Low-reflection film, optical sensing kit using same, and low-reflection molded body
A low-reflection film with a laminated structure addresses the issue of high specular gloss in conventional resin materials by ensuring low surface reflectance and gloss across wide angles, improving imaging and detection accuracy in optical sensing kits.
Patent Information
- Application Number
- JP2021508931
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-06
AI Technical Summary
Conventional resin materials used in optical sensing kits for vehicles exhibit high specular gloss on the wide-angle side, leading to unwanted light reflection that degrades image capture and detection accuracy, despite having low gloss on the low-angle side, which is unsuitable for high-precision imaging and sensing.
A low-reflection film with a laminated structure comprising a first resin layer containing a binder resin and organic particles with a specific particle diameter, achieving low surface reflectance and gloss across a wide angle range, optimized to reduce specular gloss at various angles.
The film effectively suppresses light reflection, enhancing imaging and detection accuracy of optical sensors by providing a matte finish that maintains low gloss and reflectance regardless of the viewing angle, suitable for high-precision photography and sensing in vehicles.
Smart Images

Figure 0007558927000005 
Figure 0007558927000006 
Figure 0007558927000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel low-reflection film having low surface reflectance and surface gloss on the wide-angle side, and to an optical sensing kit and a low-reflection molded article using the same. [Background technology]
[0002] Due to the remarkable progress made in sensing technology in recent years, the introduction of advanced sensing technology is being considered for various moving bodies (hereinafter sometimes referred to as "mobile vehicles") such as automobiles, trains, steam trains, ships, cargo ships, aircraft, spacecraft, rockets, transportation equipment, and vehicles.
[0003] For example, automobiles are being developed that are equipped with optical sensors, such as camera modules with image pickup elements and infrared sensors, inside the vehicle to detect obstacles (e.g., other vehicles, pedestrians, guardrails, houses, etc.) that exist ahead of the vehicle. These optical sensors capture images of the outside of the vehicle from inside the vehicle, for example, through the window glass, or detect visible light or infrared rays outside the vehicle from inside the vehicle.
[0004] Meanwhile, inside the interior of a moving vehicle in which such optical sensors are installed, there are numerous interior components installed, such as a dashboard, roof trim, sun visors, switch panels, decorative panels, steering wheels, seats, etc., and the optical sensors may also be provided with plastic accessories such as camera hoods and lens hoods (hereinafter, these may be collectively referred to as "interior parts").
[0005] In recent years, these interior parts have often been made of molded bodies made of resins such as thermoplastic resins and thermoplastic elastomers, which are lightweight and highly durable, multi-layer laminates using these resins, or nonwoven fabrics and skin materials, etc. For the interior parts of mobile vehicles, many resin materials have been proposed that suppress the gloss of the product surface and impart a matte finish from the standpoint of safety or from the standpoint of design, such as obtaining a subdued matte texture that gives a sense of luxury (see Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 06-057007 [Patent Document 2] Japanese Patent Application Publication No. 07-314519 [Patent Document 3] JP 2002-220562 A [Patent Document 4] JP 2003-020384 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the sensing technology using the optical sensors described above, if light (unwanted light) reflected from the surface of the interior parts is incident on the optical sensors, halation, lens flare, ghosting, etc. will occur, significantly degrading the captured image or significantly reducing the detection accuracy of the sensing. In contrast, the technologies of Patent Documents 1 to 4 are merely technologies for imparting a matte appearance, and the surface glossiness thereof remains high (60 degree specular glossiness of 9 to 35% (Patent Document 1), 60 degree specular glossiness of 10 to 30% (Patent Document 2), 60 degree specular glossiness of 7.3 to 15.2% (Patent Document 3), 45 degree specular glossiness of 4.7 to 18% (Patent Document 4). Therefore, there is a demand for the development of materials with lower surface glossiness.
[0008] In particular, in the use of optical sensing kits for moving vehicles, there is a trend that extremely high-precision photographing and sensing will be required in the future. Here, in low-gloss resin materials used for this type of use, the intensity of specular gloss on the wide-angle side (incident angle and reflection angle of 45° or more) is usually relatively large compared to the specular gloss on the low-angle side (incident angle and reflection angle of less than 45°). Therefore, the low-gloss resin materials of Patent Documents 1 to 4 not only have high values of 45-degree specular gloss and 60-degree specular gloss, but also have higher values of specular gloss on the wide-angle side, for example, 75-degree specular gloss and 85-degree specular gloss. For example, the surface reflectance and surface gloss of a commercially available light-shielding film (KIMOTO, product name: Carbon Feather X6B) are as follows. Therefore, when such a resin material of the conventional technology is used for an optical sensing kit, the influence of reflected light on the wide-angle side still remains large, making it difficult to perform more accurate photographing and sensing. [Table 1]
[0009] The present invention has been made in view of the above problems. That is, an object of the present invention is to provide a novel low-reflection film having a low surface reflectance and surface gloss in a wide angle range, and an optical sensing kit and a low-reflection molded body using the same. [Means for solving the problem]
[0010] In order to solve the above problems, the inventors conducted extensive research into the surface optical properties of low-reflection films suitable for more accurate photography, sensing, and the like, and as a result, discovered a new low-reflection film and low-reflection molded body that have low surface reflectance and surface gloss in a wide-angle range, thereby completing the present invention.
[0011] That is, the present invention provides various specific embodiments as shown below. [1] At least a first resin layer is provided, and the first resin layer is made of a binder resin and a binder having an average particle diameter D of 2 to 20 μm. 50and the reflectance and gloss of the surface on the first resin layer side satisfy the following relationships: (1) 70 degree regular reflectance: 0.0% or more and 2.5% or less (wavelength 550nm) (2) 60 degree specular gloss: 0.0% to 6.0% 75 degree specular gloss: 0.0% to 6.0% 85 degree specular gloss: 0.0% to 6.0% (3) The sum of the 20° specular gloss, 45° specular gloss, 60° specular gloss, 75° specular gloss, and 85° specular gloss is 7.5% or less.
[0012] [2] The organic resin particles have an average particle diameter D of 5 to 20 μm. 50 The low reflection film according to [1], [3] The low reflection film according to [1] or [2], wherein the content ratio of the organic resin particles to the binder resin is 0.6 to 2.5. [4] The thickness of the first resin layer is equal to or larger than the average particle diameter D of the organic resin particles contained in the first resin layer. 50 The low reflection film according to any one of [1] to [3], wherein the reflectance is 0.5 to 8.0 times that of the reflectance. [5] The low reflection film according to any one of [1] to [4], which has an optical density of 0.5 or more. [6] The low reflection film according to any one of [1] to [5], wherein the first resin layer further contains carbon black.
