Method for manufacturing silicon nitride substrate

By reducing grain size and controlling the sintering process, the method addresses the issue of etching solution damage in silicon nitride substrates, ensuring improved insulation and durability, even in thinner substrates.

JP7557576B2Active Publication Date: 2024-09-27NITERRA MATERIALS CO LTD

Patent Information

Application Number
JP2023102488
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-29
Filing Date
2023-06-22
Publication Date
2024-09-27
Estimated Expiration
2039-08-05

AI Technical Summary

Technical Problem

Existing silicon nitride circuit boards suffer from deteriorated insulation properties due to damage from etching solutions during the manufacturing process, which is caused by the exposure to different etching solutions for the metal plate and brazing material layer, leading to silicon nitride substrates with increased dislocation defects.

Method used

A manufacturing method that involves reducing the average grain size of silicon nitride crystal grains to 1 μm or less, controlling the sintering process at specific temperatures and pressures, and minimizing dislocation defects by limiting the grain boundary phase composition, resulting in a silicon nitride substrate with improved durability to etching solutions.

Benefits of technology

The method produces a silicon nitride substrate with reduced dislocation defects, maintaining excellent insulation properties even when made thinner, thereby enhancing durability and reducing thermal resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557576000009
    Figure 0007557576000009
  • Figure 0007557576000006
    Figure 0007557576000006
  • Figure 0007557576000007
    Figure 0007557576000007
Patent Text Reader

Abstract

To provide a method for producing a silicon nitride substrate capable of improving durability to etching liquid.SOLUTION: A method for producing a silicon nitride substrate that comprises (a) a mixing step in which silicon nitride powder and sintering aid powder are mixed over 20 hours so that the average particle diameter D50 is 1 μm or less, and a binder is added to prepare a mixture of raw materials, (b) a degreasing step in which a formed sheet of the mixture of raw materials is subjected to degreasing, and (c) a sintering step in which the degreased formed sheet is sintered under conditions that the change in pressure during the sintering from 1300°C is 0.3 MPa or less, and the sintering temperature is within the range of 1800°C to 1950°C. The thickness of the silicon nitride substrate obtained by the sintering of the formed sheet is 0.1 mm or more and 0.4 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiment relates to a method for manufacturing a silicon nitride substrate. [Background technology]

[0002] In recent years, power semiconductors have become more powerful. In addition, the power density of power modules equipped with power semiconductors has been increasing year by year. The power density of a module is expressed as: Power density = V M ×I M ×n / M v where V M is the rated withstand voltage (V). I M is the rated current @△T j-c = 125°C (A). n is the number of power semiconductors in the module. Also, M v is the volume of the module (cm 3 ). To increase the power density of a power module, it is necessary to either increase the number of power semiconductors in the module or reduce the volume of the module. As mentioned above, semiconductor elements are becoming higher in output. This has resulted in an increase in the amount of heat generated. Accordingly, there is a demand for improved heat dissipation, heat resistance, and insulation for the insulated circuit boards on which the semiconductor elements are mounted. International Publication No. WO 2015 / 060274 (Patent Document 1) discloses a silicon nitride substrate, in which the distribution amount of grain boundary phase in the thickness direction is controlled to improve the variation in insulation properties. Patent Document 1 shows the ratio of volume resistivity at room temperature (25° C.) and 250° C. when 1000 V is applied. The volume resistivity at room temperature is ρv1, and the volume resistivity at 250° C. is ρ v2 Then, ρ v2 / ρ v1 is 0.20 or more. Therefore, the silicon nitride substrate of Patent Document 1 has excellent insulation properties even in high-temperature environments. Meanwhile, semiconductor elements are being made to carry even larger currents. Circuit boards on which semiconductor elements are mounted are required to have thermal cycle resistance (TCT) characteristics in high-temperature environments. International Publication No. 2017 / 056360 (Patent Document 2) discloses a silicon nitride circuit board in which the shape of the copper plate side, the size and hardness of the protruding brazing material, etc. are controlled. Patent Document 2 shows excellent durability in a TCT test from -40°C to 250°C. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2015 / 060274 [Patent Document 2] International Publication No. 2017 / 056360 Summary of the Invention [Problem to be solved by the invention]

[0004] In Patent Document 2, etching is used to control the shape of the copper plate side surface and the size of the protruding portion of the brazing material. In the etching process, an etchant is used to remove the metal plate and the brazing material layer. Usually, the etchant for the metal plate and the etchant for the brazing material layer are different. An etchant suitable for each etching process is used. For this reason, the silicon nitride substrate is exposed to a variety of etchants. Although silicon nitride circuit boards that have been etched have excellent TCT characteristics, their insulation properties have deteriorated. When the cause of this was investigated, it was found that the silicon nitride board was damaged by the etching solution. The present invention is intended to address this issue. [Means for solving the problem]

[0005] The method for producing a silicon nitride substrate according to the embodiment of the present invention is to grow silicon nitride particles having an average grain size D over 20 hours or more. 50The method comprises a mixing step of mixing silicon nitride powder and sintering aid powder so that the particle size is 1 μm or less, and further adding a binder to adjust the raw material mixture; a degreasing step of degreasing a sheet molded body of the raw material mixture; and a sintering step of sintering the degreased sheet molded body such that the change in pressure between 1300°C and the sintering step is 0.3 MPa or less and the sintering temperature is within the range of 1800°C to 1950°C, and the thickness of the silicon nitride substrate obtained by sintering the sheet molded body is 0.1 mm to 0.4 mm. Effect of the Invention

[0006] According to the manufacturing method of the embodiment, a silicon nitride substrate is manufactured with a low ratio of silicon nitride crystal grains having dislocation defects. This improves the durability of the silicon nitride substrate to etching solutions. Therefore, even if the silicon nitride substrate is thinned, the insulation properties can be maintained. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a conceptual diagram illustrating a silicon nitride crystal grain having dislocation defects. [Diagram 2] FIG. 2 is a conceptual diagram illustrating the major axis of a silicon nitride crystal particle. [Diagram 3] 1 is a diagram showing an example of a silicon nitride circuit substrate according to an embodiment. [Figure 4] FIG. 4 is a diagram showing another example of a silicon nitride circuit board according to an embodiment. [Diagram 5] 1 is a diagram showing an example of a semiconductor device according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The method for producing a silicon nitride substrate according to the embodiment of the present invention is to grow silicon nitride particles having an average grain size D over 20 hours or more. 50The method comprises a mixing step of mixing silicon nitride powder and sintering aid powder so that the particle size is 1 μm or less, and further adding a binder to adjust the raw material mixture; a degreasing step of degreasing a sheet molded body of the raw material mixture; and a sintering step of sintering the degreased sheet molded body such that the change in pressure between 1300°C and the sintering step is 0.3 MPa or less and the sintering temperature is within the range of 1800°C to 1950°C, and the thickness of the silicon nitride substrate obtained by sintering the sheet molded body is 0.1 mm to 0.4 mm.

