Circuit board manufacturing method
By adjusting the Vickers hardness and minimum melt viscosity of the resin composition layer in resin sheets with metal foil, the method addresses resin chipping and oozing issues, resulting in improved temporary adhesion and reduced defects during circuit board manufacturing.
Patent Information
- Application Number
- JP2023196754
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-22
- Filing Date
- 2023-11-20
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2043-11-20
AI Technical Summary
The existing methods for manufacturing circuit boards using resin sheets with metal foil face issues such as resin chipping and resin oozing due to poor temporary adhesion and differences in hardness between the metal foil and resin sheet, especially during vacuum hot press treatment.
The method involves adjusting the Vickers hardness and minimum melt viscosity of the resin composition layer in the resin sheet to within specific ranges, applying heat and pressure during the manufacturing process to improve temporary adhesion and prevent resin chipping and oozing.
This approach results in a circuit board with enhanced temporary attachment properties, effectively suppressing resin chipping and resin seepage, ensuring better adhesion and integrity during the manufacturing process.
Smart Images

Figure 0007559910000007 
Figure 0007559910000008 
Figure 0007559910000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for manufacturing a circuit board. [Background technology]
[0002] BACKGROUND ART Substrates such as motherboards for portable electronic devices, system-in-package substrates, and chip-scale package substrates have been conventionally produced by laminating prepreg and copper foil onto a core layer to form a multilayer structure.
[0003] In recent years, with the increasing functionality and miniaturization of various devices, the use of resin sheets with metal foil has been considered for substrates such as motherboards for portable electronic devices in order to make the substrates thinner and allow for finer wiring while maintaining a certain level of mechanical strength. For example, Patent Document 1 describes a resin sheet with metal foil. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2022-43685 Summary of the Invention [Problem to be solved by the invention]
[0005] Metal foil-coated resin sheets are used as individual sheets, and are laminated on circuit boards in a vacuum heat press while in this state. However, resin chips can occur in individual sheets due to impacts that occur when processing the metal foil-coated resin sheets into individual sheets or when packaging and transporting the individual sheets.
[0006] One possible method for preventing resin chipping from occurring in individual sheets is to adhere a roll of a resin sheet with metal foil onto a circuit board, cut it, and then subject the cut resin sheet to a vacuum heat press. The resin sheet with metal foil is adhered to the circuit board with relatively weak adhesive strength by adhesion before cutting, and then adhered to the circuit board with relatively strong adhesive strength by vacuum heat press. Attaching the resin sheet with metal foil onto the circuit board before cutting is sometimes referred to as "temporary attachment" below. The temporary attachment of the resin sheet with metal foil can be performed using an appropriate temporary attachment device.
[0007] However, as a result of intensive research by the present inventors, it was found that when a resin sheet with a metal foil is temporarily attached to a circuit board using a temporary attachment machine, the temporary adhesion to the circuit board may be poor. It was also found that when a temporarily attached resin sheet with a metal foil is cut, resin chipping tends to occur at the cut surface due to differences in hardness between the metal foil and the resin sheet. Furthermore, it was found that when a temporarily attached resin sheet with a metal foil is pressed using a vacuum heat press, the resin contained in the resin composition layer may ooze out. Thus, the present inventors have discovered these new problems. Hereinafter, the property of a resin sheet with a metal foil temporarily adhering to a circuit board when temporarily attached to the circuit board may be referred to as "temporary attachment property," and the phenomenon in which a portion of the resin contained in the resin composition layer of a resin sheet with a metal foil flows out beyond the edge of the metal foil due to a vacuum heat press may be referred to as "resin oozing property."
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for manufacturing a circuit board that has excellent temporary attachment properties and is capable of suppressing resin chipping and resin seepage. [Means for solving the problem]
[0009] As a result of intensive research into the above-mentioned problems, the inventors discovered that the above-mentioned problems can be achieved by adjusting the Vickers hardness and minimum melt viscosity of the resin composition layer in the resin sheet with metal foil, and heating the temporarily attached resin sheet with metal foil while applying a predetermined pressure, and thus completed the present invention.
[0010] That is, the present invention includes the following. [1] (A) A step of preparing a roll-shaped resin sheet with a metal foil, the resin sheet having a metal foil and a resin composition layer, the resin composition layer having a Vickers hardness of 0.1 HV or more and 15 HV or less, and a minimum melt viscosity of 1,000 poise or more and 20,000 poise or less, wound into a roll; (B) a step of transporting a resin sheet with a metal foil from a roll-shaped resin sheet with a metal foil, arranging the resin sheet with the metal foil so that the resin composition layer of the resin sheet with the metal foil is joined to the circuit board, and attaching the resin sheet with the metal foil onto the circuit board; (C) cutting the resin sheet with the attached metal foil; and (D) heating the resin sheet with the attached metal foil while applying a pressure of 0.5 MPa or more and 1.5 MPa or less to thermally cure the resin composition layer. [2] The method for producing a circuit board according to [1], wherein the resin sheet with metal foil prepared in step (A) further comprises a protective film provided on the resin composition layer. [3] Before bonding the resin sheet with metal foil to the circuit board in step (B), (A-1) The method for producing a circuit board according to [2], comprising the step of peeling off the protective film. [4] The method for producing a circuit board according to any one of [1] to [3], wherein the thickness of the metal foil of the resin sheet with metal foil is 5 μm or less. [5] The method for producing a circuit board according to any one of [1] to [4], wherein the resin composition layer contains a thermosetting resin. [6] The method for producing a circuit board according to any one of [1] to [5], wherein the resin composition layer contains a polymer compound. [7] The method for producing a circuit board according to any one of [1] to [6], wherein the resin composition layer contains a curing accelerator. [8] The method for producing a circuit board according to any one of [1] to [7], wherein the resin composition layer contains an inorganic filler. [9] The method for producing a circuit board according to [6], wherein the polymer compound contains a thermoplastic resin.
[10] The method for producing a circuit board according to any one of [1] to [9], wherein the resin composition layer has a thickness of 3 μm or more and 60 μm or less.
[11] The resin composition layer contains a solvent, The solvent comprises an aromatic solvent having a boiling point of less than 115°C; The method for producing a circuit board according to any one of [1] to
[10] , wherein the content of aromatic solvents having a boiling point of less than 115°C is 0% by mass or more and 10% by mass or less, when the total amount of solvents contained in the resin composition layer is taken as 100% by mass.
[12] The resin composition layer contains a solvent, The solvent contains a solvent having a boiling point of 115°C or more and less than 200°C, The method for producing a circuit board according to any one of [1] to
[11] , wherein the content of the solvent having a boiling point of 115°C or more and less than 200°C is 55% by mass or more and 95% by mass or less, when the total amount of the solvent contained in the resin composition layer is 100% by mass.
[13] The resin composition layer contains a solvent, The solvent contains a solvent with a boiling point of 200°C or higher, The method for producing a circuit board according to any one of [1] to
[12] , wherein the content of the solvent having a boiling point of 200°C or higher is 0% by mass or more and 10% by mass or less, when the total amount of the solvent contained in the resin composition layer is taken as 100% by mass. [Effects of the Invention]
[0011] According to the present invention, it is possible to provide a method for manufacturing a circuit board that has excellent temporary attachment properties and is capable of suppressing resin chipping and resin seepage. [Brief explanation of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic end view of a resin sheet with a metal foil. [Figure 2] FIG. 2 is a diagram schematically illustrating the temporary attachment of a resin sheet with a metal foil to a circuit board by a temporary attachment device. DETAILED DESCRIPTION OF THE INVENTION
[0013] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that each drawing merely shows the shape, size, and arrangement of components in a schematic manner to the extent that the invention can be understood. The present invention is not limited by the following description, and each component can be modified as appropriate. In the drawings used in the following description, similar components are denoted by the same reference numerals, and redundant explanations may be omitted. Furthermore, the configuration according to the embodiments of the present invention may not necessarily be manufactured or used in the arrangement shown in the drawings.
[0014] Before describing the method for producing a circuit board of the present invention in detail, a resin sheet with a metal foil used in the method for producing a circuit board of the present invention will be described.
[0015] [Metal foil-coated resin sheet] The resin sheet with metal foil comprises a metal foil and a resin composition layer, the resin composition layer having a Vickers hardness of 0.1 HV or more and 15 HV or less and a minimum melt viscosity of 1000 poise or more and 20000 poise or less.
[0016] A resin sheet with metal foil includes a metal foil and a resin composition layer in this order. Usually, the metal foil and the resin composition layer are in direct contact with each other, and no other layer is provided between the metal foil and the resin composition layer.
[0017] FIG. 1 shows a schematic end view illustrating an example of a resin sheet with a metal foil. The resin sheet with a metal foil 1 includes a resin sheet 4 composed of a metal foil 2 and a resin composition layer 3 bonded to the metal foil 2. The resin sheet with a metal foil 1 may also include a protective film 5 provided so as to be bonded to the resin composition layer 3 of the resin sheet 4. The resin composition layer 3 and the protective film 5 are in direct contact with each other, and no other layer is provided between the resin composition layer 3 and the protective film 5. The resin composition layer 3 in FIG. 1 may be a prepreg in which a sheet-like fiber substrate such as glass cloth is impregnated with the components contained in the resin composition layer. The metal foil, resin composition layer, and protective film in the resin sheet with a metal foil will be described below.
[0018] <Metal foil> The resin sheet with metal foil of the present invention has a metal foil, and the conductor layer of the circuit board may be formed from the metal foil.
[0019] Examples of metal foils include copper foil and aluminum foil, with copper foil being preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0020] The metal foil may have a single layer structure or a multilayer structure in which two or more single metal layers or alloy layers made of different types of metals or alloys are laminated. Examples of multilayer metal foils include metal foils containing a carrier metal foil and an ultrathin metal foil bonded to the carrier metal foil. Such multilayer metal foils may include a release layer between the carrier metal foil and the ultrathin metal foil, which enables the ultrathin metal foil to be peeled from the carrier metal foil. The release layer is not particularly limited as long as it allows the ultrathin metal foil to be peeled from the carrier metal foil, and examples include an alloy layer of an element selected from the group consisting of Cr, Ni, Co, Fe, Mo, Ti, W, and P; an organic coating, etc. When a multilayer metal foil is used, a resin composition layer is provided on the ultrathin metal foil.
[0021] The thickness of the metal foil is preferably 5 μm or less, more preferably 4 μm or less, and even more preferably 3 μm or less, from the viewpoint of easily forming small diameter vias and producing a circuit board capable of fine wiring. There is no particular lower limit, but it can be 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, etc. When the metal foil has a multilayer structure including a carrier metal foil and an ultrathin metal foil bonded to the carrier metal foil, it is preferable that the thickness of the entire metal foil is in this range, and the thickness of the ultrathin metal foil may be, for example, in the range of 0.1 μm to 10 μm.
[0022] The arithmetic mean roughness (Ra) of the surface of the metal foil that is bonded to the resin composition layer is preferably 100 nm or more, preferably 200 nm or more, more preferably 300 nm or more, and even more preferably 400 nm or more, from the viewpoint of improving adhesion to the resin composition layer. There is no particular upper limit, but it is preferably 1000 nm or less, more preferably 900 nm or less, and even more preferably 800 nm or less. The arithmetic mean roughness (Ra) is a value measured in accordance with ISO 25178 and can be measured using a non-contact surface roughness meter. An example of a non-contact surface roughness meter is the "WYKO NT3300" manufactured by Veeco Instruments.
