Manufacturing method of welded joint by gas shielded arc welding of steel plate
The gas-shielded arc welding method for thick steel plates addresses weld defects and ensures high strength and low-temperature toughness, suitable for large structures like offshore platforms and shipbuilding.
Patent Information
- Application Number
- JP2024536459
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-27
AI Technical Summary
Existing welding methods for thick steel plates, particularly those with a thickness of 50 mm or more, face challenges in ensuring high strength, low-temperature impact toughness, and are prone to weld defects such as hot cracking and poor fusion, especially in cold environments like -40°C.
A gas-shielded arc welding method using multi-electrode welding with three or more electrodes, controlled groove angles and gaps, and specific chemical compositions to create a multilayer weld metal with controlled height-to-width ratios, ensuring sound welding without defects.
The method produces a welded joint with high strength and excellent low-temperature impact toughness, free from weld defects, making it suitable for large structures like offshore platforms and shipbuilding.
Smart Images

Figure 0007558479000012 
Figure 0007558479000013 
Figure 0007558479000014
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a welded joint by gas-shielded arc welding using steel plate, particularly steel plate having a thickness of 50 mm or more. [Background technology]
[0002] With the growth of the energy industry, for example, to improve the efficiency of drilling marine resources and power generation, marine structures and offshore wind turbines constructed on the sea are becoming larger. As structures and generators become larger, the foundations of the equipment are required to have high strength, and the use of thick steel plates with a plate thickness of 50 mm or more is being considered. In addition, in cold oceans, it is expected that waves and drift ice may collide with structures, so excellent toughness at -40°C is also required. When manufacturing marine structures and offshore generator equipment that use thick plates, improving the construction efficiency is an important issue, and in particular, there is a demand for highly efficient welding of such thick plates.
[0003] Large heat input welding has been proposed as one of the highly efficient welding methods for thick plates. However, when large heat input welding is used, it is often difficult to ensure the toughness of the weld metal and the heat affected zone of the base metal.
[0004] For example, Patent Document 1 discloses a "two-electrode, one-side, one-pass, large heat input submerged arc welding method with excellent toughness of weld metal." The welding method disclosed in Patent Document 1 uses a specific flux and specific welding wires for the first and second electrodes for a specific steel plate when performing one-pass welding on a steel plate having a thickness of 40 mm or more by two-electrode submerged arc welding. The steel plate contains, by mass%, C: 0.02-0.2%, Si: 0.01-1%, Mn: 0.1-2.5%, Al: 0.002-0.1%, and N: 0.001-0.015%, with P: 0.02% or less, S: 0.01% or less, and O: 0.01% or less, with the balance being Fe and unavoidable impurities. The flux contains, by mass%, SiO 2 :10~25%, MgO:5~20%, CaO:5~15%, CaF 2: 1-10%, Al 2 O 3 : 5-25%, TiO 2 : 2~20%, Fe: 10~25%, B 2 O 3 The welding wire contains, by mass%, C: 0.02-0.2%, Si: 0.01-1%, Mn: 0.5-2.5%, Al: 0.002-0.1%, Ti: 0.005-0.3%, N: 0.001-0.015%, P: 0.02% or less, S: 0.01% or less, O: 0.01% or less, and the balance is Fe and inevitable impurities. Furthermore, welding is performed under the conditions that the diameter of the welding wire of the second electrode is 6-8 mm, and the ratio of the cross-sectional area of the welding wire of the first electrode to the cross-sectional area of the welding wire of the second electrode is 35-75%. Patent Document 1 describes this as a two-electrode one-side one-pass large heat input submerged arc welding method with excellent toughness of the weld metal.
[0005] Patent Document 2 discloses a "two-electrode large heat input submerged arc welding method." The welding method described in Patent Document 2 is a two-electrode large heat input submerged arc welding method in which welding is performed using a specific wire and a specific flux. The wire contains, by mass%, C: 0.02-0.18%, Si: 0.02-0.5%, Mn: 1.15-2.2%, Mo: 0.1-1.0%, Ni: 0.1-1.5%, Ti: 0.005-0.05%, P: 0.006% or less, S: 0.003% or less, and the balance being Fe and unavoidable impurities. The flux is SiO 2 :13~25%, MgO:8~20%, CaO:5~13%, CaF 2 : 1-7%, Al 2 O 3 : 9-23%, TiO 2 : 3-11%, Fe: 11-25%, B 2 O 3With this welding method, even in high heat input submerged arc welding with a welding heat input of 500 kJ / cm or more, the mechanical performance of the weld metal is excellent, good welding workability can be obtained, and the safety of architectural structures can be significantly improved while at the same time the welding efficiency can be significantly improved.
[0006] Also, for example, Patent Document 3 discloses a "highly efficient welding method for thick steel plates." According to Patent Document 3, the method includes a processing step of processing an X-shaped groove on a pair of steel materials having a plate thickness of more than 50 mm and not more than 100 mm. Furthermore, the method includes a welding step of performing one pass of welding on each of the front and back surfaces of the pair of steel materials using a multi-electrode submerged arc welding with two or more and six or less electrodes and a flux. In the welding step, the welding current of the first electrode is an AC current with a waveform ratio of 60% or more and 90% or less, and the welding current of the other electrodes is an AC current with a waveform ratio of 70% or more or a negative DC current. The flux used here is a flux containing Al, in terms of mass ratio with respect to the total mass of the flux, and Al is used as the flux. 2 O 3 :10% or more, 50% or less, SiO 2 : Contains 16% or more and 30% or less. Also contains MgO, TiO 2 , CaF 2 , MnO in a total content of 10% or more and 60% or less, MgO in a total content of 40% or less, TiO 2 to 20% or less, CaF 2 The amount of MnO is limited to 30% or less, and MnO to 20% or less. This is the submerged arc welding method, and it is said that this method can efficiently manufacture the foundations of wind power generation facilities to be installed in cold regions because it can obtain weld metal with excellent toughness even at low temperatures.
[0007] On the other hand, narrow gap welding has been proposed as one of the highly efficient welding methods for thick plates. By reducing the cross-sectional area of the groove, it is possible to reduce the amount of welding heat input, and it is possible to ensure the toughness of the weld metal and the base metal heat-affected zone. However, simply welding thick plates using narrow gap welding has the problem that hot cracks and incomplete fusion are likely to occur.
[0008] To address this issue, for example, Patent Document 4 discloses a "narrow gap submerged arc welding method." The welding method disclosed in Patent Document 4 is a narrow gap submerged arc welding method for extra thick steel plates, in which a backing material is abutted against the back side of a narrow groove with a groove angle of 1 to 5° and a root gap of 10 to 14 mm, and steel particles are scattered in the groove to a height of 10 to 15 mm from the back side of the groove. Then, Al is added in mass % relative to the total mass of the flux. 2 O 3 , TiO 2 and CaF 2 Total: 50-70%, SiO 2 : Contains 10-20% and the rest is CaO, MnO, BaO, K 2 O, Na 2 A molten flux consisting of O and unavoidable impurities is used. This is a narrow gap submerged arc welding method in which multi-layer welding is performed with one layer and one pass. According to Patent Document 4, excellent welding workability such as good slag removability and bead shape can be obtained, and narrow gap submerged arc welding can be performed without back chipping. Patent Document 4 claims that a sound weld without welding defects such as high temperature cracking, slag inclusion, and poor fusion can be obtained with high efficiency.
[0009] In the submerged arc welding method, which is a narrow gap welding method for thick steel plates as described above, it is necessary to spray flux in front of the weld before welding and to collect the flux after welding, and these fluxes must be managed separately. Furthermore, after welding, the slag formed in the weld must be removed, which makes the work less efficient. In response to this, a narrow gap gas shielded arc welding method has been proposed that has excellent workability during on-site construction.
[0010] For example, Patent Document 5 discloses a narrow-gap gas-shielded arc welding method for joining thick steel plates by narrow-gap multi-layer welding. In the technology described in Patent Document 5, the first layer welding is performed by multi-electrode welding with two or more electrodes, the first electrode and the second electrode are positioned along a predetermined parallel welding line, and the distance between the welding wire tips of the first electrode and the second electrode is controlled to a range of 5 mm to 16 mm. In addition, the angle of the straight line connecting the welding wire tips of the first electrode and the second electrode with respect to the perpendicular direction of the welding line is controlled to a range of 45° or less. Furthermore, the melting depth perpendicular to the welding line at the bottom of the steel is set to 1.5 mm or more. As a result, even when groove processing such as gas cutting or plasma cutting is performed, there is no defect and the welding construction efficiency is improved. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Patent No. 4673710 [Patent Document 2] JP 2006-212676 A [Patent Document 3] International Publication No. 2013 / 073565 [Patent Document 4] JP 2021-126696 A [Patent Document 5] Patent No. 6137053 Summary of the Invention [Problem to be solved by the invention]
[0012] However, the invention of Patent Document 1, which aims to realize high-efficiency welding by large heat input, aims to provide a welding method that can obtain high toughness with 2 mm V-notch Charpy absorbed energy of 70 J or more at 0 ° C. In other words, it is not suitable for use in a cold environment of -40 ° C. Similarly, in Patent Document 2, the toughness evaluation is performed at 0 ° C., and use in a cold environment of -40 ° C is not assumed. In addition, in the invention of Patent Document 3, there is no reference to the low-temperature toughness value of the base metal heat affected zone (hereinafter, the base metal heat affected zone is also called "welding heat affected zone"), and it is unclear whether it can be used in a cold environment of -40 ° C. Furthermore, the invention of Patent Document 4, which aims to realize high-efficiency welding by narrow gap welding, does not refer to the mechanical properties of the weld metal and the weld heat affected zone. In addition, in the technology of the narrow gap gas shielded arc welding method disclosed in Patent Document 5, when multi-electrode welding with three or more electrodes is performed, hot cracks may occur in the center of the weld metal.
[0013] The present invention aims to solve the problems of the conventional technology and to provide a method for manufacturing a narrow gap welded joint using steel plate with a thickness of 50 mm or more by gas shielded arc welding, which is free of welding defects, has high strength, and has excellent low-temperature impact toughness.
[0014] In this context, "high strength" refers to a weld metal manufactured in accordance with the provisions of JIS Z 3111 having a room temperature yield strength (0.2% proof stress) of 325 MPa or more, a tensile strength of 520 MPa or more, and a welded joint having a room temperature tensile strength of 520 MPa or more. Also, "excellent low-temperature impact toughness" refers to the absorbed energy (vE -40 ) is 30J or more. [Means for solving the problem]
[0015] [How the present invention was made] In order to achieve the above object, the inventors first conducted intensive research into a weld metal shape that can efficiently and soundly weld a welded joint of a steel plate having a plate thickness of 50 mm or more. The weld length of a foundation for an offshore structure or an offshore wind power plant may exceed 1.0 km per structure in total length, and reducing the number of layers of weld metal is effective for highly efficient welding. However, in conventional welding methods, the welding is distributed along the groove wall, so the welding efficiency is not high. In contrast, in the present invention, it has been found that highly efficient welding can be performed by forming a multi-layer weld metal with one pass welding for each layer of weld metal without distributing the weld. However, it was noted that the low-temperature impact toughness value of the weld metal and the base metal heat-affected zone decreases when the welding heat input is large.
