Active energy ray curable resin composition, cured film and film

A polyurethane (meth)acrylate-based water-based resin composition with conductive polymers addresses storage stability issues, enabling cured films with enhanced antistatic properties, solvent resistance, and adhesion, suitable for plastic films.

JP7559708B2Active Publication Date: 2024-10-02ARAKAWA CHEM IND LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021138634
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-02
Filing Date
2021-08-27
Publication Date
2024-10-02
Estimated Expiration
2041-08-27

AI Technical Summary

Technical Problem

Water-based active energy ray-curable resin compositions containing conductive polymers face issues with storage stability due to poor dispersibility of (meth)acrylates and conductive polymers, affecting the formation of cured films with antistatic properties, solvent resistance, and adhesion to plastic substrates.

Method used

Incorporating a reaction product of hydroxyl group-containing (meth)acrylates, polyisocyanates, and hydroxyl group-containing polyalkylene glycols to form polyurethane (meth)acrylate, combined with a conductive polymer and water, enhances the stability and performance of the resin composition.

Benefits of technology

The composition achieves excellent storage stability, forming cured films with superior antistatic properties, solvent resistance, and adhesion, while maintaining safety and workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559708000001
    Figure 0007559708000001
  • Figure 0007559708000002
    Figure 0007559708000002
  • Figure 0007559708000003
    Figure 0007559708000003
Patent Text Reader

Abstract

To provide an aqueous active energy ray-curable resin composition which has excellent storage stability and can form a cured film excellent in antistatic properties, solvent resistance, and adhesion to a plastic substrate.SOLUTION: The active energy ray-curable resin composition contains: a polyurethane (meth)acrylate (A) being a reaction product of reaction components including a hydroxyl group-containing (meth)acrylate (a1), a polyisocyanate (a2), and a hydroxyl group-containing polyalkylene glycol (a3); a conductive polymer (B); and water (C).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active energy ray-curable resin composition, a cured film, and a cured layer. [Background technology]

[0002] Conventionally, plastic films such as polyester films have been used in a wide range of applications, including plate-making films, packaging films, films for optical components, films for semiconductor processing tapes, hot stamping films, and plastic molding decoration films. However, plastic films are prone to static electricity during winding and unwinding or processing, which can cause physical defects (pinholes, etc.) on the surface due to the adhesion of dust in the air, or running problems on the processing line. Therefore, various proposals have been made to suppress the static electricity of plastic films.

[0003] As one of such means, a method of applying a coating agent having an antistatic function to the surface of the film is considered. In addition to the antistatic function, the antistatic coating agent is generally required to have various properties such as the solvent resistance of the film and the adhesion between the film and the plastic substrate. As a known antistatic coating agent, for example, a coating agent using a quaternary ammonium salt type cationic compound in an active energy ray curable resin composition containing (meth)acrylates has been proposed (see Patent Document 1). In addition, as another antistatic coating agent, a coating agent using a conductive polymer such as poly(thiophene) or poly(aniline) in an active energy ray curable resin composition is also considered. Such a coating agent is a conductive polymer that is not easily affected by external environments such as humidity, so it is considered that it can exhibit a sufficient antistatic function regardless of the usage environment.

[0004] Incidentally, depending on the application, the active energy ray curable resin composition may require a low viscosity, and in that case, a method of using a large amount of a reactive diluent or using an organic solvent in combination is adopted. However, when a large amount of a reactive diluent is used, the curability decreases, making it difficult to obtain sufficient coating film properties, and when an organic solvent is used in combination, the risk of air pollution and fire increases.

[0005] In recent years, therefore, there has been an increasing demand for water-based active energy ray-curable resin compositions from the standpoint of workability and safety. For example, Patent Document 2 proposes an active energy ray-curable resin composition that is dissolved or dispersed in water to reduce viscosity. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-315373 [Patent Document 2] Japanese Patent Application Publication No. 11-279242 Summary of the Invention [Problem to be solved by the invention]

[0007] As an antistatic coating agent having good antistatic function and excellent workability and safety, it is considered to use a conductive polymer in a water-based active energy ray curable resin composition. However, the inventors have found that such a coating agent has a problem that the stability during storage (storage stability) is insufficient due to the low dispersibility of (meth)acrylates and the conductive polymer in water.

[0008] An object of the present invention is to provide an aqueous active energy ray-curable resin composition capable of forming a cured film having excellent storage stability, antistatic properties, solvent resistance and adhesion to plastic substrates. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by an active energy ray-curable resin composition containing a polyurethane (meth)acrylate, which is a reaction product of reaction components containing a specific hydroxyl group-containing (meth)acrylate, a polyisocyanate, and a hydroxyl group-containing polyalkylene glycol, and a conductive polymer and water, thereby completing the present invention.

[0010] Specifically, the present inventors have found that the use of a conductive polymer in an aqueous resin composition containing the polyurethane (meth)acrylate results in excellent storage stability in the resin composition. They have also found that such a resin composition can form a cured film that is excellent in antistatic properties, solvent resistance, and plastic adhesion. That is, the present invention relates to the following active energy ray-curable resin composition.

[0011] 1. A polyurethane (meth)acrylate (A) which is a reaction product of reaction components including a hydroxyl group-containing (meth)acrylate (a1), a polyisocyanate (a2) and a hydroxyl group-containing polyalkylene glycol (a3); An active energy ray-curable resin composition comprising a conductive polymer (B) and water (C).

[0012] 2. The active energy ray-curable resin composition according to item 1, wherein the component (a1) is a hydroxyl group-containing (meth)acrylate having at least three (meth)acryloyl groups in the molecule.

[0013] 3. The active energy ray-curable resin composition according to item 1 or 2, wherein the component (a2) is a polyisocyanate having at least three isocyanate groups in the molecule.

[0014] 4. The active energy ray-curable resin composition according to any one of items 1 to 3, wherein the component (a3) ​​is a compound represented by the following general formula (1): (chemical 1) H-(OCH2CH2)n-OR (1) (In the formula, R represents an alkyl group, an allyl group, a (meth)acryloyl group, or an acyl group, and n represents an integer of 3 to 25.)

[0015] 5. The active energy ray-curable resin composition according to any one of items 1 to 4, wherein the component (B) is a poly(thiophene).

[0016] 6. The active energy ray-curable resin composition according to any one of items 1 to 5, further comprising a (meth)acrylate (D) having at least three (meth)acryloyl groups in the molecule.

[0017] 7. The active energy ray-curable resin composition according to any one of items 1 to 6, further comprising a surface conditioner (E).

[0018] 8. The active energy ray-curable resin composition according to any one of items 1 to 7, wherein the content of the component (B) is 0.1 to 20 parts by mass, calculated as solid content, per 100 parts by mass of the total amount of the components (A) and (B).

[0019] 9. A cured film comprising the active energy ray-curable resin composition according to any one of items 1 to 8.

[0020] 10. A film comprising the cured film according to item 9 above. Effect of the Invention

[0021] The active energy ray curable resin composition of the present invention has good dispersibility and excellent storage stability. In addition, the active energy ray curable resin composition can form a cured film having excellent antistatic properties, solvent resistance, and plastic adhesion even in a thin film of 1 μm or less, so it is useful as an antistatic coating agent for plastic films. Furthermore, the active energy ray curable resin composition is an aqueous composition, so it has excellent workability and safety. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] [Active energy ray-curable resin composition] The active energy ray-curable resin composition of the present invention contains a specific polyurethane (meth)acrylate (A) (hereinafter referred to as component (A)), a conductive polymer (B) (hereinafter referred to as component (B)), and water (C) (hereinafter referred to as component (C)).

[0023] In this specification, "(meth)acrylic" means "at least one selected from the group consisting of acrylic and methacrylic". Similarly, "(meth)acrylate" means "at least one selected from the group consisting of acrylate and methacrylate", and "(meth)acryloyl group" means "at least one selected from the group consisting of acryloyl group and methacryloyl group".

[0024] <Polyurethane (meth)acrylate (A)> The component (A) is a reaction product of reaction components including a hydroxyl group-containing (meth)acrylate (a1) (hereinafter referred to as the component (a1)), a polyisocyanate (a2) (hereinafter referred to as the component (a2)), and a hydroxyl group-containing polyalkylene glycol (a3) ​​(hereinafter referred to as the component (a3)). The component (A) can be used alone or in combination of two or more types.

[0025] (Hydroxyl group-containing (meth)acrylate (a1)) As the component (a1), various known compounds having at least one hydroxyl group and at least one (meth)acryloyl group in the molecule can be used without particular limitation. As the component (a1), one type can be used alone, or two or more types can be used in combination.

[0026] The number of (meth)acryloyl groups in the molecule of component (a1) is preferably as large as possible, since the hardness and abrasion resistance of the resulting cured film will be excellent. In terms of availability, the number of (meth)acryloyl groups in the molecule of component (a1) is usually about 1 to 5.

[0027] Examples of component (a1) include hydroxyl group-containing glycerin poly(meth)acrylate, hydroxyl group-containing polyglycerin poly(meth)acrylate, hydroxyl group-containing pentaerythritol poly(meth)acrylate, hydroxyl group-containing polypentaerythritol poly(meth)acrylate, hydroxyl group-containing trimethylolpropane poly(meth)acrylate, hydroxyl group-containing polytrimethylolpropane poly(meth)acrylate, and hydroxyl group-containing mono(meth)acrylate.