[0023] Commercially available metal foils may be used, such as "Microthin MT18Ex" manufactured by Mitsui Mining & Smelting Co., Ltd.; "HA-V2," "Microthin MT18FL," "3EC-III," "3EC-M3-VLP," "3EC-M2S-VLP," "JDLC," "JTCSLC," "HA-V2," "HA," and "HG" manufactured by JX Metals Corporation; and "CF-TX4-SV," "V9," "HD," "FLEQ HD," "FUTF," "RCF-T4X," and "RCF-T5B" manufactured by Fukuda Metal Foil & Powder Co., Ltd.
[0024] <Resin composition layer> The resin sheet with metal foil has a resin composition layer, which has a thermal curing function.
[0025] The Vickers hardness of the resin composition layer is 0.1 HV or more, preferably 0.2 HV or more, more preferably 0.3 HV or more, and even more preferably 1 or more. The upper limit is 15 HV or less, preferably 14 HV or less, more preferably 13 HV or less, and even more preferably 12 HV or less, 10 HV or less, or 8 HV or less. The Vickers hardness represents the degree of hardness of the resin composition layer before curing. Adjusting the Vickers hardness of the resin composition layer within this range allows the resin composition layer to have both a certain degree of flexibility and hardness. Therefore, the resin composition layer has a certain degree of flexibility, which can prevent resin chipping when cutting the metal foil-attached resin sheet, and a certain degree of hardness, which can prevent resin exudation during heat and pressure bonding in step (D). The Vickers hardness of the resin composition layer is the Vickers hardness before curing the resin composition layer, and can be measured by the method described in the Examples below. The Vickers hardness of the resin composition layer can be adjusted within this range by adjusting (b) the type and content of the polymer compound, and (d) the content of the inorganic filler, which will be described later.
[0026] The minimum melt viscosity of the resin composition layer is 1,000 poise or more, preferably 2,000 poise or more, and more preferably 3,000 poise or more. The upper limit is 20,000 poise or less, preferably 19,000 poise or less, and more preferably 18,000 poise or less. By adjusting the Vickers hardness of the resin composition layer to 0.1 HV or more and 15 HV or less and adjusting the minimum melt viscosity of the resin composition layer within this range, it is possible to improve tackiness and suppress resin chipping. Furthermore, in addition to these conditions, by heat-pressing the circuit board and the resin composition layer under low pressure conditions of a pressure (pressing force) of 0.5 MPa or more and 1.5 MPa or less in a vacuum hot press treatment, it is possible to improve tackiness, suppress resin chipping, and suppress resin exudation. The minimum melt viscosity of the resin composition layer can be measured by the method described in the Examples below. The minimum melt viscosity of the resin composition layer can be adjusted within this range by adjusting (b) the type and content of the polymer compound, and (d) the content of the inorganic filler, which will be described later.
[0027] The thickness of the resin composition layer is preferably 60 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less, from the viewpoint of forming small vias of 100 μm or less and providing a circuit board with fine wiring. The lower limit of the thickness of the resin composition layer is not particularly limited, but is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more.
[0028] The components contained in the resin composition layer preferably have sufficient hardness and insulating properties when cured. Examples of components contained in such a resin composition layer include (a) a thermosetting resin, (b) a polymer compound, (c) a curing accelerator, (d) an inorganic filler, and (e) an organic filler. The resin composition layer may also contain a solvent as a volatile component. The components contained in the resin composition layer are adjusted so that the Vickers hardness and minimum melt viscosity of the resin composition layer fall within the ranges.
[0029] Each component that may be contained in the resin composition layer will be described below. In the present invention, unless otherwise specified, the content of each component in the resin composition layer is a value when the nonvolatile components in the resin composition layer are taken as 100 mass %, and the nonvolatile components refer to all nonvolatile components in the resin composition layer excluding the solvent.
[0030] -(a)Thermosetting resin- The resin composition layer may contain a thermosetting resin (a) as the component (a). The type of the thermosetting resin (a) is not particularly limited as long as it can be cured by heat. One type of the thermosetting resin (a) may be used alone, or two or more types may be used in combination.
[0031] Examples of (a) thermosetting resins include epoxy resins, polyphenylene ether resins, radical polymerizable resins, phenolic resins, cyanate resins, active ester resins, carbodiimide resins, acid anhydride resins, amine resins, benzoxazine resins, and thiol resins. One type of thermosetting resin may be used alone, or two or more types may be used in combination.
[0032] From the viewpoint of achieving the remarkable effects of the present invention, it is preferable to use the (a) thermosetting resin in combination with an epoxy resin and a resin capable of reacting with the epoxy resin to cure the resin composition layer. Hereinafter, a resin capable of reacting with an epoxy resin to cure the resin composition layer may be referred to as a "curing agent." Examples of curing agents include phenolic resins, cyanate resins, active ester resins, carbodiimide resins, acid anhydride resins, amine resins, benzoxazine resins, and thiol resins. Among these, phenolic resins are preferred as the curing agent. One type of curing agent may be used alone, or two or more types may be used in combination. In one embodiment, the thermosetting resin includes an epoxy resin and a phenolic resin.
[0033] Epoxy resin is a thermosetting resin having epoxy groups. Examples of epoxy resins include tetramethylbisphenol-type epoxy resins, biphenyl-type epoxy resins, naphthalene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, bisphenol AF-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol novolac-type epoxy resins, phenol novolac-type epoxy resins, tert-butyl-catechol-type epoxy resins, naphthol-type epoxy resins, anthracene-type epoxy resins, glycidylamine-type epoxy resins, glycidyl ester-type epoxy resins, cresol novolac-type epoxy resins, phenol aralkyl-type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane-type epoxy resins, cyclohexanedimethanol-type epoxy resins, naphthylene ether-type epoxy resins, trimethylol-type epoxy resins, tetraphenylethane-type epoxy resins, isocyanurate-type epoxy resins, and phenolphthalimidine-type epoxy resins. The epoxy resin may be used alone or in combination of two or more.
[0034] The (a) thermosetting resin preferably contains an epoxy resin having two or more epoxy groups per molecule as the epoxy resin. The proportion of the epoxy resin having two or more epoxy groups per molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, relative to 100% by mass of the non-volatile components of the epoxy resin.
[0035] Epoxy resins include epoxy resins that are liquid at a temperature of 20°C (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20°C (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition layer may contain only a liquid epoxy resin as the epoxy resin, or may contain only a solid epoxy resin, or may contain a combination of a liquid epoxy resin and a solid epoxy resin.
[0036] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0037] Preferred liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexanedimethanol type epoxy resins, and epoxy resins having a butadiene structure, with bisphenol A type epoxy resins and bisphenol F type epoxy resins being more preferred.
[0038] Specific examples of liquid epoxy resins include "HP4032," "HP4032D," and "HP4032SS" (naphthalene-type epoxy resins) manufactured by DIC Corporation; "828US," "828EL," "jER828EL," "825," and "Epikote 828EL" (bisphenol A-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630," "630LSD," and "604" (glycidylamine-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol-type epoxy resin) manufactured by ADEKA Corporation; and "EP-3950L" and "EP-3980S" (glycidylamine-type epoxy resins) manufactured by ADEKA Corporation. epoxy resins); "EP-4088S" (dicyclopentadiene-type epoxy resin) manufactured by ADEKA Corporation; "ZX1059" (a mixture of bisphenol A-type epoxy resin and bisphenol F-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "EX-721" (glycidyl ester-type epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" manufactured by Daicel Corporation; "JP-100" and "JP-200" (epoxy resins having a butadiene structure (epoxidized polybutadiene resin) manufactured by Nippon Soda Co., Ltd.); and "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd. These may be used alone or in combination of two or more.
[0039] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred.
[0040] Preferred solid epoxy resins are tetramethylbisphenol-type epoxy resins, naphthalene-type epoxy resins, naphthalene-type tetrafunctional epoxy resins, naphthol novolac-type epoxy resins, cresol novolac-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol-type epoxy resins, biphenyl-type epoxy resins, naphthylene ether-type epoxy resins, anthracene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol AF-type epoxy resins, phenol aralkyl-type epoxy resins, tetraphenylethane-type epoxy resins, and phenolphthalimidine-type epoxy resins, with tetramethylbisphenol-type epoxy resins, biphenyl-type epoxy resins, and naphthalene-type epoxy resins being more preferred.
[0041] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; and "EXA-7311" and "EXA- 7311-G3, EXA-7311-G4, EXA-7311-G4S, HP6000 (naphthylene ether type epoxy resin); Nippon Kayaku's "EPPN-502H" (trisphenol type epoxy resin); Nippon Kayaku's "NC7000L" (naphthol novolac type epoxy resin); Nippon Kayaku's "NC3000H", "NC3000", "NC3000L", "NC3000FH", and "NC3100" (biphenyl type epoxy resin); Nippon Steel Chemical & Material's "ESN475V" and "ESN4100V" (naphthalene ether type epoxy resin). type epoxy resin); "ESN485" (naphthol-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", and "YL7890" (tetramethylbisphenol-type epoxy resin (bixylenol-type epoxy resin)) manufactured by Mitsubishi Chemical Corporation; "YL6121" (biphenyl-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YX8800" (anthracene-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; Mitsubishi Chemical Examples of epoxy resins include "YX7700" (phenol aralkyl type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals Co., Ltd.; "YX7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.These may be used alone or in combination of two or more.
[0042] When a liquid epoxy resin and a solid epoxy resin are used in combination as the epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably 1:0.01 to 1:20, more preferably 1:0.05 to 1:10, and particularly preferably 1:0.1 to 1:7.
[0043] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 3,000 g / eq., even more preferably 80 g / eq. to 2,000 g / eq., and particularly preferably 110 g / eq. to 1,000 g / eq. The epoxy equivalent represents the mass of the resin per equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.
[0044] The weight average molecular weight (Mw) of the epoxy resin is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.
[0045] From the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulating reliability, the content of the epoxy resin as (a) thermosetting resin is preferably 1% by mass or more, more preferably 5% by mass or more, and particularly preferably 10% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less, and particularly preferably 30% by mass or less, assuming that the non-volatile components in the resin composition layer are 100% by mass.
[0046] A specific example of the polyphenylene ether resin as component (a) is "NORYL SA90" manufactured by SABIC. A specific example of the polyetherimide resin is "Ultem" manufactured by GE. The polyphenylene ether resin may have one or more (preferably two or more) styryl groups or vinylphenyl groups in one molecule. Examples of such polyphenylene ether resins include styrene monomers, as well as "OPE-2St," "OPE-2St 1200," and "OPE-2St 2200" (all manufactured by Mitsubishi Gas Chemical Company, Inc.).
[0047] The type of radical polymerizable resin as component (a) is not particularly limited, as long as it has one or more (preferably two or more) radical polymerizable unsaturated groups in one molecule. Examples of radical polymerizable resins include resins having one or more radical polymerizable unsaturated groups selected from maleimide groups, vinyl groups, allyl groups, styryl groups, vinylphenyl groups, acryloyl groups, methacryloyl groups, fumaroyl groups, and maleoyl groups. Among these, from the viewpoint of significantly achieving the effects of the present invention, the radical polymerizable resin is preferably one or more selected from maleimide resins and (meth)acrylic resins, and more preferably maleimide resins.