[0016] Next, as a result of examining the above-mentioned issues, it was found that the deposition area of the weld metal was 120.0 mm per layer. 2 It was found that if the welding heat input is less than 120.0 mm, the heat effect on the base metal is sufficiently small, and excellent low-temperature toughness characteristics of the weld can be obtained. In addition, multi-layer weld metal can be obtained by one pass welding per layer, and the welding area per layer can be 120.0 mm 2 It was found that, even if the ratio [H / W] of the height H (mm) to the width W (mm) of the weld metal of each weld layer is greater than 1.00, hot cracks are likely to occur. This occurs when the direction of solidification of the weld metal coincides with the direction of tensile strain during cooling, causing hot cracks to occur at the junction of dendrites. Therefore, it was found that the occurrence of hot cracks can be suppressed by controlling the above ratio [H / W] to 1.00 or less. Furthermore, after extensive research into groove shapes that satisfy the above, it was found that a groove angle of 20° or less and a gap between the base metals of 6 mm or less for one-sided welding and 10 mm or less for both-sided welding, respectively, are satisfactory.
[0017] On the other hand, it was found that if the gap between the base materials exceeds 6 mm, there is a possibility that poor fusion may occur during welding of the first layer. From these findings, it was found that the groove shape that can weld steel plates with a thickness of 50 mm or more with high efficiency and soundness is preferably a gap between the base materials of 6 mm or less and a groove angle of 20° or less, regardless of whether single-sided or double-sided welding is used. It was also found that the groove area can be made smaller by performing double-sided welding.
[0018] [Summary of the present invention] The present invention was completed based on these findings and through further investigation, and the gist of the present invention is as follows. [1] In a method for manufacturing a welded joint by gas-shielded arc welding of steel plates, The thickness T (mm) of the steel plate is 50 mm or more, The weld metal consists of multiple layers with one pass per layer. The cross-sectional area A (mm 2 ) and the number of weld layers p (layers) ratio [A / p] is 120.0 mm 2 / layer or lower, The ratio [H / W] of the height H (mm) to the width W (mm) of each layer in the weld metal is 1.00 or less, The gas shielded arc welding is a multi-electrode welding having three or more electrodes, The tips of the welding wires of the first electrode and the second electrode are disposed on different parallel welding lines; One of the first electrode and the second electrode is a wire negative (positive polarity), and the other is a wire positive (reverse polarity), The distance a (mm) between the welding wire tips of the first electrode and the second electrode is 5 to 16 mm, an angle α of a straight line connecting the welding wire tips of the first electrode and the second electrode with respect to a perpendicular direction of the welding line is 60° or less; A welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode that is the negative (positive) wire. A method for manufacturing welded joints by gas-shielded arc welding of steel plates. [2] In the above [1], a tilt angle Φ of a tip of each of the first electrode and the second electrode toward a groove surface side with respect to a perpendicular direction of the weld line is 0° to 15°, A distance d (mm) between a side end portion of each of the welding wire tips of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm, Each of the welding wires is a welding wire that is bent in advance to have a radius of curvature in the range of 150 to 300 mm, A third electrode and subsequent electrodes are disposed at the center of the groove behind the first electrode and the second electrode, Shielding gas: 60% or more by volume of CO 2 Using gas containing gas, A method for manufacturing welded joints by gas-shielded arc welding of steel plates. [3] In the above [1] or [2], the chemical composition of the steel plate is, in mass%, C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, O: 0.0100% or less, and N: 0.0100% or less The balance is Fe and unavoidable impurities, Ceq and plate thickness (T) defined by the following formula (1) are 0.0004T+0.25≦Ceq≦0.0004T+0.45 and having a chemical composition that satisfies the above. The dislocation density ρ at a position 1 mm below the surface of the steel plate is 4.0×10 14 m -2 is as follows: The average crystal grain size at a position 1 mm below the surface of the steel plate is 15.0 μm or less, and the average crystal grain size at the center position of the plate thickness is 20.0 μm or less; A method for manufacturing welded joints by gas-shielded arc welding of steel plates. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15...(1) However, each element symbol in the above formula (1) represents the content (mass%) of the corresponding element, and if the corresponding element is not contained, it is set to 0. [4] In the above [3], the chemical composition of the steel plate further comprises, in mass%, Cu: 2.000% or less, Ni: 2.500% or less, Cr:1.500% or less, Mo: 1.000% or less Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less A method for producing a welded joint by gas-shielded arc welding of steel plates, comprising one or more types selected from the group consisting of: [5] In any one of the above [1] to [4], the chemical composition of the weld metal is, in mass%, C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, Cu: 0.001 to 2.000%, Ni: 0.001 to 2.500%, Cr: 0.001~1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less The balance is Fe and unavoidable impurities. A method for manufacturing welded joints by gas-shielded arc welding of steel plates. [6] In the above [5], the chemical composition of the weld metal further comprises, in mass%, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less A method for producing a welded joint by gas-shielded arc welding of steel plates, comprising one or more types selected from the group consisting of: Effect of the Invention
[0019] According to the present invention, a welded joint can be obtained by welding steel plates having a thickness of 50 mm or more. This is a narrow gap welded joint that has sound weld metal without welding defects such as high-temperature cracking or incomplete fusion and has both high strength and excellent low-temperature impact toughness, and therefore has a significant industrial effect.
[0020] The welded joint of steel plates according to the present invention is not limited to marine structures and offshore wind turbines, but can also be applied to, for example, shipbuilding, line pipes, construction, and the like. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the shape of a weld metal of a welded joint according to the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a weld metal illustrating a welding process for a welded joint according to the present invention. [Diagram 3] FIG. 3 is a partially enlarged schematic cross-sectional view of a weld metal illustrating a welding process using three electrodes. [Figure 4] FIG. 4 is a schematic plan view showing a welding process using three electrodes. [Diagram 5] FIG. 5 is a schematic plan view showing a welding process using four electrodes. [Figure 6]FIG. 6 is a schematic cross-sectional view showing the groove shapes of (a) a V groove and (b) an X groove. [Figure 7] FIG. 7 is a side cross-sectional view that illustrates a schematic relationship between a gas supply nozzle and an electrode according to the present invention. [Figure 8] FIG. 8 is a plan view showing a schematic relationship between the gas supply nozzle and the electrodes according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments.
[0023] [Cross-sectional shape of welded joint] First, a welded joint of steel plates according to the present invention will be described. The welded joint of steel plates according to the present invention is a butt welded joint of steel plates having a plate thickness T (mm) of 50 mm or more, and the weld metal is made of multiple layers with one pass per layer. 2 ) and the number of weld layers p (layers) ratio [A / p] is 120.0 mm 2 / layer or less, and the ratio [H / W] of the height H (mm) to the width W (mm) of each layer in the weld metal is 1.00 or less. In the present invention, the weld metal is formed by one pass of welding per layer of weld metal, without distributing the weld along the groove wall as in conventional welding methods, thereby enabling highly efficient welding.
[0024] Here, the plate thickness T of the steel plate is specified to be 50 mm or more for application to large structures, etc. There is no particular upper limit to the plate thickness T, but it is preferably 200 mm or less due to manufacturing constraints, and more preferably 50 to 160 mm. Here, the weld line refers to a virtual line when a bead or a welded portion is represented as a single line.
[0025] The cross-sectional shape of the above-mentioned welded joint will be described with reference to FIG. Cross-sectional area A of the entire weld metal perpendicular to the weld line (mm 2 ) for the weld layer L1 (first layer)~L p When construction is performed up to the top layer (p), the cross-sectional area per layer [A / p] is 120.0 mm 2 That is, the deposition area of the weld metal is 120.0 mm per layer. 2 If the ratio [A / p] is set to 80.0 mm or less, the amount of welding heat input is not excessive, the thermal effect on the base metal is sufficiently small, and excellent low-temperature toughness characteristics of the weld metal can be obtained. 2 More preferably, the ratio [A / p] should be 60.0 mm 2 There is no particular lower limit for this ratio [A / p], but from the viewpoint of welding efficiency, it is preferably 25.0 mm 2 / layer or more.
[0026] Furthermore, the ratio [H / W] of the height H (mm) to the width W (mm) of each layer in the weld metal is 1.00 or less. For example, the i-th weld layer (L i ) is the height at H i , width W i Then, the ratio [H i / W i 〕 is 1.00 or less for all layers from the first layer (initial layer) to the pth layer (outermost layer). Here, the height H of the welded layer represents the distance between the top and bottom of each layer, and the width W represents the width of the weld metal at the center line of the height H (i.e., the distance between the fusion lines). i and width W i Measure the ratio [H i / W i ] is obtained. If this ratio [H / W] is greater than 1.00, hot cracks are more likely to occur. This is because hot cracks occur at the dendrite junctions when the solidification direction and the direction of tensile strain during cooling coincide during the solidification process of the weld metal. Therefore, hot cracks can be suppressed by controlling the maximum value of the ratio [H / W] of each layer to 1.00 or less. Preferably, the ratio [H / W] is 0.90 or less. There is no particular lower limit for this ratio [H / W], but from the viewpoint of welding efficiency, it is preferably 0.10 or more, and more preferably 0.20 or more.
[0027] [Group shape] Next, the weld metal of the welded joint according to the present invention is a weld metal constructed by multi-layer welding with one layer and one pass using a narrow groove. In the present invention, the narrow groove means that the groove angle is 20° or less and the maximum groove width between the base materials is 50% or less of the plate thickness T.
[0028] In the case of single-sided welding, if the gap between the base metals is 6 mm or less and the groove angle is 20° or less, and in the case of double-sided welding, if the gap between the base metals is 10 mm or less and the groove angle is 20° or less, the occurrence of hot cracks can be suppressed. However, if the gap between the base metals exceeds 6 mm, there is a possibility that poor fusion will occur during welding of the first layer. Therefore, the groove shape that can weld steel plates of 50 mm or more efficiently and soundly is preferably a gap between the base metals of 6 mm or less and a groove angle of 20° or less, regardless of whether single-sided welding or double-sided welding is used. Furthermore, it is more preferable that the groove angle is 4 to 20°. In addition, in the case of double-sided welding, the groove area can be made smaller, which is more preferable. Furthermore, as shown in (a) and (b) of FIG. 6, when the gap is 0 mm, that is, when the base metals are in contact with each other, as will be clear from the examples described later, the width of the weld metal becomes smaller relative to the height of the weld metal, and the bead shape approaches a pear shape. As a result, impurities segregated in the final solidification part of the weld metal lowered the melting point, causing welding strain to concentrate, resulting in hot cracking and poor fusion during welding. Therefore, it is preferable that the gap is more than 0 mm. More preferably, the gap is 2 mm or more.
[0029] [Chemical composition of steel plate] Next, the steel plate which is the base material of the welded joint of the present invention will be described. First, the steel plate may be a carbon steel or a low alloy steel. Next, the chemical composition will be described. The "%" in the chemical composition described below means "mass %" unless otherwise specified.
[0030] [Basic composition of steel plate] Among the chemical compositions of the steel plates of the welded joint according to the present invention, the basic composition is as follows.
[0031] It is preferable that the steel sheet has a chemical composition containing C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, O: 0.0100% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities.
[0032] The reason why the chemical composition of the steel sheet according to the present invention is specified as above will be explained below. [C: 0.04~0.14%] C is an element that can most inexpensively improve the strength of a steel plate, and also contributes to strengthening the austenite grain boundaries. If the C content is less than 0.04%, the grain boundary strength of austenite decreases, and hot cracking of the slab occurs, so that manufacturability is significantly reduced. In addition, there is a possibility that the strength targeted by the present invention cannot be obtained. On the other hand, if the C content exceeds 0.14%, the weldability decreases, and the toughness may also decrease. Therefore, the C content is preferably 0.04 to 0.14%. In addition, the C content is more preferably 0.05 to 0.12%.