[0009] The silicon nitride sintered body has silicon nitride crystal grains and a grain boundary phase. The grain boundary phase is mainly composed of sintering aid components. The grain boundary phase is formed by a reaction of the sintering aid during the sintering process. The reaction occurs between sintering aids, between the sintering aid and silicon nitride, or between the sintering aid and impurity oxygen. The silicon nitride substrate according to the embodiment is characterized in that, among any 50 silicon nitride crystal grains whose entire contours are visible in an observation area of ​​50 μm x 50 μm, the proportion of silicon nitride crystal grains having dislocation defects therein is between 0% and 20%.

[0010] The observation of dislocation defects is carried out on any cross section or surface of the silicon nitride sintered body. An arbitrary cross section or surface of the silicon nitride sintered body is processed by ion milling or FIB (focused ion beam) processing so that the surface roughness Ra is 1 μm or less. The processed cross section or surface is the evaluation surface. Next, the evaluation surface is observed with a transmission electron microscope (TEM). The magnification during TEM observation is 10,000 times or more. The evaluation is performed by observing a 50 μm x 50 μm area. If a 50 μm x 50 μm area cannot be observed in one field of view, the area may be divided into multiple areas for observation. In the evaluation, after observing one observation area (50 μm x 50 μm), another area located 1000 μm or more away from that area is observed. In other words, two or more 50 μm x 50 μm areas are observed to calculate the percentage of silicon nitride crystal grains having dislocation defects (defect particles). The presence or absence of dislocation defects is determined by observing the TEM images in dark and bright fields. Dislocation defects appear white in the dark field and inverted black in the bright field. In this way, the areas where the pixel color inverts when switching between dark and bright fields are considered to be dislocation defects.

[0011] Fig. 1 is a conceptual diagram illustrating a silicon nitride crystal grain having a dislocation defect. In Fig. 1, 1 is a silicon nitride crystal grain. 2 is a dislocation defect. As shown in Fig. 1, in the silicon nitride sintered body of the silicon nitride substrate according to the embodiment, a dislocation defect 2 can exist inside the silicon nitride crystal grain 1. If there are dislocation defects in silicon nitride crystal grains, the insulating properties of the silicon nitride substrate are reduced. Dislocation defects are crystal defects contained in crystals. Crystal defects are also called lattice defects. Crystal defects are caused by disturbances in the atomic arrangement or impurities. Dislocation defects occur when defects occur in a stable crystal structure, causing a decrease in insulating properties. If there are only a small number of dislocation defects, they do not adversely affect insulating properties. On the other hand, dislocation defects are easily damaged by etching solutions. When dislocation defects are damaged, they progress to larger defects in the silicon nitride structure. The thickness of the silicon nitride substrate according to the embodiment is 0.40 mm or less. If a structure defect caused by a dislocation defect occurs on the surface of such a thin substrate, the insulating properties of that part are significantly reduced. In the silicon nitride substrate according to the embodiment, the percentage of silicon nitride crystal grains having dislocation defects in any 50 μm×50 μm micro-area is 0% or more and 20% or less. The percentage of 0% or more and 20% or less in any 50 μm×50 μm observation area means that the percentage of the number is 0% or more and 20% or less in any 50 μm×50 μm area observed.

[0012] When the ratio of the number of silicon nitride crystal grains having dislocation defects exceeds 20%, the insulating properties of the silicon nitride substrate are reduced. The thickness of the silicon nitride substrate according to the embodiment is 0.4 mm or less. Since the substrate is thin, the insulating properties are reduced when there are many dislocation defects. As shown in Patent Document 1, when there is partial variation in the insulating properties of the silicon nitride substrate, electric field concentration occurs in the parts with low insulating properties. In Patent Document 1, the distribution ratio of the grain boundary phase in the thickness direction of the substrate is controlled. In contrast, in the embodiment, the ratio of the number of silicon nitride crystal grains having dislocation defects is controlled. For this reason, it is preferable that the ratio of the number of silicon nitride crystal grains having dislocation defects inside the silicon nitride crystal grains present in the observation area of ​​50 μm × 50 μm is 0% or more and 10% or less. Most preferably, the ratio is 0%. In other words, the absence of silicon nitride crystal grains having dislocation defects can improve the insulation of the silicon nitride substrate. Note that two or more regions separated from each other by 1000 μm or more are observed. In addition, in a TEM photograph of at least a part of the observation area of ​​50 μm × 50 μm, silicon nitride crystal grains whose outlines are not entirely captured are not used in the calculation of the number ratio. For example, silicon nitride crystal grains whose outlines are cut off at the edge of the photograph are not used in the calculation of the number ratio. In addition, when 50 silicon nitride crystal grains whose outlines are all captured are confirmed, the ratio of the number of silicon nitride crystal grains having dislocation defects among the 50 silicon nitride crystal grains is calculated. In other words, observation is continued until 50 silicon nitride crystal grains whose outlines are all captured are confirmed. When 50 silicon nitride crystal grains with their entire contours cannot be observed in one observation area of ​​50 μm×50 μm, 50 silicon nitride crystal grains with their entire contours are observed in another observation area of ​​50 μm×50 μm. When more than 50 silicon nitride crystal grains are observed in an observation area of ​​50 μm×50 μm, 50 silicon nitride crystal grains are selected at random. In the silicon nitride sintered body according to the embodiment, the ratio of the number of silicon nitride crystal grains having dislocation defects in any 50 silicon nitride crystal grains is 0% or more and 20% or less. This indicates that when more than 50 silicon nitride crystal grains are observed in an observation area of ​​50 μm×50 μm, the ratio of the number of silicon nitride crystal grains having dislocation defects is 0% or more and 20% or less, regardless of which 50 silicon nitride crystal grains are selected.

[0013] In addition, at the dislocation defect, the components other than silicon, oxygen, and nitrogen are 1 μm 2 It is preferable that the dislocation defects do not contain 10 mol % or more of any component other than silicon, oxygen, and nitrogen. The components other than silicon, oxygen, and nitrogen are the components that make up the grain boundary phase. The grain boundary phase is mainly composed of sintering aids. Therefore, the components other than silicon, oxygen, and nitrogen correspond to the metal components of the sintering aid. For example, when yttrium oxide (Y2O3) is used as the sintering aid, the components other than silicon, oxygen, and nitrogen are yttrium (Y). In addition, the components other than silicon, oxygen and nitrogen are 1 μm 2 The fact that the agglomerates are not larger than 1 μm means that the agglomerates of metal components that make up the grain boundary phase at the dislocation defect are smaller than 1 μm. 2 Less than (0μm 2 Even when multiple sintering aids are used, the components other than silicon, oxygen, and nitrogen are within 1 μm. 2 It is preferable that the sintering additive components do not form lumps of 1 μm or more in size. This indicates that the sintering additive components do not become the nuclei of dislocation defects. Therefore, in the dislocation defects, the lumps of metal components constituting the grain boundary phase are 1 μm or more in size. 2 Less than or even 0.2 μm 2 It is preferable that: Furthermore, not detecting 10 mol% or more of components other than silicon, oxygen, and nitrogen indicates that the metal components of the sintering aid are less than 10 mol% (including 0 mol%) in the dislocation defects. For example, when yttrium oxide (Y2O3) is used as the sintering aid, this indicates that the dislocation defects contain less than 10 mol% (including 0 mol%) of yttrium (Y). Furthermore, when multiple sintering aids are used, it is preferable that the total metal components of the sintering aids is less than 10 mol%. This indicates that the sintering aid components are not the nuclei of the dislocation defects. In addition, at the dislocation defect, the mass of the metal components that constitute the grain boundary phase is 1 μm 2 Less than (0μm 2 It is preferable that the content of the fluorine-containing compound is less than 10 mol % (including 0 mol %).

