Luminous aromatic polycarbonate resin composition, luminous resin molded article, and method for producing same
By doping an alkaline earth metal oxide with a lanthanoid rare earth element and incorporating microprotrusions, the luminescent compound addresses decomposition issues in aromatic polycarbonate resins, maintaining phosphorescence and impact strength under UV exposure.
Patent Information
- Application Number
- JP2020217894
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-25
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-12-25
AI Technical Summary
Conventional phosphorescent phosphors blended with aromatic polycarbonate resins cause decomposition, leading to poor impact strength and transparency, and are susceptible to photodecomposition under UV light, limiting their use to specific applications.
A luminescent compound is developed by doping an alkaline earth metal oxide with a lanthanoid rare earth element, incorporating microprotrusions containing phosphorus atoms, which enhances the phosphorescence properties and reduces molecular weight reduction of the polycarbonate resin.
The solution maintains excellent phosphorescence properties while significantly reducing molecular weight reduction, ensuring the resin's impact strength and transparency, even under outdoor exposure to sunlight.
Smart Images

Figure 0007557362000010 
Figure 0007557362000002 
Figure 0007557362000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a phosphorescent aromatic polycarbonate resin composition, a phosphorescent resin molded article, and a method for producing the same. [Background technology]
[0002] Phosphors that emit a long afterglow (from about 10 minutes to several hours) in a dark place and can be seen by the naked eye are called phosphorescent phosphors or luminescent agents, and examples of these include ZnS:Cu, ZnCdS:Cu, CaS:Bi, and CaSrS:Bi. These compounds emit light for a long time after they are optically excited by ultraviolet light or the like and then the irradiation is stopped. Molded products that contain phosphorescent phosphors in resin materials are widely used for evacuation signs, indicator lights, luminous signs, phosphorescent signs, and decorations.
[0003] On the other hand, aromatic polycarbonate resin has many excellent properties and is used in a wide range of fields, and is also being studied as a resin material to be combined with a phosphorescent material and put into practical use. For example, Patent Document 1 proposes a light-emitting member made of a phosphorescent material, a fluorescent material, and a transparent resin such as an aromatic polycarbonate resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-146125 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when a conventional phosphorescent phosphor (luminescent agent) is blended with an aromatic polycarbonate resin, the polycarbonate resin composition decomposes due to the properties of the phosphorescent agent, and the required properties (e.g., impact strength and transparency) of an aromatic polycarbonate resin material are not fully satisfied. In addition, conventional phosphorescent agents may be photodecomposed by ultraviolet light in the presence of moisture, resulting in a decrease in brightness, making them difficult to use in applications where they are exposed to direct sunlight (ultraviolet light) outdoors for a long period of time, and their applications are limited to evacuation guidance signs, nighttime display signs, sign buttons, clock faces, etc. In recent years, there has been a demand for polycarbonate resin composition materials that are excellent in phosphorescence and have little decrease in transparency and impact strength even when used in applications where they are exposed to direct sunlight (ultraviolet light) outdoors for a long period of time.
[0006] The present invention aims to provide a phosphorescent aromatic polycarbonate resin composition that has excellent phosphorescent properties and significantly reduces the molecular weight reduction of aromatic polycarbonate resins caused by the properties of phosphorescent agents, as well as a phosphorescent resin molded article made of the resin composition and a method for producing the same. [Means for solving the problem]
[0007] As a result of intensive research into solving the above problems, the present inventors have found that by blending a specific ratio of a phosphorescent agent having a phosphorescent compound formed by doping an alkaline earth metal oxide with a lanthanoid rare earth element and having a plurality of minute protrusions containing phosphorus atoms attached thereto, per 100 parts by mass of an aromatic polycarbonate resin (A), it is possible to obtain an aromatic polycarbonate resin composition in which the phosphorescent properties are not impaired and the decrease in molecular weight of the polycarbonate resin is sufficiently improved, and further research has led to the completion of the present invention.
[0008] That is, the phosphorescent aromatic polycarbonate resin composition according to the present invention contains 100 parts by mass of an aromatic polycarbonate resin (A) and 1 to 35 parts by mass of a phosphorescent agent (B) having a plurality of minute protrusions containing phosphorus atoms attached to a phosphorescent compound obtained by doping an alkaline earth metal oxide with a lanthanoid rare earth element. The phosphorus concentration in the phosphorescent agent (B) is 5000 ppm to 50000 ppm.The luminous resin molded article according to the present invention is made of the above-mentioned luminous aromatic polycarbonate resin composition. The method for producing the luminous resin molded article according to the present invention includes molding the above-mentioned luminous aromatic polycarbonate resin composition. Effect of the Invention
[0009] According to the present invention, it is possible to provide a phosphorescent aromatic polycarbonate resin composition which has excellent phosphorescent properties and which significantly reduces the molecular weight reduction of aromatic polycarbonate resin caused by the properties of a phosphorescent agent, a phosphorescent resin molded article made of the phosphorescent aromatic polycarbonate resin composition, and a method for producing the same. [Brief description of the drawings]
[0010] [Figure 1] SEM photo of surface-treated phosphorescent compound DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the embodiments will be described in detail. However, more detailed explanation than necessary may be omitted. For example, detailed explanation of already well-known matters or duplicate explanation of substantially the same configuration may be omitted. This is to avoid the following explanation becoming unnecessarily redundant and to facilitate understanding by those skilled in the art.
[0012] The inventors provide the following description so that those skilled in the art can fully understand the present invention, and do not intend to limit the subject matter described in the claims.
[0013] The aromatic polycarbonate resin composition according to an embodiment of the present invention contains, per 100 parts by mass of aromatic polycarbonate resin (A), 1 to 35 parts by mass of a phosphorescent agent (B) having a plurality of phosphorus-containing microscopic protrusions attached to a phosphorescent compound obtained by doping an alkaline earth metal oxide with a lanthanoid rare earth element, and may contain a polyalkylene glycol derivative (C) or other components, as necessary.