[0033] [Si: 0.03~0.70%] Although Si is an effective element for deoxidization, if the Si content is less than 0.03%, it may not be possible to obtain a sufficient effect. On the other hand, if the Si content exceeds 0.70%, the weldability may decrease. Therefore, the Si content is preferably 0.03 to 0.70%. The Si content is more preferably 0.04 to 0.60%.
[0034] [Mn: 0.30~2.50%] Mn is an element that can improve the hardenability and strength of steel at low cost. To obtain this effect, it is preferable to contain 0.30% or more of Mn. On the other hand, if the Mn content exceeds 2.50%, the weldability may decrease. Therefore, the Mn content is preferably 0.30 to 2.50%. The Mn content is more preferably 0.50 to 2.20%.
[0035] [P:0.030% or less] P is an element that has a strong effect of embrittling grain boundaries, and if contained in a large amount, it may reduce the toughness of the steel plate. Therefore, the P content is preferably 0.030% or less. Furthermore, the P content is more preferably 0.025% or less. On the other hand, since the lower the P content, the more preferable it is, the lower limit of the P content is not particularly limited and may be 0%. However, P is an element that is inevitably contained in the steel plate as an impurity, and excessively reducing the P content leads to an increase in refining time and an increase in costs, so the P content is preferably 0.001% or more.
[0036] [S:0.020% or less] Since S may reduce the toughness of the steel plate, the S content is preferably 0.020% or less. Furthermore, the S content is more preferably 0.010% or less. On the other hand, since the lower the S content, the more preferable it is, the lower limit of the S content is not particularly limited and may be 0%. However, S is an element that is inevitably contained in the steel plate as an impurity, and excessive reduction in S content leads to an increase in refining time and an increase in costs, so the S content is preferably 0.0001% or more.
[0037] [Nb: 0.001~0.100%] Nb is an element that has the effect of suppressing recrystallization when strain is applied to the austenite structure through solid solution Nb and finely precipitated NbC, and raising the non-recrystallization temperature range to the higher temperature side. In order to obtain this effect, the Nb content is preferably 0.001% or more. On the other hand, if the Nb content exceeds 0.100%, there is a possibility that the weldability will deteriorate. Therefore, the Nb content is preferably 0.001 to 0.100%. The Nb content is more preferably 0.005 to 0.075%. Furthermore, it is particularly preferably 0.005 to 0.050%.
[0038] [Al: 0.001~0.100%] Al is an element that is effective as a deoxidizer and also has the effect of forming nitrides to reduce the austenite grain size. In order to obtain this effect, the Al content is preferably 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the steel material or steel plate may decrease, and as a result, the ductility and toughness may decrease. Therefore, the Al content is preferably 0.001 to 0.100%. The Al content is more preferably 0.005 to 0.080% or less.
[0039] [O:0.0100% or less] Since O is an element that reduces ductility and toughness, the O content is preferably 0.0100% or less. On the other hand, since the lower the O content, the more preferable it is, the lower limit of the O content is not particularly limited and may be 0%. However, since O is an element that is inevitably contained in steel sheet as an impurity, and excessive reduction in O content leads to an increase in refining time and an increase in costs, the O content is preferably 0.0005% or more.
[0040] [N:0.0100% or less] Since N is an element that reduces ductility and toughness, the N content is preferably 0.0100% or less. On the other hand, since the lower the N content, the better, the lower limit of the N content is not particularly limited and may be 0%. However, since N is an element that is inevitably contained in the weld metal as an impurity, excessive reduction in N content leads to an increase in refining time and an increase in costs. Therefore, the N content is preferably 0.0005% or more.
[0041] [Optional composition of steel plate] The steel plate for the welded joint of the present invention has the above-mentioned basic composition to obtain the characteristics targeted by the present invention. However, in order to further improve the strength and weldability (specifically, the toughness of the welded part, the weldability, etc.), the steel plate may contain the following optional compositions as necessary in addition to the above-mentioned basic composition.
[0042] One or more selected from the group consisting of Cu: 2.000% or less, Ni: 2.500% or less, Cr: 1.500% or less, Mo: 1.000% or less, Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less. Since Cu, Ni, Cr, Mo, Ti, V, B, W, Ca, Mg, and REM are chemical compositions that can be contained arbitrarily, the content of these elements may be 0%.
[0043] [Cu:2.000% or less] Cu is an element that can improve the strength of the steel plate without significantly deteriorating the toughness of the steel plate. On the other hand, if the Cu content exceeds 2.000%, hot cracking due to the Cu-enriched layer formed just below the scale may become a problem. Therefore, when Cu is contained, the Cu content is preferably 2.000% or less. More preferably, the Cu content is 0.010 to 1.500%.
[0044] [Ni:2.500% or less] Ni is an element that has the effect of improving the hardenability and toughness of the steel plate. On the other hand, if the Ni content exceeds 2.500%, an increase in manufacturing costs may become a problem. Therefore, when Ni is contained, the Ni content is preferably 2.500% or less. More preferably, the Ni content is 0.010 to 2.000%.
[0045] [Cr:1.500% or less] Cr is an element that can improve the hardenability of a steel sheet, thereby improving the strength of the steel sheet. On the other hand, if the Cr content exceeds 1.500%, the weldability may be reduced. Therefore, when Cr is contained, the Cr content is preferably 1.500% or less. More preferably, the Cr content is 0.010 to 1.200%.
[0046] [Mo: 1.000% or less] Mo is an element that can improve the hardenability of a steel sheet, thereby improving the strength of the steel sheet. On the other hand, if the Mo content exceeds 1.000%, the weldability may be reduced. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. More preferably, the Mo content is 0.010 to 0.800%.
[0047] [Ti:0.100% or less] Ti is an element that has the effect of pinning the movement of grain boundaries by precipitating as TiN and suppressing grain growth. On the other hand, if the Ti content exceeds 0.100%, the cleanliness of the steel sheet structure may decrease, and as a result, the ductility and toughness may decrease. Therefore, when Ti is contained, the Ti content is preferably 0.100% or less. More preferably, the Ti content is 0.001 to 0.080%.
[0048] [V:0.300% or less] V is an element that can improve the hardenability of a steel sheet and can improve the strength of the steel sheet by forming carbonitrides. On the other hand, if the V content exceeds 0.300%, the weldability may decrease. Therefore, when V is contained, the V content is preferably 0.300% or less. More preferably, the V content is 0.010 to 0.250%.
[0049] [B:0.0100% or less] B is an element that has the effect of improving the hardenability by adding a very small amount, thereby improving the strength of the steel sheet. On the other hand, if the B content exceeds 0.0100%, the weldability may decrease. Therefore, when B is contained, the B content is preferably 0.0100% or less. More preferably, the B content is 0.0001 to 0.0070%.
[0050] [W:0.500% or less] W is an element that can improve the hardenability of steel, thereby improving the strength of the steel plate. On the other hand, if the W content exceeds 0.500%, the weldability may decrease. Therefore, when W is contained, the W content is preferably 0.500% or less. More preferably, the W content is 0.010 to 0.400%.
[0051] [Ca:0.0200% or less] Ca is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Ca content exceeds 0.0200%, the cleanliness may decrease and the toughness of the steel plate may be impaired. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. More preferably, the Ca content is 0.0001 to 0.0180%.
[0052] [Mg:0.0200% or less] Mg is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Mg content exceeds 0.0200%, the effect of adding Mg becomes saturated and an effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when Mg is contained, the Mg content is preferably 0.0200% or less. More preferably, the Mg content is 0.0001 to 0.0180%.
[0053] [REM:0.0500% or less] REM (rare earth metal) is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the REM content exceeds 0.0500%, the effect of adding REM becomes saturated and the effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when REM is contained, the REM content is preferably 0.0500% or less. More preferably, the REM content is 0.0001 to 0.0450%.
[0054] [Remainder of steel plate composition] The steel plate for the welded joint of the present invention has the above chemical composition and the remainder is Fe and inevitable impurities. Examples of inevitable impurities include H, Zn, Re, Co, Sb, Bi, etc., and a total of 0.0100% or less is acceptable. In addition, as long as the basic composition and optional composition are satisfied, elements other than these may be contained, and such embodiments are also included in the technical scope of the present invention.
[0055] [Ceq] Furthermore, it is more preferable that the chemical composition of the above steel sheet satisfies the following conditions. The relationship between Ceq and plate thickness T (mm) is as follows: 0.0004T+0.25≦Ceq≦0.0004T+0.45 It satisfies the above. Here, Ceq is defined by the following formula (1) and is an index of hardenability due to contained elements. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15...(1) In the formula (1), each element symbol represents the content (mass%) of the corresponding element, and if the corresponding element is not contained, it is set to 0.
[0056] In the present invention, in order to obtain a desired high-strength structure, it is necessary to control the cooling rate according to the plate thickness T of a certain steel plate and the amount of alloy added according to the plate thickness T. If Ceq is less than (0.0004T+0.25), the required strength cannot be obtained. On the other hand, if Ceq is greater than (0.0004T+0.45), the strength becomes too high at the surface of the steel plate, where the cooling rate is faster than at the center of the plate thickness, and the low-temperature impact toughness becomes low. For this reason, 0.0004T+0.25≦Ceq≦0.0004T+0.45 It is preferable that the above formula is satisfied. More preferably, the formula is as follows: 0.0004T+0.27≦Ceq≦0.0004T+0.43 It is.
[0057] [Steel plate properties] Here, the characteristics of the steel plate used in the welded joint according to the present invention will be described. Dislocation density ρ(m -2 ) is 4.0×10 14 m -2 The dislocation density ρ(m -2 ) refers to the dislocation length per unit volume present in a metal crystal. The reason for specifying the position 1 mm below the surface of the base material (i.e. "1 mm below the surface of the steel plate") is from the perspective of the bending workability of the steel plate. The bending workability of a steel plate is determined by the ductility of the surface layer structure of the steel plate. When the dislocation density of the surface layer structure increases due to processing strain during hot rolling, the deformation limit of the surface layer structure decreases, and bending workability decreases. For this reason, the dislocation density 1 mm below the surface of the steel plate is set to 4.0 × 10 14 m -2 In addition, since the steel structure usually inevitably contains dislocations, the above dislocation density was set to 1.0 × 10 11 m -2 Therefore, the dislocation density is preferably 1.0×10 11 m -2More preferably, it is 3.0×10 14 m -2 The following is the result.
[0058] It is also preferable that the average crystal grain size at a position 1 mm below the surface of the base material is 15.0 μm or less, and the average crystal grain size at the center position of the plate thickness of the base material is 20.0 μm or less.
[0059] The average grain size refers to the average of all grains at a position 1 mm below the surface of the steel sheet and at the center of the thickness of the sheet, when the region surrounded by the boundary with a crystal orientation difference of 15° or more is regarded as a grain, and can be measured by the method described in the examples described later. The finer the grain size of the surface layer structure of the steel sheet, the more the toughness of the surface layer of the steel sheet is improved. In order to obtain this effect, it is preferable that the average grain size at a position 1 mm below the surface of the steel sheet is 15.0 μm or less. More preferably, the average grain size at a position 1 mm below the surface of the steel sheet is 13.0 μm or less. Furthermore, the finer the grain size of the steel structure at the center of the thickness of the steel sheet, the more the toughness at the center of the thickness of the steel sheet is improved. In order to obtain this effect, it is preferable that the average grain size at the center of the thickness of the steel sheet is 20.0 μm or less. More preferably, the average grain size at a position 1 mm below the surface of the steel sheet is 15.0 μm or less. Here, in the present invention, "1 mm below the surface of the steel sheet" refers to a depth position of 1 mm in the thickness direction from the surface of the steel sheet. The "plate thickness center position" refers to the 1 / 2 position of the plate thickness.