[0014] The sintering aid components do not become the nuclei of dislocation defects, improving the resistance to etching solutions. The size and concentration of components other than silicon, oxygen, and nitrogen in the dislocation defects are analyzed by EDX (energy dispersive X-ray analysis) or WDS (wavelength dispersive X-ray analysis). Analysis may also be performed in combination with EPMA (electron probe microanalyzer).

[0015] In addition, the ratio of the number of silicon nitride crystal grains having dislocation defects with an occupied area ratio of 5% or less to the number of silicon nitride crystal grains having dislocation defects is preferably 70% or more. As described above, if the number of silicon nitride crystal grains having dislocation defects is small, it does not cause a decrease in insulation. On the other hand, if there is a large dislocation defect in one silicon nitride crystal grain, the insulation may decrease. For this reason, the occupied area ratio of the dislocation defects in one silicon nitride crystal grain is preferably 5% or less. In addition, if the ratio of the number of silicon nitride crystal grains having dislocation defects with an occupied area ratio of 5% or less to the number of silicon nitride crystal grains having dislocation defects is 70% or more, a stress relaxation effect can be obtained without decreasing the insulation. This ratio is also obtained in an observation area of ​​50 μm × 50 μm. That is, first, in one observation area of ​​50 μm×50 μm, any 50 silicon nitride crystal grains in which all the contours are captured are observed. Next, it is confirmed whether or not there are dislocation defects in each of the observed 50 silicon nitride crystal grains. The magnification of each silicon nitride crystal grain is 10,000 times for TEM observation. When one silicon nitride crystal grain does not fit in one image, it may be photographed in multiple parts. The ratio of the number of silicon nitride crystal grains having dislocation defects in the observed 50 silicon nitride crystal grains is calculated. This ratio is preferably 0% or more and 20% or less. Next, if there are silicon nitride crystal grains having dislocation defects, the occupied area ratio of the dislocation defects is calculated for each of those silicon nitride crystal grains. The ratio of the number of silicon nitride crystal grains having an occupied area ratio of 5% or less to the number of silicon nitride crystal grains having dislocation defects is calculated. This ratio is preferably 70% or more. When there are no 50 silicon nitride crystal grains whose entire contours are visible in one observation area of ​​50 μm×50 μm, 50 silicon nitride crystal grains whose entire contours are visible are searched for in another observation area of ​​50 μm×50 μm. After measuring the ratio of the number of silicon nitride crystal grains having dislocation defects and the occupied area ratio of dislocation defects in a certain observation area of ​​50 μm×50 μm, another observation area of ​​50 μm×50 μm that is 1000 μm or more away from the observation area is observed. In the silicon nitride substrate according to the embodiment, in any observation area of ​​50 μm×50 μm in any cross section, the ratio of the number of silicon nitride crystal grains having dislocation defects is 0% or more and 20% or less. Also, the ratio of the number of silicon nitride crystal grains whose occupied area ratio of dislocation defects is 5% or less is 70% or more. In other words, in the silicon nitride substrate according to the embodiment, the size of the dislocation defects in the silicon nitride crystal grains is controlled even in a microscopic region of 50 μm×50 μm.

[0016] Moreover, the dark-field image of the TEM photograph mentioned above is used to measure the area ratio of dislocation defects within a single silicon nitride crystal grain. In a dark-field image, dislocation defects are observed as white. The sum of the area of ​​the white regions and the area of ​​the black regions in a single silicon nitride crystal grain observed in a dark-field image is taken as the area of ​​that silicon nitride crystal grain. The area of ​​the white regions in the dark-field image is taken as the area of ​​the dislocation defects. The area ratio of dislocation defects is taken as (area of ​​dislocation defects / area of ​​silicon nitride crystal grain) x 100 (%). Moreover, image processing software is used to measure this area ratio. Image analysis software such as Image-j or software with an equivalent or higher resolution is used.

[0017] In addition, in an observation area of ​​300 μm×300 μm of any cross section of the silicon nitride sintered body, the long diameter of the silicon nitride crystal grains is preferably 60 μm or less, and more preferably 25 μm or less. In an observation area of ​​300 μm×300 μm of any cross section of the silicon nitride sintered body, the average long diameter of the silicon nitride crystal grains is preferably within the range of 1 μm to 10 μm. In a unit area of ​​300 μm×300 μm of any cross section of the silicon nitride sintered body, the area of ​​each grain boundary phase is preferably 9 μm or less. 2 The area of ​​the grain boundary phase means the area of ​​a region surrounded by a plurality of silicon nitride crystal grains. The fact that the long diameter of the silicon nitride crystal grains is 60 μm or less indicates that there are no silicon nitride crystal grains whose long diameter exceeds 60 μm. In other words, it indicates a state in which there are no coarse grains whose long diameter exceeds 60 μm. As mentioned above, the insulation properties are improved by reducing the number of dislocation defects. By eliminating the presence of large coarse grains, partial variations in insulation properties can be suppressed. For this reason, the long diameter of the silicon nitride crystal grains is preferably 60 μm or less, more preferably 25 μm or less. The average major axis of the silicon nitride crystal grains is preferably in the range of 1 μm to 10 μm. If the average major axis is less than 1 μm, the silicon nitride crystal grains are too small and the thermal conductivity is reduced. If the average major axis is more than 10 μm, the thermal conductivity is improved, but the strength may be reduced. In addition, in an observation area of ​​300 μm × 300 μm of an arbitrary cross section of a silicon nitride substrate, the area of ​​each grain boundary phase is 9 μm 2 It is preferable that the area of ​​the grain boundary phase is 9 μm or less. 2 If the area exceeds 9 μm, it may cause variations in insulation. The grain boundary phase and silicon nitride crystal grains have different insulation properties. Therefore, if the grain boundary phase is too large, the effect of suppressing dislocation defects in the silicon nitride crystal grains will be reduced. For this reason, the area of ​​the grain boundary phase should be less than 9 μm 2 Below that, even 5μm 2 The following is preferred:

[0018] The long diameter of silicon nitride crystal grains and the area of ​​the grain boundary phase are measured using SEM photographs. Take an SEM photograph of any cross section of the silicon nitride substrate. The cross section should be a polished surface with a surface roughness Ra of 1 μm or less. The magnification of the SEM photograph should be set to 1000x or more. The recommended magnification of the SEM photograph is 4000x. If it is not possible to photograph an area of ​​300 μm x 300 μm in one field of view, it is acceptable to photograph multiple 300 μm x 300 μm areas. If the length of the cross section in one direction is less than 300 μm, the length of the observation area in that direction should be made as long as possible, and then the observation area should be measured to be 90,000 μm. 2 The major axis of the silicon nitride crystal grain is 90,000 μm. 2 The measurement is based on the observation results in the observation area. As shown in FIG. 2, the long diameter is the length of the longest line segment among the line segments obtained by connecting any two points on the outer edge of one silicon nitride crystal particle. The long diameter of each silicon nitride crystal particle shown in an SEM photograph with an observation area of ​​300 μm × 300 μm is measured. Silicon nitride crystal particles whose outline is cut off at the edge of the SEM photograph and are not shown in their entirety are not counted. In FIG. 2, 3 indicates the long diameter of silicon nitride crystal particle 1. The maximum value of these long diameters is preferably 60 μm or less, and more preferably 25 μm or less. The average long diameter of each silicon nitride crystal particle is calculated. The average long diameter is preferably 1 μm or more and 10 μm or less. In SEM photographs, silicon nitride crystal grains and grain boundary phases can be distinguished by the difference in contrast. Silicon nitride crystal grains appear dark gray, while the grain boundary phase appears light gray. The area of ​​the grain boundary phase can be determined by image analysis of SEM photographs. Specifically, the binarized image is analyzed using image analysis software. In the binary image, silicon nitride crystal grains appear black, and the grain boundary phase appears white. The area of ​​the grain boundary phase is determined as the area surrounded by three or more silicon nitride crystal grains. In other words, the area is determined excluding the grain boundary phase that exists between two silicon nitride crystal grains. In addition, Image-j or software with an equivalent or higher resolution is used as image analysis software.

[0019] With the above configuration, it is possible to achieve a thermal conductivity of 80 W / (m K) or more and a three-point bending strength of 600 MPa or more. In other words, it is possible to improve the insulation without reducing the thermal conductivity and strength. The thermal conductivity is measured according to the flash method of JIS-R-1611 (2010), which corresponds to ISO18755 (2005). The three-point bending strength is measured according to JIS-R-1601 (2008), which corresponds to ISO14704 (2000). The content of the sintering aid is preferably 15% by mass or less in terms of oxide. If the content of the sintering aid exceeds 15% by mass, the proportion of grain boundary phase increases, and the effect of reducing silicon nitride crystal grains having dislocation defects decreases. In addition, the sintering aid is preferably one or more selected from rare earth elements, magnesium, titanium, hafnium, aluminum, and calcium. The total amount of each metal element converted into an oxide is set to 15% by mass or less. The content of the sintering aid is preferably 0.1% by mass or more. If the content of the sintering aid is less than 0.1% by mass, the effect of adding the sintering aid may be insufficient. For this reason, the content of the sintering aid is preferably 0.1% by mass or more and 15% by mass or less, and more preferably 2% by mass or more and 10% by mass or less, in terms of oxide. The thickness of the silicon nitride substrate is preferably 0.1 mm or more and 0.4 mm or less. It is also preferable to provide a circuit portion on the silicon nitride substrate to form a silicon nitride circuit substrate. Silicon nitride substrates are used to mount semiconductor elements. Methods for mounting semiconductor elements include a method of providing a circuit section. Another method is to press the semiconductor element onto the silicon nitride substrate.

[0020] The silicon nitride substrate according to the embodiment is preferably used as a silicon nitride circuit substrate having a circuit portion. Methods for forming the circuit portion include a method of joining a metal plate using a brazing material, a metallization method using a metal paste, and the like. An example of a method for joining metal plates using a brazing material is an active metal joining method. When the metal plate is a copper plate, the active metal is one or more selected from Ti (titanium), Hf (hafnium), Zr (zirconium), and Nb (niobium). The active metal is mixed with Ag (silver) and Cu (copper) to form an active metal brazing material. If necessary, one or more selected from Sn (tin), In (indium), and C (carbon) may be added. Among active metals, Ti (titanium) is preferable. Ti reacts with silicon nitride substrate to form titanium nitride (TiN), which can increase the bonding strength. Ti has good reactivity with silicon nitride substrate, and can increase the bonding strength. In addition, when Ag+Cu+active metal=100% by mass, it is preferable that the Ag content is 40% by mass or more and 80% by mass or less, the Cu content is 15% by mass or more and 60% by mass or less, and the Ti content is 1% by mass or more and 12% by mass or less. In addition, when In and Sn are added, it is preferable that the content of at least one element selected from In and Sn is 5% by mass or more and 20% by mass or less. When C is added, it is preferable that the C content is 0.1% by mass or more and 2% by mass or less. In other words, when Ag+Cu+Ti+Sn(or In)+C=100% by mass, it is preferable that the Ag content is 40% by mass or more and 73.9% by mass or less, the Cu content is 15% by mass or more and 45% by mass or less, the Ti content is 1% by mass or more and 12% by mass or less, the Sn(or In) content is 5% by mass or more and 20% by mass or less, and the C content is 0.1% by mass or more and 2% by mass or less. Although the composition of the brazing filler metal using Ti has been described here, a part or all of the Ti may be replaced with another active metal. When the metal plate is an aluminum plate, the active metal is one or two elements selected from Si (silicon) and Mg (magnesium). The active metal is mixed with Al (aluminum) to form an active metal brazing material.

[0021] An active metal brazing material is applied onto a silicon nitride substrate, and a metal plate is placed on the substrate. Next, the silicon nitride substrate on which the metal plate is placed is heated to 600°C to 900°C, and the metal plate is bonded to the silicon nitride substrate. This allows a copper plate or an aluminum plate to be bonded. The bonding is performed in a vacuum (10 -2 It is preferable to heat the substrate at a pressure of 1000 Pa or less. If necessary, a circuit pattern may be formed by an etching process or the like. A metallization method using a metal paste is a method in which a metal paste such as Cu (copper), Al (aluminum), W (tungsten), or Mo (molybdenum) is applied and heated to form a circuit portion. In the method of joining metal plates, a thick metal plate can be joined to a substrate. This can improve the current carrying capacity. On the other hand, forming a circuit pattern requires a process such as etching. In addition, in the metallization method, a paste can be applied to the location where the circuit pattern is to be formed. This allows for the formation of a pattern with a complex shape. On the other hand, it is difficult to increase the thickness of the circuit portion, making it difficult to improve the current carrying capacity. As a type of metallization method, there is also a method that uses a metal plating method. The method for forming the circuit portion can be appropriately selected depending on the purpose.