[0013] [7] The low reflection film according to any one of [1] to [6], which has a laminated structure including at least the first resin layer and an adhesive layer in this order. [8] The low reflection film according to any one of [1] to [7], which has a laminated structure including at least the first resin layer and a base film in this order. [9] The low reflection film according to any one of [1] to [8], which has a laminated structure including at least the first resin layer, a base film, and an adhesive layer in this order.
[10] The low reflection film according to any one of [1] to [9], which has a laminated structure including at least the first resin layer, a base film, a second resin layer, and an adhesive layer in this order.
[11] The low reflection film according to any one of [7] to
[10] , wherein the adhesive layer contains one or more adhesives selected from the group consisting of rubber-based adhesives, acrylic-based adhesives, olefin-based adhesives, silicone-based adhesives, and urethane-based adhesives.
[12] The low reflection film according to any one of [1] to
[11] , wherein the first resin layer has a surface roughness Ra of 0.8 to 4.0 μm.
[0014]
[13] An optical sensor arranged in a vehicle interior and capturing an image of the exterior of the vehicle or detecting visible light or infrared light outside the vehicle through a window transparent to visible light or infrared light; and a low-reflection film covering a surface of an interior part arranged in the vehicle interior and reducing reflected light of external light on the surface to improve the imaging accuracy and / or detection accuracy of the optical sensor. The low-reflection film comprises at least a first resin layer, and the first resin layer is made of a binder resin and a polymer having an average particle diameter D of 2 to 20 μm. 50 and the reflectance and gloss of the surface on the first resin layer side satisfy the following relationships: (1) 70 degree regular reflectance: 0.0% or more and 2.5% or less (wavelength 550nm) (2) 60 degree specular gloss: 0.0% to 6.0% 75 degree specular gloss: 0.0% to 6.0% 85 degree specular gloss: 0.0% to 6.0% (3) The sum of the 20° specular gloss, 45° specular gloss, 60° specular gloss, 75° specular gloss, and 85° specular gloss is 7.5% or less.
[14] The organic resin particles have an average particle diameter D of 5 to 20 μm. 50 The optical sensing kit according to
[13] , comprising:
[15] The optical sensing kit according to
[13] or
[14] , wherein the interior part is one or more selected from the group consisting of a resin molded body, a multilayer laminate using a resin molded body, a nonwoven fabric, and a skin material. Here, it is preferable that the low reflection film used in the optical sensing kit described in the above
[13] or
[14] further has one or more of the technical features described in the above [3] to
[12] .
[0015]
[16] A low-reflection molding for covering the surface of an article, the low-reflection molding comprising a binder resin and a granular material having an average particle diameter D of 2 to 20 μm. 50 and wherein the reflectance and gloss of at least one surface of the low-reflection molded body satisfy the following relationship: (1) 70 degree regular reflectance: 0.0% or more and 2.5% or less (wavelength 550nm) (2) 60 degree specular gloss: 0.0% to 6.0% 75 degree specular gloss: 0.0% to 6.0% 85 degree specular gloss: 0.0% to 6.0% (3) The sum of the 20° specular gloss, 45° specular gloss, 60° specular gloss, 75° specular gloss, and 85° specular gloss is 7.5% or less. Here, the low reflection molded body described in the above
[16] preferably further has one or more of the technical features of the above [3] to
[12] . Here, the first resin layer is to be read as the first resin layer, and the low reflection film is to be read as the low reflection molded body. Effect of the Invention
[0016] According to the present invention, a low-reflection film and a low-reflection molded body having a low surface reflectance and surface gloss in a wide angle region can be realized, and a new material that did not exist in the past can be provided. By using this low-reflection film or low-reflection molded body, for example, a matte-finished product having a low surface gloss even when viewed from the wide angle side can be realized, and by using the low-reflection film as a skin film for interior parts in optical sensing kit applications, deterioration or deterioration of the captured image and detection accuracy of optical sensors can be suppressed. Therefore, according to the present invention, a new material with excellent low reflectivity in a wide angle region can be realized, and high-precision photography and sensing can be realized in various moving vehicles such as automobiles, trains, steam trains, trains, ships, cargo ships, aircraft, spacecraft, rockets, transportation equipment, and vehicles. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a low reflection film 100 according to an embodiment. [Diagram 2] FIG. 11 is a schematic cross-sectional view showing a modified example of a low-reflection film 200. [Diagram 3] FIG. 11 is a schematic cross-sectional view showing a modified example of a low-reflection film 300. [Figure 4] FIG. 11 is a schematic cross-sectional view showing a modified low-reflection film 400. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. The positional relationships such as up, down, left and right are based on the positional relationships shown in the drawings unless otherwise specified. The dimensional ratios of the drawings are not limited to the ratios shown. However, the following embodiments are examples for explaining the present invention, and the present invention is not limited thereto. In this specification, for example, the expression of a numerical range such as "1 to 100" includes both the upper limit value "100" and the lower limit value "1". The same applies to the expression of other numerical ranges.
[0019] First embodiment FIG. 1 is a cross-sectional view showing a main part of a low reflection film 100 according to a first embodiment of the present invention. The low reflection film 100 includes a base film 11, a first resin layer 21 provided on one surface 11a of the base film 11, and an adhesive layer 31 provided on the other surface 11b of the base film 11. That is, the low reflection film 100 of this embodiment has a laminated structure (three-layer structure) in which the first resin layer 21, the base film 11, and the adhesive layer 31 are arranged at least in this order. In this laminated structure, the first resin layer 21 is disposed on the outermost surface of the front side, and the adhesive layer 31 is disposed on the outermost surface of the back side, and the first resin layer 21 and the adhesive layer 31 are disposed in a state of being exposed on the outermost surfaces of the front side and the back side, respectively. In addition, an arbitrary layer such as an antistatic layer or a protective layer may be provided on the surface of the first resin layer 21 as necessary.