[0060] [Steel plate manufacturing method] Next, a method for manufacturing the above steel sheet will be described. The steel plate to which the present invention is directed is obtained by heating, hot rolling, and cooling a slab (steel material) having the above-mentioned composition. After the cooling, an optional tempering process can be performed. Various preferable conditions are explained below. However, the manufacturing method is not limited to a specific method, and it is sufficient if it includes the above-mentioned steps.
[0061] In the following description of the manufacturing method, the temperature indicated in "°C" refers to the surface temperature of the slab or steel plate unless otherwise specified. The surface temperature can be measured, for example, by a radiation thermometer.
[0062] In the present invention, the method for producing the slab is not particularly limited, and any of the known methods for producing the slab, such as a converter, an electric furnace, a vacuum melting furnace, etc., is suitable. The slab is produced to the desired dimensions, for example, by a continuous casting method. The molten steel may further be subjected to secondary refining, such as ladle refining.
[0063] ·Heating conditions As described above, it is preferable to heat the manufactured slab to a temperature of 1000 to 1200 ° C. If the heating temperature of the slab is less than 1000 ° C., the coarse NbC precipitated inside the slab during slab casting does not redissolve and remains. As a result, the effect of increasing the temperature of the non-recrystallization temperature range by the dissolved Nb and the fine NbC reprecipitated during hot rolling cannot be obtained. Accordingly, the effect of refining the crystal grains by the controlled rolling is reduced, and the toughness is reduced. On the other hand, if the heating temperature of the slab exceeds 1200 ° C., the grain size at the start of hot rolling becomes coarse due to the grain growth of austenite, and the grain size of the final structure after hot rolling also becomes coarse accordingly, and the toughness is reduced. Therefore, the heating temperature of the slab is preferably 1000 to 1200 ° C. The heating temperature of the slab is more preferably 1030 ° C. or more, and further preferably 1170 ° C. or less.
[0064] Hot rolling conditions Next, the heated slab is preferably hot-rolled. As described above, in the present invention, the dislocation density and average grain size at a position 1 mm below the steel sheet surface, and the average grain size at the center of the sheet thickness are important. In order to obtain various properties, it is preferable to roll the slab under the following hot rolling conditions.
[0065] Here, the temperature range exceeding (8250[Nb]+770°C) at a position 1 mm below the steel plate surface or at the center of the plate thickness is referred to as the recrystallization temperature range. 3The temperature range in which the temperature reaches the center of the thickness direction of the steel plate is called the non-recrystallization temperature range. The temperature at the center of the thickness direction of the steel plate can be obtained, for example, by measuring the temperature distribution in the cross section of the steel plate by heat transfer analysis and correcting the result by the surface temperature of the steel plate. Note that the above-mentioned [Nb] represents the content (mass%) of the element in the chemical composition of the above-mentioned steel plate.
[0066] First, the temperature of the steel sheet at a position 1 mm below the surface was measured using Ar 3 Cool to below the temperature, then reheat to Ac 3 Next, for a position 1 mm below the surface of the steel plate, the temperature of the steel plate at a position 1 mm below the surface of the steel plate is (8250[Nb]+770℃)~Ar 3 The reduction ratio in the temperature range of 100°C is 25% or more. After that, the steel sheet temperature at a position 1 mm below the surface of the steel sheet is 3 The total reduction in the temperature range below this temperature is 15% or less.
[0067] The surface layer of the heated slab is temporarily heated with Ar during hot rolling. 3 By cooling the steel sheet to below the temperature, the austenite is transformed into a low-temperature structure such as ferrite. The steel sheet surface is then cooled to Ac 3 By heating the steel sheet to a temperature equal to or higher than this temperature, the steel sheet is retransformed to an austenite structure, forming a fine austenite structure on the surface layer of the steel sheet.
[0068] The cooling method in the hot rolling process may be, for example, water cooling, air cooling, or the like, and any method may be used as long as the desired temperature can be controlled. 3 Cooling was performed by water to below the temperature, and the temperature 1 mm below the steel plate surface was Ar 3 The residence time at or below the temperature is preferably 5 seconds or more and preferably 300 seconds or less. Reheating after cooling is performed by holding the steel sheet in the air, and the holding time is preferably 30 seconds or more and preferably 600 seconds or less.
[0069] Next, the steel sheet surface is in the non-recrystallization temperature range (8250[Nb]+770℃)~Ar 3By applying a reduction of 25% or more in the temperature range of 0.1 to 100° C., processing strain is introduced into the austenite in the surface layer of the steel sheet. This acts as a transformation nucleus during final cooling, resulting in a fine structure with good toughness. Preferably, the reduction rate in this temperature range is 30% or more. From the viewpoint of rolling efficiency, the reduction rate in this temperature range is preferably 80% or less, and even more preferably 70% or less.
[0070] There is no particular upper limit on the number of passes in this temperature range. In addition, as long as the above-mentioned rolling reduction condition is satisfied, the rolling may be performed, for example, in a plurality of passes.
[0071] The temperature of the steel plate surface is Ar 3 If the total reduction rate exceeds 15% in the temperature range below the Ar temperature, processing strain is introduced into the ferrite and pearlite structures in the steel sheet surface where transformation is completed, resulting in a decrease in ductility and deterioration of bending workability. 3 It is preferable that the total rolling reduction in the temperature range below this temperature be 15% or less, and more preferably, the total rolling reduction in this temperature range be 6% or less.
[0072] By controlling the structure through the above-mentioned rolling conditions for the steel sheet surface layer, it is possible to give the steel sheet surface layer a structure having a low dislocation density, a small crystal grain size, and excellent bending workability and toughness.
[0073] Next, the steel plate temperature at the center of the plate thickness is set to (8250[Nb]+770℃) or less, Ar 3 It is advisable to apply reduction so that the total reduction in the temperature range above this temperature is 25% or more.
[0074] While the heated slab is hot-rolled under the rolling conditions of the steel plate surface as described above, the center of the thickness of the steel plate is in the non-recrystallization temperature range (8250[Nb]+770℃)~Ar 3A reduction of 25% or more is applied in the temperature range of 0°C to 100°C. This introduces processing strain into the austenite at the center of the plate thickness. This acts as a transformation nucleus during final cooling, resulting in a microstructure with good toughness. For this reason, it is preferable to set the total reduction rate to 25% or more in the temperature range where the steel plate center temperature is below (8250[Nb]+770°C). More preferably, the total reduction rate in this temperature range is 30% or more. From the viewpoint of rolling efficiency, the total reduction rate in this temperature range is preferably 80% or less, and even more preferably 70% or less.
[0075] In addition, the thickness center position of the steel plate is Ar 3 If the temperature is below the Ar temperature, the ferrite that has formed will be subjected to processing strain, and the toughness will decrease. 3 It is preferable to set the temperature at or above this level.
[0076] In the present invention, the temperature ranges may overlap within the above-mentioned rolling conditions in the two types of rolling, "rolling on the steel sheet surface layer" and "rolling on the sheet thickness center position". In this case, the reduction amounts in the overlapping temperature ranges are integrated as the reduction amounts for the "steel sheet surface layer" and the "sheet thickness center position", and the integrated reduction amounts should be within the ranges of the rolling conditions.
[0077] Here, the total reduction in the recrystallization temperature range at the surface layer and the center of the plate thickness is calculated as follows in the temperature range exceeding (8250[Nb]+770℃): Total reduction = (r0-r1) / r0×100(%). Note that r0 is the plate thickness at the start of the first rolling, and r1 is the plate thickness after the final rolling. Also, Ar 3 Temperature, Ac 3 The temperature can be determined by a Formastor test or the like.
[0078] By controlling the structure through the above-mentioned rolling conditions at the center position of the thickness of the steel plate, the center position of the steel plate can have a structure with small crystal grain size and excellent toughness.
[0079] Cooling conditions After the above-mentioned hot rolling, the obtained steel plate is cooled. In the cooling, the average cooling rate in the temperature range of 700 to 550 °C at the center of the thickness of the steel plate is 2500 × T -1.7 The cooling is performed at a rate of 0.4 °C / sec or more. Examples of the cooling method include water cooling in which water is sprayed from a nozzle at a large flow rate. In the present invention, it is preferable to perform the cooling operation (treatment) on both sides of the steel sheet so that both sides of the steel sheet are cooled under the same conditions.
[0080] The average cooling rate at the center of thickness after hot rolling between 700 and 550°C is 2500×T -1.7 If the cooling rate is less than 2500×T / sec, the required strength targeted by the present invention cannot be obtained due to insufficient cooling rate in the temperature range where transformation from austenite to a low-temperature transformation structure occurs. In addition, coarse ferrite is generated, resulting in a decrease in toughness. Therefore, the average cooling rate in the temperature range of 700 to 550°C at the center of the plate thickness should be 2500×T -1.7 ° C. / sec or more is preferable.
[0081] In the present invention, after the cooling, tempering can be performed as necessary to further improve the strength and toughness. In this case, the steel sheet is tempered at a tempering temperature of 650°C or less after cooling. If the tempering temperature is higher than 650°C, significant softening may occur and the necessary strength may not be ensured. Therefore, it is preferable to set the tempering temperature to 650°C or less. On the other hand, the lower limit of the tempering temperature is not particularly limited, but it is preferable to set it to 200°C or more. The tempering time can be appropriately adjusted. The tempering temperature here refers to the temperature of the steel sheet surface.
[0082] [Chemical composition of weld metal] Next, the chemical composition of the weld metal of the weld joint of the present invention will be described. Note that "%" regarding the chemical composition means "mass %" unless otherwise specified.
[0083] [Basic composition of weld metal] The basic chemical composition of the weld metal of the weld joint according to the present invention is as follows. It is preferable that the weld metal has a chemical composition containing C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, Cu: 0.001 to 2.000%, Ni: 0.001 to 2.500%, Cr: 0.001 to 1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less, with the balance being Fe and unavoidable impurities.
[0084] The reason why the chemical composition of the weld metal in the present invention is specified as above will now be explained. Each composition can be added (contained) to the weld metal from either the steel plate or the wire, which is the welding material.
[0085] [C: 0.04~0.14%] C is an element that has the effect of increasing the strength of the weld metal by solid solution strengthening, and also contributes to strengthening the austenite grain boundary. If the C content is less than 0.04%, the grain boundary strength of the austenite decreases, and the strength targeted by the present invention may not be obtained. On the other hand, if the C content exceeds 0.14%, the occurrence of weld cracks is promoted, and the low-temperature impact toughness of the weld metal may also decrease. Therefore, the C content is preferably 0.04 to 0.14%. The C content is more preferably 0.05 to 0.12%.
[0086] [Si: 0.03~0.70%] Silicon acts as a deoxidizer and has the effect of increasing the viscosity of the weld metal and stably maintaining the bead shape. To obtain such an effect, the Si content is preferably 0.03% or more. However, if the Si content exceeds 0.70%, there is a possibility that the low-temperature impact toughness of the weld metal may decrease. In addition, silicon segregates during solidification and generates a liquid phase at the solidification cell interface, which may decrease the weld crack resistance. Therefore, the Si content is preferably 0.03 to 0.70%. The Si content is more preferably 0.04 to 0.60%.
[0087] [Mn: 0.30~2.50%] Mn is an element that can improve the hardenability and strength of the weld metal at low cost. To obtain this effect, it is preferable to contain 0.30% or more of Mn. On the other hand, if the Mn content exceeds 2.50%, Mn segregation occurs during solidification, inducing hot cracking, which may result in a decrease in weldability. Therefore, the Mn content is preferably 0.30 to 2.50%. The Mn content is more preferably 0.50 to 2.20%.