[0028] Examples of the hydroxyl group-containing glycerin poly(meth)acrylate include glycerin di(meth)acrylate, and a mixture of at least two members selected from the group consisting of glycerin mono(meth)acrylate, glycerin di(meth)acrylate, and glycerin tri(meth)acrylate.

[0029] Examples of the hydroxyl group-containing polyglycerol poly(meth)acrylate include diglycerol di(meth)acrylate, diglycerol tri(meth)acrylate, triglycerol di(meth)acrylate, triglycerol tri(meth)acrylate, and triglycerol tetra(meth)acrylate.

[0030] Examples of the hydroxyl group-containing pentaerythritol poly(meth)acrylate include pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and a mixture of at least two selected from the group consisting of pentaerythritol mono(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate.

[0031] Examples of the hydroxyl group-containing polypentaerythritol poly(meth)acrylate include dipentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol di(meth)acrylate, tripentaerythritol tri(meth)acrylate, tripentaerythritol tetra(meth)acrylate, tripentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, and mixtures of at least two of these (meth)acrylates, and mixtures of dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate, and the like.

[0032] An example of the hydroxyl group-containing trimethylolpropane poly(meth)acrylate is trimethylolpropane di(meth)acrylate.

[0033] Examples of the hydroxyl group-containing polytrimethylolpropane poly(meth)acrylate include ditrimethylolpropane di(meth)acrylate and ditrimethylolpropane tri(meth)acrylate.

[0034] Examples of the hydroxyl group-containing mono(meth)acrylate include hydroxyl group-containing linear alkyl (meth)acrylate, hydroxyl group-containing linear alkyl (meth)acrylate caprolactone adduct, hydroxyl group-containing branched alkyl (meth)acrylate, hydroxyl group-containing branched alkyl (meth)acrylate caprolactone adduct, hydroxyl group-containing cycloalkyl (meth)acrylate, hydroxyl group-containing cycloalkyl (meth)acrylate caprolactone adduct, polyalkylene glycol mono(meth)acrylate caprolactone adduct, and glycerin mono(meth)acrylate.

[0035] Examples of the hydroxyl group-containing linear alkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0036] Examples of the hydroxyl group-containing linear alkyl (meth)acrylate caprolactone adduct include 3-hydroxypropyl (meth)acrylate caprolactone adduct, 2-hydroxyethyl (meth)acrylate caprolactone adduct, and 4-hydroxybutyl (meth)acrylate caprolactone adduct.

[0037] Examples of the hydroxyl group-containing branched alkyl (meth)acrylate include 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-hydroxybutyl (meth)acrylate.

[0038] Examples of the hydroxyl group-containing branched alkyl (meth)acrylate caprolactone adduct include 2-hydroxypropyl (meth)acrylate caprolactone adduct, 2-hydroxybutyl (meth)acrylate caprolactone adduct, and 3-hydroxybutyl (meth)acrylate caprolactone adduct.

[0039] Examples of the hydroxyl group-containing cycloalkyl (meth)acrylate include hydroxycyclohexyl (meth)acrylate.

[0040] Examples of the hydroxyl group-containing cycloalkyl (meth)acrylate caprolactone adduct include (meth)acrylic acid hydroxycyclohexyl caprolactone adduct.

[0041] Examples of the polyalkylene glycol mono(meth)acrylate caprolactone adduct include polyethylene glycol mono(meth)acrylate caprolactone adduct and polypropylene glycol mono(meth)acrylate caprolactone adduct.

[0042] From the viewpoint of excellent curability and solvent resistance of the cured film, the component (a1) is preferably a hydroxyl-containing (meth)acrylate having at least three (meth)acryloyl groups in the molecule, more preferably a hydroxyl-containing (meth)acrylate having one hydroxyl group and at least three (meth)acryloyl groups in the molecule. As the hydroxyl-containing (meth)acrylate, the above-mentioned pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, a mixture of pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate, or a mixture of dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate is preferred.

[0043] The content of the (a1) component in the above reaction components is not particularly limited, but in terms of excellent solvent resistance of the cured film, the content is preferably about 20 to 80 mass%, and more preferably about 30 to 70 mass%, calculated as solid content, relative to 100 mass% of the above reaction components.

[0044] (Polyisocyanate (a2)) As the component (a2), various known compounds having at least two isocyanate groups in the molecule can be used without particular limitation. The polyisocyanates may be used alone or in combination of two or more kinds.

[0045] Examples of the component (a2) include linear aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, biuret forms, isocyanurates, allophanates, and adducts of these diisocyanates, as well as complexes obtained by reaction of two or more selected from the group consisting of biurets, isocyanurates, allophanates, and adducts.

[0046] Examples of the linear aliphatic diisocyanate include methylene diisocyanate, ethylene diisocyanate, propylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, heptamethylene diisocyanate, octamethylene diisocyanate, nonamethylene diisocyanate, and decamethylene diisocyanate.

[0047] Examples of the branched aliphatic diisocyanate include diethylpentylene diisocyanate, trimethylbutylene diisocyanate, trimethylpentylene diisocyanate, and trimethylhexamethylene diisocyanate.

[0048] Examples of the alicyclic diisocyanate include hydrogenated xylene diisocyanate, hydrogenated diphenylmethane diisocyanate, isophorone diisocyanate, cyclopentylene diisocyanate, cyclohexylene diisocyanate, cycloheptylene diisocyanate, cyclodecylene diisocyanate, tricyclodecylene diisocyanate, adamantane diisocyanate, norbornene diisocyanate, and bicyclodecylene diisocyanate.

[0049] Examples of the aromatic diisocyanate include dialkyl diphenylmethane diisocyanates such as 4,4'-diphenyldimethylmethane diisocyanate, tetraalkyl diphenylmethane diisocyanates such as 4,4'-diphenyltetramethylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, m-tetramethylxylylene diisocyanate, and 1,5-naphthylene diisocyanate.

[0050] The biuret compound of the diisocyanate is The structural formula: [ka] [where n b is an integer equal to or greater than 1, and R bA ~R bE are each independently a linear aliphatic diisocyanate residue, a branched aliphatic diisocyanate residue, an alicyclic diisocyanate residue, or an aromatic diisocyanate residue; R bα ~R bβ each independently represents an isocyanate group or [ka] (n b1 is an integer equal to or greater than 0, and R b1 ~R b5 is R bA ~R bE is the same as R b '~R b '' each independently represents an isocyanate group or R bα ~R bβ It is a radical of itself. R b4 ~R b5 , R b '' may be different groups for each structural unit. bD ~R bE , R bβ may be different groups for each structural unit.

[0051] Specific examples of the biuret derivatives of the diisocyanates include Duranate 24A-100, Duranate 22A-75P, Duranate 21S-75E (all manufactured by Asahi Kasei Corporation), and Desmodur N3200A (a biuret derivative of hexamethylene diisocyanate) (all manufactured by Sumitomo Bayer Urethane Co., Ltd.).

[0052] The isocyanurate of the diisocyanate is The structural formula: [ka] [where n i is an integer equal to or greater than 0, and R iA ~RiE are each independently a linear aliphatic diisocyanate residue, a branched aliphatic diisocyanate residue, an alicyclic diisocyanate residue, or an aromatic diisocyanate residue; R iα ~R iβ each independently represents an isocyanate group or [ka] (n i1 is an integer equal to or greater than 0, and R i1 ~R i5 is R iA ~R iE is the same as R i '~R i '' each independently represents an isocyanate group or R iα ~R iβ It is a radical of itself. R i4 ~R i5 , R i '' may be different groups for each structural unit. iD ~R iE , R iβ may be different groups for each structural unit.

[0053] Specific examples of the isocyanurate of the diisocyanate include Duranate TPA-100, Duranate TKA-100, Duranate MFA-75B, Duranate MHG-80B (all manufactured by Asahi Kasei Corporation), Coronate HXR, Coronate HX (all isocyanurate of hexamethylene diisocyanate) (all manufactured by Tosoh Corporation), Takenate D-127N (isocyanurate of hydrogenated xylylene diisocyanate) (all manufactured by Mitsui Chemicals, Inc.), and VESTANAT T1890 / 100 (isocyanurate of isophorone diisocyanate) (all manufactured by Evonik Japan Co., Ltd.).

[0054] The allophanate form of the diisocyanate is The structural formula: [ka] [where n a is an integer equal to or greater than 0, and R aA is an alkyl group, an aryl group, a polyether group, a polyester group, or a polycarbonate group, R aB ~R aG are each independently any one of a linear aliphatic diisocyanate residue, a branched aliphatic diisocyanate residue, an alicyclic diisocyanate residue, and an aromatic diisocyanate residue, and R aα ~R aγ each independently represents an isocyanate group or [ka] (n a1 is an integer equal to or greater than 0, and R a1 ~R a6 is R aB ~R aG is the same as R a '~R a ''' each independently represents an isocyanate group or R aα ~R aγ It is a radical of itself. R a1 ~R a4 , R a '~R a '' may be different groups for each structural unit. aB ~R aE , R aα ~R aβ may be different groups for each structural unit.

[0055] Specific examples of the allophanate derivatives of the diisocyanates include Coronate 2793 (manufactured by Tosoh Corporation) and Takenate D-178N (manufactured by Mitsui Chemicals, Inc.).