[0020] Here, in this specification, "provided on one (the other) surface side of" means not only an embodiment in which the first resin layer 21 or the adhesive layer 31 is directly placed on the surface (e.g., surface 11a or surface 11b) of the base film 11 as in the present embodiment, but also an embodiment in which the first resin layer 21 or the adhesive layer 31 is disposed apart from the base film 11 with an arbitrary layer (e.g., a primer layer, an adhesive layer, etc.) not shown being interposed between the surface 11a of the base film 11 and the first resin layer 21, or between the surface 11b of the base film 11 and the adhesive layer 31. In addition, a laminated structure including at least the first resin layer 21 and the adhesive layer 31 means not only a structure in which only the first resin layer 21 and the adhesive layer 31 are directly laminated on the base film 11, but also a structure in which an arbitrary layer as described above is further provided between the layers of the three-layer structure.
[0021] The type of the base film 11 is not particularly limited as long as it can support the first resin layer 21 and the adhesive layer 31. From the viewpoints of dimensional stability, mechanical strength, and weight reduction, a synthetic resin film is preferably used. Specific examples of synthetic resin films include polyester films, ABS (acrylonitrile-butadiene-styrene) films, polyimide films, polyamide films, polyamideimide films, polystyrene films, and polycarbonate films. In addition, acrylic, nylon, polyolefins such as polyethylene and polypropylene, cellulose, polysulfone, polyphenylene sulfide, polyethersulfone, and polyetheretherketone films can also be used. Among these, polyester films and polyimide films are preferably used as the base film 11. In particular, uniaxially or biaxially stretched films, especially biaxially stretched polyester films, are particularly preferred because they have excellent mechanical strength and dimensional stability. In addition, polyimide films, polyamideimide films, and polyamide films are particularly preferred for heat-resistant applications, and polyimide films and polyamideimide films are most preferred. These may be used alone or in combination of two or more.
[0022] The thickness of the base film 11 can be appropriately set depending on the required performance and application, and is not particularly limited. From the viewpoint of weight reduction and thinning, the thickness of the base film 11 is preferably 0.5 μm or more and 250 μm or less, more preferably 1 μm or more and 100 μm or less, even more preferably 5 μm or more and 50 μm or less, and particularly preferably 10 μm or more and 30 μm or less. In addition, from the viewpoint of improving the adhesion to the first resin layer 21 and the adhesive layer 31, various known surface treatments such as anchor treatment and corona treatment can be performed on the surface of the base film 11 as necessary.
[0023] The appearance of the base film 11 may be transparent, semi-transparent, or opaque, and is not particularly limited, but it is preferable that the base film 11 has light-shielding properties. For example, foamed synthetic resin films such as foamed polyester films and synthetic resin films containing various pigments can be used. For example, a synthetic resin film containing one or more dark-colored pigments or dyes such as black, gray, purple, blue, brown, red, and green can be used to form a light-shielding film with high optical density. The pigments and dyes used here can be appropriately selected from those known in the art, and the type is not particularly limited. For example, black pigments include black resin particles, magnetite black, copper-iron-manganese black, titanium black, carbon black, and the like. Among these, black resin particles, titanium black, and carbon black are preferred because of their excellent hiding properties. These can be used alone or in combination of two or more. When the base film 11 contains a pigment or dye, the content ratio can be appropriately set according to the required performance and application, and is not particularly limited. From the viewpoints of dimensional stability, mechanical strength, weight reduction, etc., the total content of pigments and dyes is preferably 0.3 to 15 mass %, more preferably 0.4 to 12 mass %, and even more preferably 0.5 to 10 mass %, relative to the total amount of the base film 11.
[0024] The first resin layer 21 is made of a binder resin 22 and a granular material having an average particle diameter D 50 The first resin layer 21 is a resin layer containing at least organic resin particles 23 having the above-mentioned predetermined reflectance and glossiness. As a material for constituting the first resin layer 21, a material known in the art can be used, and the type is not particularly limited. By using a resin layer containing a binder resin and organic resin particles 23 dispersed in the binder resin in this way, the first resin layer 21 that satisfies the above-mentioned optical characteristics can be realized. This will be described in further detail below.
[0025] Examples of the binder resin 22 include thermoplastic resins or thermosetting resins such as poly(meth)acrylic acid resins, polyester resins, polyvinyl acetate resins, polyvinyl chloride resins, polyvinyl butyral resins, cellulose resins, polystyrene / polybutadiene resins, polyurethane resins, alkyd resins, acrylic resins, unsaturated polyester resins, epoxy ester resins, epoxy resins, epoxy acrylate resins, urethane acrylate resins, polyester acrylate resins, polyether acrylate resins, phenol resins, melamine resins, urea resins, and diallyl phthalate resins, but are not limited thereto. Thermoplastic elastomers, thermosetting elastomers, ultraviolet curing resins, and electron beam curing resins can also be used. These can be used alone or in combination of two or more. The binder resin 22 can be appropriately selected and used depending on the required performance and application. For example, in applications where heat resistance is required, thermosetting resins are preferred.
[0026] The content (total amount) of the binder resin 22 in the first resin layer 21 is not particularly limited and may be appropriately adjusted to a level necessary for film formation. From the viewpoint of realizing a first resin layer 21 having a better surface reflectance and surface glossiness, the content (total amount) of the binder resin 22 is preferably 5 to 65 mass % relative to the total amount of the first resin layer 21, more preferably 15 to 55 mass %, further preferably 20 to 50 mass %, and particularly preferably 25 to 45 mass %.
[0027] In order to impart the above-mentioned reflectance and glossiness, the first resin layer 21 of the low reflection film 100 of this embodiment contains relatively coarse organic resin particles 23. From the viewpoint of reproducibly obtaining the target reflectance and glossiness, the average particle diameter D 50 The thickness is preferably 2 to 20 μm, more preferably 4 to 20 μm, even more preferably 5 to 20 μm, still more preferably 6 to 15 μm, particularly preferably 7 to 14 μm, and most preferably 10 to 14 μm.
[0028] As the material of the organic resin particles 23, those known in the art can be used, and the type is not particularly limited. Specifically, resin particles such as polymethyl methacrylate, polystyrene, polyester, polyurethane, and rubber can be used, but are not particularly limited thereto. The appearance of the organic resin particles 23 may be transparent, semi-transparent, or opaque, and is not particularly limited thereto. The appearance of the organic resin particles 23 may be colorless, or may be colored. For example, by using colored organic resin particles colored in black, gray, purple, blue, brown, red, green, or the like, a light-shielding film with high optical density can be obtained. The organic resin particles 23 can be used alone or in combination of two or more kinds.