[0088] [P:0.030% or less] P is an element that has a large effect of embrittling grain boundaries, and if contained in a large amount, it reduces the low-temperature impact toughness of the weld metal and may segregate at the interface during solidification, inducing hot cracking. Therefore, the P content is preferably 0.030% or less. Furthermore, the P content is more preferably 0.025% or less. On the other hand, since the lower the P content, the more preferable it is, the lower limit of the P content is not particularly limited and may be 0%. However, P is an element that is inevitably contained in the weld metal as an impurity, and excessively reducing the P content leads to an increase in costs, so the P content is preferably 0.001% or more.
[0089] [S:0.020% or less] Since S reduces the low-temperature impact toughness of the weld metal and may segregate at the interface during solidification, inducing hot cracking, the S content is preferably 0.020% or less. Furthermore, the S content is more preferably 0.010% or less. On the other hand, since the lower the S content, the more preferable it is, the lower limit of the S content is not particularly limited and may be 0%. However, S is an element that is inevitably contained in the weld metal as an impurity, and excessively reducing the S content leads to an increase in costs, so the S content is preferably 0.0001% or more.
[0090] [Nb: 0.001~0.100%] Nb is a carbide-forming element, and contributes to improving the strength of the weld metal by precipitating carbides. Nb also contributes to suppressing the occurrence of hot cracks by precipitating carbides at the solidification cell interface of the weld metal. In order to obtain this effect, the Nb content is preferably 0.001% or more. On the other hand, if the Nb content exceeds 0.100%, the carbides are coarsened and become the starting point of fracture, which may lead to a decrease in cryogenic impact toughness. Therefore, the Nb content is preferably 0.001 to 0.100%. The Nb content is more preferably 0.005 to 0.075%. Furthermore, the Nb content is particularly preferably 0.005 to 0.050%.
[0091] [Al: 0.001~0.100%] Al acts as a deoxidizer, increases the viscosity of the molten metal, and has an important effect of stably maintaining the bead shape. In order to obtain this effect, the Al content is preferably 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the weld metal decreases, and as a result, the ductility and toughness may decrease. Furthermore, if the viscosity of the weld metal becomes too high, the bead may not spread, and defects such as poor fusion may increase. Therefore, the Al content is preferably 0.001 to 0.100%. The Al content is more preferably 0.005 to 0.080%.
[0092] [Cu:0.001~2.000%] Cu is an element that can improve the strength of the weld metal without significantly deteriorating the toughness of the weld metal. To obtain this effect, the Cu content is preferably 0.001% or more. On the other hand, if the Cu content is greater than 2.000%, it may segregate during solidification and induce hot cracking. Therefore, when Cu is contained, the Cu content is preferably 2.000% or less. The Cu content is more preferably 0.005 to 1.500%. The Cu content is further preferably 0.005 to 1.000%, and even more preferably 0.005 to 0.500%.
[0093] [Ni:0.001~2.500%] Ni is an element that has the effect of increasing the hardenability of the weld metal and improving its toughness. To obtain this effect, the Ni content is preferably 0.001% or more. However, Ni is an expensive element, and a content of more than 2.500% is economically disadvantageous. Therefore, when Ni is contained, the Ni content is preferably 2.500% or less. The Ni content is more preferably 0.010 to 2.000%. The Ni content is further preferably 0.010 to 1.500%, and even more preferably 0.010 to 1.000%.
[0094] [Cr:0.001~1.500%] Cr is an element that can improve the hardenability of the weld metal, thereby improving the strength of the weld metal. To obtain this effect, the Cr content is preferably 0.001% or more. On the other hand, if the Cr content exceeds 1.500%, the weldability may decrease. In addition, Cr carbides may be generated, which may lead to a decrease in low-temperature impact toughness. Therefore, when Cr is contained, the Cr content is preferably 1.500% or less. The Cr content is more preferably 0.010 to 1.200%, and further preferably 0.010 to 1.000%.
[0095] [Mo:0.001~1.000%] Mo is an element that can improve the hardenability of the weld metal, thereby improving the strength of the weld metal. To obtain this effect, the Mo content is preferably 0.001% or more. On the other hand, if the Mo content exceeds 1.000%, the weldability may decrease. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. More preferably, the Mo content is 0.010 to 0.800%.
[0096] [Ti: 0.001~0.100%] Ti is an element that can precipitate as fine carbonitrides in the weld metal and improve the strength of the weld metal. To obtain this effect, the Ti content is preferably 0.001% or more. On the other hand, if the Ti content exceeds 0.100%, the cleanliness of the weld metal structure decreases, and as a result, there is a possibility that the ductility and toughness decrease. Therefore, when Ti is contained, the Ti content is preferably 0.100% or less. More preferably, the Ti content is 0.005 to 0.080%.
[0097] [V:0.001~0.300%] V is an element that can improve the hardenability of the weld metal and can improve the strength of the weld metal by forming carbonitrides. To obtain this effect, the V content is preferably 0.001% or more. On the other hand, if the V content exceeds 0.300%, the weldability may decrease. Therefore, when V is contained, the V content is preferably 0.300% or less. The V content is more preferably 0.005 to 0.250%. The V content is further preferably 0.005 to 0.150%, and even more preferably 0.005 to 0.100%.
[0098] [B: 0.001~0.020%] B is an element that has the effect of improving the hardenability by adding a very small amount, thereby improving the strength of the weld metal. In order to obtain this effect, the B content is preferably 0.001% or more. On the other hand, if the B content exceeds 0.020%, the weldability may decrease. Therefore, when B is contained, the B content is preferably 0.020% or less. More preferably, the B content is 0.005 to 0.018%.
[0099] [O:0.050% or less] Since O is an element that reduces ductility and toughness, the O content is preferably 0.050% or less. On the other hand, since the lower the O content, the more preferable it is, the lower limit of the O content is not particularly limited and may be 0%. However, since O is an element that is inevitably contained in the weld metal as an impurity, and excessive reduction in O content leads to an increase in costs, the O content is preferably 0.0005% or more.
[0100] [N:0.010% or less] Since N is an element that reduces ductility and toughness, the N content is preferably 0.010% or less. On the other hand, since the lower the N content, the better, the lower limit of the N content is not particularly limited and may be 0%. However, since N is an element that is inevitably contained in the weld metal as an impurity, excessive reduction in N content leads to an increase in costs, so the N content is preferably 0.0005% or more.
[0101] [Optional composition of weld metal] The weld metal of the present invention can obtain the characteristics targeted by the present invention by using the basic composition described above. However, for the purpose of further improving strength and weldability (specifically, toughness of the welded portion, welding workability, etc.), the weld metal may contain the following optional compositions as necessary in addition to the basic composition described above.
[0102] One or more selected from the group consisting of W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less. W, Ca, Mg, and REM are compositions that can be contained arbitrarily, so the contents of these elements may be 0%.
[0103] [W:0.500% or less] W is an element that can improve the hardenability of the weld metal, thereby improving the strength of the weld metal. On the other hand, if the W content exceeds 0.500%, the weldability may decrease. Therefore, when W is contained, the W content is preferably 0.500% or less. The W content is preferably 0.001% or more. More preferably, the W content is 0.001 to 0.300%.
[0104] [Ca:0.0200% or less] Ca is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Ca content exceeds 0.0200%, the cleanliness decreases and the toughness of the weld metal may be impaired. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. More preferably, the Ca content is 0.0001 to 0.0180%. Further preferably, the Ca content is 0.0001 to 0.0100%.
[0105] [Mg:0.0200% or less] Mg is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Mg content exceeds 0.0200%, the effect of adding Mg becomes saturated and an effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when Mg is contained, the Mg content is preferably 0.0200% or less. More preferably, the Mg content is 0.0001 to 0.0180%. Further preferably, the Mg content is 0.0001 to 0.0150%.
[0106] [REM:0.0500% or less] REM (rare earth metal) is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the REM content exceeds 0.0500%, the effect of adding REM becomes saturated and an effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when REM is contained, the REM content is preferably 0.0500% or less. More preferably, the REM content is 0.0001 to 0.0450%.
[0107] [Remainder of weld metal composition] The remainder of the weld metal of the present invention, other than the above chemical composition, is Fe and inevitable impurities. Incidentally, inevitable impurities refer to components that are mixed in from the welding wire, steel sheet, surrounding atmosphere, etc. during the welding process and are not intentionally included. Examples of inevitable impurities include H, Zn, Re, Co, Sb, Bi, etc., and a total of 0.0100% or less is acceptable. In addition, elements other than these may be contained as long as the above basic composition and optional composition are satisfied, and such embodiments are also included in the technical scope of the present invention.
[0108] [Mechanical properties of weld metal] Here, preferred mechanical properties of the welded joint according to the present invention will be described. It is preferable that the weld metal having the above-mentioned chemical composition and produced in accordance with the JIS Z 3111 standard has a room temperature yield strength (0.2% proof stress) of 325 MPa or more and a tensile strength of 520 MPa or more in a tensile test. The welded joint preferably has a tensile strength of 520 MPa or more at room temperature. In the present invention, "room temperature" refers to 25.0°C.
[0109] In addition, the absorbed energy (vE -40 ) is preferably 30 J or more. If it is less than 30 J, the toughness of the structure including the joint may be reduced and fracture may occur more easily.
[0110] [Manufacturing method for welded joints] Next, a method for manufacturing a welded joint according to the present invention will be described, that is, a method for manufacturing a welded joint formed by gas-shielded arc welding the above-mentioned steel plates will be described. First, prepare a steel plate having the above-mentioned chemical composition and a thickness of 50 mm or more. Then, perform groove processing so that the prepared steel plates form a predetermined groove shape. The groove shape to be formed does not need to be particularly limited, and examples of the groove shape that can be used for welded structures include normal V grooves, L grooves, X grooves, and K grooves.
[0111] Next, the grooved steel plates are welded together to form a weld metal having multiple layers, preferably three or more layers, with one pass per layer, to form a weld joint. If welding is performed with one or two layers of weld metal, the heat generated during welding does not spread uniformly within the groove, inducing welding defects. The welding wire used is not particularly limited as long as it can form a weld metal having the desired characteristics.
[0112] [Gas shielded arc welding method] The welding method used in the present invention is a multi-electrode gas-shielded arc welding method that can stably obtain narrow gap welded joints that have weld metal free of welding defects and have high strength and excellent low-temperature impact toughness.
[0113] As the welding conditions for the gas-shielded arc welding method of the present invention, it is necessary to properly control the welding conditions described below with reference to the drawings.
[0114] [Welding conditions (basic conditions and optional conditions)] (1) Basic welding conditions (a) Multi-layer welding is performed using three or more electrodes. (b) The tips of the welding wires of the first electrode and the second electrode are arranged on different parallel welding lines (see FIG. 4). (c) One of the first electrode and the second electrode is set as a wire negative (positive polarity), and the other is set as a wire positive (reverse polarity). (d) The distance a (mm) between the tips of the welding wires of the first electrode and the second electrode is 5 to 16 mm (see FIG. 4). (e) The angle α of the straight line connecting the tips of the welding wires of the first electrode and the second electrode with respect to the perpendicular direction to the welding line is 60° or less (see FIG. 4). (f) A welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode serving as the negative wire (positive polarity). (2) Optional welding conditions (g) The inclination angle Φ of the tip of each of the first and second electrodes toward the groove surface with respect to the perpendicular direction of the weld line is 0° to 15° (see FIG. 3). (h) The distance d (mm) between the side end of the tip of the welding wire of each of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm (see Figs. 2 and 3). (i) Each welding wire is curved in advance to have a radius of curvature in the range of 150 to 300 mm. (j) The third and subsequent electrodes are placed in the center of the groove behind the first and second electrodes (see Figures 4 and 5). (k) Shielding gas containing 60% or more by volume of CO 2 A gas containing gas is used.