[0056] The adduct of the diisocyanate is The structural formula: [ka] [where n ad is an integer equal to or greater than 0, and R adA ~RadE are each independently a linear aliphatic diisocyanate residue, a branched aliphatic diisocyanate residue, an alicyclic diisocyanate residue, or an aromatic diisocyanate residue; R ad1 ~R ad2 are each independently [ka] (In the formula, n ad’ is an integer equal to or greater than 0, and R ad’ ~R ad’’ is R adA ~R adE is the same as R ad’’’ is R ad1 ~R ad2 It is the base of itself, R ad’ ~R ad’’’ may have different groups for each structural unit. and R adD ~R adE , R ad2 may be different for each structural unit.] An adduct of trimethylolpropane and diisocyanate represented by the formula: The following structural formula [ka] [where n ad1 is an integer equal to or greater than 0, and R adα ~R adε are each independently a linear aliphatic diisocyanate residue, a branched aliphatic diisocyanate residue, an alicyclic diisocyanate residue, or an aromatic diisocyanate residue; R adA ~R adB are each independently [ka] (In the formula, n ad1’ is an integer equal to or greater than 0, and R adδ’ ~R adε’ is R adα ~R adε is the same as R adB’ is R adA ~R adBIt is the base of itself, R adδ’ ~R adε’ , R adB’ may have different groups for each structural unit. R adδ ~R adε , R adB may be different for each structural unit.] Examples of the compound include an adduct of glycerin and a diisocyanate represented by the following formula:

[0057] Specific examples of the adducts of the diisocyanates include Duranate P301-75E (both manufactured by Asahi Kasei Corporation), Takenate D-110N, Takenate D-160N (both manufactured by Mitsui Chemicals, Inc.), Coronate L, Coronate HL (both manufactured by Tosoh Corporation).

[0058] In the above formulas, "linear aliphatic diisocyanate residue, branched aliphatic diisocyanate residue, alicyclic diisocyanate residue, and aromatic diisocyanate residue" means the remaining groups of the linear aliphatic diisocyanate, branched aliphatic diisocyanate, alicyclic diisocyanate, and aromatic diisocyanate excluding isocyanate groups.

[0059] In view of excellent solvent resistance of the cured film, the component (a2) is preferably a polyisocyanate having at least three isocyanate groups in the molecule. As the polyisocyanate having at least three isocyanate groups in the molecule, the biuret, isocyanurate, allophanate, and adduct are preferable.

[0060] The isocyanate group content (NCO%) of the component (a2) is not particularly limited, but is preferably about 10 to 30% in order to provide a cured film with excellent solvent resistance.

[0061] The molar ratio (NCO / OH) of the isocyanate groups contained in the (a2) component to the hydroxyl groups contained in the (a1) component is not particularly limited, but from the viewpoint of excellent solvent resistance of the cured film, it is preferably about 1.2 to 6.0, and more preferably about 1.5 to 3.0.

[0062] The content of the (a2) component in the above reaction components is not particularly limited, but in terms of excellent solvent resistance of the cured film, the content is preferably about 15 to 75 mass%, and more preferably about 15 to 60 mass%, calculated as solid content, relative to 100 mass% of the above reaction components.

[0063] (Hydroxyl-containing polyalkylene glycols (a3)) As the component (a3), various known polyalkylene glycols having at least one hydroxyl group in the molecule can be used without particular limitation. As the component (a3), one type may be used alone, or two or more types may be used in combination.

[0064] Examples of the component (a3) ​​include polyalkylene glycol, polyalkylene glycol monoalkyl ether, polyalkylene glycol mono(meth)acrylate, polyalkylene glycol monoallyl ether, and polyalkylene glycol monoacylate.

[0065] Examples of the polyalkylene glycol include polyethylene glycol, polypropylene glycol, polybutylene glycol, polyether glycol having at least one structure of block or random copolymerization of ethylene oxide / propylene oxide / butylene oxide, polyoxytetramethylene glycol, polyethylene glycol polypropylene glycol polyethylene glycol (block copolymer), polypropylene glycol polyethylene glycol polypropylene glycol (block copolymer), polyethylene glycol polypropylene glycol (random copolymer), polyoxytetramethylene glycol polyethylene glycol polyoxytetramethylene glycol (block copolymer), polyethylene glycol polyoxytetramethylene glycol polyethylene glycol (block copolymer), polyethylene glycol polyoxytetramethylene glycol (random copolymer), polypropylene glycol polyoxytetramethylene glycol polypropylene glycol (block copolymer), polyoxytetramethylene glycol polyoxytetramethylene glycol polypropylene glycol (block copolymer), polypropylene glycol polyoxytetramethylene glycol (random copolymer), and the like.

[0066] Examples of the polyalkylene glycol monoalkyl ether include polyethylene glycol derivatives such as polyethylene glycol monomethyl ether, polyethylene glycol monoethyl ether, polyethylene glycol monopropyl ether, polyethylene glycol monobutyl ether, polyethylene glycol monopentyl ether, polyethylene glycol monohexyl ether, polyethylene glycol monoheptyl ether, polyethylene glycol monooctyl ether, polyethylene glycol lauryl ether, polyethylene glycol cetyl ether, polyethylene glycol stearyl ether, polyethylene glycol nonylphenyl ether, polyethylene glycol tridecyl ether, polyethylene glycol oleyl ether, polyethylene glycol octylphenyl ether, and polyoxyethylene oleyl cetyl ether; and polypropylene glycol derivatives such as polypropylene glycol monomethyl ether.

[0067] Examples of the polyalkylene glycol mono(meth)acrylate include polyethylene glycol derivatives such as polyethylene glycol mono(meth)acrylate, polypropylene glycol derivatives such as polypropylene glycol mono(meth)acrylate, polyethylene glycol polypropylene glycol mono(meth)acrylate, poly(ethylene glycol tetramethylene glycol) mono(meth)acrylate, and poly(propylene glycol tetramethylene glycol) mono(meth)acrylate.

[0068] Examples of the polyalkylene glycol monoallyl ether include polyethylene glycol derivatives such as polyethylene glycol monoallyl ether, polypropylene glycol derivatives such as polypropylene glycol monoallyl ether, and polyethylene glycol polypropylene glycol monoallyl ether.

[0069] Examples of the polyalkylene glycol monoacylate include polyethylene glycol derivatives such as polyethylene glycol monolaurate, polyethylene glycol monostearate, and polyethylene glycol monooleate.

[0070] The component (a3) ​​is preferably one represented by the following general formula (1) from the viewpoint of excellent storage stability.

[0071] (C13) H-(OCH2CH2)n-OR (1) (In the formula, R represents an alkyl group, an allyl group, a (meth)acryloyl group, or an acyl group, and n represents an integer of 3 to 25.)

[0072] As the component (a3), polyethylene glycol monomethyl ether and polyethylene glycol mono(meth)acrylate are particularly preferred because they have excellent storage stability.

[0073] Examples of commercially available products of component (a3) ​​include PEG#200T, PEG#200, PEG#300, PEG#400, PEG#600, PEG#1000, PEG#1500, PEG#1540, PEG#2000, PEG#4000, PEG#4000P, PEG#6000, PEG#6000P,PEG#11000, PEG#20000, Uniox M-400, Uniox M-550, Uniox M-1000, Uniox M-2000, Uniox M-2500, Uniox M-3000, Uniox M-4000, Blenmer PE-90, Blenmer PE-200, Blenmer PE-300, Blenmer AE-90, Blenmer AE-200, and Blenmer AE-400 (all manufactured by NOF Corporation).

[0074] The physical properties of the (a3) ​​component are not particularly limited. The (a3) ​​component has a hydroxyl value (JIS K0070; the same applies hereinafter when referring to the hydroxyl value) of about 10 to 300 mgKOH / g is preferable from the viewpoint of excellent storage stability, and from the same viewpoint, about 30 to 140 mgKOH / g is more preferable.

[0075] From the viewpoint of excellent storage stability and solvent resistance of the cured film, the number average molecular weight of the (a3) ​​component is preferably about 200 to 3,000, and more preferably about 400 to 2,000. The number average molecular weight refers to a polystyrene-equivalent value in gel permeation chromatography, but the method for measuring it is not particularly limited, and various known means can be used, and commercially available measuring machines can also be used.

[0076] The amount of the (a3) ​​component in the reaction components is not particularly limited, but is preferably about 5 to 50 mass% and more preferably about 10 to 30 mass% in terms of solid content relative to 100 mass% of the reaction components in terms of excellent storage stability. If the amount of the (a3) ​​component is 5 mass% or more, the storage stability of the active energy ray curable resin composition is excellent and separation of the composition over time can be suppressed, which is preferable. In addition, if the amount of the (a3) ​​component is 50 mass% or less, the crosslink density is high, the curability is sufficient, and the water resistance of the obtained cured film is high, which is preferable.

[0077] In the component (A), the molar ratio of the hydroxyl groups of the component (a1), the isocyanate groups of the component (a2), and the hydroxyl groups of the component (a3) ​​is not particularly limited, but from the viewpoint of excellent storage stability and solvent resistance of the cured film, it is preferably 0.1-0.9:1:0.1-0.9, and more preferably about 0.4-0.8:1:0.1-0.6.

[0078] The reactive component in the (A) component may contain other components (hereinafter referred to as other components) that do not fall under any of the (a1), (a2), and (a3) ​​components. The other components are not particularly limited, but may be any compound having at least one functional group capable of reacting with an isocyanate group in the molecule. Examples of the functional group capable of reacting with an isocyanate group include a hydroxyl group and an amino group.

[0079] In addition, when the component (A) has a salt structure, the storage stability of the active energy ray curable resin composition is reduced, which is not preferable. Examples of such a component (A) include salts of polyurethane (meth)acrylate obtained by neutralizing a polyurethane (meth)acrylate obtained from a reaction component containing a carboxyl group-containing compound such as hydroxycarboxylic acid with a basic substance such as a metal hydroxide, ammonia, or amines.