[0029] The content (total amount) of the organic resin particles 23 in the first resin layer 21 is not particularly limited as long as the above-mentioned surface reflectance and surface glossiness are obtained. From the viewpoint of realizing a first resin layer 21 having a better surface reflectance and surface glossiness, the content (total amount) of the organic resin particles 23 is preferably 35 to 95 mass % relative to the total amount of the first resin layer 21, more preferably 40 to 85 mass %, further preferably 45 to 80 mass %, and particularly preferably 50 to 75 mass %. At this time, the type of organic resin particles 23 used and the average particle diameter D 50 From the viewpoint of reproducibly achieving the above-mentioned preferred surface reflectance and surface glossiness, it is preferable to set the content of the organic resin particles 23 within the above range, taking into consideration the usage ratio of the binder resin 22. That is, the content ratio of the organic resin particles to the total mass of the binder resin in the first resin layer 21 is preferably 0.6 to 2.5, more preferably 0.7 to 2.3, and even more preferably 0.8 to 2.0.
[0030] The first resin layer 21 may contain inorganic particles 24 in addition to the organic resin particles 23. By using the inorganic particles 24 in combination, it is possible to further increase the light blocking property and further reduce the surface reflectance and surface glossiness. As the inorganic particles 24, various pigments and dyes known in the art can be used, and the type is not particularly limited. For example, kaolin, calcined kaolin, calcined clay, uncalcined clay, silica (e.g., natural silica, fused silica, amorphous silica, hollow silica, wet silica, synthetic silica, aerosil, etc.), aluminum compounds (e.g., boehmite, aluminum hydroxide, alumina, hydrotalcite, aluminum borate, aluminum nitride, etc.), magnesium compounds (e.g., magnesium aluminometasilicate, magnesium carbonate, magnesium oxide, magnesium hydroxide, etc.), calcium compounds (e.g., calcium carbonate, magnesium oxide, magnesium hydroxide, etc.), calcium carbonate, magnesium oxide, magnesium hydroxide, magnesium hydroxide, calcium carbonate, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, calcium carbonate, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, calcium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, calcium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, calcium hydroxide, calcium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, calcium hydroxide, calcium hydroxide, calcium hydroxide, calcium hydroxide, calcium hydroxide, calcium hydroxide, calcium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, magnesium hydroxide, calcium ... Examples of the black inorganic pigment include, but are not limited to, titanium oxide, zinc oxide, zirconium oxide, barium sulfate, zinc borate, barium metaborate, sodium borate, boron nitride, agglomerated boron nitride, silicon nitride, carbon nitride, strontium titanate, barium titanate, and zinc stannate. In addition, black inorganic pigments are preferably used from the viewpoint of improving light-shielding and hiding properties. Examples of the black inorganic pigment include, but are not limited to, black resin particles, magnetite black, copper-iron-manganese black, titanium black, carbon black, and aniline black. Among these, black inorganic pigments are preferably black resin particles, titanium black, carbon black, and aniline black, and more preferably carbon black and aniline black. On the other hand, in recent years, from the viewpoint of design, there has been an increase in popularity of luxurious, low-gloss, dark designs, and there is a demand for harmony with these designs.To meet such demands, hollow particles such as hollow silica can be used as the inorganic particles 24 to increase light scattering in the first resin layer 21 and reduce the surface reflectance of the first resin layer 21, particularly the surface reflectance in the wide-angle region, thereby realizing a darker, blacker first resin layer 21. These inorganic particles can be used alone or in combination of two or more types.
[0031] Carbon black includes oil furnace black, lamp black, channel black, gas furnace black, acetylene black, thermal black, ketjen black, etc., which are produced by various known methods, but the type is not particularly limited. Conductive carbon black is particularly preferably used from the viewpoint of imparting electrical conductivity to the first resin layer 21 and preventing static electricity from charging. Carbon black has a long history, and various grades of carbon black and carbon black dispersions are commercially available from, for example, Mitsubishi Chemical Corporation, Asahi Carbon Co., Ltd., Mikuni Color Co., Ltd., Resino Color Kogyo Co., Ltd., Cabot Corporation, DEGUSSA Corporation, etc., and may be appropriately selected from these depending on the required performance and application. The particle size of carbon black can be appropriately set depending on the required performance, etc., and is not particularly limited. The average particle diameter D of carbon black 50 In this specification, the average particle diameter D is preferably 0.01 to 2.0 μm, more preferably 0.05 to 1.0 μm, and further preferably 0.08 to 0.5 μm. 50 is the volume-based median diameter (D) measured using a laser diffraction particle size distribution analyzer (e.g., Shimadzu Corporation: SALD-7000, etc.). 50 )
[0032] When inorganic particles 24 are used, from the viewpoints of dispersibility, film-forming properties, handleability, light-shielding properties, matte properties, etc., and from the viewpoint of the blending balance with the above-mentioned binder resin 22 and organic resin particles 23, the content (total amount) of inorganic particles 24 is preferably 1 to 55 mass % relative to the total amount of first resin layer 21, more preferably 5 to 45 mass %, even more preferably 7 to 40 mass %, and particularly preferably 7 to 30 mass %.
[0033] The first resin layer 21 may contain various additives known in the art. Specific examples thereof include, but are not limited to, lubricants, conductive agents, flame retardants, antibacterial agents, antifungal agents, antioxidants, plasticizers, resin curing agents, curing accelerators, leveling agents, flow control agents, antifoaming agents, dispersants, and the like. Examples of lubricants include, but are not limited to, hydrocarbon-based lubricants such as polyethylene, paraffin, and wax; fatty acid-based lubricants such as stearic acid and 12-hydroxystearic acid; amide-based lubricants such as stearic acid amide, oleic acid amide, and erucic acid amide; ester-based lubricants such as butyl stearate and monoglyceride stearate; alcohol-based lubricants; solid lubricants such as metal soap, talc, and molybdenum disulfide; silicone resin particles; and fluororesin particles such as polytetrafluoroethylene wax and polyvinylidene fluoride. Among these, organic lubricants are particularly preferably used. When an ultraviolet-curable resin or an electron beam-curable resin is used as the binder resin, a sensitizer or an ultraviolet absorber, such as n-butylamine, triethylamine, or tri-n-butylphosphine, may be used. These may be used alone or in combination of two or more. The content of these is not particularly limited, but is generally preferably 0.01 to 5 mass% each in terms of solid content relative to the total resin components contained in the first resin layer 21.