[0014] The aromatic polycarbonate resin (A) used in the present invention is a polycarbonate resin having a structural unit derived from an aromatic compound, and is not particularly limited as long as it can obtain the aromatic polycarbonate resin composition of the present invention. Examples of such aromatic polycarbonate resins include polymers obtained by the phosgene method in which various dihydroxydiaryl compounds are reacted with phosgene, or the ester exchange method in which a dihydroxydiaryl compound is reacted with a carbonate ester such as diphenyl carbonate. A representative example includes a polycarbonate resin produced from 2,2-bis(4-hydroxyphenyl)propane (bisphenol A).
[0015] Examples of dihydroxydiaryl compounds include, in addition to bisphenol A, bis(hydroxyaryl)alkanes such as bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)phenylmethane, 2,2-bis(4-hydroxyphenyl-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, and 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane; Examples of the cycloalkanes include bis(hydroxyaryl)cycloalkanes such as (4-hydroxyphenyl)cyclopentane and 1,1-bis(4-hydroxyphenyl)cyclohexane; dihydroxydiaryl ethers such as 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether; dihydroxydiaryl sulfides such as 4,4'-dihydroxydiphenyl sulfide; dihydroxydiaryl sulfoxides such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; and dihydroxydiaryl sulfones such as 4,4'-dihydroxydiphenyl sulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone. These can be used alone or in combination. In addition to these, piperazine, dipiperidyl hydroquinone, resorcin, 4,4'-dihydroxydiphenyl, etc. can be used in combination.
[0016] Furthermore, the dihydroxydiaryl compound may be used in combination with, for example, the following trivalent or higher aromatic compounds.
[0017] Examples of trivalent or higher phenolic compounds include phloroglucin, 4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptene, 2,4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptane, 1,3,5-tri-(4-hydroxyphenyl)-benzene, 1,1,1-tri-(4-hydroxyphenyl)-ethane, and 2,2-bis-[4,4-(4,4'-dihydroxydiphenyl)-cyclohexyl]-propane.
[0018] The viscosity average molecular weight of the aromatic polycarbonate resin (A) is preferably 10,000 to 100,000, and more preferably 12,000 to 30,000. When producing such an aromatic polycarbonate resin (A), a molecular weight regulator, a catalyst, etc. may be used as necessary.
[0019] The luminescent agent (B) used in the present invention is SrAl 2 O 4 Or Sr 4 Al 14 O 25 The phosphorescent agent is a phosphorescent compound in which a plurality of minute protrusions containing phosphorus atoms are attached (or fixed) to a phosphorescent compound in which an alkaline earth metal oxide such as a strontium aluminate compound is doped with a lanthanoid rare earth element such as Eu or Dy.
[0020] In general, a phosphorescent compound refers to a compound that stores light such as ultraviolet light and continues to emit light for a long time even after the irradiation of light is stopped, and has a persistence of afterglow of about several minutes to several tens of hours after the end of photoexcitation. Among phosphorescent compounds, it is particularly preferable to use an aluminate-based phosphorescent compound as the raw material for the phosphorescent agent (B). An aluminate-based phosphorescent compound is, for example, SrAl 2 O 4 Or Sr 4 Al 14 O 25The compound represented by the formula (I) is used as the mother crystal, europium Eu is added as an activator in a specific range of mole percent, dysprosium Dy is added as a co-activator in a specific molar ratio to Eu, and further the proportion of Al is set within a specific range with respect to the total number of moles of Sr, Eu, and Dy.
[0021] In the present invention, a phosphorescent compound obtained by surface-treating a raw material powder of a phosphorescent compound in which an alkaline earth metal oxide such as an aluminate is doped with a lanthanoid rare earth element is used as the phosphorescent agent (B). This surface treatment modifies the surface of the phosphorescent compound to prevent defects such as denaturation (including photolysis by ultraviolet light) of the phosphorescent compound due to contact with water (moisture) and adverse effects such as a decrease in molecular weight on the polycarbonate resin material to be mixed.
[0022] The surface treatment may, for example, include a treatment including the following steps as necessary: A step of adding the phosphorescent pigment raw material powder to an aqueous solution containing at least one inorganic acid selected from hydrochloric acid, nitric acid, and sulfuric acid, and at least one phosphate selected from sodium dihydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate, and stirring at a temperature of 20 to 30°C to perform an acid / phosphate treatment. At this time, the mass ratio of the phosphorescent pigment raw material powder to the phosphate in the aqueous solution is 100:4 to 14, and the amount of the inorganic acid in the aqueous solution is such that the pH of the aqueous solution is 5.0 or less. If necessary, the phosphorescent pigment obtained by the acid / phosphate treatment may be washed with water or neutralized with an alkaline aqueous solution (pH adjusted to a range of 6.8 to 7.2), and then dried. It is preferable that the inorganic acid contained in the aqueous solution used in the acid / phosphate treatment is nitric acid, and the phosphate is sodium dihydrogen phosphate.