[0048] The type of maleimide resin is not particularly limited as long as it has one or more (preferably two or more) maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule. Examples of maleimide resins include: (1) maleimide resins containing an aliphatic skeleton (preferably an aliphatic skeleton having 36 carbon atoms derived from dimer diamine), such as "BMI-3000J," "BMI-5000," "BMI-1400," "BMI-1500," "BMI-1700," and "BMI-689" (all manufactured by Designer Molecules), and "SLK6895-T90" (manufactured by Shin-Etsu Chemical Co., Ltd.); (2) maleimide resins containing an indane skeleton, as described in the Japan Institute of Invention and Innovation's Technical Disclosure Bulletin No. 2020-500211; and (3) maleimide resins containing an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000" (manufactured by Daiwa Kasei Co., Ltd.), and "BMI-80" (manufactured by Keiai Kasei Co., Ltd.).
[0049] The (meth)acrylic resin may be a monomer or an oligomer, and may be any type of (meth)acrylic resin, as long as it has one or more (preferably two or more) (meth)acryloyl groups in one molecule. Here, the term "(meth)acryloyl group" is a general term for acryloyl groups and methacryloyl groups. Examples of methacrylic resins include (meth)acrylate monomers, as well as (meth)acrylic resins such as "A-DOG" (manufactured by Shin-Nakamura Chemical Co., Ltd.), "DCP-A" (manufactured by Kyoeisha Chemical Co., Ltd.), "NPDGA," "FM-400," "R-687," "THE-330," "PET-30," and "DPHA" (all manufactured by Nippon Kayaku Co., Ltd.).
[0050] The phenolic resin may be a compound having one or more, preferably two or more, hydroxyl groups bonded to an aromatic ring such as a benzene ring or a naphthalene ring per molecule. When combined with an epoxy resin, the phenolic resin may react with the epoxy resin to harden the resin composition layer, and is therefore sometimes referred to as a "phenolic curing agent." From the viewpoint of achieving the remarkable effects of the present invention, the phenolic resin is preferably a phenolic resin having a novolac structure. Furthermore, from the viewpoint of adhesion, nitrogen-containing phenolic resins are preferred, and triazine skeleton-containing phenolic resins are more preferred. Of these, triazine skeleton-containing phenolic novolac resins are preferred from the viewpoint of achieving the remarkable effects of the present invention. Specific examples of phenolic resins include "MEH-7700," "MEH-7810," and "MEH-7851" manufactured by Meiwa Chemical Industry Co., Ltd.; "NHN," "CBN," and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "SN-170," "SN-180," "SN-190," "SN-475," "SN-485," "SN-495," "SN-375," and "SN-395" manufactured by Nippon Steel Chemical & Material Co., Ltd.; and "LA-7052," "LA-7054," "LA-3018," "LA-3018-50P," "LA-1356," "TD2090," "TD-2090-60M," and "KA-1163" manufactured by DIC Corporation.
[0051] The cyanate resin may be a compound having one or more, preferably two or more, cyanate groups in one molecule. When combined with an epoxy resin, the cyanate resin reacts with the epoxy resin to harden the resin composition layer, and therefore is sometimes called a "cyanate-based curing agent." Examples of cyanate resins include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylidene))benzene, bis(4-cyanatephenyl)thioether, and bis(4-cyanatephenyl)ether; multifunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate resins include "PT30" and "PT60" manufactured by Lonza (both of which are phenol novolac-type multifunctional cyanate resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been triazine-converted to form a trimer).
[0052] As the active ester resin, compounds having two or more highly reactive ester groups per molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are generally preferred. When combined with an epoxy resin, active ester resins can react with the epoxy resin to cure the resin composition layer, and are therefore sometimes referred to as "active ester curing agents." The active ester resin is preferably one obtained by the condensation reaction of a carboxylic acid compound and / or a thiocarboxylic acid compound with a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving resistance to high-temperature reflow blistering, active ester resins obtained from a carboxylic acid compound and a hydroxy compound are preferred, and active ester resins obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound are more preferred. Examples of carboxylic acid compounds include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalene, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, and phenol novolak. Here, "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one dicyclopentadiene molecule with two phenol molecules.
[0053] Specifically, the active ester resin is preferably a dicyclopentadiene-type active ester resin, a naphthalene-type active ester resin containing a naphthalene structure, an active ester resin containing an acetylated product of phenol novolac, or an active ester resin containing a benzoylated product of phenol novolac, and among these, at least one selected from a dicyclopentadiene-type active ester resin and a naphthalene-type active ester resin is more preferred. As the dicyclopentadiene-type active ester resin, an active ester resin containing a dicyclopentadiene-type diphenol structure is preferred.
[0054] Commercially available active ester resins include, for example, activated ester resins containing a dicyclopentadiene-type diphenol structure such as "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000L-65T", "HPC-8000", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation); activated ester resins containing a naphthalene structure such as "HP-B-8151-62T", "EXB-8100L-65T", and "EXB-8150-60T"; Examples of such active ester resins include "EXB-8150-62T," "EXB-9416-70BK," "HPC-8150-60T," "HPC-8150-62T," and "EXB-8" (manufactured by DIC Corporation); "EXB9401" (manufactured by DIC Corporation) as a phosphorus-containing active ester resin; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester resin which is an acetylated product of phenol novolac; "YLH1026," "YLH1030," and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester resins which are benzoylated products of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Inc.) as an active ester resin containing a styryl group and a naphthalene structure.
[0055] As the carbodiimide resin, a compound having one or more, preferably two or more, carbodiimide structures in one molecule can be used. When combined with an epoxy resin, the carbodiimide resin can react with the epoxy resin to harden the resin composition layer, and therefore is sometimes called a "carbodiimide-based curing agent." Specific examples of carbodiimide resins include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane-bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), poly(naphthalenecarbodiimide); Examples of polycarbodiimides include aromatic polycarbodiimides such as poly(methylenediphenylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide]. Commercially available carbodiimide resins include, for example, "Carbodilite V-02B," "Carbodilite V-03," "Carbodilite V-04K," "Carbodilite V-07," and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; and "Stavaxol P," "Stavaxol P400," and "Hykasil 510" manufactured by Lanxess AG.
[0056] As the acid anhydride resin, a compound having one or more, preferably two or more, acid anhydride groups in one molecule can be used. When combined with an epoxy group, the acid anhydride resin can react with the epoxy resin to harden the resin composition layer, and therefore is sometimes called an "acid anhydride curing agent." Specific examples of acid anhydride resins include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic anhydride. Examples of suitable anhydrides include hydrates, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid. Commercially available acid anhydride resins include, for example, "HNA-100," "MH-700," "MTA-15," "DDSA," and "OSA" manufactured by New Japan Chemical Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; "HN-2200" and "HN-5500" manufactured by Resonac Corporation; and "EF-30," "EF-40," "EF-60," and "EF-80" manufactured by Cray Valley Chemical Industries, Ltd.
[0057] The amine resin may be a compound having one or more, preferably two or more, amino groups in one molecule. When combined with an epoxy group, the amine resin may react with the epoxy resin to harden the resin composition layer, and is therefore sometimes referred to as an "amine-based curing agent." Examples of the amine resin include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines, with aromatic amines being preferred. The amine resin is preferably a primary amine or secondary amine, with primary amines being more preferred. Specific examples of amine resins include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-hydroxyphenyl)propionate. Examples of suitable bis(4-aminophenoxy)benzene include bis(4-aminophenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, and bis(4-(3-aminophenoxy)phenyl)sulfone. Commercially available amine resins include, for example, "SEIKACURE-S" manufactured by Seika Corporation; "KAYABOND C-200S," "KAYABOND C-100," "KAYAHARD AA," "KAYAHARD AB," and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd.; "Epicure W" manufactured by Mitsubishi Chemical Corporation; and "DTDA" manufactured by Sumitomo Seika Chemicals Co., Ltd.
[0058] Benzoxazine resins, when combined with epoxy resins, can react with the epoxy resin to cure the resin composition layer, and are therefore sometimes referred to as "benzoxazine-based curing agents." Specific examples of benzoxazine resins include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemicals Corporation.
[0059] Thiol resins, when combined with epoxy resins, can react with the epoxy resin to harden the resin composition layer, and are therefore sometimes referred to as "thiol-based curing agents." Examples of thiol resins include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.
[0060] The active group equivalent of the curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., still more preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The active group equivalent is the mass of the curing agent per equivalent of the active group.
[0061] The weight average molecular weight (Mw) of the curing agent is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.
[0062] When the number of epoxy groups in the epoxy resin is taken as 1, the number of active groups in the curing agent is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.1 or more, and preferably 5 or less, more preferably 3 or less, and particularly preferably 2 or less. The "number of epoxy groups in the epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile components of the epoxy resin present in the resin composition layer by the epoxy equivalent. Furthermore, the "number of active groups in the curing agent" refers to the total value obtained by dividing the mass of the non-volatile components of the curing agent present in the resin composition layer by the active group equivalent.
[0063] From the viewpoint of achieving a significant effect of the present invention, the content of the curing agent as (a) thermosetting resin is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 12% by mass or less, when the non-volatile components in the resin composition layer are taken as 100% by mass.
[0064] From the viewpoint of achieving a significant effect of the present invention, the content of the (a) thermosetting resin is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, and is preferably 65% by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less, or 50% by mass or less, when the non-volatile components in the resin composition layer are taken as 100% by mass.
[0065] -(b) High molecular compound- The resin composition layer may contain a (b) polymer compound as the (b) component. By including the polymer compound in the resin composition layer, the toughness and compatibility of the resin composition layer can be improved, and as a result, resin chipping can be suppressed. The (b) polymer compound may be used alone or in combination of two or more.
[0066] The (b) polymer compound can be one having a high weight-average molecular weight or a high number-average molecular weight. Such a component is preferably a thermoplastic resin. Examples of the thermoplastic resin include polyimide resin, polycarbonate resin, phenoxy resin, butyral resin, and copolymer. Of these, the (b) component is preferably at least one selected from phenoxy resin and butyral resin, from the viewpoint of setting the Vickers hardness of the resin composition layer within a desired range and reducing the minimum melt viscosity of the resin composition layer.
[0067] The polyimide resin may be a resin having an imide structure, and generally includes those obtained by an imidization reaction between a diamine compound and an acid anhydride.
[0068] The diamine compound for preparing the polyimide resin is not particularly limited, but examples thereof include aliphatic diamine compounds and aromatic diamine compounds.
[0069] Examples of the aliphatic diamine compound include linear aliphatic diamine compounds such as 1,2-ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-hexamethylenediamine, 1,5-diaminopentane, and 1,10-diaminodecane; branched aliphatic diamine compounds such as 1,2-diamino-2-methylpropane, 2,3-diamino-2,3-butane, and 2-methyl-1,5-diaminopentane; alicyclic diamine compounds such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,4-diaminocyclohexane, and 4,4'-methylenebis(cyclohexylamine); and dimer acid diamines (hereinafter also referred to as "dimer diamines"). The dimer acid diamine refers to a diamine compound obtained by substituting two terminal carboxylic acid groups (-COOH) of a dimer acid with an aminomethyl group (-CH2-NH2) or an amino group (-NH2). Dimer acid is a compound obtained by dimerizing an unsaturated fatty acid (preferably one having 11 to 22 carbon atoms, particularly preferably one having 18 carbon atoms), and its industrial production process is also known.
[0070] Examples of the aromatic diamine compound include a phenylenediamine compound, a naphthalenediamine compound, and a dianiline compound.
[0071] The phenylenediamine compound refers to a compound consisting of a benzene ring having two amino groups, and further, the benzene ring here may have 1 to 3 optional substituents. The substituents here are not particularly limited. Specific examples of the phenylenediamine compound include 1,4-phenylenediamine, 1,2-phenylenediamine, 1,3-phenylenediamine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobiphenyl, and 2,4,5,6-tetrafluoro-1,3-phenylenediamine.