[0115] [Individual welding conditions] The above welding conditions will be explained in more detail below.
[0116] (a) Multi-layer welding with three or more electrodes In narrow-gap multi-pass welding, when one pass is performed per layer, heat tends to concentrate at the center of the groove with one electrode, resulting in insufficient melting of the steel material at the groove surface, and defects due to poor fusion (cold lap) and spatter and slag entrapment on the groove surface are likely to occur. In particular, the temperature of the steel material is low in the first layer welding, and the melting depth is small, so defects due to poor fusion are likely to occur. In addition, from the viewpoint of improving welding efficiency, it is advantageous to use multi-electrode welding with three or more electrodes. Note that, from the viewpoint of welding efficiency, four or less electrodes are preferable. Three electrodes are most preferable.
[0117] (b) Electrode placement The welding wire tips of the first electrode and the second electrode are arranged on different parallel welding lines. Fig. 4 shows an example of the arrangement of the welding wire tips in the case of three electrodes, and Fig. 5 shows an example of the arrangement of the welding wire tips in the case of four electrodes. As shown in these figures, the welding wire tip 5c of the first electrode 5 and the welding wire tip 6c of the second electrode 6 are arranged on different parallel welding lines 9. In this way, the arcs emitted from the welding wires of the first electrode and the second electrode spread in the width direction of the weld metal being formed.
[0118] (c) Electrode polarity One of the first electrode and the second electrode is wire negative (positive polarity), and the other is wire positive (negative polarity). If the first electrode and the second electrode have the same polarity, for example, if both the first electrode and the second electrode are wire positive, the arcs of each electrode will be inward due to the electromagnetic force of attraction, and heat will be concentrated in the center of the groove, and sufficient melting will not be obtained on the groove surface. However, if the first electrode and the second electrode have different polarities and the tips of the welding wires described in (b) above are arranged on different lines parallel to the welding line, the magnetic fields due to the welding currents of each electrode will generate strong outward electromagnetic forces, and the arcs will repel each other. As a result, it is possible to obtain a sufficient melting depth on the groove surface. From this result, in the present invention, the polarities of the first electrode and the second electrode are one of wire negative (positive polarity) and the other of wire positive (negative polarity).
[0119] (d) Distance between 1st and 2nd electrode tips a: 5~16mm Distance a between the tips of welding wires 5b and 6b supplied from power feed tips 5a and 6a at the tips of the welding torches of first electrode 5 and second electrode 6 (hereinafter simply referred to as "first-second electrode tip distance") needs to be controlled within the range of 5 to 16 mm. Note that distance a between the tips of welding wires 5b and 6b here refers to the distance between the centers of welding wire tips 5c and 6c of each electrode, as shown in FIG. 4.
[0120] If the distance a between the first and second electrode tips is less than 5 mm, the current (electrons) flowing between the electrodes reduces the heat of the arc itself, and sufficient melting of the groove surface is not achieved. On the other hand, if the distance a exceeds 16 mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance, and the arc repulsive force sufficient to overcome the inward electromagnetic force generated by the current flowing through the groove surface is not obtained, so the arcs face inward and heat is concentrated in the center of the groove. As a result, sufficient melting of the groove surface is not achieved.
[0121] Furthermore, in narrow gap welding, suppressing welding defects caused by spatter adhesion to the groove surface is an issue, but by controlling the above-mentioned welding conditions (b), (c), and (d), the spatter is absorbed into the molten metal. This suppresses the adhesion of spatter to the groove surface, making it possible to obtain a sound weld.
[0122] From the above, the distance a between the first and second electrode tips is controlled to be in the range of 5 to 16 mm. However, in order to obtain a deeper and more stable melting depth at the groove face by stronger arc repulsion, it is preferable to control the distance a between the first and second electrode tips to be in the range of 5 to 8 mm.
[0123] (e) 1st-2nd electrode tip arrangement angle α: 60° or less In the narrow gap gas shielded arc welding method of the present invention, the melting of the groove surface is ensured by utilizing the repulsion of the arc. Here, in FIG. 4, the angle α of the straight line connecting the welding wire tips 5c and 6c of the first electrode 5 and the second electrode 6 with respect to the perpendicular direction of the welding line 9 (hereinafter, also simply referred to as the "first-second electrode tip arrangement angle") will be described. If this angle α exceeds 60°, a sufficient repulsive force of the arc cannot be obtained, and sufficient melting cannot be obtained at the groove surface. Therefore, the angle α is limited to 60° or less. Preferably, the angle α is 45° or less. The angle α may be 0° (i.e., parallel to the perpendicular direction of the welding line). More preferably, the angle α is 25° or more.
[0124] (f) REM content of the welding wire used for the positive electrode REM (rare earth elements) are effective elements for refining inclusions during steelmaking and casting, and for improving the toughness of weld metal during welding. Furthermore, when welding is performed by supplying a welding wire containing REM to an electrode with a negative (positive) polarity, it is possible to refine droplets and stabilize transfer. This refinement of droplet transfer suppresses the generation of spatters, and enables stable gas shielded arc welding even with a positive polarity. For this reason, in the present invention, a steel wire containing 0.015 to 0.100 mass% of REM (rare earth elements) is supplied to an electrode with a positive polarity. Note that elements other than REM (rare earth elements) are intended to contain appropriate amounts that are normally contained according to the grade (steel type) of the welding wire, as specified in JIS Z 3312. If the content of REM (rare earth elements) is less than 0.015 mass%, the above-mentioned refinement of droplets and stabilization of transfer cannot be achieved. On the other hand, if the REM content exceeds 0.100 mass%, cracks will occur during the wire manufacturing process, making it difficult to manufacture the welding wire. For this reason, the REM (rare earth element) content is limited to the range of 0.015 to 0.100 mass%. The REM content is preferably 0.025 to 0.050 mass%.
[0125] In addition, welding wire for gas shielded arc welding is generally manufactured in a diameter range of 0.6 to 2.0 mm, but when welding with the same current, generally, the thinner the wire diameter, the higher the deposition rate due to Joule heat. Therefore, in order to realize highly efficient welding work, it is preferable to select a relatively thin wire diameter. On the other hand, if the wire diameter is too thin, the wire will soften due to Joule heat, making the welding unstable. Therefore, it is preferable that the diameter of the welding wire used is in the range of 1.0 to 1.6 mm.
[0126] The above welding conditions are the basic welding conditions for gas-shielded arc welding of the present invention, and by performing welding under the above-mentioned conditions, it is possible to produce a narrow gap welded joint that is free of welding defects, has high strength, and has excellent low-temperature impact toughness.
[0127] Furthermore, in the present invention, by satisfying the optional welding conditions described below in addition to the basic welding conditions described above, it becomes possible to more stably obtain narrow gap welded joints that are free of welding defects, have high strength, and have excellent low-temperature impact toughness.
[0128] (g) Tilt angle of power supply tip Φ: 0°~15° The arc has a directivity and tends to point in the direction in which the tip of the welding wire of the electrode points. In order to effectively utilize the directivity of the arc in melting the groove surface, it is advantageous to point the direction of the welding wire tip toward the groove surface, and the direction in which the tip of the welding wire points varies greatly depending on the feed angle of the welding wire supplied from the power feed tip at the tip of the electrode. As shown in FIG. 3, the feed angle of the welding wires 5b and 6b of the first electrode 5 and the second electrode 6 with respect to the bottom of the weld metal 2 is the same as the inclination of the tips of the power feed tips 5a and 6a of the electrodes. Therefore, by adjusting the inclination angle Φ of the tip of the power feed tip toward the groove surface 4 (hereinafter also referred to as the "inclination angle Φ of the power feed tip"), the feed angle of the welding wire supplied from each power feed tip with respect to the bottom of the weld metal can be controlled. Here, the bottom of the weld metal refers to the bottom of each weld layer of the weld metal, and refers to the vicinity of the boundary with the previous weld layer.
[0129] When the inclination angle Φ of the power feed tips of the first and second electrodes is less than 0° (i.e., when the inclination angle Φ is inclined away from the groove surface), the current flows through a path with less resistance. As a result, the arc creeps up the wire electrode (i.e., also called "arc creeping"), making it difficult to maintain the targeted melting at the groove surface, especially the bottom. On the other hand, when the inclination angle Φ of the power feed tip exceeds 15°, the arc faces too far toward the groove surface, resulting in a convex weld bead shape, and melting by the arc in the first layer and subsequent welding layers becomes insufficient, which makes it easy for welding defects to occur. For this reason, the inclination angle Φ of the power feed tip is preferably set in the range of 0° to 15°. More preferably, the inclination angle Φ of the power feed tip is 5° to 12°.
[0130] (h) Distance d between the tip of the welding wire and the groove surface: 0.5 to 3.0 mm In order to obtain a deeper and more stable fusion depth at the bottom of the weld metal, it is preferable that the distance d between the side ends of the welding wire tips 5c and 6c of the first electrode 5 and the second electrode 6 and the groove surface 4 of the steel plate is 0.5 to 3.0 mm, as shown in Figures 2 and 3. If the distance d is less than 0.5 mm, the arc will be generated not between the wire and the bottom of the weld metal but between the wire and the groove surface, and the previous weld layer and the groove surface will not be efficiently fused at the bottom of the weld metal.
[0131] On the other hand, if the distance d exceeds 3.0 mm, the arc will be away from the groove surface, and the groove surface will not be melted efficiently. More preferably, the distance d is in the range of 0.5 to 2.0 mm, and even more preferably, in the range of 0.5 to 1.0 mm. Note that the "side end of the tip of the welding wire" referred to here refers to the side end closest to the groove surface of the steel sheet to be melted by each electrode, and the distance d refers to the shortest distance between the side end and the groove surface 4.
[0132] (i) Curvature radius of the welding wire to be fed: 150 to 300 mm In the present invention, in order to control the feed angle (Φ) of the welding wires 5b, 6b supplied from the power feed tips at the tips of the welding torches of the first electrode 5 and the second electrode 6, power feed tips 5a, 6a with their tips inclined toward the groove surface are used as shown in Fig. 3. At this time, the welding wires 5b, 6b pass through the power feed tips with their tips inclined toward the groove surface, and in order to pass through them more smoothly, it is preferable to curve the supplied welding wire in advance using a so-called three-point roller or the like (not shown).
[0133] The radius of curvature when bending in advance is preferably 150 to 300 mm. If the radius of curvature is less than 150 mm, the wire feed resistance increases, the welding wire cannot be stably fed, and it becomes difficult to maintain an arc. On the other hand, if the radius of curvature of the welding wire exceeds 300 mm, there is no effect in reducing the wire feed resistance when the tip of the power feed tip is bent, so the welding wire cannot be stably fed, and it becomes difficult to maintain an arc. Therefore, the radius of curvature of the welding wire fed to the power feed tips of the first electrode and the second electrode is preferably 150 to 300 mm. More preferably, the radius of curvature of the welding wire is 175 to 275 mm.
[0134] (j) Arrangement of the third and subsequent electrodes To avoid the risk of hot cracking, it is effective to position the welding wire tips (7c and 8c) of the third and subsequent electrodes in the center of the groove behind the welding wire tips (5c and 6c) of the first and second electrodes, as shown in Figures 4 and 5. This also makes it possible to further reduce the number of layers, greatly reducing the risk of stacking defects in multi-layer welding.