[0023] The phosphorescent compound obtained by doping a lanthanoid rare earth element on an alkaline earth metal oxide such as an aluminate-based surface treatment can be obtained as a phosphorescent compound to which a plurality of minute protrusions containing phosphorus atoms are attached (or fixed). The phosphorescent compound after the surface treatment is highly stable against contact with water (moisture), and has excellent water resistance (moisture resistance), has excellent afterglow characteristics, has a higher initial afterglow luminance than an untreated phosphorescent compound, is sufficiently excited even at low illuminance, emits light effectively, and is suitable for outdoor use. As a result of X-ray fluorescence (XRF) analysis (NEX-CG manufactured by Rigaku), phosphorus was not detected on the surface of the phosphorescent compound before the surface treatment, but was detected on the surface of the phosphorescent compound after the surface treatment. Here, the concentration range of the detected phosphorus is preferably 5000 ppm to 50000 ppm when calculated by FP quantitative analysis. If the content is less than 5000 ppm, the water resistance is low, and if the content is more than 50000 ppm, the thermal stability of the polycarbonate may be affected. More preferably, the content is 5000 ppm to 40000 ppm, and most preferably, the content is 10000 ppm to 20000 ppm. In addition, when the surface state was observed with a SEM / EDX (JSM-IT500HR manufactured by JEOL Ltd.) at an accelerating voltage of 5 kV, no minute protrusions containing phosphorus were observed on the surface of the phosphorescent compound before the surface treatment, but multiple (many) minute protrusions containing phosphorus with a size (major axis) of about 0.1 to 1.5 μm were observed on the surface of the phosphorescent compound after the surface treatment, as shown in FIG. 1. In addition, the results of elemental analysis of the surface of the phosphorescent compound after the surface treatment with the same device at an accelerating voltage of 15 kV were as follows. The units of the values in Table 1 are mass %.
[0024] [Table 1]
[0025] As shown in Table 1, it was confirmed that the phosphorescent compound used in the present invention, to which a plurality of micro-pillars containing phosphorus atoms are attached (or fixed), contains phosphorus atoms concentrated in the micro-pillar portion. Dysprosium was also localized in the micro-pillar portion of the phosphorescent compound. Furthermore, in the phosphorescent compound containing phosphorus in a portion other than the micro-pillar, phosphorus was relatively more abundant in the micro-pillar portion.
[0026] The inventors speculate that by forming a large number of minute protrusions containing phosphorus atoms on the surface of the raw powder of the phosphorescent compound after the surface treatment, these numerous minute protrusions work together to act like a film that blocks water (moisture) from wetting (absorbing) the surface or inside of the phosphorescent compound, effectively preventing aggregation of the raw powders and denaturation due to contact with water (moisture), and thus the luminance characteristics of the phosphorescent compound are not lost for a long period of time, and there is no adverse effect on the polycarbonate resin material to be melt-kneaded, such as a decrease in the molecular weight of the resin. In fact, in the examples described below, it was confirmed that even when the phosphorescent agent (B) used in the present invention is melt-kneaded with an aromatic polycarbonate resin, excellent phosphorescence is continuously maintained, and the possibility of a decrease in hydrolysis characteristics (molecular weight decrease) for the polycarbonate resin is also significantly reduced. From these results, it can be understood that the phosphorescent agent (B) used in the present invention is prevented from absorbing moisture even when it comes into contact with moisture (water vapor) generated under various environments, and that denaturation is suppressed even when exposed to sunlight. Furthermore, the luminous agent (B) used in the present invention is also inhibited from absorbing moisture during storage.
[0027] The luminescent agent (B) preferably has an average particle size of 1 to 500 μm. Those less than 1 μm or larger than 500 μm are difficult to manufacture, are not practical, and are difficult to obtain, so they are not preferred. Those in the range of 10 to 60 μm are more preferred from a practical standpoint. Furthermore, two or more types of luminescent agents with different average particle sizes can be used in combination.
[0028] The amount of the luminescent agent (B) is 1 to 35 parts by mass, preferably 2 to 25 parts by mass, based on 100 parts by mass of the aromatic polycarbonate resin (A) of the present invention. If the amount of the luminescent agent (B) is less than 1 part by mass, it is difficult to obtain the luminescent effect of the luminescent agent, which is not preferable. On the other hand, if the amount exceeds 35 parts by mass, the molecular weight is significantly reduced, which is not preferable because the transparency and impact resistance are reduced.
[0029] As a result of elemental analysis of the surface of the phosphorescent compound after the surface treatment by SEM / EDX, it is sufficient that the phosphorus atoms are 2.0% or more in the microprojection part, and less than 1.0% in the part other than the microprojection. When phosphorus atoms are detected in the part other than the microprojection, the ratio of phosphorus atoms detected in the microprojection part is at least twice as high as the phosphorus atoms detected in the part other than the microprojection. Furthermore, it is sufficient that dysprosium atoms are 1.0% or more in the microprojection part, and the ratio of dysprosium atoms in the part other than the microprojection is less than 0.5% of the phosphorescent compound. When dysprosium atoms are detected in the part other than the microprojection, the ratio of dysprosium atoms detected in the microprojection part is at least twice as high as the dysprosium atoms detected in the part other than the microprojection.
[0030] As the luminescent agent (B), for example, GDK11010WP (composition formula: SrAl 2 O 4 : Eu, Dy, average particle size 10μm, green emission color), GDK11025WP (composition formula: SrAl 2 O 4 : Eu, Dy, average particle size 25 μm, green emission color), GDK11060WP (composition formula: SrAl 2 O 4 : Eu, Dy, average particle size 60μm, green emission color), GDK13010WP (composition formula: SrAl 2 O 4 : Eu, Dy, average particle size 10 μm, green emission color), GDK13025WP (composition formula: SrAl 2 O 4 : Eu, Dy, average particle size 25μm, green emission color, phosphorus atom 34600ppm,), GDK13060WP (composition formula: SrAl 2 O4 : Eu, Dy, average particle size 60 μm, green emission color), or GDK13100WP (composition formula: SrAl 2 O 4 : Eu, Dy, average particle size 100 μm, green emission color), BDK11025WP (composition formula: Sr 4 Al 14 O 25 : Eu, Dy, average particle size 25 μm, blue emission color), BDK13015WP (composition formula: Sr 4 Al 14 O 25 : Eu, Dy, average particle size 15 μm, blue emission color), BDK13030WP (composition formula: Sr 4 Al 14 O 25 : Eu, Dy, average particle size 30 μm, blue emission color) are commercially available.