[0034] The thickness T of the first resin layer 21 can be appropriately set according to the required performance and the application, and is not particularly limited. From the viewpoint of a balance between high optical density, light weight and thin film, the thickness T of the first resin layer 21 is preferably 0.1 μm or more, more preferably 0.2 μm or more, even more preferably 0.5 μm or more, particularly preferably 1.0 μm or more, and most preferably 4.0 μm or more, and the upper limit side is preferably 40 μm or less, more preferably 35 μm or less, even more preferably 30 μm or less, and particularly preferably 25 μm or less. Here, the thickness T of the first resin layer 21 is the maximum thickness when there are surface irregularities as shown in the figure. At this time, from the viewpoint of realizing the above-mentioned preferable surface reflectance and surface glossiness with good reproducibility, the average particle diameter D of the organic resin particles 23 used is set to 10 μm or more. 50 In consideration of the above, it is desirable to set the thickness T of the first resin layer 21 within the above range. 50 When t (μm) is used, the thickness T (μm) of the first resin layer 21 is preferably adjusted so that T / t is within the range of 0.5 to 8.0. Although it varies depending on the film formation method, generally, T / t is preferably 0.5 to 3.0, more preferably 0.6 to 2.5, even more preferably 0.9 to 2.4, particularly preferably 1.0 to 2.3, and most preferably 1.3 to 2.2. Depending on the coating method, T / t is preferably 1.5 or more, more preferably 2.0 or more, and even more preferably 3.0 or more, and the upper limit is preferably 8.0 or less, and more preferably 7.5 or less. If necessary, various known surface treatments such as anchor treatment and corona treatment can be performed on the surface of the first resin layer 21.
[0035] On the other hand, from the viewpoints of weight reduction, thinning, ease of handling, etc., the total thickness of the low-reflection film 100 is preferably 0.5 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and particularly preferably 25 μm or more, and the upper limit is preferably 500 μm or less, more preferably 400 μm or less, even more preferably 300 μm or less, and particularly preferably 250 μm or less.
[0036] From the viewpoint of providing high light-shielding properties as a light-shielding member, the optical density (OD) of the first resin layer 21 is preferably 0.5 or more, more preferably 1.0 or more, even more preferably 1.7 or more, and particularly preferably 2.0 or more. In this specification, the optical density (OD) is a value obtained by measurement using an optical densitometer (X-Rite361T: X-Rite Corporation) and an orthofilter in accordance with ISO 5-2.
[0037] Here, as described above, the low reflection film 100 of this embodiment has its surface shape adjusted to be uneven in order to reduce the surface reflectance and surface glossiness in the wide angle region. The surface roughness Ra of the surface on the first resin layer 21 side of the low reflection film 100 (the surface of the first resin layer 21 in this embodiment) can be appropriately set according to the required performance and application, and is not particularly limited. From the viewpoint of achieving a better surface reflectance and surface glossiness, and from the viewpoint of a balance between high optical density, weight reduction and thinning, it is preferably 0.8 to 4.0 μm, more preferably 1.0 to 3.6 μm, even more preferably 1.5 to 3.3 μm, and particularly preferably 2.0 to 3.0 μm. In this specification, the surface roughness Ra is a value measured in accordance with the measurement method of arithmetic mean roughness (Ra) of JIS-B0601 (2001). For example, it can be measured by a stylus surface roughness tester (SURFCOM 1500SD2-3DF: Tokyo Seimitsu Co., Ltd.).
[0038] As described above, the surface reflectance of the low reflection film 100 of this embodiment is adjusted to a 70 degree regular reflectance of 0.0% to 2.5% (wavelength 550 nm) on the surface of the low reflection film 100 on the first resin layer 21 side (the surface of the first resin layer 21 in this embodiment) in order to reduce the surface reflection in the wide angle region. From the viewpoint of realizing a higher matte finish and low surface reflection, the 70 degree regular reflectance is preferably 0.0% to 2.0% (wavelength 550 nm), more preferably 0.0% to 1.5% (wavelength 550 nm), even more preferably 0.0% to 1.0% (wavelength 550 nm), and particularly preferably 0.0% to 0.5% (wavelength 550 nm). In this specification, the 70-degree regular reflectance is a value obtained by measuring the regular reflectance (specular reflectance) (%) of the surface of the first resin layer 21 at an incident and receiving angle of 70° for light with a wavelength of 550 nm using a spectrophotometer (SolidSpec-3700: Shimadzu Corporation).
[0039] Furthermore, as described above, in order to reduce the specular gloss in the wide-angle range, the specular gloss of the surface of the low-reflection film 100 on the first resin layer 21 side (the surface of the first resin layer 21 in this embodiment) is adjusted so that the 60-degree specular gloss is 0.0% or more and 6.0% or less, the 75-degree specular gloss is 0.0% or more and 6.0% or less, and the 85-degree specular gloss is 0.0% or more and 6.0% or less. From the viewpoint of achieving higher matteness and lower gloss, the 60 degree specular gloss is preferably 0.0% or more and 4.0% or less, the 75 degree specular gloss is preferably 0.0% or more and 4.0% or less, and the 85 degree specular gloss is preferably 0.0% or more and 4.0% or less, and more preferably the 60 degree specular gloss is 0.0% or more and 3.0% or less, the 75 degree specular gloss is 0.0% or more and 3.0% or less, and the 85 degree specular gloss is more preferably 0.0% or more and 2.0% or less, the 75 degree specular gloss is 0.0% or more and 2.0% or less, and the 85 degree specular gloss is more preferably 0.0% or more and 2.0% or less.
[0040] In this case, from the viewpoint of realizing a wide range of low gloss from a low angle region to a wide angle region, and from the viewpoint of the balance of light blocking property, low gloss, low reflectivity, light absorption, etc., the specular gloss of the low reflection film 100 of this embodiment is preferably 7.5% or less, more preferably 6.0% or less, even more preferably 5.0% or less, particularly preferably 4.0% or less, and most preferably 3.0% or less, as a sum of the 20 ° specular gloss, 45 ° specular gloss, 60 ° specular gloss, 75 ° specular gloss, and 85 ° specular gloss. In this specification, the specular gloss is a value obtained by measuring the gloss (specular gloss) (%) of the surface of the first resin layer 21 at each of the specified incident and receiving angles (20 °, 45 °, 60 °, 75 °, 85 °) using a digital variable angle gloss meter (Gloss Meter VG7000: Nippon Denshoku Co., Ltd.) in accordance with JIS-Z8741:1997.
