porous and dense parts] Fig. 7 is a schematic diagram of an example of a one-piece composite ceramic part 403 made of a porous part 401 and a dense part 402 for holding the porous part 401. In Fig. 7, the porous part 401 is surrounded by the dense part 402 and is integrated into one piece. These composite ceramic parts 403 can be used as an adsorption plate by connecting an intake / exhaust member. The example in Fig. 7 is merely one example, and a plurality of porous parts 401 may be independently arranged in the dense part 402, or the dense part 402 may be arranged inside the porous part 401.

[0073] In the present invention, the dense portion 402 constituting the composite ceramic part 403 is made of a metal oxide containing aluminum and zirconium, and the proportion of zirconium in the metal components constituting the metal oxide is smaller than that of the porous portion 401. EXAMPLES

[0074] The method for producing a shaped object according to the present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0075] Example 1 In this example, a porous portion having a lattice pattern was fabricated. This roughly corresponds to a lattice pattern with holes spaced at a pitch of 175 μm.

[0076] <Step (i), Step (ii) and Step (iii)> α-Al 2 O 3 Powder, Gd 2 O 3 Powder, Tb 2 O 3.5 Powder (Tb 4 O 7 Powder) was prepared, and the molar ratio was Al 2 O 3 :Gd 2 O 3 :Tb 2 O 3.5 The powders were weighed out so that the ratio of the powder mass to the total mass was 77.4:20.8:1.8. The weighed powders were mixed in a dry ball mill for 30 minutes to obtain a mixed powder (material powder). The composition of the powdered material was analyzed by ICP emission spectrometry, and the zirconium oxide content was found to be less than 0.1 mol %.

[0077] Next, a shaped object of Example 1 was formed through steps basically similar to those shown in FIGS. 1A to 1H described above. To form the object, a 3D SYSTEMS ProX DMP 100 (product name) equipped with a 50 W Nd:YAG laser (beam diameter 65 μm) was used.

[0078] First, a roller was used to form a 20 μm-thick first powder layer of the above-mentioned material powder on a base made of pure alumina (step (i)). Next, a 30 W laser beam was irradiated onto the powder layer, and the material powder in a 10 mm × 10 mm square area was melted and solidified in a mesh-like pattern. The drawing speed was 180 mm / s and the drawing pitch was 175 μm (step (ii)). The drawing lines were angled at 45 degrees to each side of the square. Next, a new 20 μm-thick powder layer was formed with a roller so as to cover the above-mentioned melted and solidified part (step (i)). The laser was irradiated onto the powder layer directly above the above-mentioned square area, so as to be perpendicular to the drawing lines of the first layer, and the powder in the 10 mm × 10 mm area was melted and solidified (step (ii)).

[0079] By repeating this process (iii), a molded object with a base dimension of 10 mm × 10 mm and a height of 3 mm was formed. The molded object contained unsolidified powder, and by removing the unsolidified powder, a molded object with a porous structure was obtained.

[0080] <Process (iv)> The zirconium component-containing liquid was prepared as follows: 85% by weight of zirconium (IV) butoxide (hereinafter, Zr(On-Bu) 4 A solution of Zr(On-Bu) was prepared by dissolving the above Zr(On-Bu) in 1-butanol. 4 The solution was dissolved in 2-propanol (IPA) and ethyl acetoacetate (EAcAc) was added as a stabilizer. The molar ratio of each component was Zr(On-Bu) 4 The mixture was stirred at room temperature for about 3 hours to prepare a zirconium component-containing liquid, the weight concentration of which was 8% zirconia solid matter.

[0081] The above-mentioned shaped article processed for testing was immersed in the zirconium component-containing liquid, degassed under reduced pressure for 1 minute to allow the liquid to penetrate (impregnate) into the interior of the shaped article, and then naturally dried for 1 hour.

[0082] The shaped object impregnated (absorbed) with the zirconium component-containing liquid as described above was placed on a platinum wire provided on an alumina plate, and then heated in an electric furnace. Specifically, the temperature was raised to 1670°C in an air atmosphere over 2.5 hours, and the object was held at 1670°C for 50 minutes. Then, the current was stopped and the object was cooled to 200°C or less over 1.5 hours (step (iv)).