[0022] When a metal plate is used for the circuit portion as described above, two types of etching are required: etching of the metal plate and etching of the brazing material layer. For example, when etching a copper plate, cupric chloride or ferric chloride is used. When etching an active metal brazing material layer, hydrogen peroxide, ammonium fluoride, hydrogen fluoride, etc. are used. In addition, acid solutions such as sulfuric acid, hydrochloric acid, and nitric acid may be used as chemical polishing liquids. In addition, silicon nitride circuit boards may be immersed in chemical solutions to remove the etching resist. In this way, silicon nitride circuit boards are exposed to two or more chemical solutions. In addition, the number of etchings may be increased to optimize the side shape of the copper plate and the size of the brazing material protruding part. In particular, when the thickness of the copper plate is 0.8 mm or more, it is necessary to take measures such as increasing the number of etchings, prolonging the etching time, or increasing the concentration of the etching solution. In addition, an etching solution with a pH of about 5 to 6 is usually used as an etching solution for active metal brazing material. The etching time is also shortened by using an etching solution with a pH of 5 or less or by combining it with a chemical polishing solution with a pH of about 1. For this reason, the number of etching processes using an etching solution with a pH of 5 or less tends to increase. However, etching of the active brazing metal material places a large load on the silicon nitride substrate. The silicon nitride substrate according to the embodiment has fewer dislocation defects, so that damage to silicon nitride crystal grains caused by etching can be reduced. Therefore, deterioration of the insulating properties of the silicon nitride substrate due to etching can be suppressed. Therefore, the silicon nitride substrate according to the embodiment is suitable for a silicon nitride circuit substrate using a metal plate having a thickness of 0.8 mm or more in the circuit section, which is particularly subject to an increased load due to etching. Furthermore, by thinning the silicon nitride substrate to 0.40 mm or less, the thermal resistance of the silicon nitride substrate can be reduced. By thinning the silicon nitride substrate to 0.30 mm or less, the thermal resistance can be further reduced. The silicon nitride substrate according to the embodiment has fewer dislocation defects, so that it has excellent durability against etching solutions. Therefore, even when the silicon nitride substrate has a thin thickness, deterioration of the insulating properties due to etching can be suppressed. The thickness of the silicon nitride substrate is preferably 0.1 mm or more. If the thickness is less than 0.1 mm, the strength of the silicon nitride substrate decreases.

[0023] Next, a method for manufacturing a silicon nitride substrate according to an embodiment will be described. The method for manufacturing a silicon nitride substrate is not limited to the following example. The following manufacturing method can be used as a method for obtaining silicon nitride substrates with a high yield. First, raw material powder is prepared. The raw material powder requires silicon nitride powder and sintering aid powder. The sintering aid is preferably one or more selected from rare earth elements, magnesium, titanium, hafnium, aluminum, and calcium. The total amount of each metal element converted into an oxide is 15 mass% or less. The lower limit of the amount of sintering aid added is preferably 0.1 mass% or more. If the amount of sintering aid is less than 0.1 mass%, the effect of adding the sintering aid may be insufficient. For this reason, the amount of sintering aid added is preferably 0.1 mass% or more and 15 mass% or less.

[0024] In addition, it is preferable that the silicon nitride powder has an alpha conversion rate of 80 mass% or more, an average particle size of 0.4 μm to 2.5 μm, and an impurity oxygen content of 2 mass% or less. The impurity oxygen content is 1.0 mass% or less, and more preferably 0.1 mass% to 0.8 mass%. If the impurity oxygen content exceeds 2 mass%, a reaction between the impurity oxygen and the sintering aid occurs, and there is a possibility that more grain boundary phases than necessary are formed. In addition, it is preferable to use a rare earth compound as a sintering aid. Rare earth compounds are important materials for controlling the major axis of silicon nitride crystal particles. The amount of rare earth compound powder added is preferably controlled to 3% by mass or more and 10% by mass or less, and more preferably 5% by mass or more and 9% by mass or less, calculated as oxide. The oxide conversion is calculated as R2O3, where R is the rare earth element. In addition, in the process of grain growth of silicon nitride crystal particles, it is necessary to create a state in which the rare earth element can be easily coordinated to the surface of the silicon nitride crystal particles. Coordination to the surface means that the rare earth element (including rare earth element compounds) is adjacent to the surface element of silicon nitride. Coordination of the rare earth element to the surface of silicon nitride crystal particles can promote the reaction between the silicon nitride crystal particles and the rare earth element, and the reaction between sintering aids. The raw material powder is preferably in the form of a fine powder, and has an average particle diameter D 50 It is preferable to control the size of the silicon nitride crystal particles to 1.0 μm or less, and more preferably 0.4 μm or less. Another effective method is to use a solution of an alkoxide compound or the like instead of a powder and mix the rare earth element in a wet state to chemically bond the rare earth element to the surface of the silicon nitride crystal particles. If necessary, powder of a compound containing one or more selected from magnesium, titanium, hafnium, aluminum, and calcium is added. The total amount of these compounds added is preferably 5 mass% or less. These compounds are preferably oxides or carbonates. If the sintering aid contains oxygen as a constituent element, an oxide liquid phase is formed by reaction between the sintering aids themselves or by reaction between the sintering aids and impurity oxygen in the silicon nitride powder. This can promote densification of silicon nitride crystal particles. The rare earth compound has the effect of promoting sintering, and the compound containing magnesium, titanium, hafnium, aluminum, or calcium has the effect of lowering the sintering temperature and strengthening the grain boundary phase.

[0025] The above raw material powders are mixed and a binder is added to prepare a raw material mixture. The raw material powder is a mixed powder of silicon nitride powder and sintering aid powder. In order to control the grain growth of silicon nitride crystal particles in the sintering process, the mixed powder needs to be mixed uniformly. In the mixing process, the powder is crushed and mixed using a ball mill or the like. If the crushing stress is too large, dislocation defects will be formed in the silicon nitride powder, and dislocation defects will tend to remain in the silicon nitride particles after sintering. For this reason, the mixing process is carried out for 20 hours or more until the average particle size D 50 It is preferable to carry out the mixing so that the average particle diameter D is 1 μm or less. The upper limit of the mixing time is not particularly limited, but it is preferable that it is 60 hours or less. Mixing for more than 60 hours may be possible, but the production time will be too long. 50 The measurement is preferably performed using a laser diffraction / scattering type particle size distribution measuring device (manufactured by Horiba, Ltd.).