[0041] From the viewpoint of realizing a luxurious, low-gloss, dark-colored design, the luminous reflectance Y value in the CIE 1976 XYZ color system of one surface of the low-reflection film 100 of the embodiment is preferably 0.1 to 4.0%, more preferably 0.1 to 3.0%, even more preferably 0.1 to 2.0%, and particularly preferably 0.1 to 1.0%, based on the diffuse reflectance using an integrating sphere. The luminous reflectance Y value corresponds to a quantitative value that directly expresses the intensity of reflected light felt by humans, and the smaller this value, the smaller the intensity of reflected light, resulting in a low-reflectance, dark-colored design. The luminous reflectance Y value is the luminous reflectance Y (%) of the XYZ (Yxy) color system measured in accordance with JIS Z 8701, and can be measured using a spectrophotometer (for example, spectrophotometer U-4100 (manufactured by Hitachi High-Technologies Corporation)). In order to realize a low-gloss, dark design over a wide range from low angle to wide angle, it is preferable that the luminous reflectance Y value based on the specular reflectance at each angle satisfy the following relationship. 5°: 0.01 to 0.10% (preferably 0.01 to 0.05%) 20°: 0.01 to 0.10% (preferably 0.01 to 0.05%) 45°: 0.01 to 0.20% (preferably 0.01 to 0.06%) 60°: 0.01 to 0.50% (preferably 0.01 to 0.25%) 70°: 0.01 to 1.50% (preferably 0.01 to 0.40%)
[0042] On the other hand, the electrical conductivity (Ω / □) of the surface on the first resin layer 21 side of the low reflection film 100 (the surface of the first resin layer 21 in this embodiment) can be appropriately set according to the required performance and application, and is not particularly limited. From the viewpoint of handling, etc., it is preferably 1.0×10 8 (Ω / □) or less is preferable, and 1.0×10 7 (Ω / □) or less, more preferably 1.0×10 6 (Ω / □) or less, particularly preferably 1.0×10 5 Ω or less. In this specification, the electrical conductivity is a value measured in accordance with JIS-K6911:1995. Such a first resin layer 21 can be obtained, for example, by using conductive carbon black as a pigment or by carrying out an antistatic treatment of applying conductive carbon black to the surface of the first resin layer 21.
[0043] To provide high light-shielding properties as a light-shielding member, the low reflection film 100 preferably has an overall optical density (OD) of 0.5 or more, more preferably 1.0 or more, even more preferably 1.7 or more, and particularly preferably 2.0 or more.
[0044] The adhesive layer 31 is provided on the surface 11b of the above-mentioned base film 11, and is a layer that adhesively bonds to an adherend (not shown). By adhesively bonding the adhesive layer 31 side to the adherend in this manner, it is possible to impart a surface with low reflectance and low gloss in the wide-angle region. The type of adherend is not particularly limited, but is preferably an interior part of a mobile vehicle, such as a dashboard, roof trim, sun visor, switch panel, decoration panel, steering wheel, seat, camera hood or lens hood for optical sensors, etc.
[0045] The material constituting the adhesive layer 31 may be any known material in the art, and may be appropriately selected depending on the surface material of the adherend (resin molded body, multi-layer laminate using this resin molded body, nonwoven fabric, skin material, etc.), and the type is not particularly limited. For example, rubber-based adhesives, acrylic-based adhesives, olefin-based adhesives, silicone-based adhesives, and urethane-based adhesives are preferably used.
[0046] The method for producing the low reflection film 100 of this embodiment is not particularly limited as long as the above-mentioned configuration can be obtained. Conventionally known coating methods such as doctor coating, dip coating, roll coating, bar coating, die coating, blade coating, air knife coating, kiss coating, spray coating, and spin coating are preferably used.
[0047] Specifically, a coating liquid containing the above-mentioned binder resin 22 and organic resin particles 23, as well as optional components (inorganic particles 24, various additives) blended as necessary in a solvent is applied to the surface 11a of the base film 11, dried, and then heat treatment, pressure treatment, or the like is performed as necessary, to form the first resin layer 21 on the base film 11. Also, a coating liquid containing an adhesive in a solvent is applied to the surface 11b of the base film 11, dried, and then heat treatment, pressure treatment, or the like is performed as necessary, to form the adhesive layer 31 on the base film 11. At this time, in order to improve the adhesion between the base film 11 and the first resin layer 21 and / or the adhesive layer 31, anchor treatment, corona treatment, or the like can be performed as necessary. Also, an intermediate layer such as a primer layer or an adhesive layer can be provided between the base film 11 and the first resin layer 21 and / or the adhesive layer 31 as necessary. Then, after being formed into a sheet, vacuum forming, pressure forming, or the like can be performed.
[0048] Examples of the solvent for the coating solution used herein include water; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate; ether-based solvents such as methyl cellosolve and ethyl cellosolve; alcohol-based solvents such as methyl alcohol, ethyl alcohol, and isopropyl alcohol; nonpolar solvents such as hexane and cyclohexane; aprotic polar solvents such as dimethylformamide; aromatic solvents such as toluene; and mixed solvents of these.
[0049] (action) In the low reflection film 100 of this embodiment, the 70-degree regular reflectance and specular gloss of the surface of the low reflection film 100 on the first resin layer 21 side (the surface of the first resin layer 21 in this embodiment) are adjusted within a predetermined range, so that the surface reflectance and surface gloss are small not only in the wide angle region but also from the low angle region to the wide angle region. Therefore, by using this low reflection film 100, a matte-finished product with low surface reflectance and surface gloss when viewed from both the wide angle side and the low angle side can be realized. In addition, by using the low reflection film 100 of this embodiment as a low reflection film that covers the surface of an interior part arranged in the interior of a moving vehicle, reduces the reflected light of external light on the surface, and improves the imaging accuracy and / or detection accuracy of an optical sensor arranged in the interior, the deterioration or decrease of the imaging image and detection accuracy of the optical sensors can be suppressed. Therefore, the low reflection film 100 of this embodiment can realize highly accurate imaging, sensing, and the like in various moving vehicles such as automobiles, trains, steam trains, ships, cargo ships, airplanes, spacecraft, rockets, transportation equipment, and vehicles.