[0080] <Properties and Production Method of Polyurethane (Meth)acrylate (A)> The physical properties of the (A) component are not particularly limited. From the viewpoint of curability, the weight average molecular weight of the (A) component is more preferably about 1,000 to 10,000. The weight average molecular weight refers to a polystyrene equivalent value in a gel permeation chromatography method, but the measurement method is not particularly limited, and various known means can be adopted, and a commercially available measuring device can also be used.

[0081] From the viewpoint of excellent curability, the component (A) is preferably a compound having at least two (meth)acryloyl groups in the molecule.

[0082] The method for producing the component (A) is not particularly limited as long as it is a method for reacting the components (a1), (a2), and (a3), and various known production methods are exemplified. Specifically, for example, the components (a2) and (a3) ​​are reacted in the presence of a catalyst at an appropriate reaction temperature (for example, 60 to 90 ° C., etc.), and then the component (a1) is added, and similarly in the presence of a catalyst, the reaction is carried out at an appropriate reaction temperature (for example, 60 to 90 ° C., etc.). The order in which the components (a1), (a2), and (a3) ​​are reacted is not particularly limited, and examples thereof include a method in which each of them is mixed and reacted in any order, and a method in which all the components are mixed and reacted at once.

[0083] Examples of the catalyst include organic tin catalysts such as dibutyltin dilaurate and dioctyltin dilaurate, organic acid tin catalysts such as tin octoate, organic titanium catalysts such as titanium ethylacetoacetate, organic zirconium catalysts such as zirconium tetraacetylacetonate, organic iron catalysts such as iron acetylacetonate, etc. The catalysts may be used alone or in combination of two or more.

[0084] The content of the component (A) in the active energy ray-curable resin composition is not particularly limited, but in terms of an excellent balance between the hardness and abrasion resistance of the cured film, the content is preferably about 20 to 90 parts by mass, and more preferably about 40 to 85 parts by mass, calculated as the solid content, relative to 100 parts by mass of the active energy ray-curable resin composition.

[0085] <Conductive polymer (B)> Component (B) is a conductive polymer, which is a substance that imparts antistatic properties to the cured film.

[0086] The component (B) is not particularly limited as long as it is a conductive polymer. The component (B) is preferably a π-conjugated conductive polymer containing various known heteroatoms. The term "heteroatom" refers to an atom other than hydrogen and carbon (e.g., nitrogen atom, sulfur atom, etc.), and the term "heteroatom-containing π-conjugated conductive polymer" refers to an organic polymer compound having the heteroatom in the molecule and having a molecular main chain that forms a π-conjugated structure. In this specification, the component (B) is in a state doped with various dopants. The component (B) may be used alone or in combination of two or more.

[0087] Examples of the heteroatom-containing π-conjugated conductive polymer include poly(thiophenes), poly(thiophenevinylenes), poly(pyrroles), etc., which are π-conjugated conductive polymers having a heterocycle containing a heteroatom. Examples of the heteroatom-containing π-conjugated conductive polymer include poly(anilines), etc., which are π-conjugated conductive polymers having an aromatic ring.

[0088] The heterocycle or aromatic ring may have an alkyl group, an alkoxy group, or an alkylenedioxy group bonded in a branched or cyclic manner. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, and an octadecyl group. Examples of the alkoxy group include a methoxy group, an ethoxy group, a butoxy group, a hexyloxy group, a decyloxy group, and an octadecyloxy group. Examples of the alkylenedioxy group include an ethylenedioxy group, a propylenedioxy group, and a butenedioxy group.

[0089] The poly(thiophene)s are not particularly limited, and examples of the poly(thiophene)s include poly(thiophene), poly(alkylthiophene), poly(monoalkoxythiophene), poly(dialkoxythiophene), and poly(alkylenedioxythiophene).

[0090] Examples of the poly(alkylthiophene)s include poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3,4-dimethylthiophene), and poly(3,4-dibutylthiophene). Examples of the poly(monoalkoxythiophenes) include poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), and poly(3-octadecyloxythiophene). Examples of the poly(dialkoxythiophenes) include poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-didecyloxythiophene), and poly(3,4-didodecyloxythiophene). Examples of the poly(alkylenedioxythiophenes) include poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), and poly(3,4-butenedioxythiophene).

[0091] Examples of the poly(thiophene vinylene)s include poly(thiophene vinylene), poly(alkylthiophene vinylenes), poly(monoalkoxythiophene vinylenes), poly(dialkoxythiophene vinylenes), and poly(alkylenedioxythiophene vinylenes).

[0092] Examples of the poly(alkylthiophene vinylene)s include poly(3-methylthiophene vinylene), poly(3-ethylthiophene vinylene), poly(3-propylthiophene vinylene), poly(3-butylthiophene vinylene), poly(3-hexylthiophene vinylene), poly(3-heptylthiophene vinylene), poly(3-octylthiophene vinylene), poly(3-decylthiophene vinylene), poly(3-dodecylthiophene vinylene), poly(3-octadecylthiophene vinylene), poly(3,4-dimethylthiophene vinylene), and poly(3,4-dibutylthiophene vinylene). Examples of the poly(monoalkoxythiophene vinylene)s include poly(3-methoxythiophene vinylene), poly(3-ethoxythiophene vinylene), poly(3-butoxythiophene vinylene), poly(3-hexyloxythiophene vinylene), poly(3-heptyloxythiophene vinylene), poly(3-octyloxythiophene vinylene), poly(3-decyloxythiophene vinylene), poly(3-dodecyloxythiophene vinylene), and poly(3-octadecyloxythiophene vinylene). Examples of the poly(dialkoxythiophene vinylene)s include poly(3,4-dimethoxythiophene vinylene), poly(3,4-diethoxythiophene vinylene), poly(3,4-dipropoxythiophene vinylene), poly(3,4-dibutoxythiophene vinylene), poly(3,4-dihexyloxythiophene vinylene), poly(3,4-diheptyloxythiophene vinylene), poly(3,4-dioctyloxythiophene vinylene), poly(3,4-didecyloxythiophene vinylene), poly(3,4-didecyloxythiophene vinylene), poly(3,4-didodecyloxythiophene vinylene), etc. Examples of the poly(alkylenedioxythiophene vinylene)s include poly(3,4-ethylenedioxythiophene vinylene), poly(3,4-propylenedioxythiophene vinylene), poly(3,4-butenedioxythiophene vinylene), etc.

[0093] Examples of the poly(pyrrole)s include poly(pyrrole), poly(alkylpyrroles), poly(monoalkoxypyrroles), poly(dialkoxypyrroles), and poly(alkylenedioxypyrroles).

[0094] Examples of the poly(alkylpyrrole)s include poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-propylpyrrole), poly(3-butylpyrrole), poly(3-hexylpyrrole), poly(3-heptylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3-octadecylpyrrole), poly(3,4-dimethylpyrrole), and poly(3,4-dibutylpyrrole). Examples of the poly(monoalkoxypyrrole)s include poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), poly(3-heptyloxypyrrole), poly(3-octyloxypyrrole), poly(3-decyloxypyrrole), poly(3-dodecyloxypyrrole), and poly(3-octadecyloxypyrrole). Examples of the poly(dialkoxypyrrole)s include poly(3,4-dimethoxypyrrole), poly(3,4-diethoxypyrrole), poly(3,4-dipropoxypyrrole), poly(3,4-dibutoxypyrrole), poly(3,4-dihexyloxypyrrole), poly(3,4-diheptyloxypyrrole), poly(3,4-dioctyloxypyrrole), poly(3,4-didecyloxypyrrole), poly(3,4-didodecyloxypyrrole), etc. Examples of the poly(alkylenedioxypyrrole)s include poly(3,4-ethylenedioxypyrrole), poly(3,4-propylenedioxypyrrole), poly(3,4-butenedioxypyrrole), etc.

[0095] Examples of the poly(anilines) include poly(aniline), poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid).

[0096] Examples of the dopant include Lewis acids (PF5, AsF5, SbF5, etc.), protonic acids (HF, HCl, H2SO4, paratoluenesulfonic acid, etc.), electrolyte anions (Cl - , Br - , sulfoanion, etc.), anionic polymers, etc.

[0097] Examples of the anionic polymer include at least one selected from the group consisting of polystyrene sulfonic acid (hereinafter referred to as PSS), polyvinyl sulfonic acid, polyallyl sulfonic acid, polyethyl acrylate sulfonic acid, polybutyl acrylate sulfonic acid, poly-2-acrylamido-2-methylpropane sulfonic acid, polyisoprene sulfonic acid, polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic carboxylic acid, polymethacrylic carboxylic acid, poly-2-acrylamido-2-methylpropane carboxylic acid, and polyisoprene carboxylic acid, polyacrylic acid, and salts thereof.

[0098] The component (B) is usually used as an aqueous dispersion or solution, and in such cases, the solids concentration of the component (B) is usually about 0.1 to 10% by weight.

[0099] As the component (B), poly(thiophenes) and / or poly(anilines) are preferred, particularly poly(thiophenes), in view of the excellent antistatic properties of the cured film. In addition, poly(thiophenes) may include alkylenedioxypoly(thiophenes) doped with PSS (particularly 3,4-ethylenedioxythiophene (PEDOT)) and self-doped ethylenedioxypoly(thiophenes) obtained from thiophenes with sulfonic acid groups bonded to the ethylenedioxy moieties, in consideration of availability.