[0026] Next, a molding process is performed to mold the raw material mixture. The raw material mixture can be molded by a general-purpose die pressing method, a cold isostatic pressing (CIP) method, or a sheet molding method (e.g., a doctor blade method, a roll molding method, etc.). If necessary, the raw material mixture is mixed with a solvent such as toluene, ethanol, or butanol. The doctor blade method is suitable for mass production of substrates with a thickness of 0.40 mm or less. Next, after the molding process, the molded body is degreased. In the degreasing process, the molded body is heated in a non-oxidizing atmosphere at a temperature of 500°C to 800°C for 1 hour to 4 hours to degrease most of the organic binder that was added beforehand. Examples of non-oxidizing atmospheres include a nitrogen gas atmosphere and an argon gas atmosphere. If necessary, the molded body is treated in an oxidizing atmosphere such as air to control the amount of organic matter remaining in the degreased body. Examples of the organic binder include butyl methacrylate, polyvinyl butyral, polymethyl methacrylate, etc. When the raw material mixture (the total amount of silicon nitride powder and sintering aid powder) is taken as 100 mass%, the amount of the organic binder added is preferably 3 mass% or more and 28 mass% or less. If the amount of the organic binder added is less than 3 mass %, the amount of binder is too small, making it difficult to maintain the shape of the molded body, and in such a case, it becomes difficult to improve mass productivity by forming a multi-layered molded body. On the other hand, if the amount of binder exceeds 28% by mass, the voids in the molded body after the degreasing process become large, and the pores in the silicon nitride substrate become large. Therefore, the amount of organic binder added is preferably within a range of 3% by mass to 28% by mass, more preferably 3% by mass to 17% by mass. Next, the degreased green body is placed in a sintering vessel, and a sintering process is carried out in a sintering furnace in a non-oxidizing atmosphere. The temperature in the sintering process is preferably in the range of 1800°C to 1950°C. The non-oxidizing atmosphere is preferably a nitrogen gas atmosphere or a reducing atmosphere containing nitrogen gas. In addition, the inside of the sintering furnace is preferably a pressurized atmosphere. If the sintering temperature is lower than 1800°C, the grain growth of silicon nitride crystal grains is insufficient, making it difficult to obtain a dense sintered body. On the other hand, if the sintering temperature is higher than 1950°C, silicon nitride may decompose into Si and N2 if the atmospheric pressure in the furnace is low. For this reason, it is preferable to control the sintering temperature within the above range. In addition, the sintering time is preferably within a range of 7 hours to 20 hours.

[0027] During the sintering process, it is preferable to set the heating rate from 1350°C to 1600°C at 50°C / h or less. In the temperature range from 1350°C to 1600°C, a liquid phase mainly composed of the sintering aid is generated. Therefore, by controlling the heating rate, it is possible to promote the diffusion of the liquid phase to the surfaces of the silicon nitride crystal particles. The rate of temperature rise from 1650°C to the sintering temperature is preferably 50°C / h or less. By setting the rate of temperature rise to 50°C / h or less, uniform grain growth is promoted, and the generation of coarse grains can be suppressed, and the formation of dislocation defects in silicon nitride crystal grains can be suppressed. The heating rate from 1300°C to 1650°C is defined as the first heating rate. The heating rate from 1650°C to the sintering temperature is defined as the second heating rate. The first heating rate is preferably equal to or greater than the second heating rate. By making the second heating rate equal to or slower than the first heating rate, the effect of suppressing the generation of coarse grains can be improved. Grain growth proceeds via the liquid phase diffused on the surface of silicon nitride crystal grains. Therefore, by maintaining the heating rate from 1650°C to the sintering temperature at the first heating rate that is effective for the diffusion of the liquid phase, or by setting it to a second heating rate that is slower than the first heating rate, uniform grain growth is promoted. This improves the effect of suppressing the generation of coarse grains. Furthermore, in the sintering step, it is preferable to control the pressure so that the amount of change in pressure is 0.3 MPa or less. By suppressing the amount of change in pressure, it is possible to suppress the formation of dislocation defects in silicon nitride crystal grains. The change in pressure affects the grain growth of silicon nitride crystal grains. When the sintering step is performed at normal pressure or under pressure, it is preferable to set the amount of change in pressure to 0.3 MPa or less, and further to 0.1 MPa or less. In order to control the amount of change in pressure, it is effective to control the gas pressure in the sintering atmosphere. Gas is easily generated during the sintering step of the silicon nitride substrate. In the sintering step, the binder in the molded body, the sintering aid, impurity oxygen in the silicon nitride powder, etc. become gas components. The pressure of the sintering atmosphere changes depending on the generated gas components. In other words, even in normal pressure sintering where no pressure is applied, the pressure of the sintering atmosphere changes depending on the generated gas components. For this reason, it is necessary to control the atmosphere pressure during the sintering step by removing the generated gas components, etc., so that the pressure does not change. In particular, it is preferable to set the amount of change in pressure between the heat treatment step at 1300°C or more and the sintering step to 0.3 MPa or less.

[0028] In this way, by controlling the rate of temperature rise or suppressing pressure changes, abnormal grain growth of silicon nitride crystal grains can be suppressed. This makes it possible to control the maximum long diameter of silicon nitride crystal grains to 60 μm or less, or even 25 μm or less, in an observation area of ​​300 μm×300 μm of any cross section of the silicon nitride sintered body. Also, in an observation area of ​​300 μm×300 μm of any cross section of the silicon nitride sintered body, the average long diameter of silicon nitride crystal grains can be controlled within the range of 1 μm to 10 μm. Furthermore, since abnormal grain growth can be suppressed, the area of ​​each grain boundary phase can be controlled to 9 μm or less in an observation area of ​​300 μm×300 μm of any cross section of the silicon nitride sintered body. 2 Below that, even 5μm 2 It can be controlled as follows: The cooling rate after the sintering step can be appropriately set. In order to promote the crystallization of the grain boundary phase, it is preferable to set the cooling rate to 100° C. / h or less.