[0050] (Modification) In the first embodiment, the low-reflection film 100 having a three-layer laminate structure in which the first resin layer 21, the base film 11, and the adhesive layer 31 are arranged at least in this order is exemplified, but two or more resin layers may be provided. For example, as shown in Fig. 2, the low-reflection film 200 may have a laminate structure (four-layer structure) in which the first resin layer 21, the base film 11, the second resin layer 41, and the adhesive layer 31 are arranged at least in this order. In addition, the low-reflection film 200 may have a laminate structure (four-layer structure) in which the first resin layer 21, the second resin layer 41, the base film 11, and the adhesive layer 31 are arranged at least in this order.
[0051] In this case, the second resin layer 41 may be a conventionally known resin layer, or may be a resin layer or a light-shielding film having the same composition as the first resin layer 21 (however, the regular reflectance and specular gloss of these are not particularly limited), and the type is not particularly limited. The optical density (OD) of the second resin layer 41 is not particularly limited, but is preferably 0.5 or more, more preferably 1.0 or more, even more preferably 1.7 or more, and particularly preferably 2.0 or more. In addition, when the resin layers 21 and 31 are laminated, the overall optical density (OD) of the low reflection film 100 is preferably 1.5 to 6.0, more preferably 2.0 to 6.0, even more preferably 2.3 to 6.0, particularly preferably 4.5 to 6.0, and most preferably 5.0 to 6.0.
[0052] Also, as shown in Fig. 3, a low-reflection film 300 having a two-layer laminate structure omitting the adhesive layer 31 may be used, or as shown in Fig. 4, a low-reflection film 400 having a two-layer laminate structure omitting the base film 11 may be used. In the above first embodiment, an example has been shown in which the first resin layer 21 is provided on a flat surface (base film 11), but the first resin layer 21 may also be provided on a curved surface or an uneven surface.
[0053] The first resin layer 21 in the above-mentioned embodiment and each modified example can be recognized as an article expressed as a low reflection molded body by itself. That is, the first resin layer 21 of the present invention can be realized not only as a low reflection film but also as a thicker low reflection molded body. In this case, the thickness of the low reflection molded body is not limited to the thickness in the above-mentioned film form (thickness T of the first resin layer 21) and can be set arbitrarily. For example, the low reflection molded body can be a low reflection molded body having a thickness of 50 to 1000 μm, a low reflection molded body having a thickness of 1 to 10 mm, or a low reflection molded body having a thickness of 1 cm or more. EXAMPLES
[0054] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The present invention can adopt various conditions as long as the object of the present invention is achieved without departing from the gist of the present invention. In the following, "parts" refers to "parts by mass" unless otherwise specified.
[0055] Example 1 The substrate was a biaxially oriented PET film having a thickness of 50 μm (Toray Industries, Inc., product name: Lumirror T60, highly transparent type, total light transmittance (550 nm): 89.1%). One side of the substrate was coated with the following resin layer coating solution by a bar coating method so that the thickness after drying would be 8 μm, and then dried to form a first resin layer having a thickness of 8 μm on the substrate film, thereby producing the low reflection film of Example 1.
[0056] <Coating solution for resin layer> Binder resin 16.4 parts by weight (DIC, Acrydic A807, solid content: 50% by weight) ·Organic resin particles 9.0 parts by mass (Acrylic beads, average particle size D 50 :8μm) ·Inorganic particles 2.4 parts by mass (Tokai Carbon Co., Ltd., Toka Black #5500, average particle size D 50 :25nm) Resin hardener 2.4 parts by weight (DIC, Burnock DN980, solid content: 75% by weight) ·Dilution solvent 77.0 parts by mass (MEK:toluene = 50:50 mixed solvent)
[0057] (Examples 2 to 30, Comparative Examples 1 to 9, and Example 31) As shown in Tables 2 to 4, the type and average particle diameter D 50 Except for changing the amount of binder resin, the amount of dilution solvent, and the thickness of the resin layer, the low reflection films of Examples 2 to 30 and Comparative Examples 1 to 9 were produced in the same manner as in Example 1. In addition, the resin layer coating liquid shown in Table 4 was applied to one side of a 50 μm-thick biaxially stretched PET film (Toray Industries, Inc., product name: Lumirror T60, highly transparent type, total light transmittance (550 nm): 89.1%) as a substrate so as to have a thickness of 15 μm after drying, and then dried to form a first resin layer having a thickness of 15 μm on the substrate film, thereby producing the low reflection film of Example 31.
[0058] The physical properties of the obtained low reflection films of Examples 1 to 31 and Comparative Examples 1 to 9 were measured and evaluated under the following conditions. The evaluation results are shown in Tables 2 to 4.
[0059] (1) Film thickness / particle size The thickness of the low reflection film is the average particle diameter D of the organic resin particles. 50 This was calculated by dividing by .
[0060] (2) Specular gloss In accordance with JIS-Z8741:1997, a digital variable angle glossmeter (Gloss Meter VG7000: Nippon Denshoku Co., Ltd.) was used to measure the gloss (specular gloss) (%) of the surface on the first resin layer 21 side at each specified incident light angle (20°, 45°, 60°, 75°, 85°).
[0061] (3)70 degree specular reflectance Using a spectrophotometer (SolidSpec-3700: Shimadzu Corporation), the regular reflectance (specular reflectance) (%) of the surface on the first resin layer 21 side was measured at an incident light receiving angle of 70° for light with a wavelength of 550 nm.
[0062] (4) Optical density OD The optical density of the first resin layer 21 was measured using an optical densitometer (X-Rite361T: X-Rite Corporation) based on ISO 5-2. An ortho filter was used during the measurement.
[0063] (4) Surface roughness Ra The surface roughness Ra (μm) of the surface on the first resin layer 21 side was measured using a stylus surface roughness measuring instrument (SURFCOM 1500SD2-3DF: Tokyo Seimitsu Co., Ltd.) in accordance with the method for measuring arithmetic mean roughness (Ra) of JIS-B0601 (2001).