[0031] The aromatic polycarbonate resin composition of the embodiment of the present invention may further contain a polyalkylene glycol derivative (C). The polyalkylene glycol derivative (C) is a derivative of a polyalkylene glycol compound, and is not particularly limited as long as the aromatic polycarbonate resin composition of the present invention can be obtained. Representative examples of such polyalkylene glycol derivatives include polyalkylene glycol derivatives represented by the following formula (1).
[0032] Formula (1): RO-(X'-O)m(Y'-O)n-R' (In the formula, R and R' each independently represent a hydrogen atom or an alkyl group having 1 to 30 carbon atoms, X' represents a linear or branched alkylene group having 2 to 4 carbon atoms, Y' represents a linear or branched alkylene group having 2 to 5 carbon atoms, X' and Y' may be the same or different, m and n each independently represent 3 to 60, and m+n represents 6 to 120.)
[0033] The weight average molecular weight of the polyalkylene glycol derivative represented by the formula (1) is preferably 500-8,000, and more preferably 1,000-4,000.
[0034] The polyalkylene glycol derivative represented by formula (1) preferably contains a polyalkylene glycol derivative represented by the following formula (2).
[0035] Formula (2): HO-(CH 2 CH 2 CH 2 CH 2 O)m(CH(CH 3 )CH 2 O)nH (In the formula, m and n each independently represent 3 to 60, and m+n represents 8 to 90.)
[0036] As the polyalkylene glycol derivative represented by formula (2), modified glycols containing tetramethylene glycol units and propylene glycol units are suitable. As such polyalkylene glycol derivatives, commercially available products can be used, such as polyserine DCB-1000 (weight average molecular weight 1000), polyserine DCB-2000 (weight average molecular weight 2000), and polyserine DCB-4000 (weight average molecular weight 4000) manufactured by NOF Corp.
[0037] The weight average molecular weight of the polyalkylene glycol derivative represented by the formula (2) is preferably 500-8,000, and more preferably 1,000-4,000.
[0038] By blending the polyalkylene glycol derivative (C) represented by the general formula (1), the generation of excessive shear heat during molding of the polycarbonate resin composition is suppressed, and the thermal stability is improved, resulting in a good hue and improved brightness.
[0039] The amount of the polyalkylene glycol derivative (C) is preferably 0.05 to 5.0 parts by weight, more preferably 0.1 to 2.0 parts by weight, based on 100 parts by weight of the polycarbonate resin (A). If the amount of the polyalkylene glycol derivative (C) is less than 0.05 parts by weight, the effect of improving thermal stability is insufficient. Conversely, if the amount of the polyalkylene glycol derivative (C) is more than 5.0 parts by weight, the moist heat resistance is reduced.
[0040] In addition, modified glycols containing tetramethylene glycol units and 2-methyltetramethylene glycol units are also preferred as polyalkylene glycols represented by general formula (1). Commercially available products can be used as such polyalkylene glycol derivatives, and examples of such products include PTG-L1000 (weight average molecular weight 1000), PTG-L2000 (weight average molecular weight 2000), and PTG-L3000 (weight average molecular weight 3000) manufactured by Hodogaya Chemical Co., Ltd. In addition, modified glycols containing ethylene glycol units and propylene glycol units are also preferred as polyalkylene glycols represented by general formula (1). Commercially available products can be used as such polyalkylene glycol derivatives, and examples of such products include Unilube 50DE-25 (weight average molecular weight 1750) and Unilube 75DE-25 (weight average molecular weight 1400) manufactured by NOF Corp.
[0041] In addition, other polyalkylene glycol derivatives such as modified glycols, such as one-terminal butyl ether in which a butyl group is bonded to a hydroxyl group at one end of a polyalkylene glycol, and one-terminal stearyl ether in which a stearyl group is bonded to a hydroxyl group at one end of a polyalkylene glycol, are also suitable. As other polyalkylene glycol derivatives, commercially available products can be used, such as Polyserine BC-1000 (one-terminal butyl group, weight average molecular weight 1000) and Polyserine SC-1000 (one-terminal stearyl group, weight average molecular weight 1000) manufactured by NOF Corporation.
[0042] In addition, as other polyalkylene glycol derivatives, modified glycols of polyalkylene glycols containing ethylene glycol units and propylene glycol units and having one terminal butyl ether or one terminal stearyl ether are also suitable. As other polyalkylene glycol derivatives, commercially available products can be used, such as NOF Corp.'s Unilube 50MB-11 (one terminal butyl group, weight average molecular weight 1000), Unilube 50MB-26 (one terminal butyl group, weight average molecular weight 2000), Unilube 50MB-72 (one terminal butyl group, weight average molecular weight 3000), Unilube 10MS-250KB (one terminal stearyl group, weight average molecular weight 2000), etc.
[0043] In addition, modified glycols containing tetramethylene glycol units and ethylene glycol units are also preferred as other polyalkylene glycol derivatives. Commercially available products can be used as other polyalkylene glycol derivatives, such as Polyserine DC3000E (weight average molecular weight 3000) and Polyserine DC1800E (weight average molecular weight 1800) manufactured by NOF Corp.
[0044] The aromatic polycarbonate resin composition according to an embodiment of the present invention may further contain a phosphorus-based antioxidant (D). When the aromatic polycarbonate resin composition contains the luminescent agent (B) and the phosphorus-based antioxidant (D) at the same time, it is possible to maintain and improve the excellent luminescent properties required for luminescent molded articles, in particular to prevent deterioration of the initial luminescent properties of the luminescent molded article made of the obtained aromatic polycarbonate resin composition, and in addition to this, it is possible to prevent deterioration such as deterioration due to usage conditions and aging deterioration.
[0045] The phosphorus-based antioxidant (D) is not particularly limited as long as it can provide the aromatic polycarbonate resin composition of the present invention, but it preferably contains a phosphite compound having the following phosphite structure: [ka]
[0046] In the aromatic polycarbonate resin composition according to an embodiment of the present invention, the phosphorus-based antioxidant (D) preferably contains at least one compound selected from the group consisting of a phosphite compound represented by formula (3) below, a phosphite compound represented by formula (4) below, a phosphite compound represented by formula (5) below, and a phosphite compound represented by formula (6) below.