[0072] The naphthalene diamine compound refers to a compound consisting of a naphthalene ring having two amino groups, and the naphthalene ring may have 1 to 3 optional substituents. The substituents are not particularly limited. Specific examples of the naphthalene diamine compound include 1,5-diaminonaphthalene, 1,8-diaminonaphthalene, 2,6-diaminonaphthalene, and 2,3-diaminonaphthalene.
[0073] A dianiline compound refers to a compound containing two aniline structures in the molecule, and each of the two benzene rings in the two aniline structures may further have one to three optional substituents. The substituents are not particularly limited. The two aniline structures in the dianiline compound may be bonded via a direct bond and / or one or two linker structures having 1 to 100 skeletal atoms selected from carbon, oxygen, sulfur, and nitrogen atoms. Dianiline compounds also include those in which two aniline structures are bonded via two bonds.
[0074] Specific examples of the "linker structure" in the dianiline compound include -NHCO-, -CONH-, -OCO-, -COO-, -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -CH=CH-, -O-, -S-, and -CO- , -SO2-, -NH-, -Ph-, -Ph-Ph-, -C(CH3)2-Ph-C(CH3)2-, -O-Ph-O-, -O-Ph-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-C(CH3)2-Ph-O-, -C(CH3)2-Ph-C(CH3)2-, groups represented by the following formulas (I) and (II), and groups consisting of combinations thereof. In this specification, "Ph" represents a 1,4-phenylene group, a 1,3-phenylene group, or a 1,2-phenylene group. [ka]
[0075] In one embodiment, specific examples of the dianiline compound include 4,4'-diamino-2,2'-ditrifluoromethyl-1,1'-biphenyl, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 4-aminophenyl 4-aminobenzoate, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis(4-aminophenyl)propane, 4,4'-(hexafluoroisopropylidene)dianiline, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-
[0033] 4,4'-(9-fluorenylidene)dianiline, 2,2-bis(3-methyl-4-aminophenyl)propane, 2,2-bis(3-methyl-4-aminophenyl)benzene, 4,4'-diamino-3,3'-dimethyl-1,1'-biphenyl, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 9,9'-bis(3-methyl-4-aminophenyl)fluorene, 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane, and the like.
[0076] The diamine compound may be a commercially available product or may be synthesized by a known method. The diamine compound may be used alone or in combination of two or more.
[0077] The acid anhydride used to prepare the polyimide resin is not particularly limited, but in a preferred embodiment, it is an aromatic tetracarboxylic dianhydride, such as benzenetetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, anthracenetetracarboxylic dianhydride, or diphthalic dianhydride, preferably diphthalic dianhydride.
[0078] Benzenetetracarboxylic dianhydride means a dianhydride of benzene having four carboxy groups, and further, the benzene ring here may have 1 to 3 optional substituents, such as a halogen atom, a cyano group, and -X 33 -R 33 (The same definition as in the following formula (B1)) Specific examples of the benzenetetracarboxylic dianhydride include pyromellitic dianhydride and 1,2,3,4-benzenetetracarboxylic dianhydride.
[0079] Naphthalenetetracarboxylic dianhydride refers to a dianhydride of naphthalene having four carboxy groups, and the naphthalene ring here may optionally have 1 to 3 substituents, such as halogen atoms, cyano groups, and -X 33 -R 33 (The same definition as in the following formula (B1)) Specific examples of the naphthalenetetracarboxylic dianhydride include 1,4,5,8-naphthalenetetracarboxylic dianhydride and 2,3,6,7-naphthalenetetracarboxylic dianhydride.
[0080] Anthracenetetracarboxylic dianhydride refers to a dianhydride of anthracene having four carboxy groups, and the anthracene ring here may optionally have 1 to 3 substituents, such as halogen atoms, cyano groups, and -X 33 -R 33(The same definition as in the following formula (B1)) is preferred. Specific examples of the anthracenetetracarboxylic dianhydride include 2,3,6,7-anthracenetetracarboxylic dianhydride.
[0081] Diphthalic dianhydride refers to a compound containing two phthalic anhydrides in the molecule, and each of the two benzene rings in the two phthalic anhydrides may have one to three optional substituents. The substituents include halogen atoms, cyano groups, and -X 33 -R 33 (the same as the definition in the following formula (B1)) is preferred. The two phthalic anhydrides in the diphthalic dianhydride may be bonded to each other by a direct bond or via a linker structure having 1 to 100 skeletal atoms selected from carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms. Examples of diphthalic dianhydrides include those represented by the formula (B1): [ka] [In formula (B1), R 11 and R 12 are each independently a halogen atom, a cyano group, a nitro group, or -X 33 -R 33 indicates, X 33 are each independently a single bond, -NR 33’ -, -O-, -S-, -CO-, -SO2-, -NR 33’ CO-, -CONR 33’ -, -OCO-, or -COO-; R 33 each independently represents a substituted or unsubstituted alkyl group or a substituted or unsubstituted alkenyl group, R 33’ each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted alkenyl group, Y represents a single bond or a linker structure having 1 to 100 skeletal atoms selected from carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms; n1 and m1 each independently represent an integer of 0 to 3.] Examples of the compound include compounds represented by the following formula:
[0082] Y is preferably a linker structure having 1 to 100 skeletal atoms selected from carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms. n1 and m1 are preferably 0.
[0083] The "linker structure" in Y has 1 to 100 skeletal atoms selected from carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms. The "linker structure" is preferably -[A1-Ph] a10 -A1-[Ph-A1] b10 - (wherein each A1 independently represents a single bond, -(substituted or unsubstituted alkylene group)-, -O-, -S-, -CO-, -SO2-, -CONH-, -NHCO-, -COO-, or -OCO-, and each a10 and b10 independently represents an integer of 0 to 2 (preferably 0 or 1).)
[0084] Specific examples of the "linker structure" for Y include -CH-, -CHCH-, -CHCHCH-, -CHCHCHCH-, -CHCHCHCHCH-, -CHCHCHCHCHCH-, -CH(CH)-, -C(CH)-, -O-, -CO-, -SO-, -Ph-, -O-Ph-O-, -O-Ph-SO-Ph-O-, -O-Ph-C(CH)-Ph-O-, etc. In this specification, "Ph" represents a 1,4-phenylene group, a 1,3-phenylene group, or a 1,2-phenylene group.
[0085] Specific examples of diphthalic dianhydrides include 4,4'-oxydiphthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2, 3,3',4'-Biphenyltetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-diphenylethertetracarboxylic dianhydride, 2,3,3',4'-diphenylsulfonetetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenoxyphenyl)sulfone dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethynylidene-4 ,4'-Diphthalic dianhydride, 2,2-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenyl)benzene dianhydride Examples of the dianhydride include 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, and 4,4'-(4,4'-isopropylidenediphenoxy)bisphthalic dianhydride.
[0086] The acid anhydride may be commercially available or may be synthesized by a known method or a method similar thereto. The acid anhydride may be used alone or in combination of two or more.
[0087] Commercially available polyimide resins can be used, including "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd.
[0088] Polycarbonate resins are resins having a carbonate structure. Examples of such resins include carbonate resins without reactive groups, hydroxyl group-containing carbonate resins, phenolic hydroxyl group-containing carbonate resins, carboxyl group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, urethane group-containing carbonate resins, and epoxy group-containing carbonate resins. Here, the reactive group refers to a functional group that can react with other components, such as a hydroxy group, a phenolic hydroxyl group, a carboxy group, an acid anhydride group, an isocyanate group, a urethane group, or an epoxy group.
[0089] Commercially available carbonate resins can be used, including "FPC0220" and "FPC2136" manufactured by Mitsubishi Gas Chemical Co., Inc., and "T6002" and "T6001" (polycarbonate diol) manufactured by Asahi Kasei Corporation.
[0090] Examples of phenoxy resins include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A, bisphenol F, bisphenol S, bisphenolacetophenone, novolac, biphenyl, fluorene, dicyclopentadiene, norbornene, naphthalene, anthracene, adamantane, terpene, and trimethylcyclohexane. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.
[0091] Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both of which are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YL7500BH30," "YX6954BH30," "YX7553," "YX7553BH30," "YL7769BH30," "YL6794," "YL7213," "YL7290," and "YL7482" manufactured by Mitsubishi Chemical Corporation.
[0092] Butyral resins are resins having butyral groups in their molecules. Specific examples of butyral resins include the S-LEC BH series, BX series (e.g., BX-5Z), KS series (e.g., KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0093] The copolymer is preferably a copolymer containing at least two or more selected from repeating units having a structure obtained by polymerizing styrene (styrene units), repeating units having a structure obtained by polymerizing ethylene (ethylene units), repeating units having a structure obtained by polymerizing propylene (propylene units), repeating units having a structure obtained by polymerizing isoprene (isoprene units), repeating units having a structure obtained by polymerizing butadiene (butadiene units), repeating units having a structure obtained by polymerizing hydrogenated butadiene (hydrogenated butadiene units), repeating units having a structure obtained by polymerizing acrylic acid (acrylate units), and repeating units having a structure obtained by polymerizing methacrylic acid (methacrylate units).
[0094] Specific examples of the copolymer include styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), styrene-butadiene-butylene-styrene block copolymer (SBBS), styrene-butadiene diblock copolymer, hydrogenated styrene-butadiene block copolymer, hydrogenated styrene-isoprene block copolymer, hydrogenated styrene-butadiene random copolymer, and styrene-maleic anhydride copolymer.
[0095] From the viewpoint of obtaining a cured product that more significantly exhibits the intended effects of the present invention, the weight average molecular weight (Mw) of component (b) is preferably greater than 5,000, more preferably at least 8,000, and particularly preferably at least 10,000, and is preferably not more than 100,000, more preferably not more than 80,000, and particularly preferably not more than 50,000. The weight average molecular weight of component (b) is the weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0096] From the viewpoint of reducing the minimum melt viscosity of the resin composition layer, the number average molecular weight (Mn) of component (b) is preferably 5,000 or more, more preferably 8,000 or more, particularly preferably 10,000 or more, and preferably 100,000 or less, more preferably 80,000 or less, particularly preferably 50,000 or less. The number average molecular weight can be measured as described below. It should be noted that component (b) only needs to have either the weight average molecular weight or the number average molecular weight within the above-mentioned range. For example, when the molecular weight of component (b) is generally handled in terms of the weight average molecular weight, the number average molecular weight does not need to be within the above-mentioned range. Similarly, when the molecular weight of component (b) is generally handled in terms of the number average molecular weight, the weight average molecular weight does not need to be within the above-mentioned range.
[0097] The number average molecular weight can be measured by the following method: 100 mg of component (b) and 5 g of dispersant (N-methylpyrrolidone, manufactured by Kanto Chemical Co., Ltd.) are weighed into a vial and dispersed ultrasonically for 20 minutes. The mixture is then filtered using a membrane filter (Advantec, manufactured by Toyo Roshi Kaisha, Ltd., 0.5 μm cutoff), and the number average molecular weight (Mn) is calculated using a gel permeation chromatograph (Shodex GPC-101, manufactured by Shoko Scientific Co., Ltd.).
[0098] The content of component (b) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, and is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, when the non-volatile components in the resin composition layer are taken as 100% by mass, from the viewpoint of setting the Vickers hardness of the resin composition layer within the desired range and reducing the minimum melt viscosity of the resin composition layer.
[0099] -(c) Curing accelerator- The resin composition layer may contain a (c) curing accelerator as the (c) component. The (c) curing accelerator as the (c) component does not include those corresponding to the above-mentioned (a) and (b). The (c) curing accelerator functions as a curing catalyst that accelerates the curing of the epoxy resin in the (a) component.