[0083] In Example 1, the step of causing the shaped article to absorb the zirconium component-containing liquid (step (iii)) and the heating step (step (iv)) were alternately repeated five times each to obtain a ceramic article having a porous portion.

[0084] <Evaluation> [Evaluation method] The average pore size was evaluated by the following method. A scanning electron microscope (SEM) was used to obtain an SEM image of the polished surface of a molded object having a porous portion. The average pore size was calculated as follows. First, the area S and the maximum distance (2a) of the hole contour were obtained from the SEM image for each hole, and b=S / (πa) was calculated. The average value of the minor axis diameter of the ellipse with the major axis diameter 2a and the minor axis diameter 2b thus obtained was taken as the average pore size. The average pore size described in this specification has the same meaning.

[0085] The porosity was measured by the mercury injection method. Therefore, the porosity in the present invention refers to the ratio of open pores to the volume of the ceramic article, and does not include closed pores.

[0086] The Zr content and the average grain size of the Zr region were evaluated by the following method. A compositional analysis of the porous portion was performed in an area of ​​2 mm x 2 mm using SEM-EDX analysis, and the ratio of Zr components to all metal elements was taken as the Zr content. For the average grain size, mapping of the compositional distribution of the porous portion in the same area was performed, and the area of ​​a continuous region containing Zr components as the main component was calculated by regarding it as one zirconia region, and the diameter of a circle equivalent to that area (equivalent circle diameter) was calculated. The equivalent circle diameters were calculated for multiple zirconia regions, and the average value was taken as the average equivalent circle diameter of the zirconia regions.

[0087] The molding accuracy and mechanical strength were evaluated using the following method. The molding accuracy refers to the difference between the dimensions of the ceramic article after the firing process and the design dimensions. For a molded object measuring 10 mm x 10 mm and 3 mm high, the maximum change rate on the top surface of the molded object in steps (iii) and (iv) was compared, and the change rate was expressed in order of quality as A, B, and C. That is, a molded object with a change rate of 3% or less was expressed as molding accuracy A, a molded object with a change rate of 3% or more but less than 5% was expressed as molding accuracy B, a molded object with a change rate of more than 5% was expressed as molding accuracy C, and a molded object with damage or the like and not suitable for practical use was expressed as molding accuracy D. Specifically, the molded object with molding accuracy A had a dent on the top surface of 0.3 mm or less, the molded object with molding accuracy B had a dent on the top surface of more than 0.3 and less than 0.5 mm, and the molded object with molding accuracy C had a dent on the top surface of more than 0.5 mm.

[0088] The mechanical strength was measured as follows. First, after the porous portion was impregnated and sintered (step (iv)), the surface of the sample was polished using abrasive papers from No. 250 to No. 15,000, and finally polished using No. 15,000 lapping film abrasive paper, and SEM image 1 was obtained. Next, the sample from which SEM image 1 was obtained was placed on a No. 600 diamond polishing disk (manufactured by Musashino Electronics Co., Ltd.) rotating at 80 rpm, cut with a load of 0.5 kg, and SEM image 2 was obtained. The loss ratio of SEM image 2 to SEM image 1 was expressed as mechanical strength A or less, that of SEM image 2 was greater than 10% and less than 20%, and that of SEM image 2 was expressed as mechanical strength B, and that of SEM image 2 was expressed as mechanical strength C.

[0089] [Evaluation Results] An optical microscope image of the porous part of the produced ceramic article is shown in Figure 4A. An SEM image is shown in Figure 5A, and a mapping image of the composition distribution of the Zr component of the same area by SEM-EDX is shown in Figure 5B. The obtained porous part had open pores that communicated from one surface to the opposite surface. The average pore size in the porous part was 115 μm, and the porosity was 31 vol. %. The closed pores were 0.4 vol. %. The Zr content was 1.56 mol. %. The average equivalent circle diameter of the zirconia region was 20 μm, and the zirconia region was distributed so as to extend from the bridge part to the outside of the bridge part. The porous part of the obtained ceramic article had a molding accuracy of B and mechanical strength of A.