[0047] Formula (3): [ka] (In formula (3), R 1 represents an alkyl group having 1 to 20 carbon atoms, and a represents an integer of 0 to 3.
[0048] In formula (3), R 1 is an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms.
[0049] Examples of the compound represented by formula (3) include triphenyl phosphite, tricresyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, trisnonylphenyl phosphite, etc. Among these, tris(2,4-di-t-butylphenyl)phosphite is particularly suitable, and is commercially available as, for example, Irgafos 168 manufactured by BASF ("Irgafos" is a registered trademark of BASF Societas Europea).
[0050] Formula (4): [ka] (In formula (4), R 2 , R 3 , R 5 and R 6 R each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. 4represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; X represents a single bond, a sulfur atom, or a group represented by the formula: -CHR 7 - (where R 7 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. A represents an alkylene group having 1 to 8 carbon atoms or a group represented by the formula: *-COR 8 - (where R 8 represents a single bond or an alkylene group having 1 to 8 carbon atoms, and * represents a bond on the oxygen side. Either Y or Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms.
[0051] Examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, a t-pentyl group, an i-octyl group, a t-octyl group, and a 2-ethylhexyl group. Examples of the cycloalkyl group having 5 to 8 carbon atoms include a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. Examples of the alkylcycloalkyl group having 6 to 12 carbon atoms include a 1-methylcyclopentyl group, a 1-methylcyclohexyl group, and a 1-methyl-4-i-propylcyclohexyl group. Examples of the aralkyl group having 7 to 12 carbon atoms include a benzyl group, an α-methylbenzyl group, and an α,α-dimethylbenzyl group.
[0052] R 2 , R 3 and R 5 are each preferably independently an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, or an alkylcycloalkyl group having 6 to 12 carbon atoms. 2 and R 5 are each preferably independently a t-alkyl group such as a t-butyl group, a t-pentyl group, or a t-octyl group, a cyclohexyl group, or a 1-methylcyclohexyl group. 3is preferably an alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, or a t-pentyl group, and more preferably a methyl group, a t-butyl group, or a t-pentyl group.
[0053] R 6 is preferably a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms, and more preferably a hydrogen atom, or an alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, or a t-pentyl group.
[0054] In formula (4), R 4 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. Examples of the alkyl group having 1 to 8 carbon atoms include R 2 , R 3 , R 5 and R 6 In particular, R 4 is preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and more preferably a hydrogen atom or a methyl group.
[0055] In formula (4), X represents a single bond, a sulfur atom or a group represented by the formula: -CHR 7 -, where the formula is -CHR 7 -R in 7 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. Examples of the alkyl group having 1 to 8 carbon atoms and the cycloalkyl group having 5 to 8 carbon atoms include R 2 , R 3 , R 5 and R 6 In particular, X is preferably a single bond, a methylene group, or a methylene group substituted with a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a t-butyl group, or the like, and more preferably a single bond.
[0056] In formula (4), A is an alkylene group having 1 to 8 carbon atoms or a group represented by the formula: 8 Examples of the alkylene group having 1 to 8 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a 2,2-dimethyl-1,3-propylene group, and the like, with a propylene group being preferred. 8 -R in 8 R represents a single bond or an alkylene group having 1 to 8 carbon atoms. 8 Examples of the alkylene group having 1 to 8 carbon atoms represented by the formula (I) include the alkylene groups exemplified in the description of A. 8 is preferably a single bond or an ethylene group. 8 The * in - is a bond on the oxygen side, indicating that the carbonyl group is bonded to the oxygen atom of the phosphite group.
[0057] In formula (4), one of Y and Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. Examples of the alkoxy group having 1 to 8 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, a t-butoxy group, and a pentyloxy group. Examples of the aralkyloxy group having 7 to 12 carbon atoms include a benzyloxy group, an α-methylbenzyloxy group, and an α,α-dimethylbenzyloxy group. Examples of the alkyl group having 1 to 8 carbon atoms include R 2 , R 3 , R 5 and R 6 Examples of the alkyl group include those exemplified in the explanation of the above.
[0058] Examples of the compound represented by formula (4) include 2,4,8,10-tetra-t-butyl-6-[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine, 6 -[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, and the like. Among these, when the resulting aromatic polycarbonate resin composition is to be used in fields where optical properties are particularly required, 2,4,8,10-tetra-t-butyl-6-[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine is suitable, and is commercially available, for example, as Sumilizer GP manufactured by Sumitomo Chemical Co., Ltd. ("Sumilizer" is a registered trademark).
[0059] Formula (5): [ka] (In the formula, R 9 and R 10 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group which may be substituted with an alkyl group, and b and c each independently represent an integer of 0 to 3.
[0060] Examples of the compound represented by formula (5) include bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, etc. Bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite is commercially available under the trade name "ADK STAB PEP-24G" manufactured by ADEKA CORPORATION. ADK STAB PEP-36 ("ADK STAB" is a registered trademark) manufactured by ADEKA CORPORATION is commercially available.
[0061] Formula (6): [ka]
[0062] (In the formula, R 11 ~R 18 R each independently represents an alkyl group or an alkenyl group having 1 to 3 carbon atoms. 11 and R 12 , R 13 and R 14 , R 15 and R 16 , R 17 and R 18 may be bonded to each other to form a ring. 19 ~R 22 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. each of d to g independently represents an integer of 0 to 5. X 1 ~X 4 Each of X independently represents a single bond or a carbon atom. 1 ~X 4 is a single bond, R 11 ~R 22 The functional group connected to the single bond is excluded from the general formula (14).