[0100] As the (c) curing accelerator, a compound that accelerates the curing of the epoxy resin can be used. Examples of such (c) curing accelerators include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators, with imidazole-based curing accelerators being preferred. One type of (c) curing accelerator may be used alone, or two or more types may be used in combination.
[0101] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitate, tetrabutylphosphonium hydrogenhexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butyldimethylphosphonium tetraphenylborate; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, p-tolyltriphenylphosphonium tetra-p-tolylborate, and tetraphenylphosphonium tetra-p-tolylborate. aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine aromatic phosphines such as benzene, tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether;
[0102] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as toluene bis(dimethylurea), 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].
[0103] Examples of guanidine curing accelerators include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.
[0104] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct Examples of imidazole compounds include 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds with epoxy resins. Commercially available imidazole curing accelerators include "1B2PZ," "2E4MZ," "2MZA-PW," "2MZ-OK," "2MA-OK," "2MA-OK-PW," "2PHZ," "2PHZ-PW," "Cl1Z," "Cl1Z-CN," "Cl1Z-CNS," and "C11Z-A" manufactured by Shikoku Chemicals Corporation; and "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0105] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organic cobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organic copper complexes such as copper(II) acetylacetonate, organic zinc complexes such as zinc(II) acetylacetonate, organic iron complexes such as iron(III) acetylacetonate, organic nickel complexes such as nickel(II) acetylacetonate, and organic manganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0106] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, etc. Commercially available amine curing accelerators may be used, such as "MY-25" manufactured by Ajinomoto Fine-Techno Co., Inc.
[0107] In order to obtain the effects of the present invention more significantly, the content of the (c) curing accelerator is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and even more preferably 0.04% by mass or more, and is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.3% by mass or less, when the non-volatile components in the resin composition layer are taken as 100% by mass.
[0108] -(d) Inorganic filler- The resin composition layer may contain an inorganic filler as component (d). The (d) inorganic filler is contained in the resin composition layer in the form of particles. An inorganic compound is used as the material for the (d) inorganic filler. Examples of materials for the (d) inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium titanate zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Spherical silica is preferred. (d) The inorganic filler may be used alone or in any combination of two or more types in any ratio.
[0109] (d) Examples of commercially available inorganic fillers include "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C," "YA050C," "YA050C-MJE," "YA010C," "SC2500SQ," "SO-C4," "SO-C2," and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30," "DAW-03," and "FB-105FD" manufactured by Denka Company, Limited; "Silfil NSS-3N," "Silfil NSS-4N," and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "CellSpheres" and "MGH-005" manufactured by Taiheiyo Cement Corporation; and "Sfereek" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0110] The average particle size of the (d) inorganic filler is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less, even more preferably 2 μm or less, and particularly preferably 1.5 μm or less. The lower limit of the average particle size of the (d) inorganic filler is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more. The average particle size of the (d) inorganic filler can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, a particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution analyzer, and the median diameter is used as the average particle size. A measurement sample can be prepared by weighing 100 mg of inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it ultrasonically for 10 minutes. The measurement sample was measured using a laser diffraction particle size distribution analyzer, with blue and red light source wavelengths used, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell system, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution analyzer is the "LA-960" manufactured by Horiba, Ltd.
[0111] (d) The specific surface area of the inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 The upper limit of the specific surface area of the (A) inorganic filler is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, and even more preferably 30m 2 / g or less, particularly preferably 10m 2The specific surface area of the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and then calculating the specific surface area using the BET multipoint method.
[0112] (d) From the viewpoint of improving moisture resistance and dispersibility, the inorganic filler is preferably treated with a surface treatment agent. Examples of the surface treatment agent include a fluorine-containing silane coupling agent, an aminosilane coupling agent, an epoxysilane coupling agent, a mercaptosilane coupling agent, a silane coupling agent, an alkoxysilane, an organosilazane compound, and a titanate coupling agent. The surface treatment agent may be used alone or in any combination of two or more.
[0113] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).
[0114] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably 0.2% to 3% by mass, and even more preferably 0.3% to 2% by mass.
[0115] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition layer or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1.0 mg / m 2 Less than 0.8 mg / m is preferred 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:
[0116] (d) The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.
[0117] From the viewpoint of setting the Vickers hardness of the resin composition layer within a desired range and reducing the minimum melt viscosity of the resin composition layer, the content of the (d) inorganic filler is preferably 25% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, when the nonvolatile components of the resin composition layer are taken as 100% by mass. The upper limit is preferably 85% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less.
[0118] -(e)Organic filler- The resin composition layer may contain an organic filler (e) as component (e). The organic filler (e) as component (e) does not include those corresponding to the above-mentioned components (a) to (d). As the organic filler, any organic filler that can be used when forming an insulating layer of a printed wiring board may be used, and examples thereof include rubber particles, polyamide fine particles, silicone particles, etc.
[0119] As the rubber particles, commercially available products may be used, such as "EXL2655" manufactured by Dow Chemical Japan, and "AC3401N" and "AC3816N" manufactured by Aica Kogyo Co., Ltd.
[0120] In order to obtain a significant effect of the present invention, the content of (e) the organic filler is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, and is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, when the non-volatile components in the resin composition layer are taken as 100% by mass.
[0121] -(f) Other additives- The resin composition layer may contain (f) other additives as an optional non-volatile component. Examples of the optional additives (f) include organic fillers, polymerization initiators, organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds, colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black, polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine, leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents, thickeners such as bentone and montmorillonite, antifoaming agents such as silicone-based antifoaming agents, acrylic-based antifoaming agents, fluorine-based antifoaming agents, and vinyl resin-based antifoaming agents, ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers, adhesion improvers such as urea silanes, adhesion promoters such as triazole-based adhesion promoters, tetrazole-based adhesion promoters, and triazine-based adhesion promoters, and hindered phenolic acids. surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, and red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers; photopolymerization initiation aids such as tertiary amines; and photosensitizers such as pyrarizones, anthracenes, coumarins, xanthones, and thioxanthones. (f) The optional additives may be used singly or in combination of two or more.
[0122] The resin composition layer may contain a solvent as a volatile component. An organic solvent is typically used as the solvent. Solvents can be classified into solvents with a boiling point of less than 115°C, solvents with a boiling point of 115°C or higher but lower than 200°C, and solvents with a boiling point of 200°C or higher. These may be used alone or in combination of two or more. The boiling point here refers to the boiling point under atmospheric pressure (760 mmHg).
[0123] Solvents with a boiling point of less than 115°C include aromatic solvents that contain an aromatic ring in the molecule and have a boiling point of less than 115°C, and non-aromatic solvents that do not contain an aromatic ring in the molecule and have a boiling point of less than 115°C. Examples of solvents with a boiling point of less than 115°C include non-aromatic solvents such as methyl ethyl ketone (MEK) (boiling point 80°C), ethyl acetate (boiling point 77°C), and cyclohexane (boiling point 80.7°C); and aromatic solvents such as toluene (boiling point 111°C).
[0124] Solvents having a boiling point of 115°C or higher and lower than 200°C include aromatic solvents that contain an aromatic ring in the molecule and have a boiling point of 115°C or higher and lower than 200°C, and non-aromatic solvents that do not contain an aromatic ring in the molecule and have a boiling point of 115°C or higher and lower than 200°C. Examples of solvents having a boiling point of 115°C or higher and lower than 200°C include cyclohexanone (boiling point 153°C), 2-methoxypropanol (boiling point 119°C), methyl cellosolve (boiling point 124.5°C), butyl cellosolve (boiling point 171.2°C), methyl carbitol (boiling point 194°C), butyl acetate (boiling point 126°C), butyl cellosolve acetate (boiling point 191°C), propylene glycol monomethyl ether (boiling point 120°C), propylene glycol monoethyl ether (boiling point 132°C), and propylene glycol. Examples of suitable solvents include non-aromatic solvents such as dipropylene glycol monopropyl ether (boiling point 150°C), propylene glycol monobutyl ether (boiling point 170°C), dipropylene glycol monomethyl ether (boiling point 188°C), dipropylene glycol monoethyl ether (boiling point 198°C), dipropylene glycol monoethyl ether (boiling point 132.8°C), octane (boiling point 125°C), and decane (boiling point 174.2°C); and aromatic solvents such as xylene (boiling point 138°C to 144°C) and tetramethylbenzene (boiling point 197°C).
[0125] Solvents with a boiling point of 200°C or higher include aromatic solvents that contain an aromatic ring in the molecule and have a boiling point of 200°C or higher, and non-aromatic solvents that do not contain an aromatic ring in the molecule and have a boiling point of 200°C or higher. Examples of solvents with a boiling point of 200°C or higher include non-aromatic solvents such as N-methyl-2-pyrrolidone (NMP) (boiling point 204°C), butyl carbitol (boiling point 230.6°C), carbitol acetate (boiling point 217°C), dipropylene glycol monopropyl ether (boiling point 210°C), dipropylene glycol monobutyl ether (boiling point 215°C), and triethylene glycol monoethyl ether (boiling point 256°C); and aromatic solvents such as acetophenone (boiling point 202°C), benzyl alcohol (boiling point 205°C), anisole (boiling point 154°C), phenetole (boiling point 169°C), methyl benzoate (boiling point 198-200°C), and ethyl benzoate (boiling point 211-213°C).
[0126] The amount of the solvent having a boiling point of less than 115°C is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 37% by mass or less, when the total amount of solvents contained in the resin composition layer is taken as 100% by mass. The lower limit is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more. The amount of the solvent can be measured by the method described in the Examples below.
[0127] The amount of aromatic solvents having a boiling point of less than 115°C is preferably 15% by mass or less, more preferably 14% by mass or less, even more preferably 10% by mass or less, 5% by mass or less, or 1% by mass or less, when the total amount of solvents contained in the resin composition layer is taken as 100% by mass. The lower limit is preferably 0% by mass, more preferably 0% by mass or more, and even more preferably 0.5% by mass or more. The amount of the solvent can be measured by the method described in the Examples below.
[0128] The amount of the non-aromatic solvent having a boiling point of less than 115°C is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 37% by mass or less, when the total amount of solvents contained in the resin composition layer is taken as 100% by mass. The lower limit is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more. The amount of the solvent can be measured by the method described in the Examples below.
[0129] The solvent having a boiling point of 115°C or higher but lower than 200°C preferably accounts for 95% by mass or less, more preferably 93% by mass or less, and even more preferably 90% by mass or less, when the total amount of solvents contained in the resin composition layer is taken as 100% by mass. The lower limit is preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 63% by mass or more. The amount of the solvent can be measured by the method described in the Examples below.
[0130] The amount of the solvent having a boiling point of 200°C or higher is preferably 10% by mass or less, more preferably 8% by mass or less, even more preferably 5% by mass or less, 3% by mass or less, or 1% by mass or less, when the total amount of the solvent contained in the resin composition layer is taken as 100% by mass. The lower limit is preferably 0% by mass, more preferably 0% by mass or more, and even more preferably 0.5% by mass or more. The amount of the solvent can be measured by the method described in the examples below.
[0131] The amount of solvent contained in the resin sheet with metal foil (residual solvent amount) is preferably small from the viewpoint of adjusting the minimum melt viscosity of the resin composition layer. The amount of solvent in the resin composition layer (residual solvent amount) is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2.5% by mass or less, and even more preferably 2% by mass or less, when the mass of the entire resin composition layer is taken as 100% by mass. There is no particular lower limit, but it is preferably 0.0001% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.1% by mass or more. The residual solvent amount can be determined from the mass loss rate, and specifically can be measured by the method described in the Examples below.