[0029] 3 to 5 are diagrams showing an example of a silicon nitride circuit board according to an embodiment. In FIG. 3, 10 is a silicon nitride circuit board. 12 is a silicon nitride board. 13 is a front metal plate. 14 is a bonding layer. 15 is a rear metal plate. FIG. 3 shows an example in which two front metal plates 13 are bonded to a silicon nitride board 12. The embodiment is not limited to this form, and one or three or more front metal plates 13 may be bonded to the silicon nitride board 12. Each front metal plate 13 may be processed into a wiring pattern. In the example of FIG. 3, a rear metal plate 15 is further bonded to the silicon nitride board 12. The rear metal plate 15 functions as a heat sink rather than a circuit. The rear metal plate 15 can be provided as necessary. The silicon nitride substrate may have a through hole. The silicon nitride circuit substrate preferably has a structure in which the front metal plate and the rear metal plate are electrically connected through the through hole. FIG. 4 shows an example of a silicon nitride circuit substrate having a through hole. FIG. 4 is a cross-sectional view of a portion in which a through hole is provided. In FIG. 4, 10 is a silicon nitride circuit substrate. 12 is a silicon nitride substrate. 13 is a front metal plate. 14 is a bonding layer. 18 is a rear metal plate. 19 is a through hole. In FIG. 4, the front metal plate 13 and the rear metal plate 18 are electrically connected through the through hole 19. In FIG. 4, a plurality of through holes 19 respectively connect a plurality of front metal plates 13 and a plurality of rear metal plates 18. The embodiment is not limited to such a structure. In the silicon nitride circuit substrate 10, the through hole 19 may be provided only for a portion of the plurality of front metal plates 13. The through hole 19 may be provided only for a portion of the plurality of rear metal plates 18. The inside of the through hole 19 is preferably filled with the same material as the bonding layer 14. The internal structure of the through hole 19 is not particularly limited as long as it can electrically connect the front metal plate and the back metal plate. For this reason, a metal thin film may be provided only on the inner wall of the through hole 19. On the other hand, by filling the through hole 19 with the same material as the bonding layer 14, the bonding strength can be improved. The silicon nitride circuit board according to the embodiment is suitable for a semiconductor device. In the semiconductor device, a semiconductor element is mounted on the metal plate of the silicon nitride circuit board via a bonding layer. FIG. 5 shows an example of a semiconductor device. In FIG. 5, 10 is a silicon nitride circuit board. 20 is a semiconductor device. 21 is a semiconductor element. 22 is a bonding layer. 23 is a wire bonding. 24 is a metal terminal. In FIG. 5, a semiconductor element 21 is bonded onto the metal plate of the silicon nitride circuit board 10 via a bonding layer 22. Similarly, a metal terminal 24 is bonded via the bonding layer 22. Adjacent metal plates are electrically connected to each other by a wire bonding 23. In FIG. 5, in addition to the semiconductor element 21, a wire bonding 23 and a metal terminal 24 are bonded. The semiconductor device according to the embodiment is not limited to such a structure. For example, only one of the wire bonding 23 and the metal terminal 24 may be provided. A plurality of semiconductor elements 21, bonding wires 23, and metal terminals 24 may be provided on the front metal plate 13. The semiconductor elements 21, bonding wires 23, and metal terminals 24 can be bonded to the back metal plate 18 as necessary. The metal terminals 24 can have various shapes, such as a lead frame shape or a convex shape. The bonding layer 22 for bonding the semiconductor element 21 or the metal terminal 24 may be made of solder, brazing material, or the like. The solder is preferably lead-free. The melting point of the solder is preferably 450°C or less. The melting point of the brazing material is preferably 450°C or less. A brazing material with a melting point of 500°C or more is called a high-temperature brazing material. An example of a high-temperature brazing material is one containing Ag as a main component.

[0030] (Example) (Examples 1 to 5, Reference Example 1) A mixed raw material powder was prepared by mixing silicon nitride powder and sintering aid powder. The mixed raw material powder was then crushed and mixed to prepare mixed raw material powders 1 to 3. The crushing and mixing was performed using a ball mill. The results are shown in Table 1.

[0031] [Table 1]

[0032] The mixed raw powders 1 to 3 have an average particle size D 50 The mixed raw material powder 4 was crushed and mixed for 20 hours or more until the average particle size D 50 The crushing and mixing was carried out for a short period of 10 hours until the average particle size D 50 The measurement was performed using a laser diffraction / scattering type particle size distribution measuring device (manufactured by Horiba, Ltd.). Next, 5% to 10% by mass of binder was added to the mixed raw material powder to prepare a mixed raw material paste. The mixed raw material paste was formed into a sheet by the doctor blade method. The sheet-formed body was subjected to a degreasing process at 500°C to 800°C for 1 hour to 4 hours to prepare a degreased body. Next, the sintering process shown in Table 2 was carried out in a nitrogen atmosphere. The silicon nitride substrate after the sintering process was divided to obtain silicon nitride substrates of 50 mm length x 40 mm width. The pressure of 0.1 MPa indicates normal pressure.

[0033] [Table 2]

[0034] The silicon nitride substrates according to the examples and reference examples were measured for dislocation defects, the major axis of silicon nitride crystal grains, the area of ​​the grain boundary phase, thermal conductivity, three-point bending strength, fracture toughness value, and dielectric strength voltage. In the measurement of the dislocation defect, an arbitrary cross section was processed by ion milling to a surface roughness of Ra 1 μm or less, and used as the evaluation surface. The evaluation surface was observed by TEM. In the observation by TEM, adjacent regions were photographed in sequence in an arbitrary observation region of 50 μm × 50 μm. The magnification when taking the TEM photograph was set to 10,000 times, and bright-field images and dark-field images were taken. The region that appears white in the dark-field image was used as the dislocation defect. The presence or absence of dislocation defects in one silicon nitride crystal grain and the occupied area ratio were determined by comparing the bright-field image and the dark-field image. In addition, the occupied area ratio of the dislocation defect was measured by binarizing the dark-field image using image processing software and calculating (area of ​​white pixel clusters / (area of ​​white pixel clusters + area of ​​black pixel clusters)) × 100. Observation in one observation region of 50 μm × 50 μm was continued until 50 silicon nitride crystal grains with visible outlines were confirmed. Silicon nitride crystal particles that were cut off at the edge of the TEM photograph (i.e. silicon nitride crystal particles whose entire outline was not visible) were excluded from the count of the number ratio. When 50 silicon nitride crystal particles whose entire outline was visible were confirmed, a separate observation area was observed by TEM, even if the entire observation area of ​​50 μm x 50 μm was not observed. As the separate observation area, an area more than 1000 μm away from the previous observation area was selected. A total of two or more observation areas were photographed. Image-j was used as the image analysis software. In addition, the elements at the core of the dislocation defects were analyzed. EDX was used to analyze the dislocation defects. This revealed that elements other than silicon, oxygen, and nitrogen were present within 1 μm of the dislocation defects. 2 It was measured whether the particles were agglomerated to 10 mol % or more and whether they were detected at 10 mol % or more.

[0035] The long diameter of silicon nitride crystal particles was measured based on SEM observation of an arbitrary cross section. The magnification for taking SEM photographs was set to 3000 times, and an area of ​​300 μm × 300 μm was photographed. In the SEM photograph, the length of the longest line segment obtained by connecting any two points on the outer edge of one silicon nitride crystal particle was taken as the long diameter. The average of the long diameters of silicon nitride crystal particles shown in the SEM photograph (observation area 300 μm × 300 μm) was calculated. In addition, the longest long diameter of each silicon nitride crystal particle was extracted as the maximum long diameter. The SEM photograph (observation area 300 μm × 300 μm) was binarized using image analysis software, and the binary image was analyzed. In the binary image, the area surrounded by three or more silicon nitride crystal particles was determined as the grain boundary phase, and its area was calculated. Image-j was used as the image analysis software. Thermal conductivity was measured according to the flash method of JIS-R-1611 (2010). JIS-R-1611 (2010) corresponds to ISO18755 (2005). Three-point bending strength was measured according to JIS-R-1601 (2008). Fracture toughness was measured using the Niihara formula according to the IF method of JIS-R-1607 (2015). Dielectric strength was measured by the two-terminal method according to JIS-C-2141. JIS-C-2141 corresponds to IEC672-2 (1980). For the dielectric strength measurement, a measuring terminal with a flat electrode with a diameter of 25 mm at the tip was used. The dielectric strength was measured in Fluorinert. The results are shown in Tables 3 and 4.