[0090] Example 2 This embodiment is an example in which the content of the zirconium component in the porous portion is different. A porous ceramic was produced under the same conditions as in Example 1, except that the step of immersing in a zirconium component-containing liquid (step (iii)) and the step of heating (step (iv)) were alternately repeated twice each. The produced ceramic article having porosity was evaluated in the same manner as in Example 1.

[0091] Example 3 This embodiment is an example in which the arrangement of openings in the porous portion is random. A porous ceramic article was produced under the same conditions as in Example 1, except that the drawing speed was 220 mm / s and the drawing pitch was 125 μm to obtain a porous portion having randomly arranged openings. An optical microscope image of the porous portion is shown in FIG. 4B. The produced porous ceramic was evaluated in the same manner as in Example 1.

[0092] Example 4 This example is an example of the fabrication of a composite ceramic part consisting of a ceramic porous portion and a ceramic dense portion for supporting the porous portion. In Fig. 7, the porous portion has a lattice pattern with a period of 175 μm, and the dense portion surrounds and integrates the porous portion.

[0093] The porous portion was produced under the same laser irradiation conditions as in Example 1. The dense portion was produced by irradiating a 30 W laser beam at a drawing speed of 100 mm / s to 140 mm / s and a drawing pitch of 100 μm. FIG. 6A shows an SEM image of the boundary between the porous portion and the dense portion of the obtained composite ceramic part. FIG. 6B and FIG. 6C show mapping images of the composition distribution of the Zr component by SEM-EDX in the regions corresponding to a part 601 of the porous portion and a part 602 of the dense portion shown in FIG. 6A, respectively. The porous portion and the dense portion of the produced ceramic article were evaluated in the same manner as in Example 1.

[0094] (Examples 5 to 8) This example is an example in which the content of the zirconium component in the lattice-like porous portion is different. The conditions are the same as in Example 1, except that the step of immersing in the zirconium component-containing liquid was repeated 3, 4, 6, and 8 times, respectively.

[0095] (Examples 9 to 14) This example is an example in which the content of the zirconium component in the porous portion having randomly arranged pores is different. The conditions are the same as in Example 3, except that the step of immersing in the zirconium component-containing liquid was repeated 2, 3, 4, 6, 7, and 8 times, respectively.

[0096] (Examples 15 and 16) This example is an example of a composite ceramic part consisting of a ceramic porous part and a ceramic dense part for supporting the porous part, the content of the zirconium component being different. The conditions are the same as in Example 4, except that the step of immersing in the zirconium component-containing liquid was repeated 4 and 6 times, respectively.

[0097] (Comparative Examples 1 to 3) Porous ceramics were obtained in the same manner as in Example 1, except that the step of immersing the intermediate shaped article in a zirconium component-containing liquid (step (iii)) and the step of heating the intermediate shaped article that has absorbed the zirconium component-containing liquid (step (iv)) were not performed in Comparative Example 1, were performed once in Comparative Example 2, and were performed eight times in Comparative Example 3. The produced ceramic articles having porous portions were evaluated in the same manner as in Example 1.

[0098] Comparative Example 4 This comparative example is an example in which the content of the zirconium component in the porous portion having randomly arranged pores is different, and the conditions are the same as those of Example 3, except that the step of immersing in the zirconium component-containing liquid was performed once.

[0099] (Examples 17 to 19) This example is an example of a composite ceramic part having a porous portion and a dense portion for supporting the porous portion, the content of the zirconium component being different. The conditions are the same as in Example 4, except that the step of immersing in the zirconium component-containing liquid was repeated 2, 3, and 7 times, respectively.

[0100] Comparative Example 5 This comparative example is an example of a composite ceramic part consisting of a porous portion and a dense portion for supporting the porous portion, with a different content of zirconium component. The conditions are the same as in Example 4, except that the step of immersing in the zirconium component-containing liquid was repeated nine times each.