[0132] <Protective film> The resin sheet with metal foil may have a protective film. By laminating the protective film on the resin sheet with metal foil, adhesion of dust and the like to the surface of the resin composition layer and scratches can be suppressed.
[0133] Examples of the protective film include films made of plastic materials, metal foils, and release papers, with films made of plastic materials being preferred.
[0134] When a film made of a plastic material is used as the protective film, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, with inexpensive polyethylene terephthalate being particularly preferred.
[0135] When a metal foil is used as the protective film, examples of the metal foil include copper foil and aluminum foil, with copper foil being preferred. The copper foil may be a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).
[0136] The surface of the protective film that is to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0137] The protective film may also be a protective film with a release layer, which has a release layer on the surface that bonds to the resin composition layer. Examples of the release agent used in the release layer of the protective film with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Commercially available protective films with a release layer may be used, including, for example, "SK-1," "AL-5," and "AL-7" manufactured by Lintec Corporation, "Lumirror T60," "Lumirror R80," and "Lumirror" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Uni-Peel" manufactured by Unitika Limited, which are PET films having a release layer primarily composed of an alkyd resin-based release agent.
[0138] The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. When the protective film has a multi-layer structure such as a protective film with a release layer, it is preferable that the thickness of the entire protective film is in this range.
[0139] <Method for manufacturing a resin sheet with a metal foil, and method for manufacturing a roll-shaped resin sheet with a metal foil> A method for producing a resin sheet with metal foil includes, for example, preparing a resin varnish by dissolving the components contained in the resin composition layer in a solvent, applying the resin varnish to a protective film using a die coater or the like, and then drying the varnish to form a resin composition layer on the protective film. Next, a metal foil is laminated to the surface of the resin composition layer using a roll laminator or the like, thereby producing a resin sheet with metal foil. The solvent may be one of those described above.
[0140] Drying may be carried out by known methods such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is carried out so that the content of organic solvent in the resin composition layer becomes 10% by mass or less, preferably 5% by mass or less. Although this varies depending on the boiling point of the solvent in the resin varnish, for example, when a resin varnish containing 30% by mass to 60% by mass of solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 to 10 minutes.
[0141] The resin sheet with metal foil may be produced by applying a resin varnish onto a metal foil and then drying it to form a resin composition layer.
[0142] When the resin composition layer in the metal foil-attached resin sheet is a prepreg, a sheet-like fiber substrate is impregnated with a resin varnish or components contained in the resin composition layer by a known method such as a hot melt method or a solvent method, and then dried to produce a prepreg. The prepreg is then laminated with a metal foil to produce a prepreg. The sheet-like fiber substrate can be a commonly used substrate for prepregs, such as glass cloth.
[0143] The resin sheet with metal foil can be produced in roll form by winding it into a roll. The resin sheet with metal foil is preferably wound with the metal foil on the outside and the protective film on the inside. Usually, the resin sheet with metal foil is wound around a cylindrical or cylindrical winding core.
[0144] From the viewpoint of significantly obtaining the effects of the present invention, the winding diameter of the roll-shaped resin sheet with metal foil is preferably 5 cm or more, more preferably 6 cm or more, and even more preferably 7 cm or more, and is preferably 20 cm or less, more preferably 16 cm or less, and even more preferably 12 cm or less. The winding diameter of the roll-shaped resin sheet with metal foil refers to the diameter of the winding core.
[0145] [Circuit board manufacturing method] The method for manufacturing a circuit board of the present invention comprises the steps of: (A) preparing a roll-shaped resin sheet with a metal foil; (B) a step of transporting a resin sheet with a metal foil from a roll-shaped resin sheet with a metal foil, arranging the resin sheet with the metal foil so that the resin composition layer of the resin sheet with the metal foil is joined to the circuit board, and attaching the resin sheet with the metal foil onto the circuit board; (C) cutting the resin sheet with the attached metal foil; and (D) A step of heating the resin sheet with the attached metal foil while applying a pressure of 0.5 MPa or more and 1.5 MPa or less to thermally cure the resin composition layer.
[0146] Furthermore, the method for manufacturing a circuit board of the present invention may, if necessary, include the following step (A-1) after step (A) and before attaching (temporarily attaching) the resin sheet with metal foil to the circuit board in step (B): (A-1) A step of peeling off the protective film.
[0147] This method of manufacturing a circuit board provides excellent temporary attachment properties, suppresses resin chipping and resin seepage, and generally enables the manufacture of a circuit board having an insulating layer with excellent reflow resistance.
[0148] In step (A), a roll-shaped resin sheet with a metal foil is prepared as described above.
[0149] When the roll-shaped resin sheet with metal foil further comprises a protective film, after step (A), the protective film is peeled off from the resin sheet with metal foil in step (A-1) before the resin sheet with metal foil is attached to a circuit board in step (B).
[0150] FIG. 2 is a schematic diagram showing an example of a temporary bonding device. The temporary bonding device (auto-cutter device) 10 peels off the protective film 5 from a roll-shaped resin sheet 11 with a metal foil and temporarily bonds the resin sheet 4, with the resin composition layer exposed, to a circuit board 6 so that the resin composition layer is bonded to the circuit board 6. As shown in FIG. 2, in step (A), a roll-shaped resin sheet 11 with a metal foil, which has been pre-slit to an appropriate width, is set in the temporary bonding device 10. The metal foil-equipped resin sheet 1 is transported from the roll-shaped resin sheet 11 with the metal foil, and step (A-1) is performed to peel off the protective film 5 from the resin sheet 1 with the metal foil. In detail, step (A-1) is performed in which the protective film 5 is peeled off from the resin sheet 1 with the metal foil as the resin sheet 1 with the metal foil passes through a protective film removal tool (jig) 13. The peeled protective film 5 can be collected by a protective film take-up roll 12. The shape and mechanism of the protective film remover 13 are not particularly limited, and may be, for example, cylindrical (such as a roll) or prismatic (such as a blade). The angle at which the protective film is removed relative to the conveyance direction of the metal foil-coated resin sheet 1 is not particularly limited, and may be set arbitrarily.
[0151] In step (B), the resin sheet with metal foil is transported from the roll-shaped resin sheet with metal foil, and positioned so that the resin composition layer of the resin sheet with metal foil is joined to the circuit board, and the resin sheet with metal foil is attached (temporarily attached) onto the circuit board.
[0152] 2 shows an embodiment in which a resin sheet 4 from which a protective film 5 has been peeled off is provided on one side (the upper side in FIG. 2) of a circuit board 6, and a roll of a resin sheet 11 with a metal foil is set above the circuit board 6. Below, an embodiment in which a resin sheet 4 is provided on one side of the circuit board 6 will be described based on the description of FIG. 2, but it is also possible to set another roll of an adhesive sheet 11 with a metal foil below the circuit board 6, and provide resin sheets 4 on both sides of the circuit board 6.
[0153] The conveying speed of the metal foil-attached resin sheet 1 (or resin sheet 4) in step (B) is not particularly limited, but from the viewpoint of contributing to an improvement in the production speed of circuit boards, the conveying speed is preferably 1 m / min or more, more preferably 2 m / min or more, and even more preferably 3 m / min or more. The upper limit is not particularly limited, but it can be 10 m / min or more.
[0154] The means for transporting the resin sheet 1 (or resin sheet 4) with metal foil in step (B) is not particularly limited, and can be carried out mechanically, for example, by fixing the resin sheet by vacuum adsorption from the metal foil side.
[0155] In step (B), the transported resin sheet 4 with the exposed resin composition layer is arranged so that the resin composition layer is bonded to the circuit board 6. For example, the resin sheet 4 can be aligned with the circuit board 6 transported by a conveyor device 15 using guide rolls 16 and 17.
[0156] The circuit board 6 mainly refers to a substrate such as a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, etc., on one or both sides of which a patterned conductor layer (circuit) is formed. In addition, the "circuit board" of the present invention also includes an inner layer circuit board, which is an intermediate product on which an insulating layer and / or a conductor layer is to be further formed when manufacturing a printed wiring board.
[0157] After the resin composition layer is positioned so as to be bonded to the circuit board 6, the metal foil-attached resin sheet (resin sheet) 4 from which the protective film 5 has been peeled off is attached (temporarily attached) to the circuit board 6. The temporary attachment can be performed, for example, by heating and pressurizing a portion of the resin sheet 4 from the metal foil side using a heater (not shown) or the like in an unnecessary portion that does not overlap with the circuit board 6 and requires heat pressing treatment, among a portion of the front in the feeding direction of the circuit board 6 (a portion on the right side of the circuit board 6 in FIG. 2 ), thereby partially temporarily attaching the resin sheet 4 to the circuit board 6. The heating temperature when partially press-bonding the resin sheet 4 to the circuit board 6 depends on the melt viscosity characteristics of the resin composition layer, but is preferably 60°C to 130°C, more preferably 60°C to 120°C. The heating time is preferably 1 second to 20 seconds, more preferably 5 seconds to 15 seconds. The pressure during press-bonding is preferably 0.02 kgf / cm 2 ~0.25kgf / cm 2 (0.196N / m 2 ~2.45N / m 2 ), more preferably 0.05 kgf / cm 2 ~0.20kgf / cm 2 (0.49N / m 2 ~1.96N / m 2 )
[0158] After step (B) is completed, the resin sheet 4 is cut by a cutter 14 according to the size of the circuit board 6. When cutting, it is preferable to install a cutter backup heater heated to a temperature in the range of 40°C to 80°C in order to significantly obtain the effects of the present invention.
[0159] All of the above steps (A) to (C) can be performed continuously in a temporary bonding device. Examples of commercially available temporary bonding devices include the Mach series dry film laminator manufactured by Hakuto Co., Ltd., the auto cutter FAC500, SAC-500, and SAC-500 / 600 manufactured by Shin-ei Kiko Co., Ltd., and the NT-100 and NT-300 manufactured by Nikko Materials Co., Ltd.
[0160] In step (D), the resin sheet with the attached (temporarily attached) metal foil is heated while applying a pressure of 0.5 MPa to 1.5 MPa to thermally cure the resin composition layer. Step (D) is usually performed using a vacuum heat press treatment device, and the details of step (D) are as follows: the temporarily attached metal foil resin sheet is placed in the vacuum heat press treatment device, and a vacuum heat press treatment is performed to heat and press-bond the circuit board and the resin composition layer together under a pressure of 0.5 MPa to 1.5 MPa. Next, the resin composition layer is thermally cured.
[0161] In step (D), the circuit board and the resin composition layer are heat-pressed together under a low pressure of 0.5 MPa to 1.5 MPa in a vacuum hot press treatment. By heat-pressing a resin composition layer having a Vickers hardness of 0.1 HV to 15 HV and a minimum melt viscosity of 1,000 poise to 20,000 poise at a pressure within this range, it is possible to suppress the exudation of the resin in the resin composition layer.
[0162] In the vacuum hot press treatment, the pressure (pressing force) is 0.3 MPa or more, preferably 0.5 MPa or more, more preferably 0.7 MPa or more, even more preferably 0.8 MPa or more, or 0.9 MPa or more, from the viewpoint of suppressing resin exudation. The upper limit is 1.5 MPa or less, preferably 1.4 MPa or less, more preferably 1.3 MPa or less.