[0100] PEDOT doped with PSS can be obtained, for example, as an aqueous dispersion of a complex of poly(3,4-ethylenedioxythiophene) and polystyrenesulfonic acid (PEDOT / PSS) by polymerizing the monomer 3,4-ethylenedioxythiophene (EDOT) in an aqueous phase in the presence of PSS as a dopant using an oxidizing agent.

[0101] As the aqueous dispersion of PEDOT / PSS, for example, commercially available products such as Baytron P (manufactured by Starck), Clevios P ​​(manufactured by Heraeus), and Orgacon ICP1010 (manufactured by Agfa-Gevaert Japan KK) can be used.

[0102] Furthermore, the self-doped ethylenedioxypoly(thiophene) can be obtained as an aqueous solution of the self-doped ethylenedioxypoly(thiophene) by, for example, reacting a monomer in which a hydroxymethyl group is bonded to the ethylene moiety of 3,4-ethylenedioxythiophene with 2,4-butanesultone, purifying the monomer, and obtaining 3,4-ethylenedioxythiophene having a sulfonic acid group introduced therein, and then polymerizing the resulting 3,4-ethylenedioxythiophene with an oxidizing agent in an aqueous phase.

[0103] As an aqueous solution of self-doped ethylenedioxypoly(thiophene) obtained from thiophene having a sulfonic acid group bonded to the ethylenedioxy moiety, a commercially available product such as SELFTRON (manufactured by Tosoh Corporation) can also be used.

[0104] In addition, the active energy ray-curable resin composition of the present invention can also be used in combination with a non-heteroatom-based conductive polymer, such as poly(acetylenes), poly(phenylenes), poly(phenylenevinylenes), poly(acenes), etc., as long as the desired effects are not impaired.

[0105] The content of the (B) component in the active energy ray-curable resin composition is not particularly limited, but in terms of excellent antistatic properties of the cured film, it is preferably 0.1 to 20 parts by mass, calculated as solid content, per 100 parts by mass of the active energy ray-curable resin composition.

[0106] The content of the (B) component in the active energy ray-curable resin composition is not particularly limited, but in terms of excellent antistatic properties of the cured film, the content is preferably 0.05 to 25 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 4 to 10 parts by mass, relative to 100 parts by mass of the total amount of the (A) component and the (B) component, calculated as solid content.

[0107] <Water(C)> The component (C) is not particularly limited as long as it is water, and examples thereof include distilled water, ion-exchanged water, ion-exchanged distilled water, etc. The component (C) also includes the water contained in the component (B).

[0108] From the viewpoint of coatability, the content of the component (C) in the active energy ray-curable resin composition is preferably in the range such that the solid content concentration of the active energy ray-curable resin composition is about 0.5 to 50 mass %.

[0109] ((Meth)acrylate (D)) The active energy ray-curable resin composition may contain a (meth)acrylate (D) having at least three (meth)acryloyl groups in the molecule.

[0110] The number of (meth)acryloyl groups in the molecule of component (D) is preferably as large as possible, since the resulting cured film will have excellent solvent resistance. In terms of ease of availability, the number of (meth)acryloyl groups in the molecule of component (D) is usually about 3 to 5.

[0111] Examples of the component (D) include poly(meth)acrylates having at least three (meth)acryloyl groups in the molecule of the component (a1), trimethylolpropane tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate and epichlorohydrin-modified trimethylolpropane tri(meth)acrylate, and glycerin tri(meth)acrylate. Acrylates, glycerin tri(meth)acrylates such as ethylene oxide modified glycerin tri(meth)acrylate and propylene oxide modified glycerin tri(meth)acrylate, pentaerythritol tetra(meth)acrylates such as ethylene oxide modified pentaerythritol tetra(meth)acrylate and propylene oxide modified pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylates such as dipentaerythritol hexa(meth)acrylate and caprolactone modified dipentaerythritol hexa(meth)acrylate, diglycerin Examples of the poly(meth)acrylate include (poly)glycerin poly(meth)acrylates such as triglycerin tetra(meth)acrylate, triglycerin penta(meth)acrylate, etc., (poly)pentaerythritol poly(meth)acrylates such as tripentaerythritol octa(meth)acrylate and tetrapentaerythritol deca(meth)acrylate, (poly)trimethylolpropane poly(meth)acrylates such as ditrimethylolpropane tetra(meth)acrylate, polyester (meth)acrylate, urethane (meth)acrylate, epoxy (meth)acrylate, polyether (meth)acrylate, polyol (meth)acrylate, and polyacryl (meth)acrylate.

[0112] Examples of the urethane (meth)acrylate include a reaction product of a hydroxyl group-containing (meth)acrylate with a polyisocyanate, a reaction product of a hydroxyl group-containing (meth)acrylate with a polyol and a polyisocyanate, etc. The urethane (meth)acrylate is different from the component (A).

[0113] Examples of the hydroxyl group-containing (meth)acrylate include the same as those in the component (a1). Examples of the polyisocyanate include the same as those in the component (a2).

[0114] Examples of the polyol include aliphatic diols such as alkylene glycol, alicyclic diols such as 1,4-cyclohexanedimethanol, glycerin, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, polyether polyols, polyester polyols, polycarbonate polyols, acrylic polyols, and polyolefin polyols.

[0115] The polyacryl(meth)acrylate may be, for example, a reaction product of an acrylic copolymer obtained by polymerizing an epoxy group-containing mono(meth)acrylate and, if necessary, a mono(meth)acrylate, with (meth)acrylic acid.

[0116] Examples of the epoxy group-containing mono(meth)acrylate include glycidyl(meth)acrylate, β-methylglycidyl(meth)acrylate, 3,4-epoxycyclohexylmethyl(meth)acrylate, and vinylcyclohexene monoxide (that is, 1,2-epoxy-4-vinylcyclohexane).

[0117] Of the components (a1), pentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, and glycerin poly(meth)acrylate, each of which has a hydroxyl group, are preferred as the component (D) from the viewpoint of excellent storage stability.

[0118] Examples of the pentaerythritol poly(meth)acrylate include pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and a mixture of at least two selected from the group consisting of pentaerythritol mono(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate.

[0119] Examples of the dipentaerythritol poly(meth)acrylate include dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and a mixture of at least two selected from the group consisting of dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0120] Examples of the glycerin poly(meth)acrylate include glycerin di(meth)acrylate, and a mixture of at least two selected from the group consisting of glycerin mono(meth)acrylate, glycerin di(meth)acrylate, and glycerin tri(meth)acrylate.

[0121] Commercially available products of the pentaerythritol poly(meth)acrylate include, for example, Aronix M-933, Aronix M-934, Aronix M-306, and Aronix M-305 (all manufactured by Toagosei Co., Ltd.). Commercially available products of the dipentaerythritol poly(meth)acrylate include, for example, Aronix M-403, Aronix M-402, and Aronix M-400 (all manufactured by Toagosei Co., Ltd.). Commercially available products of the glycerin poly(meth)acrylate include, for example, Aronix M920 (manufactured by Toagosei Co., Ltd.).

[0122] (Physical Properties of (Meth)Acrylate (D)) The physical properties of component (D) are not particularly limited. From the viewpoints of excellent curability and solvent resistance of the cured film, the molecular weight of component (D) is preferably about 300 to 10,000, and more preferably about 300 to 5,000.

[0123] In this specification, when simply referring to "molecular weight", it has the following meaning. That is, when the structure of a compound can be expressed unequivocally by a specific chemical formula, such as pentaerythritol tetra(meth)acrylate, the molecular weight means the formula weight. On the other hand, when the structure of a compound cannot be expressed unequivocally by a specific chemical formula, such as polymer poly(meth)acrylate, the molecular weight means the weight average molecular weight.

[0124] The hydroxyl value of the component (D) is preferably about 80 to 300 mgKOH / g, and more preferably about 200 to 300 mgKOH / g, in view of excellent storage stability of the active energy ray-curable resin composition.

[0125] The content of the (D) component in the active energy ray-curable resin composition is not particularly limited, but in terms of the balance between the antistatic property and hardness of the cured film, it is preferably about 0 to 50 parts by mass, calculated as the solid content, per 100 parts by mass of the active energy ray-curable resin composition.

[0126] (Surface conditioner (E)) The active energy ray-curable resin composition may contain a surface conditioner (E) (hereinafter referred to as component (E)).

[0127] The component (E) may be used alone or in combination of two or more thereof. Examples of the component (E) include acrylic, silicone, fluorine-based, and acetylene diol-based compounds.

[0128] The content of the component (E) in the active energy ray-curable resin composition is not particularly limited, but in terms of the solvent resistance of the cured film, it is preferably about 0 to 10 parts by mass, calculated as solid content, per 100 parts by mass of the active energy ray-curable resin composition.

[0129] ((Meth)acrylate) The active energy ray-curable resin composition may contain a (meth)acrylate other than the component (D). The (meth)acrylate may be used alone or in combination of two or more kinds.

[0130] Examples of the (meth)acrylate include a mono(meth)acrylate having one (meth)acryloyl group in the molecule, and a di(meth)acrylate having two (meth)acryloyl groups in the molecule.

[0131] Examples of the mono(meth)acrylate include compounds of the component (a1) having one (meth)acryloyl group in the molecule, and mono(meth)acrylates that do not contain a hydroxyl group.