[0101] The above evaluation results of the examples and comparative examples are shown in Table 1. [Table 1]

[0102] (Consideration) [Zr content and Zr components] Comparing Example 1, Example 2, and Comparative Examples 1 to 3, the Zr content increased with an increase in the number of Zr impregnations in the porous ceramic portion (0, 1, 2, 5, 8 times). It was found that the average grain size of the Zr region also increased with an increase in the Zr content, and precipitated crystal grains with an average grain size of 10 μm or more were bonded to form a continuous mesh. Most of the Zr component was zirconium oxide (ZrO 2 Evaluations using SEM-EDX and XRD revealed that the ZnO does not remain as a single metal but forms a complex oxide with Gd.

[0103] Furthermore, as is apparent from the results of Example 4 in Table 1 and from Figures 6B and 6C, when Zr impregnation was performed under similar conditions, the Zr content was higher in the porous portion than in the dense portion. This is believed to be because the zirconium component-containing liquid penetrates into the inside of the molded object through the open pores in the porous portion, and because the porous portion has a large surface area, more zirconium component penetrates into the dense portion.

[0104] [Relationship between Zr concentration, molding accuracy, and mechanical strength] The ceramic articles with molding accuracy of A, B, and C were free of damage and were sufficient for practical use as ceramic articles. In particular, the ceramic articles with molding accuracy of A and B had good molding accuracy and were suitable as examples for obtaining ceramic articles with complex or fine shapes. On the other hand, the comparative ceramic article with molding accuracy of D had poor molding accuracy and a large difference from the designed dimensions, and also showed damage such as cracks, making it impossible to obtain specifications sufficient for practical use.

[0105] Examples 1 to 3, Examples 5 to 14, and Comparative Examples 1 to 4 in which ceramic articles composed only of a porous part were shaped are compared, and the relationship between the zirconium content rate of the porous part and the shaping accuracy is considered. Regarding the shaping accuracy, it is good when Zr is not contained or when the Zr content rate is 1.5 mol% or less (0 ≦ Zr ≦ 1.5 mol%), and the change rate between the dimensions of the ceramic article after the firing process after shaping and the designed dimensions is 3% or less (shaping accuracy A). When the Zr content rate increases, the shaping accuracy decreases. In the range where 1.5 < Zr ≦ 2.0 mol%, the change rate is greater than 3% and 5% or less (shaping accuracy B). Further, when the Zr content rate increases and becomes greater than 2.0 mol%, the change rate becomes greater than 5% (shaping accuracy C). As the Zr content rate increases, the melting point decreases, so the portion where crystals melt increases, and the bridges in the porous part deform, resulting in loss of shaping accuracy. As a result, the porosity and the average pore diameter also vary from the designed values.

[0106] On the other hand, regarding the mechanical strength, it improves as the Zr content rate increases. When the Zr content rate is less than 0.3 mol% (0 ≦ Zr < 0.3 mol%), the mechanical strength is weak, and the defect ratio is greater than 20% (mechanical strength C). As the Zr content rate increases (0.3 ≦ Zr < 0.7 mol%), the defect ratio decreases (greater than 10% and 20% or less), and sufficient mechanical strength is obtained (mechanical strength B). Further, when the Zr content rate increases and becomes 0.7 mol% or more, the defect ratio becomes 10% or less, and the mechanical strength further improves (mechanical strength A). When the degree of improvement in mechanical strength is small, the ratio of the porous part being defective during processing or in the use environment increases.

[0107] From the above, it was found that in order to simultaneously achieve molding accuracy and mechanical strength in the porous part (both molding accuracy and mechanical strength are A or B), the ratio of the zirconium component in the metal components constituting the metal oxide must be 0.3 mol% or more and 2.0 mol% or less. Furthermore, it was found that the zirconium component under this condition forms crystal grains with an average grain size of 10 μm or more as a metal oxide composite with other metal components, and the crystal grains are connected to form a mesh-like structure. The crystal grains mainly composed of zirconium form crystals composite with Gd, forming a complex network that permeates the inside of the eutectic structure. As a result, the high mechanical strength that the crystal grains mainly composed of zirconium originally have is effectively imparted to the eutectic structure, so that sufficient mechanical strength can be obtained even in the porous part composed of fine bridge parts. It was found that in order to simultaneously achieve further preferable molding accuracy and mechanical strength (both molding accuracy and mechanical strength are A), the ratio of the zirconium component in the metal components constituting the metal oxide must be 0.7 mol% or more and 1.5 mol% or less.