[0135] The distance b between the welding wire tip 6c of the second electrode and the welding wire tip 7c of the third electrode is preferably in the range of 10 to 100 mm, more preferably 10 to 60 mm, even more preferably 10 to 40 mm, and most preferably 10 to 25 mm. Furthermore, the distance c between the welding wire tip 7c of the third electrode and the welding wire tip 8c of the fourth electrode is also preferably in the range of 10 to 100 mm, more preferably 10 to 60 mm, even more preferably 10 to 40 mm, and most preferably 10 to 25 mm.
[0136] Furthermore, the polarity of the third electrode and thereafter is not particularly limited, and may be either wire negative (positive polarity) or wire positive (negative polarity).
[0137] (k) Shielding gas composition The oxygen content in the weld metal is also greatly affected by the shielding gas composition.2 It is preferable to use a gas containing 60% by volume or more of gas, with the remainder being an inert gas such as Ar. More preferably, 2 The gas is 100% by volume.
[0138] The nozzles for supplying the shielding gas are preferably arranged as follows.
[0139] In order to ensure good shielding in gas-shielded arc welding, which is the object of the present invention, suppress the inclusion of nitrogen from the atmosphere, and reduce the deterioration of the low-temperature toughness of the weld metal and the occurrence of welding defects, a shielding gas supply nozzle 11 is positioned in front of the welding direction of the first electrode 5 in the groove.
[0140] A detailed description will be given based on Figs. 7 and 8. Fig. 7 is a side cross-sectional view showing a schematic arrangement of the shielding gas supply nozzle and the electrodes, and Fig. 8 is a plan view showing the same arrangement as Fig. 7 from above. These figures show an example of three-electrode welding in which a first electrode 5, a second electrode 6, and a third electrode 7 are arranged. A shielding gas supply nozzle 11 is arranged in front of the first electrode 5 in the welding direction, and a gas discharge port 11a from which the shielding gas is discharged is directed toward the first electrode 5. During welding, the shielding gas supply nozzle 11 moves in conjunction with the three electrodes along the welding direction, and arc welding is performed while supplying the shielding gas.
[0141] The cross-sectional area N of the gas discharge port 11a is 100 mm 2 ~350mm 2 It is preferable that the range is 100%.
[0142] The cross-sectional area N of the gas discharge port 11a is 100 mm 2 If the cross-sectional area N of the gas discharge port 11a is less than 350 mm, the area onto which the gas is blown becomes small, and the shielding performance becomes insufficient. 2 If the cross-sectional area exceeds 100 mm, the gas will disperse to areas other than the bottom of the groove, resulting in insufficient shielding. 2 ~350mm 2More preferably, the cross-sectional area N is 125 mm 2 ~300mm 2 It is.
[0143] Moreover, the supply flow rate Q of the shielding gas is preferably in the range of 35 L / min to 70 L / min.
[0144] If the supply flow rate Q of the shielding gas is less than 35 L / min, the amount of gas supplied to the molten pool 12 becomes insufficient, and the shielding performance deteriorates. On the other hand, if the supply flow rate Q of the shielding gas exceeds 70 L / min, the flow rate of the shielding gas becomes excessive, and the possibility of occurrence of welding defects increases. Therefore, the supply flow rate Q of the shielding gas is preferably 35 L / min to 70 L / min. This supply flow rate Q is more preferably 40 L / min to 65 L / min. Note that the flow rate of the shielding gas changes depending on the combination of the supply flow rate Q of the shielding gas and the cross-sectional area N of the gas outlet, but the flow rate is preferably 2 m / s to 7 m / s.
[0145] The preferred cross-sectional shape of the tip of the gas discharge port is as follows.
[0146] 7 and 8 show only the tip portion of the shielding gas supply nozzle 11, but the cross-sectional shape of the tip portion of the gas discharge port 11a is not particularly limited. However, since a nozzle with a larger cross-sectional area can be inserted into the groove when the cross-sectional shape of the tip portion is rectangular rather than circular, it is preferable that the cross-sectional shape of the tip portion of the gas discharge port be rectangular.
[0147] The angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is preferably 40° to 80° (see FIG. 7).
[0148] If the angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is less than 40°, the shielding gas does not reach the third electrode 7 sufficiently, resulting in insufficient shielding. On the other hand, if the angle X exceeds 80°, the gas is dispersed to areas other than the bottom of the groove, resulting in insufficient shielding. Therefore, the angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is preferably 40° to 80°. This angle X is more preferably 45° to 75°.
[0149] Furthermore, the distance Y between the tip of the gas discharge port 11a and the welding wire tip 5c of the first electrode 5 is preferably 40 mm or less (see Figs. 7 and 8). The distance between the gas discharge port 11a and the electrodes is also effective for shielding. That is, if the distance Y between the tip of the gas discharge port 11a (specifically, the part closest to the electrode) and the welding wire tip 5c of the first electrode 5 exceeds 40 mm, the shielding gas does not reach the entire electrode sufficiently, and the gas is dispersed to areas other than the bottom of the groove, resulting in insufficient shielding. Therefore, the distance Y is preferably 40 mm or less. The distance Y is more preferably 5 mm to 35 mm.
[0150] [Other welding conditions] The welding conditions other than those mentioned above are not particularly specified, but may be, for example, a welding current of 280 to 360 A, a welding voltage of 32 to 37 V, a welding speed of 30 to 90 (cm / min), a wire extension length of 15 to 30 (mm), and a welding heat input per pass of 10 to 50 (kJ / cm).
[0151] In addition, when multi-layer welding is performed using three electrodes, the following welding current conditions are more suitable. First, the current value I1 of the first electrode and the current value I2 of the second electrode are set to a range of 280A to 360A. If the current values I1 and I2 of the first and second electrodes are less than 280A, the groove face cannot be melted sufficiently, and there is a high possibility of incomplete fusion. On the other hand, if the current values I1 and I2 exceed 360A, the height of the weld bead increases and the bead becomes elongated, increasing the risk of hot cracking. Therefore, the range of the current value I1 of the first electrode and the current value I2 of the second electrode is preferably 280A to 360A, and more preferably 280A to 340A.
[0152] Next, the current value I3 of the third electrode is controlled for each layer of the multi-layer welding based on the relationship with the width of the weld bead of each layer, thereby suppressing hot cracks that occur in each weld layer, which is the object of the present invention. i is set to a range that satisfies the following formula (2). I3 i ≦30×G i-1 -10 ··· (2) Here, I3 i : Current value of the third electrode of the i-th layer [A], G i-1 is the width [mm] of the weld bead formed by welding the layer before the i-th layer (i.e. the i-1th layer), and i is a natural number greater than or equal to 2.
[0153] Current value I3 of the third electrode i When the weld bead width G becomes larger, the height of the weld bead becomes larger and the bead becomes longer, which increases the risk of hot cracking. i is the width G of the weld bead formed by welding one layer before (i.e., the i-1th layer) i-1 As the number of layers increases, the width of the weld bead also increases due to the influence of the current value of the third electrode. Based on this, the relationship between the width of the weld bead and the current value of the third electrode was examined, and a favorable range was found, from which the above formula (2) was derived. In other words, if the range satisfies formula (2), the formation of a vertically elongated weld bead is suppressed, and the excellent effect of preventing hot cracks can be obtained. EXAMPLES
[0154] The present invention will be further described below with reference to examples. However, the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.
[0155] First, molten steel having the chemical composition shown in Table 1 was produced, and steel material (slab) was manufactured by continuous casting or the like. This composition in Table 1 becomes the chemical composition of the steel plate that will become the base material. Note that the "-" column in Table 1 indicates that the element is not intentionally added, and includes not only cases where the element is not contained (0%), but also cases where the element is unavoidably contained.
[0156] [Table 1]
[0157] Next, the obtained slab was subjected to the steps of heating, hot rolling, and cooling in order to obtain steel plates having thicknesses T (mm) shown in Tables 2-1 and 2-2. The rolling start temperature in the hot rolling step was in the range of 990 to 1140°C at the surface layer of the steel plate, and the rolling finish temperature was in the range of 670 to 830°C at the surface layer of the steel plate. The above steel plate temperatures were measured by an emissivity thermometer for the surface layer temperature and by attaching a thermocouple to the center of the thickness of the steel plate. Cooling after hot rolling was performed by spraying water at a large flow rate from the front and back sides of the steel plate.
[0158] On the other hand, molten steel was melted in a vacuum melting furnace and cast to obtain a steel ingot, which was heated to 1200°C and then hot and cold worked to produce a 1.2 mmΦ gas shielded arc welding wire. In addition to YGW18, G 59J A 1 was used as the wire steel type (grade).
[0159] Next, the above steel plate was subjected to groove processing to obtain the groove shapes shown in Tables 2-1 and 2-2. Note that the groove shapes V (groove) in Tables 2-1 and 2-2 are the shapes shown in FIG. 6(a), and X (groove) are the shapes shown in FIG. 6(b). Furthermore, gas-shielded arc welding was performed using the welding wire obtained above to form a weld metal in the above-mentioned groove, and a welded joint was obtained. The layering conditions at this time (specifically, whether one pass or two passes per layer was performed) are also shown.
[0160] [Table 2-1]
[0161] [Table 2-2]
[0162] The specific welding conditions for the gas shielded arc welding were as follows: no preheating, downward welding, welding current: 180-390 A, welding voltage: 22-38 V, welding speed: 40-120 cm / min, interpass temperature: 200° C. or less. The number of weld metal layers was 3 or more.
[0163] Tables 3-1 to 3-4 show the welding conditions for each electrode in gas shielded arc welding. The welding electrodes were arranged as shown in Figures 4 and 5. Here, the distance b between the welding wire tips of the second and third electrodes was 18 mm, and the distance c between the welding wire tips of the third and fourth electrodes was 10 mm. The "2-4 passes per layer" shown in the lamination conditions for joint No. 35 in Table 3-3 specifically means 1 pass from the first to second layers, 2 passes from the third to eighth layers, 3 passes from the ninth to fourteenth layers, and 4 passes from the fifteenth to the final layer. In the "Polarity" column in Tables 3-1 and 3-3, "positive polarity" is written for negative wire, and "reverse polarity" is written for positive wire.
[0164] [Table 3-1]
[0165] [Table 3-2]
[0166] [Table 3-3]
[0167] [Table 3-4]
[0168] [Evaluation of weld metal shape] Vertical cross-sectional macros were taken and observed at positions 1 / 4D, 2 / 4D, and 3 / 4D in the weld line direction of the welded joint. Here, D above refers to the length from one end of the weld line to the other end. The 1 / 4D position represents a position 1 / 4 of D moved in the welding direction from one end of the weld line, and similarly, the 2 / 4D position is the center position of the weld line, and the 3 / 4D position represents a position 3 / 4 of D moved in the welding direction.
[0169] Then, the cross-sectional area A (mm 2 ) was measured and divided by the number of weld layers p (layers), to obtain the ratio [A / p] of the cross-sectional area A of the weld metal to the number of weld layers p.
[0170] The distance between the top and bottom of each layer of the weld metal was measured to determine the height H (mm) of each layer of the weld metal, and the width of the weld metal at the center line of each height H (i.e., the distance between the fusion lines) was measured to determine the width W (mm) of the weld metal. The ratio [H / W] was calculated for each layer, and the maximum ratio [H / W] for the entire weld metal was recorded. Furthermore, as mentioned above, a narrow groove means that the groove angle is 20° or less and the maximum groove width between the base metals is 50% or less of the plate thickness T, so the ratio [Wmax / T] of the maximum groove width Wmax to the plate thickness T was calculated.