[0163] In the vacuum hot press treatment, the heating temperature varies depending on the composition of the resin composition layer, but is preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher. The upper limit of the heating temperature is not particularly limited, but can usually be set to 300°C or lower. Note that the resin composition layer may be thermally cured by heating in the vacuum hot press treatment to form an insulating layer.
[0164] In the vacuum hot pressing treatment, the heat-bonding time (pressing time) is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 15 minutes or more. There is no particular upper limit, but it is preferably 300 minutes or less, more preferably 200 minutes or less, and even more preferably 150 minutes or less.
[0165] The resin sheet with the metal foil from which the circuit board and protective film have been peeled off may be set in a vacuum heat press device via cushion paper, a metal plate such as a stainless steel plate (SUS plate), a release film, or the like.
[0166] The vacuum heat press treatment can be carried out using a conventionally known vacuum heat press device that presses the circuit board and the resin sheet with metal foil from which the protective film has been peeled off from both sides using a heated metal plate such as a SUS plate. An example of a commercially available vacuum heat press device is the "VH1-1603" manufactured by Kitagawa Seiki Co., Ltd.
[0167] The vacuum hot pressing treatment may be carried out only once or may be repeated two or more times. When the treatment is repeated two or more times, the pressure, heating temperature, pressing time, etc. may be the same or different.
[0168] In the vacuum heat press treatment, the atmospheric pressure, that is, the pressure (degree of decompression) during decompression in the chamber in which the resin sheet with metal foil attached (temporarily attached) to the circuit board to be treated is stored, is preferably 3×10 -2 MPa or less, more preferably 1×10 -2 MPa or less. There is no particular lower limit, but it is 1×10 -10 MPa or more.
[0169] The resin sheet with the metal foil from which the protective film has been peeled off is laminated on the circuit board by vacuum pressing, and then the resin composition layer is thermally cured to form an insulating layer. For example, when performing pressing by vacuum hot pressing, an example of a method for thermally curing the resin composition layer is a method in which the resin composition layer is thermally cured using heat generated during pressing to form an insulating layer.
[0170] The conditions for thermally curing the resin composition layer are not particularly limited, and conditions that are usually employed when forming an insulating layer for a printed wiring board may be used.
[0171] For example, although the thermal curing conditions for the resin composition layer vary depending on the type of resin composition layer, the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.
[0172] Before thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50°C or higher but lower than 120°C (preferably 60°C or higher but 115°C or lower, more preferably 70°C or higher but 110°C or lower) for 5 minutes or longer (preferably 5 to 150 minutes, more preferably 15 to 120 minutes, and even more preferably 15 to 100 minutes).
[0173] Since the resin sheet with metal foil used in the present invention contains metal foil, after completion of step (D), it may include step (E) of forming a conductor layer (circuit) by a subtractive method or a modified semi-additive method.
[0174] In the step (E), the metal foil in the resin sheet with metal foil can be used to form a conductor layer by a subtractive method or a modified semi-additive method.
[0175] In the subtractive method, unnecessary portions of the metal foil (non-circuit forming portions) are selectively removed by etching or the like to form a circuit. The circuit formation by the subtractive method may be carried out according to a known procedure. For example, the circuit formation by the subtractive method can be carried out by a method including: i) providing an etching resist on the surface of the metal foil (i.e., the surface opposite to the surface bonded to the resin composition layer); ii) exposing and developing the etching resist to form a wiring pattern; iii) etching and removing the exposed metal foil portions; and iv) removing the etching resist.
[0176] In the modified semi-additive process, non-circuit forming portions of a metal foil are protected with a plating resist, and a thick layer of a metal such as copper is applied to the circuit forming portions by electrolytic plating. The plating resist is then removed, and the metal foil other than the circuit forming portions is removed by etching to form a circuit. Circuit formation using the modified semi-additive process may be carried out according to known procedures. For example, circuit formation using the modified semi-additive process can be carried out by a method including: i) providing a plating resist on the surface of the metal foil (i.e., the surface opposite to the surface bonded to the resin composition layer); ii) exposing and developing the plating resist to form a wiring pattern; iii) electroplating through the plating resist; iv) removing the plating resist; and v) etching and removing the metal foil other than the circuit forming portions. If the metal foil is thick, the entire surface of the metal foil may be thinned by etching or the like before step i) to a desired thickness (usually 5 μm or less, 4 μm or less, or 3 μm or less).
[0177] When manufacturing a circuit board, a step (F) of drilling holes and a step (G) of roughening the insulating layer may be further performed. These steps (F) to (G) may be performed according to various methods known to those skilled in the art and used in the manufacture of printed wiring boards. Furthermore, if necessary, the formation of insulating layers and conductor layers in steps (A) to (G) may be repeated to form a multilayer wiring board.
[0178] The method for manufacturing a circuit board of the present invention uses a resin sheet with metal foil in which the resin composition layer has a Vickers hardness of 0.1 HV or more and 15 HV or less and a minimum melt viscosity of 1,000 poise or more and 20,000 poise or less, and therefore exhibits the characteristic of suppressing the occurrence of resin chipping. The resin sheet with metal foil is cut using a temporary bonding device, and the cut edge portions are visually inspected for cracks and chips. At this time, there are no cracks or chips in the resin sheet with metal foil. The evaluation of resin chipping can be performed using the method described in the examples below.
[0179] The method for manufacturing a circuit board of the present invention uses a resin sheet with a metal foil in which the resin composition layer has a Vickers hardness of 0.1 HV or more and 15 HV or less and a minimum melt viscosity of 1,000 poise or more and 20,000 poise or less, and therefore exhibits excellent tackiness. The resin sheet with a metal foil is positioned so as to be joined to the circuit board using a tackiness device, and the resin sheet with a metal foil and the circuit board are tackiness-attached. After tackiness, the resin sheet is tilted 90 degrees from the surface positioned so as to be joined to the circuit board, and the presence or absence of peeling between the resin composition layer and the circuit board is confirmed. At this time, the resin sheet with a metal foil does not peel from the circuit board. The tackiness can be evaluated by the method described in the examples below.
[0180] The method for manufacturing a circuit board of the present invention involves heating a resin sheet with a temporarily attached metal foil while applying a pressure of 0.5 MPa to 1.5 MPa, thereby exhibiting the characteristic of suppressing resin exudation. After temporarily attaching the resin sheet with metal foil to the circuit board, it is heated at 180°C for 2 hours while applying pressure, and the resin flow after heating is obtained as the average value of 100 points of the exudation distance of the resin from the edge of the metal foil. At this time, the resin flow amount is 20 mm or less. Resin exudation can be evaluated using the method described in the Examples below.
[0181] The circuit board manufacturing method of the present invention uses a metal foil-attached resin sheet in which the resin composition layer has a Vickers hardness of 0.1 HV to 15 HV and a minimum melt viscosity of 1,000 poise to 20,000 poise, and therefore typically exhibits excellent reflow resistance. This results in an insulating layer with excellent reflow resistance. The metal foil-attached resin sheet is laminated on both sides of a copper-clad laminate so that the resin composition layer contacts the copper-clad laminate. The pressure is evacuated, the temperature is raised from room temperature by 5°C each time, and the laminate is heated and pressed at 180°C for 120 minutes to obtain a laminate substrate. A reflow test is performed in which the laminate substrate is passed through a reflow device three times. No abnormalities such as swelling occur during this test. Reflow resistance can be evaluated using the method described in the Examples below. [Example]
[0182] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the following description, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, the operations described below were carried out in an environment of normal temperature and pressure, unless otherwise specified.
[0183] [Example 1] <Preparation of Resin Sheet A with Metal Foil> Bisphenol type epoxy resin (Nippon Steel Chemical Co., Ltd. "ZX1059", epoxy equivalent approximately 165g / eq.) 15 parts, tetramethylbisphenol type epoxy resin (Mitsubishi Chemical Co., Ltd. "YX4000H", epoxy equivalent approximately 194g / eq.) 10 parts, biphenyl type epoxy resin (Nippon Kayaku Co., Ltd. "NC3000L", epoxy equivalent approximately 271g / eq.) 18 parts, naphthalene type epoxy resin (DIC Corporation "HP4710", 5 parts of epoxy equivalent (approx. 170 g / eq.), 15 parts of a phenolic hardener with a triazine skeleton and a cresol novolac structure (DIC Corporation "LA-3018-50P", phenol equivalent (approx. 151 g / eq.), 50% solids solution in 2-methoxypropanol), 15 parts of a naphthol aralkyl phenolic resin MEK solution (Nippon Steel Chemical Co., Ltd. "SN485", phenol equivalent (approx. 215 g / eq.), 60% solids solution in MEK) ), 10 parts of phenoxy resin ("YL7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 mixed solution of MEK with a 30% solid content and cyclohexanone), 10 parts of butyral resin ("BL-1" manufactured by Sekisui Chemical Co., Ltd., a 1:1 mixed solution of MEK and cyclohexanone with a 15% solid content), 30 parts of methyl ethyl ketone (MEK), and an amino-based silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminomethyl-2- ... 130 parts of inorganic filler that had been surface-treated with aminopropyltrimethoxysilane (amount of surface treatment: 0.6% by mass of amino silane coupling agent per 100% by mass of inorganic filler) and 6 parts of organic filler ("AC3816N" manufactured by Aica Kogyo Co., Ltd.) were uniformly dispersed using a mixer, and then 3 parts of imidazole curing accelerator (5% solids solution of "1B2PZ" manufactured by Shikoku Chemicals Corporation in MEK) were added to prepare a varnish of the resin composition.
[0184] Next, the resin composition varnish was uniformly applied to a PET film ("AL5" manufactured by Lintec Corporation, 38 μm thick) using a die coater so that the dried thickness would be 30 μm, and then dried at 110°C for 5 minutes to produce a resin roll. This was then laminated with copper foil ("MT18Ex" manufactured by Mitsui Mining & Smelting Co., Ltd., "3 μm ultra-thin copper foil / 18 μm carrier foil") to obtain a roll-shaped resin sheet A with metal foil. The minimum melt viscosity of the resin composition layer was 6000 poise, the adhesion to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 3 HV.
[0185] <Measurement of Adhesion of Resin Composition Layer to Copper Foil> The PET film was peeled off from the resulting resin sheet with metal foil, and 31B tape was attached to it. Then, the sheet was cut into a 25 mm wide, 10 cm long piece. The copper foil carrier was peeled off, and 31B tape was attached to the copper remaining on the resin after the carrier layer was peeled off. The adhesion of the resin composition layer to the copper foil was measured using a TSE tensile tester (AUTO COM AC-C) at a peel speed of 300 mm / min and a peel angle of 180°.
[0186] <Measurement of Vickers hardness of resin composition layer> The Vickers hardness of the resin composition layer of the metal foil-attached resin sheet A was confirmed at a test force of 0.1 N using a micro-Vickers-Vickers hardness tester manufactured by Mitutoyo Corporation.
[0187] <Measurement of Minimum Melt Viscosity of Resin Composition Layer> Multiple resin composition layers of metal foil-attached resin sheet A were stacked and processed into pellets, yielding 18 mm thick, 1.2 g pellet-shaped measurement samples. The minimum melt viscosity of the obtained samples was measured using a dynamic viscoelasticity measuring device (Rheosol-G3000, manufactured by UBM). Specifically, the samples were heated from a starting temperature of 60°C to 200°C, and the dynamic viscoelastic modulus was measured to calculate the minimum melt viscosity (poise). The measurement conditions were a heating rate of 5°C / min, a measurement temperature interval of 2.5°C, a vibration frequency of 1 Hz, and a strain of 1 deg.