[0132] Examples of the di(meth)acrylate include compounds of the component (a1) having two (meth)acryloyl groups in the molecule, and di(meth)acrylates not containing hydroxyl groups. Examples of the di(meth)acrylates not containing hydroxyl groups include 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, ethylene ... acrylate, neopentyl glycol di(meth)acrylate, dicyclopentadiene di(meth)acrylate, bisphenol A ethylene oxide modified di(meth)acrylate, propylene oxide modified bisphenol A type di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, phthalic acid diglycidyl ester di(meth)acrylate, hydroxypivalic acid modified neopentyl glycol di(meth)acrylate, etc.

[0133] The content of the (meth)acrylate in the active energy ray-curable resin composition is not particularly limited, but is preferably about 0 to 300 parts by mass, calculated as solid content, per 100 parts by mass of the active energy ray-curable resin composition.

[0134] (Photopolymerization initiator) The active energy ray-curable resin composition may contain a photopolymerization initiator. The photopolymerization initiator may be used alone or in combination of two or more kinds. Examples of the photopolymerization initiator include 1-hydroxy-cyclohexyl-phenyl ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, a mixture of oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and 4-methylbenzophenone.

[0135] The photopolymerization initiators used were 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester and oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester from the viewpoints of curability and antistatic properties of the cured film. It is preferred to use a mixture of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester.

[0136] The content of the photopolymerization initiator in the active energy ray-curable resin composition is not particularly limited, but from the viewpoint of a balance between antistatic properties, solvent resistance, and the like of the cured film, the content is preferably 0 to 20 parts by mass, calculated as a solid content, relative to 100 parts by mass of the active energy ray-curable resin composition.

[0137] (solvent) The active energy ray curable resin composition may also use a solvent as long as it does not impair the effects of the present invention. Examples of the solvent include methyl ethyl ketone, methyl isobutyl ketone, methyl acetate, ethyl acetate, butyl acetate, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, isobutyl alcohol, tert-butyl alcohol, diacetone alcohol, acetone, acetylacetone, toluene, xylene, n-hexane, cyclohexane, methylcyclohexane, n-heptane, isopropyl ether, methyl cellosolve, ethyl cellosolve, 1,4-dioxane, propylene glycol monomethyl ether, ethylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate. The above solvents may be used alone or in combination of two or more. The solvent is preferably a water-miscible solvent such as ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, isobutyl alcohol, tert-butyl alcohol, diacetone alcohol, acetone, methyl cellosolve, ethyl cellosolve, 1,4-dioxane, or propylene glycol monomethyl ether.

[0138] In order to improve the electrical conductivity of the (B) component, the active energy ray curable resin composition is preferably used in combination with a high boiling point, highly polar solvent. Examples of high boiling point, highly polar solvent include ethylene glycol, dimethyl sulfoxide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, tetrahydrothiophene-1,1-dioxide, ethylene carbonate, propylene carbonate, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether. In particular, from the viewpoint of the antistatic property of the cured film, it is preferable to use 1,3-dimethyl-2-imidazolidinone in combination.

[0139] The content of the solvent in the active energy ray curable resin composition is not particularly limited. From the viewpoint of coatability, the content of the solvent is preferably about 0 to 200 parts by mass relative to 100 parts by mass of the active energy ray curable resin composition. From the viewpoint of coatability, the content of the solvent is preferably in a range such that the solid content concentration of the active energy ray curable resin composition is about 0.5 to 50% by mass.

[0140] (Additives) The active energy ray curable resin composition may contain the above (meth)acrylate, photopolymerization initiator, and non-solvent additives as long as the effect of the present invention is not impaired. The additives may be used alone or in combination of two or more. Examples of the additives include binders, curing agents, antioxidants, active energy ray absorbers, light stabilizers, defoamers, antifouling agents, preservatives, rust inhibitors, pH adjusters, lubricants, antiblocking agents, pigments, dyes, metal oxide fine particle dispersions, and organic fine particle dispersions.

[0141] The content of the additive in the active energy ray-curable resin composition is not particularly limited. The content of the additive is preferably about 0 to 50 parts by mass, calculated as a solid content, relative to 100 parts by mass of the curable resin composition.

[0142] [Physical properties and production method of active energy ray-curable resin composition]

[0143] The physical properties of the active energy ray curable resin composition are not particularly limited. The solid content concentration of the active energy ray curable resin composition is preferably about 0.5 to 50 mass% from the viewpoint of coatability. The viscosity of the active energy ray curable resin composition at a temperature of 25°C is preferably about 0.5 to 1000 mPa·s, more preferably about 0.5 to 100 mPa·s, from the viewpoint of coatability.

[0144] The active energy ray curable resin composition is obtained by mixing the (A) component and the (C) component, and optionally the (D) component, the (meth)acrylate, the photopolymerization initiator, and additives, emulsifying (or dispersing), and then mixing the (B) component and the (E) component, and optionally a solvent. The emulsification method is not particularly limited, and various known methods such as an inversion emulsification method and a mechanical emulsification method can be applied. Furthermore, various known emulsifiers and dispersants may be used as necessary within a range that does not impair the effects of the present invention. The emulsification conditions are also not particularly limited, and for example, the temperature is usually about 5 to 70°C, preferably about 10 to 50°C. Furthermore, the time is usually about 1 to 24 hours, preferably about 1 to 12 hours. Before emulsification, a mixture of the (A) component, the (D) component, and the photopolymerization initiator may be pre-emulsified.

[0145] The apparatus used for the above emulsification is not particularly limited, and examples thereof include a propeller mixer, a turbine mixer, a homomixer, a disperser mixer, an ultra mixer, a colloid mill, a high-pressure homogenizer, and an ultrasonic wave. A single apparatus can be used, or multiple apparatuses can be used in appropriate combination.

[0146] The active energy ray-curable resin composition can be used as a coating agent for various plastic films, particularly as a coating agent (hard coating agent) for preventing scratching, and can also be used as various coating agents such as wood paints and printing inks.

[0147] [Cured film] The cured film of the present invention is obtained from the active energy ray-curable resin composition. Specifically, for example, the coating agent is applied onto various plastic substrates in a range of 0.05 to 30 g / m2 after drying. 2 Approximately, preferably 0.1 to 20 g / m 2 The cured film is obtained by applying the composition to a thickness of about 100 nm, drying the composition, and then curing the composition by irradiating the composition with active energy rays such as ultraviolet rays, electron beams, and radiation. The cured film is formed, for example, by applying the composition to a plastic substrate as a coating agent for preventing scratches and curing the coating agent.

[0148] Examples of the plastic substrate include polycarbonate, polymethyl methacrylate, polystyrene, polyethylene terephthalate (PET), polyimide, polyolefin, nylon, epoxy resin, melamine resin, triacetyl cellulose resin, ABS resin, AS resin, norbornene resin, etc. Examples of the form of the plastic substrate include a film, a molded product, etc.

[0149] The cured film can be produced by various known methods.Specifically, for example, the active energy ray curable resin composition is applied to the plastic substrate, dried as necessary, and then cured by irradiating with active energy rays such as ultraviolet rays, electron beams, and radiation.In addition, there is also a method in which the coating agent is applied to a release film, cured by irradiating with active energy rays, an adhesive layer is provided thereon, the plastic substrate is bonded thereon, and then the release film is peeled off, and the cured film is transferred onto the plastic substrate.

[0150] Examples of active energy rays used in the curing reaction include ultraviolet rays and electron beams. As a light source for ultraviolet rays, an ultraviolet ray irradiation device having a xenon lamp, a high-pressure mercury lamp, a metal halide lamp, or an LED lamp can be used. The light amount, light source arrangement, transport speed, etc. can be adjusted as necessary. For example, when a high-pressure mercury lamp is used, it is preferable to perform curing at a transport speed of about 5 to 50 m / min for one lamp having a lamp output of about 80 to 160 W / cm.

[0151] Examples of the coating method include bar coater coating, wire bar coating, Mayer bar coating, air knife coating, gravure coating, reverse gravure coating, offset printing, flexographic printing, screen printing, and spray coating.

[0152] The active energy ray-curable resin composition can form a cured film by curing with active energy rays, and is therefore suitable for use with plastics that are easily deformed by heat.

[0153] [film] The film of the present invention includes the cured film. The film is an article having the cured film and various substrate films as components.

[0154] The above-mentioned base film may be, for example, a plastic film, and various known films may be used. Examples of the plastic film include polycarbonate film, polyester film, polyolefin film, polystyrene film, epoxy resin film, melamine resin film, triacetyl cellulose film, ABS resin film, AS resin film, acrylic resin film, and alicyclic polyolefin resin film. From the viewpoint of transparency and adhesion to the cured film, the plastic film is preferably one film selected from the group consisting of polycarbonate film, triacetyl cellulose film, acrylic resin film, and alicyclic polyolefin resin film. The average thickness of the base film is not particularly limited, but is usually about 20 to 1000 μm, preferably 20 to 200 μm.

[0155] The film can be produced by various known methods.Specific examples include a method of coating the active energy ray curable resin composition on the substrate film, drying it as necessary, and then irradiating it with the active energy ray to cure it.Also, a laminated film can be produced by coating the active energy ray curable resin composition of the present invention on the non-coated surface of the obtained substrate film, laminating another substrate film thereon, and then irradiating it with the active energy ray.

[0156] Examples of the coating method include the above-mentioned methods.