[0171] [Measurement of dislocation density in steel sheets] Samples were taken from each steel plate at the center in the longitudinal and transverse directions, 1 mm below the surface of the steel plate, to be the evaluation surface. The surfaces of the samples were mirror-polished by mechanical polishing and electrolytic polishing, and the dislocation density ρ(m -2 ) was evaluated. (Reference 1) GKWilliams and WHHall:Acta Metall.,1(1953),22
[0172] [Average grain size] Similarly to the above, samples were taken so that the evaluation surfaces were 1 mm below the surface of the steel plate at the center of the longitudinal and width directions of each steel plate and the longitudinal cross section of the steel plate at the center of the plate thickness. The surfaces of the obtained samples were mirror-polished with colloidal silica finish and measured by EBSP (electron backscatter diffraction) under the following conditions. The measurement area was 300 μm × 400 μm, and the measurement step size was 1 μm. From the obtained crystal orientation map, the circle equivalent diameter of the structure surrounded by high-angle grain boundaries where the crystal orientation difference with adjacent crystal grains is 15° or more was obtained, and the average value of the circle equivalent diameter in the measurement area was taken as the average crystal grain size. Note that the surface layer and the center of the plate thickness of the steel plate of the present invention were mainly composed of bainite and pseudo-polygonal ferrite.
[0173] [Evaluation of welding defects] In addition, radiographic testing was performed on the obtained welded joints in accordance with JIS Z 3104 to evaluate the presence or absence of weld defects. Weld defects were judged as falling under JIS Z3104 Class 1 with a "○", Class 2 with a "△", and Class 3 or 4 with an "×". Class 1 or 2 was deemed to be pass, and Class 3 or 4 was deemed to be fail.
[0174] [Evaluation of mechanical properties of weld metal] From the welded joints thus obtained, tensile test pieces (parallel diameter 6 mm) and Charpy impact test pieces (V notch) were taken from the welded metal and tensile tests and impact tests were carried out in accordance with the provisions of JIS Z 3111. Tensile tests were carried out on three pieces each at room temperature (normal temperature), and the average values obtained (0.2% proof stress, tensile strength) were regarded as the tensile properties of the welded metal of the welded joint. Charpy impact tests were also carried out on three pieces each in the same way, and the absorbed energy (vE -40 ) was obtained, and the average value was regarded as the cryogenic impact toughness of the weld metal of the welded joint. A value of 30 J or more was evaluated as "○", and a value less than this was evaluated as "×".
[0175] In addition, tensile tests were also conducted at room temperature on the welded joints in accordance with the provisions of JIS Z 3121. The test pieces were taken perpendicular to the weld axis so that the weld axis was in the center of the parallel length of the test piece, and the thickness was the full thickness of the welded joint, which was a No. 1A test piece. Three test pieces were taken, and the individual yield stress values were all 325 MPa or more, and were evaluated as "○", while the average was 325 MPa or more but some individual values did not reach 325 MPa, and those less than that were evaluated as "×". The individual tensile strength values were all 520 MPa or more, and were evaluated as "○", while the average was 520 MPa or more but some individual values did not reach 520 MPa, and those less than that were evaluated as "×".
[0176] Furthermore, Charpy impact tests were also conducted on the heat-affected zones of welded joints in accordance with the provisions of JIS Z 3128. The V-notch direction of the test specimen was perpendicular to the steel plate surface, and the test specimens were taken from the center of the plate thickness, the center of the weld metal, on the fusion line, and 1 mm from the fusion line. Three test specimens were taken, and the evaluation was carried out as follows: if all individual values were 30J or more, they were marked as "○", if the average was 30J or more but some individual values did not reach 30J, they were marked as "△", and if they were less than that, they were marked as "×".
[0177] As described above, the target values in the present invention are a room temperature yield strength (0.2% proof stress) of the weld metal of 325 MPa or more, a tensile strength of the weld metal of 520 MPa or more, and a room temperature tensile strength of the welded joint of 520 MPa or more. Furthermore, the absorbed energy (vE -40 ) is 30J or more.
[0178] [Welding efficiency] The wire diameter (mm) used during welding and the wire feed speed (mm / min) during welding were measured, and the deposition amount (g) divided by the unit welding time (min) was recorded as the deposition efficiency (g / min). If this value was 250g / min or more, it was evaluated as "○", and if it was less than that, it was evaluated as "×".
[0179] Of the above measurement and evaluation results, the results of the chemical composition of the weld metal are shown in Tables 4-1 and 4-2, and the results of the properties of the weld metal and steel plate, the performance of the welded joints, etc. are shown in Tables 5-1 and 5-2.
[0180] [Table 4-1]
[0181] [Table 4-2]
[0182] [Table 5-1]
[0183] [Table 5-2]
[0184] All of the examples of the present invention have sound welded joints with no welding defects such as hot cracks or incomplete fusion. Furthermore, all of the examples of the present invention have a room temperature yield strength (0.2% proof stress) of the weld metal of 325 MPa or more, a tensile strength of 520 MPa or more, and a room temperature tensile strength of the welded joint of 520 MPa or more. In addition, the absorbed energy (vE -40 ) is 30 J or more, and the weld metal has both high strength and excellent low-temperature impact toughness.
[0185] On the other hand, in the examples that are outside the preferred range of the steel plate and welded weld metal of the present invention, hot cracking occurs, lowering hot cracking resistance, or insufficient fusion occurs. In addition, the room temperature yield strength (0.2% proof stress) and tensile strength of the weld metal, the room temperature tensile strength of the welded joint, and the absorbed energy (vE -40 ) and other mechanical properties were at slightly lower levels.
[0186] Although joints No. 5-2, No. 22-2, and No. 22-3 may be economically disadvantageous due to the REM content of the welding wire or weld metal, they showed good results in the characteristics and performance shown in Tables 5-1 and 5-2. Also, joint No. 18-2 may be economically disadvantageous due to the shielding gas composition, but it showed good results in the characteristics and performance shown in Tables 5-1 and 5-2. [Explanation of symbols]
[0187] 1 steel plate 2. Weld metal 3. Welding Line 4 Bevel surface 5 1st electrode 6 Second electrode 7 Third electrode 8 4th electrode 5a, 6a, 7a, 8a: Power supply chips for the first electrode, the second electrode, the third electrode, and the fourth electrode 5b, 6b, 7b, 8b Welding wires for the first electrode, second electrode, third electrode, and fourth electrode 5c, 6c, 7c, 8c Welding wire tips of the first electrode, second electrode, third electrode, and fourth electrode 9 Welding Lines 10 Backing material 11 Shielding gas supply nozzle 11a Gas outlet 12 Molten pool T plate thickness A Cross-sectional area of the entire weld metal L i Welding layer (i = 1 to p layers), (L 1 :First layer, L P : outermost layer) W i Width of weld layer (i=1 to p layers) a) Distance between tip 5c of the welding wire of the first electrode and tip 6c of the welding wire of the second electrode b Distance between tip 6c of the welding wire of the second electrode and tip 7c of the welding wire of the third electrode c) Distance between tip 7c of the welding wire of the third electrode and tip 8c of the welding wire of the fourth electrode d Distance between the tip end 5c or 6c of the welding wire and the groove surface 4 α The angle of the straight line connecting the tips of the welding wires of the first and second electrodes with respect to the perpendicular direction of the welding line θ Bevel angle, θ f Surface groove angle, θ b Back bevel angle Φ Tilt angle of the tip of the power supply tip G Gap T f Surface thickness, T m Intermediate thickness, T b Back Thickness
Claims
1. In a method for manufacturing a welded joint by gas shielded arc welding of steel plates, The thickness T (mm) of the steel plate is 50 mm or more, The weld metal consists of multiple layers with one pass per layer. The cross-sectional area A (mm 2 The ratio [A / p] of the number of weld layers p (layers) to the number of layers p (layers) is 120.0 mm 2 Below / layer, The ratio [H / W] of the height H (mm) to the width W (mm) of each layer in the weld metal is 1.00 or less, The gas shielded arc welding is a multi-electrode welding having three or more electrodes, The tips of the welding wires of the first electrode and the second electrode are disposed on different parallel welding lines; One of the first electrode and the second electrode is a wire negative (positive polarity), and the other is a wire positive (reverse polarity), The distance a (mm) between the welding wire tips of the first electrode and the second electrode is 5 to 16 mm, an angle α of a straight line connecting the welding wire tips of the first electrode and the second electrode with respect to a perpendicular direction to the welding line is 60° or less; A welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode that is the negative wire (positive polarity). A method for manufacturing welded joints by gas-shielded arc welding of steel plates.
2. The inclination angle Φ of the tip of each of the first electrode and the second electrode toward the groove surface side with respect to the perpendicular direction of the weld line is 0° to 15°, A distance d (mm) between a side end portion of each welding wire tip of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm, Each of the welding wires is a welding wire that is bent in advance to have a radius of curvature in the range of 150 to 300 mm, A third electrode and subsequent electrodes are disposed at the center of the groove behind the first electrode and the second electrode, Shielding gas containing 60% or more by volume of CO 2Using gas containing gas, A method for producing a welded joint by gas shielded arc welding of the steel plate according to claim 1.
3. The chemical composition of the steel sheet is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001-0.100%, O: 0.0100% or less, and N: 0.0100% or less; The balance is Fe and unavoidable impurities, Ceq and plate thickness (T) defined by the following formula (1) 0.0004T+0.25≦Ceq≦0.0004T+0.45 and having a chemical composition that satisfies the above. The dislocation density ρ at a position 1 mm below the surface of the steel plate is 4.0 × 10 14 m -2 is as follows: The average crystal grain size at a position 1 mm below the surface of the steel plate is 15.0 μm or less, and the average crystal grain size at the center position of the plate thickness is 20.0 μm or less; A method for producing a welded joint by gas-shielded arc welding of the steel plate according to claim 1 or 2. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15...(1) However, each element symbol in the above formula (1) represents the content (mass%) of the corresponding element, and if the corresponding element is not contained, it is set to 0.
4. The chemical composition of the steel sheet further comprises, in mass%, Cu: 2.000% or less, Ni: 2.500% or less, Cr: 1.500% or less, Mo: 1.000% or less, Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 3, comprising one or more selected from the group consisting of:
5. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001 to 2.500%, Cr: 0.001-1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less; The balance is Fe and inevitable impurities. A method for producing a welded joint by gas-shielded arc welding of the steel plate according to claim 1 or 2.
6. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001 to 2.500%, Cr: 0.001-1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less; The balance is Fe and inevitable impurities. A method for producing a welded joint by gas shielded arc welding of the steel plate according to claim 3.
7. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001 to 2.500%, Cr: 0.001-1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001-0.020%, O: 0.050% or less, and N: 0.010% or less; The balance is Fe and inevitable impurities. A method for producing a welded joint by gas shielded arc welding of steel plates according to claim 4.
8. The chemical composition of the weld metal further comprises, in mass %, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 5, comprising one or more selected from the group consisting of:
9. The chemical composition of the weld metal further comprises, in mass %, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 6, comprising one or more selected from the group consisting of:
10. The chemical composition of the weld metal further comprises, in mass %, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 7, comprising one or more selected from the group consisting of:
Citation Information
Patent Citations
Shallow penetration submerged arc welding method
JP1980084278A
Three electrode two layer submerged arc welding of thick plate
JP1996257752A
Method and apparatus for submerged arc welding
JP2011200920A
Narrow groove gas-shield arc-welding method
JP2015223605A
Thick steel sheet, and method for producing thick steel sheet
WO2021054344A1