[0063] A specific example of the compound represented by formula (6) is bis(2,4-dicumylphenyl)pentaerythritol diphosphite, which is commercially available under the trade name "Doverphos (registered trademark) S-9228" manufactured by Dover Chemical Co., and under the trade name "ADEKA STAB PEP-45" (bis(2,4-dicumylphenyl)pentaerythritol diphosphite) manufactured by ADEKA Corporation.
[0064] In addition to the above, there may be mentioned tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene-di-phosphonite, etc. Specific examples of such organic phosphonite compounds include Sandstab PEPQ manufactured by Clariant Japan.
[0065] The amount of the phosphorus-based antioxidant is preferably 0.5 parts by mass or less, and more preferably 0.02 to 0.2 parts by mass, based on 100 parts by mass of the aromatic polycarbonate resin (A).
[0066] The aromatic polycarbonate resin composition according to the embodiment of the present invention may further contain a mold release agent. When the aromatic polycarbonate resin composition contains the luminescent agent (B) and the mold release agent at the same time, it is possible to obtain the effects of suppressing yellowing, improving the hue, and imparting extrusion moldability while maintaining and improving the excellent luminescent properties required for luminescent molded articles.
[0067] The release agent is not particularly limited as long as it can provide the aromatic polycarbonate resin composition of the present invention, but fatty acid esters are preferred.
[0068] Specific examples of fatty acid esters include behenyl behenate, octyldodecyl behenate, stearyl stearate, glycerin monopalmitate, glycerin monostearate, glycerin monooleate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate, etc., which can be used alone or in combination of two or more. Among these, stearic acid esters such as glycerin monostearate and pentaerythritol distearate are suitable, and for example, Rikemal S-100A (trade name) manufactured by Riken Vitamin Co., Ltd. and Unistar H476DP ("Unistar" is a registered trademark) manufactured by NOF Corporation are commercially available.
[0069] The amount of the release agent is 0.03 to 0.5 parts by mass, preferably 0.05 to 0.2 parts by mass, based on 100 parts by mass of the polycarbonate resin (A). If the amount of the release agent is less than 0.03 parts by mass, the effect of suppressing yellowing, improving the hue, and the effect of imparting extrusion moldability are insufficient. If the amount of the release agent is more than 0.5 parts by mass, the effect of improving the hue and the effect of imparting extrusion moldability are also insufficient.
[0070] Furthermore, in addition to the above components, the aromatic polycarbonate resin composition according to the embodiment may be appropriately blended with various additives such as ultraviolet absorbers, colorants, softeners, antistatic agents, heat stabilizers, light diffusing agents, fluorescent brighteners, impact modifiers, and polymers other than the aromatic polycarbonate resin (A), within the scope that does not impair the effects of the present invention. For example, an ultraviolet absorber, which is a component that further improves the weather resistance of the aromatic polycarbonate resin composition, can be appropriately used depending on the application of the molded product obtained by molding the aromatic polycarbonate resin composition.
[0071] As the ultraviolet absorbent, for example, ultraviolet absorbents that are usually blended with polycarbonate resins, such as benzotriazole-based compounds, triazine-based compounds, benzophenone-based compounds, and anilide oxalate-based compounds, can be used alone or in combination of two or more kinds.
[0072] Examples of benzotriazole compounds include 2-(2-hydroxy-5-t-octylphenyl)benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-pentyl-2-hydroxyphenyl)-2H-benzotriazole, and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)benzotriazole. phenol, 2-(2-hydroxy-4-octyloxyphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)-2H-benzotriazole, 2-[2'-hydroxy-3,5-di(1,1-dimethylbenzyl)phenyl]-2H-benzotriazole, 2,2'-Methylenbis[6-(2H-benzotriazol-2-yl)4-(1,1,3,3-tetramethylbutyl)phenol], etc. Among them, 2-(2-hydroxy-5-t-octylphenyl)benzotriazole, etc. are particularly suitable, and for example, TINUVIN 329 (TINUVIN is a registered trademark) manufactured by BASF, Seesorb 709 manufactured by Shipro Kasei Co., Ltd., Chemisorb 79 manufactured by Chemipro Kasei Co., Ltd., etc. are commercially available.
[0073] Examples of triazine compounds include 2,4-diphenyl-6-(2-hydroxyphenyl-4-hexyloxyphenyl)-1,3,5-triazine, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-(octyloxy)phenol, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]phenol. For example, TINUVIN 1577 manufactured by BASF is commercially available.
[0074] As an example of an oxalic acid anilide compound, commercially available products include Sanduvor VSU manufactured by Clariant Japan Co., Ltd. As an example of a benzophenone compound, 2,4-dihydroxybenzophenone, 2-hydroxy-4-n-octoxybenzophenone, etc. can be mentioned.
[0075] The amount of the ultraviolet absorber is preferably 0 to 1.0 part by mass, more preferably 0 to 0.5 part by mass, relative to 100 parts by mass of the aromatic polycarbonate resin (A). If the amount of the ultraviolet absorber exceeds 1.0 part by mass, the initial color of the resulting aromatic polycarbonate resin composition may be deteriorated. If the amount of the ultraviolet absorber is 0.1 part by mass or more, the effect of improving the weather resistance of the aromatic polycarbonate resin composition is particularly enhanced.
[0076] The aromatic polycarbonate resin composition of the embodiment of the present invention can be produced by mixing the aromatic polycarbonate resin (A), the luminescent agent (B) and various other additives. As long as the aromatic polycarbonate resin composition of the present invention can be obtained, the production method is not particularly limited, and the type and amount of each component can be appropriately adjusted. The method of mixing the components is also not particularly limited, and examples thereof include a method of mixing using a known mixer such as a tumbler or a ribbon blender, and a method of melt kneading using an extruder. Pellets of the aromatic polycarbonate resin composition can be easily obtained by these methods.