[0157] The amount of coating is not particularly limited, but the amount of coating after drying is preferably 0.1 to 30 g / m 2 The preferred thickness is 1 to 20 g / m 2 The cured film formed on the substrate film usually has an average thickness of about 0.05 to 30 μm, and preferably about 0.1 to 20 μm. EXAMPLES

[0158] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In each example, parts and % are by weight unless otherwise specified.

[0159] <Synthesis of polyurethane (meth)acrylate (A)> Manufacturing Example 1 In a reaction vessel equipped with a stirrer and a cooling tube, 47.9 parts of an isocyanurate modified product of hexamethylene diisocyanate (manufactured by Tosoh Corporation under the trade name "Coronate HXR"), 84.0 parts of polyethylene glycol monomethyl ether (manufactured by NOF Corporation under the trade name "Uniox M-1000"), 117.6 parts of a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aronix M-403"), 0.06 parts of tin octylate, and 0.15 parts of 4-methoxyphenol were charged, and the temperature in the system was raised to 70°C over about 15 minutes. Next, the reaction system was kept at the same temperature for 1.5 hours, and then cooled to 60°C. Then, 50.4 parts of a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (manufactured by Toagosei Co., Ltd., product name "Aronix M-403") and 0.12 parts of tin octylate were charged, and the temperature in the system was raised to 75°C over about 15 minutes. Next, the reaction system was held at the same temperature for 1 hour, after which 0.15 parts of 4-methoxyphenol was charged and the system was cooled to obtain polyurethane (meth)acrylate 1 with a solid content of 100%.

[0160] Manufacturing Example 2 In a reaction vessel equipped with a stirrer and a cooling tube, 42.9 parts of an isocyanurate modified product of hexamethylene diisocyanate (manufactured by Tosoh Corporation under the trade name "Coronate HXR"), 50.7 parts of polyethylene glycol monomethyl ether (manufactured by NOF Corporation under the trade name "Uniox M-1000"), 66.3 parts of a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aronix M-305"), 0.12 parts of tin octylate, and 0.15 parts of 4-methoxyphenol were charged, and the temperature in the system was raised to 70°C over about 15 minutes. Next, the reaction system was kept at the same temperature for 1.5 hours and then cooled to 60°C. Then, 28.8 parts of a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate (manufactured by Toagosei Co., Ltd., product name "Aronix M-305") and 0.12 parts of tin octylate were charged, and the temperature in the system was raised to 75°C over about 15 minutes. Next, the reaction system was held at the same temperature for 1 hour, after which 0.15 parts of 4-methoxyphenol was charged and the system was cooled to obtain polyurethane (meth)acrylate 2 with a solid content of 100%.

[0161] Comparative Manufacturing Example 1 In a reaction vessel equipped with a stirrer and a cooling tube, 137.8 parts of an isocyanurate modified product of hexamethylene diisocyanate (manufactured by Tosoh Corporation, trade name "Coronate HXR"), 63.5 parts of rosin epoxy acrylate (manufactured by Arakawa Chemical Industries, Ltd., trade name "Beamset 101"), 37.8 parts of 2-hydroxyethyl acrylate, 9.5 parts of polyethylene glycol monomethyl ether (manufactured by NOF Corporation, trade name "Uniox M-1000") and 0.15 parts of 4-methoxyphenol were charged, and then 0.12 parts of tin octylate were charged under stirring, and the temperature in the system was raised. After keeping the temperature at 70°C for 1.5 hours, 11.8 parts of 2-hydroxyethyl acrylate was added and kept warm for another 1 hour. Then, 39.6 parts of castor oil fatty acid (Toyokuni Oil Mills, trade name "CO-FA") was added, and the reaction system was maintained at the same temperature for 1 hour, after which 0.15 parts of 4-methoxyphenol was added to obtain polyurethane acrylate. The acid value of the polyurethane acrylate was 24.2 mgKOH / g. 200 parts of the polyurethane acrylate were kept at 60-70°C, neutralized with 6.1 parts of triethylamine added under stirring, and cooled to obtain a polyurethane (meth)acrylate salt with a solid content of 100%.

[0162] [Preparation of active energy ray-curable resin composition] Example 1 76.9 parts of the polyurethane (meth)acrylate 1, 9.0 parts of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (manufactured by IGM Resins BV, product name "OMNIRAD2959", solid content 100%) as a photopolymerization initiator, and 4.5 parts of a mixture of oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester (manufactured by IGM Resins BV, product name "OMNIRAD754", solid content 100%) were mixed and dissolved, and then 135.6 parts of water was gradually added while stirring to emulsify, and an emulsion with a solid content of 40% was obtained. Next, 400.0 parts (4.8 parts as solids) of a PEDOT / PSS water dispersion (trade name "Orgacon ICP1010", manufactured by Agfa-Gevaert Japan, 1.2% solids) as a conductive polymer, 6.4 parts (4.8 parts as solids) of an acetylene diol-based surface conditioner (trade name "Olfine EXP.4200", manufactured by Nissin Chemical Industry Co., Ltd., 75% solids), and 367.6 parts of water were blended into the emulsion to obtain an active energy ray-curable resin composition with a solids content of 10%.

[0163] Example 2 and Comparative Examples 3-4 An active energy ray-curable resin composition having a solid content of 10% was produced in the same manner as in Example 1, except that the composition was changed to that shown in Table 1.

[0164] Example 3 The polyurethane (meth)acrylate 1 was 45.3 parts, dipentaerythritol poly(meth)acrylate (Toagosei Co., Ltd., product name "Aronix M-403", 100% solids), 22.6 parts, pentaerythritol poly(meth)acrylate (Toagosei Co., Ltd., product name "Aronix M-306", 100% solids), 9.0 parts, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (IGM Resins BV, product name "OMNIRAD2959", 100% solids) as a photopolymerization initiator, and a mixture of oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester (IGM After mixing and dissolving 4.5 parts of Resins BV's product name "OMNIRAD754" (100% solids), 135.6 parts of water were gradually added while stirring to emulsify, obtaining an emulsion with a solids content of 40%. Next, 400.0 parts (4.8 parts as solids) of PEDOT / PSS water dispersion (Japan Agfa-Gevaert Co., Ltd. product name "Orgacon ICP1010" solids content 1.2%) as a conductive polymer, 6.4 parts (4.8 parts as solids) of acetylene diol-based surface conditioner (Nissin Chemical Industry Co., Ltd. product name "Olfine EXP.4200" solids content 75%), and 367.6 parts of water were mixed into the emulsion to obtain an active energy ray curable resin composition with a solids content of 10%.

[0165] Examples 4 to 9 and 11 Except for changing the composition to that shown in Table 1, an active energy ray-curable resin composition having a solid content of 10% was produced in the same manner as in Example 3.

[0166] Example 10 The polyurethane (meth)acrylate 2 was 44.0 parts, pentaerythritol poly(meth)acrylate (manufactured by Toagosei Co., Ltd., product name "Aronix M-306", 19.0 parts, photopolymerization initiator 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (manufactured by IGM Resins BV, product name "OMNIRAD2959", 100% solids), 8.0 parts, oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester mixture (manufactured by IGM Resins BV, product name "OMNIRAD754") After mixing and dissolving 4.0 parts of 100% solids, 112.5 parts of water were gradually added while stirring to emulsify, and an emulsion with a solid content of 40% was obtained. Next, 1666.7 parts (20.0 parts as solids) of PEDOT / PSS water dispersion (Agfa-Gevaert Japan Co., Ltd., trade name "Orgacon ICP1010", solid content 1.2%) as a conductive polymer, 6.7 parts (5.0 parts as solids) of an acetylene diol-based surface conditioner (Nissin Chemical Industry Co., Ltd., trade name "Olfine EXP.4200", solid content 75%), and 139.1 parts of water were mixed into the emulsion to obtain an active energy ray curable resin composition with a solid content of 5%.

[0167] Comparative Example 1 An active energy ray curable resin composition with a solid content of 1.5% was obtained by blending 6,250.0 parts (75.0 parts as solid content) of a PEDOT / PSS water dispersion as a conductive polymer (manufactured by Agfa-Gevaert Japan, product name "Orgacon ICP1010", solid content 1.2%), 33.3 parts (25.0 parts as solid content) of an acetylene diol-based surface conditioner (manufactured by Nissin Chemical Industry Co., Ltd., product name "Olfine EXP.4200", solid content 75%), and 382.7 parts of water.

[0168] Comparative Example 2 An active energy ray-curable resin composition with a solid content of 10% was produced in the same manner as in Example 3, except that the composition was changed to that in Table 1 and a mixed solvent of water and isopropanol (IPA) (water / IPA (mass ratio) = 54 / 46) was used instead of water.

[0169] (Storage Stability of Active Energy Ray-Curable Resin Composition) The active energy ray curable resin compositions of Examples 1 to 8 and Comparative Examples 1 to 4 were placed in screw tubes and stored for one week at room temperature in the dark. The state of the active energy ray curable resin compositions was visually evaluated according to the following criteria. The results are shown in Table 1. ○: The appearance remains unchanged and the liquid remains even after storage for one week at room temperature and protected from light. ×: After storing for one week in the dark at room temperature, the resin separates and / or the conductive polymer aggregates. do.