[0064] (5) Luminous reflectance Y value The luminous reflectance Y value of the low reflection film of Example 1 was measured based on the diffuse reflectance using a spectrophotometer (e.g., a spectrophotometer U-4100 (manufactured by Hitachi High-Technologies Corporation)) and an integrating sphere in accordance with JIS Z 8701, and was 0.81%. The luminous reflectance Y values based on the specular reflectance at the incident light receiving angles (5°, 20°, 45°, 60°, 70°) were as follows. 5°: 0.03% 20°: 0.02% 45°: 0.04% 60°: 0.10% 70°: 0.37% [Table 2]
[0065] [Table 3]
[0066] [Table 4] [Industrial Applicability]
[0067] The present invention can be widely and effectively used as a high-performance low-reflection film in the fields of precision machinery, semiconductors, optical equipment, electronic devices, etc. For example, the present invention can be widely and effectively used as a low-reflection film for use in lens units, camera modules, sensor units, etc. mounted on high-performance single-lens reflex cameras, compact cameras, video cameras, mobile phones, projectors, vehicle-mounted cameras, vehicle-mounted sensors, optical sensors, etc., and can be particularly effectively used as a low-reflection film for interior parts of moving vehicles, such as dashboards, roof trims, sun visors, switch panels, decorative panels, steering wheels, seats, camera hoods and lens hoods for optical sensors, etc. [Explanation of symbols]
[0068] 11...Base material (base material film) 11a...plane 11b...plane 21...First resin layer 22 Binder resin 23...Organic resin particles 24...Inorganic particles 31...adhesive layer 41...Second resin layer T: Thickness of the first resin layer t: Average particle size of organic resin particles 100 ···Low reflection film 200 ···Low reflection film 300 ···Low reflection film 400 ···Low reflection film
Claims
1. At least a first resin layer is provided, The first resin layer is made of a binder resin and a polymer having an average particle diameter D 50 The composition contains at least organic resin particles having the formula: The reflectance and gloss of the surface on the first resin layer side have the following relationship: (1) 70 degree regular reflectance: 0.0% or more and 2.5% or less (wavelength 550nm) (2) 60 degree specular gloss: 0.0% to 6.0% 75 degree specular gloss: 0.0% to 6.0% 85 degree specular gloss: 0.0% to 6.0% (3) The sum of the 20° specular gloss, 45° specular gloss, 60° specular gloss, 75° specular gloss, and 85° specular gloss is 7.5% or less. Fulfilling The thickness T of the first resin layer is 0.5 to 2.4 times or 3.0 to 8.0 times the average particle diameter D 50 of the organic resin particles contained in the first resin layer. Low reflection film.
2. The organic resin particles have an average particle diameter D of 5 to 14 μm. 50 have The low reflection film according to claim 1 .
3. The content ratio of the organic resin particles to the total mass of the binder resin is 0.6 to 2.
5. The low reflection film according to claim 1 or 2.
4. Has an optical density of 0.5 or more The low reflection film according to any one of claims 1 to 3.
5. The first resin layer further contains carbon black. The low reflection film according to any one of claims 1 to 4.
6. The laminate structure has at least the first resin layer and an adhesive layer in this order. The low reflection film according to any one of claims 1 to 5.
7. The laminate structure has at least the first resin layer and a base film in this order. The low reflection film according to any one of claims 1 to 5.
8. The laminate structure has at least the first resin layer, the base film, and the adhesive layer in this order. The low reflection film according to any one of claims 1 to 5.
9. The laminated structure has at least the first resin layer, the base film, the second resin layer, and the adhesive layer in this order. The low reflection film according to any one of claims 1 to 5.
10. The adhesive layer contains one or more adhesives selected from the group consisting of rubber-based adhesives, acrylic-based adhesives, olefin-based adhesives, silicone-based adhesives, and urethane-based adhesives. The low reflection film according to any one of claims 6, 8 and 9.
11. The surface roughness Ra of the first resin layer is 0.8 to 4.0 μm. The low reflection film according to any one of claims 1 to 10.
12. an optical sensor disposed in a vehicle interior and configured to capture an image of the exterior of the vehicle interior through a window transparent to visible light or infrared light or to detect visible light or infrared light from the exterior of the vehicle interior; a low-reflection film that covers a surface of an interior part arranged in the room and reduces reflected light of external light on the surface to improve imaging accuracy and / or detection accuracy of the optical sensor; At least The low reflection film is At least a first resin layer is provided, The first resin layer is made of a binder resin and a polymer having an average particle diameter D 50 The composition contains at least organic resin particles having the formula: The reflectance and gloss of the surface on the first resin layer side have the following relationship: (1) 70 degree regular reflectance: 0.0% or more and 2.5% or less (wavelength 550nm) (2) 60 degree specular gloss: 0.0% to 6.0% 75 degree specular gloss: 0.0% to 6.0% 85 degree specular gloss: 0.0% to 6.0% (3) The sum of the 20° specular gloss, 45° specular gloss, 60° specular gloss, 75° specular gloss, and 85° specular gloss is 7.5% or less. Fulfilling The thickness T of the first resin layer is 0.5 to 2.4 times or 3.0 to 8.0 times the average particle diameter D 50 of the organic resin particles contained in the first resin layer. Optical sensing kit.
13. The organic resin particles have an average particle diameter D of 5 to 14 μm. 50 have The optical sensing kit of claim 12.
14. The interior part is at least one selected from the group consisting of a resin molded body, a multi-layer laminate using a resin molded body, a nonwoven fabric, and a skin material. The optical sensing kit according to claim 12 or 13.
15. A low-reflection molding that covers a surface of an article, The low reflection molding comprises a binder resin and a particle diameter D 50 The low reflection molding contains at least organic resin particles having the following relationship: (1) 70 degree regular reflectance: 0.0% or more and 2.5% or less (wavelength 550nm) (2) 60 degree specular gloss: 0.0% to 6.0% 75 degree specular gloss: 0.0% to 6.0% 85 degree specular gloss: 0.0% to 6.0% (3) The sum of the 20° specular gloss, 45° specular gloss, 60° specular gloss, 75° specular gloss, and 85° specular gloss is 7.5% or less. Fulfilling The thickness T of the first resin layer is 0.5 to 2.4 times or 3.0 to 8.0 times the average particle diameter D 50 of the organic resin particles contained in the first resin layer. Low reflection molded body.
Citation Information
Patent Citations
Method for delustering resin
JP1994057007A
Production of matted thermoplastic resin molding
JP1995314519A
Antireflection film
JP1998268105A
Flatting material composition
JP2002220562A
Matte resin composition, and matte resin molding having uniform matte surface, obtained by molding it
JP2003020384A