[0077] When the viscosity average molecular weight of the aromatic polycarbonate resin (A) is MW0 and the viscosity average molecular weight of the aromatic polycarbonate resin composition is MW1, the value obtained by subtracting MW1 from MW0 is preferably not more than 1000. If the value obtained by subtracting MW1 from MW0 exceeds 1000, the transparency and impact strength of the resulting polycarbonate resin composition may be reduced.
[0078] The luminous molded article according to the embodiment of the present invention can be obtained by molding the aromatic polycarbonate resin composition. As long as the luminous molded article according to the present invention can be obtained, the method for producing the luminous molded article is not particularly limited, and examples thereof include a method for molding the aromatic polycarbonate resin composition by known injection molding, compression molding, etc.
[0079] The luminous molded article according to the present invention is suitable for use as, for example, evacuation guidance signs, nighttime display signs, indicator buttons, clock faces, switches, connector parts, accessories, and the like.
[0080] As described above, the embodiments of the present invention have been described as examples of the present invention. However, the technology of the present invention is not limited to the above, and can be applied to embodiments in which appropriate changes, substitutions, additions, omissions, etc. are made. EXAMPLES
[0081] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" and "%" are based on mass.
[0082] The following raw materials were used: 1. Aromatic polycarbonate resin (A): Polycarbonate resin synthesized from bisphenol A and carbonyl chloride. Viscosity average molecular weight: 18,800, SD Polyca 200-20 (product name) manufactured by Sumika Polycarbonate Co., Ltd., hereinafter also referred to as "PC" or (A1).
[0083] 2. Luminous agent (B): 2-1) GDK13025WP(SrAl 2 O 4 Eu, Dy) (Manufactured by LTI Co., Ltd., average particle size 25 μm, contains minute protrusions containing phosphorus atoms, hereafter abbreviated as PP-1) 2-2) GDK11010WP(SrAl 2 O 4 Eu, Dy) (Manufactured by LTI Co., Ltd., average particle size 10 μm, contains minute protrusions containing phosphorus atoms, hereafter abbreviated as PP-2) 2-3)BDK11025WP(Sr 4 Al 14 O 25 Eu, Dy) (Manufactured by LTI Co., Ltd., average particle size 25 μm, contains minute protrusions containing phosphorus atoms, hereafter abbreviated as PP-3)
[0084] 3. Antioxidants (phosphorus antioxidants:) Tris(2,4-di-t-butylphenyl)phosphite represented by the following formula: [ka] (BASF Irgafos 168 (product name), hereafter referred to as "P168")
[0085] 4. Release agent (fatty acid ester:) Glycerin Monostearate (Rikemal S-100A (hereinafter referred to as S100A) manufactured by Riken Vitamin Co., Ltd.)
[0086] 5. Polyalkylene glycol derivatives (C) Modified glycol (random copolymer) consisting of tetramethylene glycol units and propylene glycol units. Weight average molecular weight: 2000, also known as Polyserine DCB-2000 (product name) manufactured by NOF Corporation (hereinafter referred to as DCB2000).
[0087] 6.Others (used for comparison purposes) GDK13025(SrAl 2 O 4 Eu, Dy) (Manufactured by LTI Co., Ltd., average particle size 25 μm, no minute protrusions containing phosphorus atoms, hereafter abbreviated as PP-4)
[0088] The polycarbonate resin, the luminescent agent, and various additives were dry mixed by hand blending in the compounding ratios shown in Tables 2 and 3 below, and then melt-kneaded at a melting temperature of 250°C using a twin-screw extruder (TEX30α, manufactured by The Japan Steel Works, Ltd.) to obtain pellets of the aromatic polycarbonate resin composition of each of Examples 1 to 8 and Comparative Examples 1 to 3. The obtained pellets were evaluated in the following various ways. The results are shown in Tables 2 and 3.
[0089] The methods for measuring various evaluation items in the present invention will be described below.
[0090] (Brightness evaluation) The pellets obtained were dried at 120°C for 4 hours or more, and then a flat test piece (80mm x 50mm x 2mm thick) was prepared using an injection molding machine (FANUC Co., Ltd., ROBOSHOT S2000i100B) at a molding temperature of 280°C, a mold temperature of 80°C, and a cylinder set temperature of 280°C. The test piece was stored in a dark place for 48 hours or more and completely blocked from light, and then irradiated with light from a D65 light source at an illuminance of 200lx for 20 minutes. The luminance of the test piece surface 20 minutes after the end of irradiation was measured with a luminance meter (SR-3, Topcon Co., Ltd.) at a measurement distance of 30cm and a viewing angle of 2°. The evaluation criteria were as follows: a luminance measurement value of 100 or more was excellent (◎), a luminance measurement value of 5 or more but less than 100 was good (○), and a luminance measurement value of less than 5 was poor (×).
[0091] (Melt Volume Rate (MVR)) The melt volume rate (MVR) of each of the obtained pellets was measured at 300°C under a load of 1.2 kg using a semi-automatic melt indexer 2A manufactured by Toyo Seiki Co., Ltd., in accordance with ISO 1133. The MVR of the PC used as the raw material was also measured under the above conditions, and the value obtained by subtracting the MVR of the PC from the MVR of the obtained pellets (hereinafter referred to as ΔMVR) was calculated. ΔMVR values of less than 10 were rated as excellent (◎), values between 10 and 15 were rated as good (○), and values of 15 or more were rated as poor (×).
[0092] (molecular weight reduction) The polycarbonate resin (A) and the obtained pellets were each dissolved in methylene chloride to prepare a solution with a pellet concentration of 0.38% by weight. The viscosity of the obtained solution was measured at a temperature of 20°C using a Cannon-Fenske viscometer. The viscosity average molecular weight was calculated according to the following formula. [η]=1.23×10 -4 M 0.83 however, [η]: Intrinsic viscosity M: Viscosity average molecular weight When the viscosity average molecular weight of the polycarbonate resin (A) is MW0 and the viscosity average molecular weight of the polycarbonate resin composition is MW1, the value obtained by subtracting MW1 from MW0 (hereinafter abbreviated as ΔMW) of less than 500 was rated as excellent (◎), 500 or more and less than 1000 was rated as good (○), and 1000 or more was rated as poor (×).