[0170] [Creating a hardened film] 15 parts of the active energy ray curable resin composition of Example 1 was diluted with 84 parts of water and 1 part of 1,3-dimethyl-2-imidazolidinone until the aqueous dispersion had a solid content of 1.5%. This aqueous dispersion was applied to a polyethylene terephthalate film (manufactured by Toray Industries, Inc., product name "Lumirror 50T60") with a thickness of 50 μm, so that the thickness of the coating film after curing was 0.1 μm, using a #3 bar coater, and dried at 80° C. for 2 minutes to produce a film. Thereafter, a film with a cured film was obtained under the conditions of a high pressure mercury lamp of 120 W / cm (1 lamp), an irradiation distance of 24 cm, and a belt speed of 22 m / min, with one pass and an accumulated irradiation amount of 50 mJ / cm2. A film with a cured film was obtained in the same manner from the active energy ray curable resin compositions of Examples 3, 5 to 9, and 11 and Comparative Examples 3 to 4.

[0171] 15 parts of the active energy ray curable resin composition of Example 2 was diluted with 84 parts of isopropyl alcohol and 1 part of 1,3-dimethyl-2-imidazolidinone until the aqueous dispersion had a solid content of 1.5%. This aqueous dispersion was applied to a polyethylene terephthalate film (manufactured by Toray Industries, Inc., product name "Lumirror 50T60") with a thickness of 50 μm using a #3 bar coater so that the thickness of the coating film after curing was 0.1 μm, and the film was dried at 80° C. for 1 minute to produce a film. Thereafter, a film with a cured film was obtained under the conditions of a high pressure mercury lamp of 120 W / cm (1 lamp), irradiation distance of 24 cm, and belt speed of 22 m / min, with one pass and an accumulated irradiation amount of 50 mJ / cm2.

[0172] 15 parts of the active energy ray curable resin composition of Example 4 was diluted with water to an aqueous dispersion with a solid content of 1.5%. This aqueous dispersion was applied to a polyethylene terephthalate film (manufactured by Toray Industries, Inc., product name "Lumirror 50T60") with a thickness of 50 μm using a #3 bar coater so that the thickness of the coating after curing was 0.1 μm, and the film was dried at 80° C. for 2 minutes to prepare a film. Then, a film with a cured film was obtained under the conditions of a high pressure mercury lamp of 120 W / cm (1 lamp), irradiation distance of 24 cm, and belt speed of 22 m / min, with one pass and an accumulated irradiation amount of 50 mJ / cm2.

[0173] 30 parts of the active energy ray curable resin composition of Example 10 was diluted with 70 parts of water until it became an aqueous dispersion with a solid content of 1.5%. This aqueous dispersion was applied to a polyethylene terephthalate film (manufactured by Toray Industries, Inc., product name "Lumirror 50T60") with a thickness of 50 μm using a #3 bar coater so that the thickness of the coating film after curing was 0.1 μm, and the film was dried at 80° C. for 2 minutes to prepare a film. Then, a film with a cured film was obtained under the conditions of a high pressure mercury lamp of 120 W / cm (1 lamp), irradiation distance of 24 cm, and belt speed of 22 m / min, one pass, and an accumulated irradiation amount of 50 mJ / cm2.

[0174] The resin composition of Comparative Example 1 was directly applied as an aqueous dispersion having a solid content of 1.5% onto a 50 μm-thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., product name "Lumirror 50T60") using a #3 bar coater so that the thickness of the coating after curing would be 0.1 μm. The coating was then dried at 80° C. for 2 minutes to produce a membrane-coated film.

[0175] 15 parts of the active energy ray curable resin composition of Comparative Example 2 was diluted with 84 parts of water and 1 part of 1,3-dimethyl-2-imidazolidinone to an aqueous dispersion with a solid content of 1.5%. However, the obtained aqueous dispersion separated, so it could not be applied to a polyethylene terephthalate film, and the following evaluations could not be performed.

[0176] (Antistatic) The surface resistivity of the cured film of the cured film of Example 1 was measured using a surface resistivity meter (manufactured by Mitsubishi Chemical Corporation, product name "Hiresta MCP-HT-450") in accordance with JIS K 6911 at an applied voltage of 10 to 500 V. The results are shown in Table 1. The cured films of Examples 2 to 11 and Comparative Examples 1, 3 and 4 were also evaluated in the same manner.

[0177] (Solvent resistance) The cured film of the cured film of Example 1 was observed for dissolution or not by 10 reciprocations of a cotton swab soaked in methyl ethyl ketone over a width of 5 cm, and the solvent resistance was evaluated according to the following criteria. The results are shown in Table 1. The cured films of Examples 2 to 11 and Comparative Examples 1, 3 and 4 were also evaluated in the same manner. ◯: The cured film does not dissolve at all. △: Traces of the cotton swab left on the cured film. ×: The cured film was dissolved.

[0178] (Adhesion) In the cured film of the cured film-attached film according to Example 1, 11 scratches were made at 1 mm intervals reaching the film substrate using a cutter guide and a cutter, and scratches were also made perpendicular to each other to make 100 grids. Cellophane tape was firmly pressed onto the grids and then peeled off in one go, and the state of the grids was visually observed and evaluated. The results are shown in Table 1. The cured films according to Examples 2 to 11 and Comparative Examples 1, 3 and 4 were also evaluated in the same manner. ◯: No peeling of the cured film at all. ×: Peeling of the cured film occurred.

[0179] [Table 1]

[0180] The blend amounts in Table 1 are values ​​in parts by mass converted into solid content. The notes and abbreviations in Table 1 are as follows. *Evaluation was not possible because the aqueous dispersion of the active energy ray-curable resin composition could not be applied. (Compound abbreviations and details) ICP1010: PEDOT / PSS water dispersion (product name "Orgacon ICP1010", solid content 1.2%) manufactured by Agfa-Gevaert Japan Ltd. SELFTRON: Self-doped ethylenedioxypoly(thiophene) aqueous solution (product name "SELFTRON H" solid content 1.2%) manufactured by Tosoh Corporation AQUAPASS: Polyaniline sulfonic acid aqueous solution (product name "AQUAPASS 01-x" solid content 5%) manufactured by Mitsubishi Chemical Corporation M403: Dipentaerythritol poly(meth)acrylate with a hydroxyl value of 90 mgKOH / g (product name "Aronix M-403", solid content 100%) manufactured by Toagosei Co., Ltd. M306: Pentaerythritol poly(meth)acrylate with a hydroxyl value of 160 mgKOH / g (product name "Aronix M-306", 100% solids), manufactured by Toagosei Co., Ltd. M3150: Trimethylolpropane EO modified acrylate (product name "MIRAMER M-3150" solid content 100%) manufactured by MIWON EXP4200: Acetylene diol-based surface conditioner (product name "Olfine EXP.4200", solid content 75%) manufactured by Nissin Chemical Industry Co., Ltd. OMNI2959: 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (product name "OMNIRAD2959" solid content 100%) manufactured by IGM Resins BV OMNI1173: 2-hydroxy-2-methyl-1-phenyl-propan-1-one (product name "OMNIRAD1173" solid content 100%) manufactured by IGM Resins BV OMNI754: Mixture of oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester (trade name "OMNIRAD754" solid content 100%) manufactured by IGM Resins BV

Claims

1. a polyurethane (meth)acrylate (A) (excluding a salt structure) which is a reaction product of reaction components including a hydroxyl group-containing (meth)acrylate (a1), a polyisocyanate (a2) and a hydroxyl group-containing polyalkylene glycol (a3); An active energy ray-curable resin composition comprising a conductive polymer (B), water (C), and optionally a solvent, the hydroxyl group-containing (meth)acrylate (a1) is a hydroxyl group-containing (meth)acrylate having at least three (meth)acryloyl groups in the molecule, The polyisocyanate (a2) is a polyisocyanate having at least three isocyanate groups in the molecule, The hydroxyl group-containing polyalkylene glycol (a3) ​​is a compound represented by the following general formula (1): The content of the polyurethane (meth)acrylate (A) is 20 to 90 parts by mass, calculated as a solid content, relative to 100 parts by mass of the active energy ray-curable resin composition; The content of the conductive polymer (B) is 0.1 to 20 parts by mass, in terms of solid content, relative to 100 parts by mass of the active energy ray-curable resin composition; The solvent is at least one selected from the group consisting of ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, isobutyl alcohol, tert-butyl alcohol, diacetone alcohol, acetone, methyl cellosolve, ethyl cellosolve, 1,4-dioxane, and propylene glycol monomethyl ether; An active energy ray-curable resin composition. (Chem.1) H-(OCH) 2 CH 2 )n -OR (1) (In the formula, R represents an alkyl group, an allyl group, a (meth)acryloyl group, or an acyl group, and n represents an integer of 3 to 25.)

2. 2. The active energy ray-curable resin composition according to claim 1, wherein the component (B) is a poly(thiophene).

3. The active energy ray-curable resin composition according to claim 1 or 2, further comprising a (meth)acrylate (D) having at least three (meth)acryloyl groups in the molecule.

4. The active energy ray-curable resin composition according to any one of claims 1 to 3, further comprising a surface conditioner (E).

5. The active energy ray-curable resin composition according to any one of claims 1 to 4, wherein the content of the component (B) is, in terms of solid content, 0.1 to 20 parts by mass per 100 parts by mass of the total amount of the component (A) and the component (B).

6. A cured film comprising the active energy ray-curable resin composition according to any one of claims 1 to 5.

7. A film comprising the cured film according to claim 6.

Citation Information

Patent Citations

  • Mold release film

    JP1998315373A

  • Aqueous resin composition curable with active energy ray, and its production

    JP1999279242A

  • Production of urethane(Meth)Acrylate and water-based coating material

    JP2000109533A

  • Radiation curable conductive composition

    JP2005170996A

  • Conductive hard coat composition

    JP2005298624A