[0108] As described above, the method for producing a porous ceramic object according to the present invention makes it possible to obtain high shaping accuracy while greatly improving the mechanical strength of the object. [Industrial Applicability]

[0109] According to the present invention, it is possible to improve the mechanical strength of a ceramic article having a porous portion while still taking advantage of the characteristics of the direct molding method that allows for the production of objects with dense and complex shapes.

[0110] The present invention is not limited to the above-described embodiments, and various modifications and variations can be made without departing from the spirit and scope of the present invention. Therefore, the following claims are appended to apprise the public of the scope of the present invention.

[0111] This application claims priority based on Japanese Patent Application No. 2018-229383, filed on December 6, 2018, the entire contents of which are incorporated herein by reference. [Explanation of symbols]

[0112] 101…Powder 102…Powder layer 103...Solidification section 110…Sculpted object 130…Foundation 151...Stage 152…Roller 180…Energy beam source 181…Scanner section 190...Liquid injection nozzle 201…Cladding nozzle 202…Powder supply hole 203…Energy beam 301...Porous ceramics 302...Open hole 303…pore diameter 304...Period of opening 401...Porous part 402…Dense part 403...Composite ceramic parts

Claims

1. 1. A method for making a ceramic article, comprising the steps of: (i) smoothing a powder of a metal oxide mainly composed of aluminum oxide to form a powder layer; (ii) irradiating the powder layer with an energy beam based on modeling data to melt and solidify or sinter the powder; (iii) a step of allowing a liquid containing zirconium to be absorbed into a shaped object having a porous portion formed by repeating the steps (i) and (ii); (iv) heating the shaped object that has absorbed the liquid containing the zirconium element, the porous portion is composed of a bridge portion which is a structural portion forming holes and a plurality of openings, the thickness of the bridge portion is 1 mm or less, the pore diameter of the openings is 50 μm or more and 1000 μm or less, and the porosity of the porous portion is 5 volume % or more; A method for manufacturing a ceramic article, characterized in that in the absorbing step, the liquid is absorbed so that the ratio of zirconium elements to all metal elements contained in the porous portion is 0.3 mol % or more and 2.0 mol % or less.

2. 1. A method for making a ceramic article, comprising the steps of: (i) irradiating a powder of a metal oxide mainly composed of aluminum oxide with an energy beam based on modeling data, and melting and solidifying or sintering the powder to form a model having a porous portion; (ii) allowing the shaped object formed in step (i) to absorb a liquid containing zirconium; (iii) heating the shaped object that has absorbed the liquid containing the zirconium element, the porous portion is composed of a bridge portion which is a structural portion forming holes and a plurality of openings, the thickness of the bridge portion is 1 mm or less, the pore diameter of the openings is 50 μm or more and 1000 μm or less, and the porosity of the porous portion is 5 volume % or more; A method for manufacturing a ceramic article, characterized in that in the absorbing step, the liquid is absorbed so that the ratio of zirconium elements to all metal elements contained in the porous portion is 0.3 mol % or more and 2.0 mol % or less.

3. 3. The method for producing a ceramic article according to claim 1, wherein the proportion of zirconium in the metal elements contained in the metal oxide powder is less than 0.15 mol %.

4. The method for producing a ceramic article according to any one of claims 1 to 3, wherein the metal oxide powder contains a rare earth oxide.

5. 5. The method for producing a ceramic article according to claim 4, wherein the rare earth oxide further contains at least one oxide selected from the group consisting of gadolinium oxide, terbium oxide and praseodymium oxide.