[0036] [Table 3]

[0037] [Table 4]

[0038] The silicon nitride substrates according to the examples had a dislocation defect ratio of 20% or less, and even 10% or less. In the examples in which dislocation defects were observed (Examples 2, 4, 5, and 7), the size of the nucleus of the dislocation defect (elements other than silicon, oxygen, and nitrogen) was within the range of 0.2 μm or less. Furthermore, in the nucleus of the dislocation defect of the silicon nitride sintered body according to the examples, the elements other than silicon, oxygen, and nitrogen were less than 10 mol %. The maximum value of the long diameter of the silicon nitride crystal grains was 60 μm or less. In the silicon nitride substrate according to the embodiment, the maximum value of the area of ​​the grain boundary phase was 9 μm. 2 The results were smaller than those of the reference example. In addition, excellent values ​​were obtained for the thermal conductivity, three-point bending strength, and dielectric strength. Next, copper plates (thickness 0.8 mm) were bonded to both sides of the silicon nitride substrate according to the embodiment and the reference example using an active metal brazing material. The active metal brazing material used was made of Ag (60 mass%), Cu (28 mass%), Sn (9 mass%), and Ti (3 mass%). The thickness of the active metal bonding layer was 30 μm.

[0039] Next, the front copper plate was etched and patterned. A cupric chloride solution was used for etching the copper plate. An etching solution containing ammonium fluoride and hydrogen peroxide (H2O2) was used for etching the active metal brazing material layer. In etching condition 1, the pH of the etching solution for the active metal brazing material was set to a range of 5.2 to 5.8. In etching condition 2, the pH of the etching solution for the active metal brazing material was set to a range of 4.5 to 5.0. In addition, in etching condition 2, a chemical polishing solution containing hydrochloric acid and having a pH of 1 to 2 was also used. In other words, etching under etching condition 2 is more likely to damage the silicon nitride substrate than etching under etching condition 1. The insulation of the silicon nitride circuit board after etching was compared with that of the silicon nitride circuit board before etching to measure the rate of decrease. The rate of decrease in insulation was measured by measuring the leakage current. The leakage current was measured by applying an AC voltage of 1.5Kv-100Hz between the front and back of the silicon nitride board under conditions of a temperature of 25°C and a humidity of 70%. A silicon nitride circuit board in which the change in leakage current before and after etching was 5% or less was determined to be a good product (○). A silicon nitride circuit board in which the change in leakage current was more than 5% and less than 10% was determined to be a fair product (△). A silicon nitride circuit board in which the change in leakage current was more than 10% was determined to be a defective product (×). The results are shown in Table 5.

[0040] [Table 5]

[0041] The silicon nitride substrates according to the Examples showed little deterioration in insulation properties after etching under either etching condition 1 or 2. For the silicon nitride substrate according to Reference Example 1, the deterioration in insulation properties was small when etched under etching condition 1. However, when etched under etching condition 2, a deterioration in insulation properties was observed. Furthermore, in the silicon nitride substrate according to Example 7, the coarse grains exceeded 25 μm and the area of ​​the grain boundary phase was 9 μm. 2 Therefore, when etching was performed under etching condition 2, the insulating property was slightly decreased. Etching condition 2 is necessary when the copper plate thickness is 0.8 mm or more. In other words, etching condition 2 is suitable for etching a silicon nitride circuit board having a copper plate thickness of 0.8 mm or more.

[0042] Although several embodiments of the present invention have been illustrated above, these embodiments are merely examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other.

Claims

1. Average particle size D 50 a mixing step of mixing silicon nitride powder and sintering aid powder so that the particle size is 1 μm or less, and further adding a binder to prepare a raw material mixture; A degreasing step of degreasing a sheet molded body of the raw material mixture; a sintering step of sintering the degreased sheet compact at a sintering temperature in the range of 1800° C. to 1950° C.; A cooling step after the sintering step, The change in pressure from 1300° C. during the sintering step is 0.3 MPa or less, and the change in pressure during the sintering step until before the cooling step is performed is 0.3 MPa or less; During the sintering step, the heating rate from 1350° C. to 1600° C. is 50° C. / h or less, and the heating rate from 1650° C. to the sintering temperature is 50° C. / h or less; The method for producing a silicon nitride substrate, wherein the thickness of the silicon nitride substrate obtained by sintering the sheet compact is 0.1 mm or more and 0.4 mm or less.

2. in an observation region of 50 μm×50 μm on any cross section or surface of the silicon nitride substrate, the ratio of the number of silicon nitride crystal grains having dislocation defects therein among any 50 silicon nitride crystal grains whose entire contours are visible is 0% or more and 10% or less, 2. The method for producing a silicon nitride substrate according to claim 1, wherein a ratio of the number of silicon nitride crystal grains in which the occupied area ratio of the dislocation defects is 5% or less to the number of the silicon nitride crystal grains having the dislocation defects is 70% or more.

3. 3. The method for producing a silicon nitride substrate according to claim 2, wherein components other than silicon, oxygen and nitrogen are not detected in the dislocation defects at an amount of 10 mol % or more.

4. 4. The method for producing a silicon nitride substrate according to claim 1, wherein in an observation area of ​​300 μm×300 μm of any cross section of said silicon nitride substrate, the maximum value of the major axis of silicon nitride crystal grains is 60 μm or less.

5. In an observation area of ​​300 μm×300 μm of an arbitrary cross section of the silicon nitride substrate, the area of ​​each grain boundary phase is 9 μm 2 5. The method for producing a silicon nitride substrate according to claim 1, wherein the silicon nitride substrate is formed by:

6. 6. The method for producing a silicon nitride substrate according to claim 1, wherein the silicon nitride substrate has a dielectric strength of 25 kV / mm or more.

7. 7. The method for producing a silicon nitride substrate according to claim 1, wherein the silicon nitride substrate has a thermal conductivity of 80 W / (m·K) or more.

8. 8. The method for producing a silicon nitride substrate according to claim 1, wherein the silicon nitride substrate has a three-point bending strength of 600 MPa or more.

Citation Information

Patent Citations

  • Silicon nitride substrate and silicon nitride circuit substrate using same

    WO2015060274A1

  • Silicon nitride sintered compact having high thermal conductivity, silicon nitride substrate and silicon nitride circuit substrate using same, and semiconductor device

    WO2016117553A1

  • Circuit substrate and semiconductor device

    WO2017056360A1

Cited By

  • Insulation withstand voltage test method and silicon nitride substrate

    JP2026164263A