[0093] (thermal stability) The pellets according to Examples 3, 7, and 8 were pre-dried at 120°C for 4 hours, and then flat test pieces (80 mm long, 50 mm wide, 2 mm thick) were prepared at a molding temperature of 300°C using an injection molding machine (ROBOSHOT S2000i100B, manufactured by Fanuc Corporation), and the YI was measured using a spectrophotometer (CMS-35SP, manufactured by Murakami Color Research Laboratory Co., Ltd.). The smaller the YI, the less yellowing due to molding and the better the thermal stability.
[0094] [Table 2]
[0095] [Table 3]
[0096] As shown in Table 2, when the configuration of the present invention was satisfied (Examples 1 to 8), sufficient performance was obtained in all evaluation items.
[0097] On the other hand, as shown in Table 3, when the configuration of the present invention was not satisfied (Comparative Examples 1 to 3), all of them had some kind of defect. Comparative Example 1 used a conventional luminous compound (without micro-protrusions containing phosphorus atoms), and molecular weight reduction (MVR, ΔMw) occurred. Comparative Example 2 was a case where the blending amount of luminous agent (B) was less than the specified amount, and the brightness was poor. Comparative Example 3 was a case where the blending amount of luminous agent (B) was more than the specified amount, and molecular weight reduction (ΔMw) occurred.
[0098] The embodiments have been described above as examples of the technology of the present invention, and detailed descriptions have been provided for this purpose.
[0099] Therefore, the components described in the detailed description may include not only essential components for solving the problem, but also components that are not essential for solving the problem in order to illustrate the above technology. Therefore, the fact that those non-essential components are described in the detailed description should not be interpreted as immediately being essential.
[0100] Furthermore, since the above-described embodiment is intended to illustrate the technology of the present invention, various modifications, substitutions, additions, omissions, and the like can be made within the scope of the claims or their equivalents. [Industrial Applicability]
[0101] The luminous aromatic polycarbonate resin composition of the present invention has excellent luminous properties and is highly valuable in industrial applications, since it does not lose the inherent transparency and impact strength properties of polycarbonate resins even when used outdoors for applications in which it is exposed to direct sunlight (ultraviolet light) for a long period of time.
Claims
1. A phosphorescent aromatic polycarbonate resin composition comprising 100 parts by mass of an aromatic polycarbonate resin (A) and 1 to 35 parts by mass of a phosphorescent agent (B) comprising a phosphorescent compound having a plurality of phosphorus atom-containing microprojections attached thereto, the phosphorescent agent being an alkaline earth metal oxide doped with a lanthanoid rare earth element, The phosphorus element contained in the phosphorescent agent (B) has a concentration of 5,000 ppm to 50,000 ppm.
2. 2. The phosphorescent aromatic polycarbonate resin composition according to claim 1, wherein the alkaline earth metal oxide is a strontium aluminate compound.
3. The luminous aromatic polycarbonate resin composition according to claim 1, wherein the long diameter of the minute projections of the luminous agent (B) is 0.1 μm to 1.5 μm.
4. The luminous aromatic polycarbonate resin composition according to claim 1, wherein the luminous agent (B) has an average particle size of 1 to 60 μm.
5. The luminous aromatic polycarbonate resin composition according to claim 1, further comprising 0.05 to 5.0 parts by mass of a polyalkylene glycol derivative represented by the following formula (1): Formula (1): RO-(X'-O)m(Y'-O)n-R' (In the formula, R and R' each independently represent a hydrogen atom or an alkyl group having 1 to 30 carbon atoms, X' represents a linear or branched alkylene group having 2 to 4 carbon atoms, Y' represents a linear or branched alkylene group having 2 to 5 carbon atoms, X' and Y' may be the same or different, m and n each independently represent 3 to 60, and m+n represents 6 to 120.)
6. 6. The light-storing aromatic polycarbonate resin composition according to claim 5, wherein the polyalkylene glycol derivative comprises a polyalkylene glycol derivative represented by formula (2): Formula (2): HO-(CH 2 CH 2 CH 2 CH 2 O)m(CH(CH 3 ) CH 2 O) n-H (In the formula, m and n each independently represent 3 to 60, and m+n represents 8 to 90.)
7. The phosphorescent aromatic polycarbonate resin composition according to claim 1, wherein, when the viscosity average molecular weight of the aromatic polycarbonate resin (A) is MW0 and the viscosity average molecular weight of the phosphorescent aromatic polycarbonate resin composition is MW1, the value obtained by subtracting MW1 from MW0 is 1000 or less.
8. The phosphorescent aromatic polycarbonate resin composition according to any one of claims 1 to 7, further comprising at least one selected from the group consisting of a heat stabilizer, an antioxidant, a release agent, an ultraviolet absorber, a colorant, a softener, an antistatic agent, a light diffusing agent, a fluorescent brightening agent, and an impact modifier.
9. A luminous resin molded article comprising the luminous aromatic polycarbonate resin composition according to any one of claims 1 to 8.
10. 10. The luminescent resin molded article according to claim 9, which is an evacuation guide sign, a nighttime display sign, a display button, a clock face, a switch, a connector part or an accessory.
11. A method for producing a luminous resin molded article, comprising molding the luminous aromatic polycarbonate resin composition according to any one of claims 1 to 8.
Citation Information
Patent Citations
Polycarbonate resin composition
JP2003041110A
Polycarbonate resin composition
JP2005082647A
Light-emitting member
JP2005146125A
Luminosity fluorescent polycarbonate resin composition and molded article
JP2010159318A
Polycarbonate resin composition for optical component and molded article formed of same
JP2017002295A