6. A ceramic article made of a metal oxide containing aluminum oxide as a main component and having a porous portion, the porous portion is composed of a bridge portion which is a structural portion forming holes and a plurality of openings, the thickness of the bridge portion is 1 mm or less, the pore size of the openings is 50 μm or more and 1000 μm or less, the porosity of the porous portion is 5 vol % or more, and the ratio of closed pores contained in the porous portion is 0.5 vol % or less, The ratio of zirconium to all metal elements contained in the porous portion is 0.3 mol% or more and 2.0 mol% or less, When a composition analysis of the porous portion is performed in an area of ​​2 mm x 2 mm by SEM-EDX analysis and a composition distribution of the porous portion is mapped in the area, the porous portion has a continuous region containing zirconium as a main component with respect to all metal elements, In the region, at least a part of the zirconium element contained in the porous portion forms a composite metal oxide with a rare earth element constituting the porous portion, an average equivalent circle diameter calculated from the diameter of a circle corresponding to the area of ​​each of the regions is 10 μm or more; A ceramic article, characterized in that in the porous portion, the surface of the bridge portion has the region.

7. 7. The ceramic article according to claim 6, wherein the ratio of zirconium to all metal elements contained in the porous portion is 0.3 mol % or more and 1.5 mol % or less.

8. 8. The ceramic article according to claim 6, wherein the porous portion contains gadolinium in an amount equal to or greater than the amount of zirconium, and the region is made of a composite metal oxide of zirconium and gadolinium.

9. 9. The ceramic article according to claim 6, wherein the porous portion has a porosity of 5 volume % or more and 60 volume % or less.

10. 10. The ceramic article according to claim 6, wherein the porous portion contains closed pores at a ratio of 0.5 volume % or less.

11. A ceramic article made of a metal oxide containing aluminum oxide as a main component and having a dense portion and a porous portion, the porous portion is composed of a bridge portion which is a structural portion forming holes and a plurality of openings, the thickness of the bridge portion is 1 mm or less, the pore size of the openings is 50 μm or more and 1000 μm or less, the porosity of the porous portion is 5 vol % or more, and the ratio of closed pores contained in the porous portion is 0.5 vol % or less, The dense portion is a portion of the bridge portion having a thickness of 1 mm or more and a porosity of less than 5 volume %, a ratio (mol %) of zirconium in all metal elements contained in the porous portion is higher than a ratio (mol %) of zirconium in all metal elements contained in the dense portion, When a composition analysis of the porous portion is performed in an area of ​​2 mm x 2 mm by SEM-EDX analysis and a composition distribution of the porous portion is mapped in the area, the porous portion has a continuous region containing zirconium as a main component with respect to all metal elements, In the region, at least a part of the zirconium element contained in the porous portion forms a composite metal oxide with a rare earth element constituting the porous portion, A ceramic article characterized in that an average equivalent circle diameter calculated from the diameter of a circle equivalent to the area of ​​each of the regions is 10 μm or more, and in the porous portion, a surface of the bridge portion has the regions.

12. 12. The ceramic article according to claim 11, wherein a ratio of zirconium to all metal elements contained in the porous portion is 0.3 mol % or more and 2.0 mol % or less.

13. 13. The ceramic article according to claim 11, wherein the porous portion contains gadolinium in an amount equal to or greater than the amount of zirconium, and the region is made of a composite metal oxide of zirconium and gadolinium.

14. The ceramic article according to claim 11 , wherein the porous portion has pores communicating with the outside.

15. The ceramic article according to any one of claims 11 to 14, wherein the porosity of the porous portion is 5 volume % or more and 60 volume % or less.

16. 16. The ceramic article according to claim 11, wherein the porous portion contains closed pores at a ratio of 0.5 volume % or less.

17. The ceramic article according to claim 11 , wherein the dense portion is provided so as to support the porous portion.

18. The ceramic article according to claim 11 , which is an adsorption plate having the porous portion as an intake and exhaust portion.

Citation Information

Patent Citations

  • Member for heat treatment consisting of alumina sintered compact having excellent durability

    JP2002316866A

  • A member for fusing the vertebral bodies

    JP2017529297A

  • Laminate-molding sintered body, method for producing laminate-molding sintered body, and kit for producing laminate-molding sintered body

    JP2018031050A

  • vacuum suction pad

    JP3213127U