[0188] <Evaluation of resin chipping> The metal foil-attached resin sheet A was cut using a temporary bonding device, and the cut edge portions were visually inspected for cracks and chips. The resin chipping was evaluated based on the following evaluation criteria. Good: No cracks or chips in the resin sheet with metal foil. ×: There are cracks and chips in the resin sheet with metal foil.
[0189] <Evaluation of temporary attachment> Using a temporary bonding device (manufactured by Shin-ei Kiko Co., Ltd.), the resin composition layer of the metal foil-attached resin sheet A was positioned so as to be joined to a circuit board (manufactured by Panasonic, R1515A), and the metal foil-attached resin sheet A was temporarily bonded to the circuit board. The temporarily attached metal foil resin sheet A was tilted 90 degrees with the surface positioned so as to be joined to the circuit board as a reference, and the presence or absence of peeling between the resin composition layer and the circuit board was confirmed, and the temporary bondability was evaluated based on the following evaluation criteria. Good: The resin sheet with metal foil does not peel off. ×: The resin sheet with the metal foil peeled off.
[0190] <Evaluation of resin exudation> After temporarily attaching the metal foil-attached resin sheet A to the circuit board, it was heated at 180°C for 2 hours while applying a pressure of 1.0 MPa. The amount of resin flow after heating was calculated as the average of 100 points of the resin seepage distance from the copper foil edge. The resin seepage rate was determined based on this amount of resin flow. 〇: Resin flow amount is 20mm or less. ×: Resin flow amount is greater than 20 mm.
[0191] <Reflow resistance evaluation> Both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.8 mm, Panasonic R1515A) with an inner layer circuit formed on it were immersed in MEC CZ8100 to roughen the copper surface.
[0192] The resin composition layer of the metal foil-attached resin sheet A was laminated on both sides of the copper-clad laminate so that it was in contact with the copper-clad laminate. The lamination was performed using a test press machine "KVHC" manufactured by Kitagawa Seiki Co., Ltd. The pressure was vacuum (1.0 MPa), and the temperature was raised from room temperature at 5°C per degree, and the sheets were heated and pressed at 180°C for 120 minutes.
[0193] The laminated substrate obtained as described above was cut into small pieces of 100 mm x 50 mm, and passed through a reflow device ("HAS-6116" manufactured by Nippon Antom Co., Ltd.) that reproduces a solder reflow temperature of a peak temperature of 260°C three times (the reflow temperature profile conforms to IPC / JEDEC J-STD-020C), and evaluated by visual observation according to the following criteria. ○: 2 or less abnormalities such as swelling △: 3 or more, 4 or less abnormalities such as swelling ×: 5 or more abnormalities such as swelling
[0194] <Measurement of residual solvent amount> The mass of a sheet sample cut from the metal foil-attached resin sheet A before lamination with the copper clad laminate was measured, and the mass of the PET film and copper foil was subtracted to determine the mass of the resin composition layer before the drying test, W0. The sheet sample was then subjected to a drying test in which it was dried at 130°C for 15 minutes. After the drying test, the mass of the sheet sample was measured, and the mass of the PET film and copper foil was subtracted to determine the mass of the resin composition layer after the drying test, W1. The masses of the PET film and copper foil were measured using PET film and copper foil of the same dimensions as those contained in the sheet sample. The mass loss rate of the resin composition due to the drying test ((W0-W1) / W0) was calculated using the mass W0 before the drying test and the mass W1 after the drying test. This mass loss rate was taken as the amount of residual solvent.
[0195] <Method for measuring solvent composition in resin sheet> A 5 mg portion of the resin composition layer was measured from resin sheet A with metal foil, and the measured sample was processed in an oven at 250°C for 10 minutes using a GCMS-QP2020-NX (Shimadzu Corporation). The sample was then measured under conditions of a sample line temperature of 260°C, a transfer line temperature of 260°C, and a cycle time of 55 minutes. The solvent type was identified from each detected peak, and the type and amount of solvent contained in the resin composition layer of the resin sheet with metal foil were analyzed by comparing the results with a calibration curve prepared in advance.
[0196] [Example 2] The pressure used in the evaluation of resin seepage was changed from 1.0 MPa to 1.3 MPa in Example 1. Other than the above, the resin chipping, tackiness, resin seepage, and reflow resistance were evaluated in the same manner as in Example 1.
[0197] [Example 3] The pressure used in the evaluation of resin seepage was changed from 1.0 MPa to 0.7 MPa in Example 1. Other than the above, the resin chipping, tackiness, resin seepage, and reflow resistance were evaluated in the same manner as in Example 1.
[0198] [Example 4] In Example 1, metal foil-attached resin sheet A was replaced with metal foil-attached resin sheet B prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0199] <Preparation of Resin Sheet B with Metal Foil> In preparing the resin sheet A with metal foil, 1) The amount of phenoxy resin (Mitsubishi Chemical Corporation's "YL7553BH30", a 1:1 mixed solution of MEK with a solid content of 30% and cyclohexanone) was changed from 10 parts to 40 parts. 2) The amount of inorganic filler surface-treated with an amino-silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (amount of surface treatment: 0.6% by mass of amino-silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 150 parts. A resin sheet B with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points.
[0200] The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet B was 18,000 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 5.0 HV.
[0201] [Example 5] In Example 1, metal foil-attached resin sheet A was replaced with metal foil-attached resin sheet C prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0202] <Preparation of Resin Sheet C with Metal Foil> In preparing resin sheet A with metal foil, the amount of inorganic filler surface-treated with an amino-silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (surface treatment amount: 0.6% by mass of amino-silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 50 parts. A resin sheet C with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet C was 1200 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 1.5 HV.
[0203] [Example 6] In Example 1, metal foil-attached resin sheet A was replaced with metal foil-attached resin sheet D prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0204] <Preparation of Resin Sheet D with Metal Foil> In preparing resin sheet A with metal foil, the amount of inorganic filler surface-treated with an amino-silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (surface treatment amount: 0.6% by mass of amino-silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 180 parts. A resin sheet D with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of metal foil-attached resin sheet D was 12,000 poise, the adhesion to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 14.0 HV.
[0205] [Example 7] In Example 1, metal foil-attached resin sheet A was replaced with metal foil-attached resin sheet E prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0206] <Preparation of Resin Sheet E with Metal Foil> In preparing the resin sheet A with metal foil, 1) The amount of phenoxy resin (Mitsubishi Chemical Corporation's "YL7553BH30", a 1:1 mixed solution of MEK with a solid content of 30% and cyclohexanone) was changed from 10 parts to 40 parts. 2) The amount of inorganic filler surface-treated with an amino-based silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (surface treatment amount: 0.6% by mass of amino-based silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 50 parts. A resin sheet E with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet E was 4000 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 0.3 HV.
[0207] [Example 8] In Example 1, metal foil-attached resin sheet A was replaced with metal foil-attached resin sheet F prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0208] <Preparation of Resin Sheet F with Metal Foil> In the preparation of resin sheet A with metal foil, the amount of methyl ethyl ketone was changed from 30 parts to 20 parts, and 10 parts of toluene was further used. A resin sheet F with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet F was 6000 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 3 HV.
[0209] [Example 9] In Example 1, metal foil-attached resin sheet A was replaced with metal foil-attached resin sheet G prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0210] <Preparation of Resin Sheet G with Metal Foil> In the preparation of resin sheet A with metal foil, the amount of methyl ethyl ketone was changed from 30 parts to 27 parts, and 3 parts of NMP (N-methyl-2-pyrrolidone) was used. A resin sheet G with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet G was 5000 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 3 HV.
[0211] [Example 10] In Example 1, the metal foil-attached resin sheet A was replaced with the metal foil-attached resin sheet H prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0212] <Preparation of Resin Sheet H with Metal Foil> In the preparation of resin sheet A with metal foil, the amount of methyl ethyl ketone was changed from 30 parts to 15 parts, and 15 parts of toluene was used. A resin sheet H with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet H was 6000 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 3 HV.
[0213] [Example 11] In Example 1, metal foil-attached resin sheet A was replaced with metal foil-attached resin sheet I prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0214] <Preparation of Metal Foil-Attached Resin Sheet I> In the preparation of resin sheet A with metal foil, the amount of methyl ethyl ketone was changed from 30 parts to 23 parts, and 5 parts of NMP (N-methyl-2-pyrrolidone) was used. Resin sheet I with metal foil was obtained in the same manner as in the preparation of resin sheet A with metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet I was 2500 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 3 HV.
[0215] [Comparative Example 1] In Example 1, the pressure used in the evaluation of resin exudation was changed from 1.0 MPa to 2.0 MPa. Except for the above, the same procedures as in Example 1 were carried out to evaluate resin chipping, tackiness, resin exudation, and reflow resistance.
[0216] Comparative Example 2 In Example 5, the pressure used in the evaluation of resin exudation was changed from 1.0 MPa to 0.3 MPa. Other than the above, the same procedures as in Example 1 were carried out to evaluate resin chipping, tackiness, resin exudation, and reflow resistance.
[0217] Comparative Example 3 In Example 1, the metal foil-attached resin sheet A was replaced with the metal foil-attached resin sheet J prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0218] <Preparation of Resin Sheet J with Metal Foil> In preparing the resin sheet A with metal foil, 1) The amount of phenoxy resin (Mitsubishi Chemical Corporation's "YL7553BH30", MEK and cyclohexanone solution with a solid content of 30%) was changed from 10 parts to 40 parts. 2) The amount of inorganic filler surface-treated with an amino-based silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (surface treatment amount: 0.6% by mass of amino-based silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 200 parts. A resin sheet J with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet J was 29,000 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 8.0 HV.
[0219] Comparative Example 4 In Example 1, the metal foil-attached resin sheet A was replaced with the metal foil-attached resin sheet K prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0220] <Preparation of Resin Sheet K with Metal Foil> In preparing the resin sheet A with metal foil, 1) The amount of phenoxy resin (Mitsubishi Chemical Corporation's "YL7553BH30", MEK and cyclohexanone solution with a solid content of 30%) was changed from 10 parts to 40 parts. 2) The amount of inorganic filler surface-treated with an amino-based silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (surface treatment amount: 0.6% by mass of amino-based silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 20 parts. A resin sheet K with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet K was 400 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 0.2 HV.
[0221] Comparative Example 5 In Example 1, the metal foil-attached resin sheet A was replaced with the metal foil-attached resin sheet L prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0222] <Preparation of Resin Sheet L with Metal Foil> In preparing resin sheet A with metal foil, the amount of inorganic filler surface-treated with an amino-silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (surface treatment amount: 0.6% by mass of amino-silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 250 parts. A resin sheet L with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet L was 17,000 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 16.0 HV.
[0223] Comparative Example 6 In Example 1, the metal foil-attached resin sheet A was replaced with the metal foil-attached resin sheet M prepared as follows. Other than the above, the Vickers hardness, minimum melt viscosity, resin chipping, tackiness, resin exudation, and reflow resistance were evaluated in the same manner as in Example 1.
[0224] <Preparation of Resin Sheet M with Metal Foil> In preparing the resin sheet A with metal foil, 1) The amount of inorganic filler surface-treated with an amino-based silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane) (surface treatment amount: 0.6% by mass of amino-based silane coupling agent per 100% by mass of inorganic filler) was changed from 130 parts to 50 parts. 2) The amount of organic filler ("AC3816N" manufactured by Aica Kogyo Co., Ltd.) was changed from 6 parts to 1 part. A resin sheet M with a metal foil was obtained in the same manner as in the preparation of the resin sheet A with a metal foil, except for the above points. The minimum melt viscosity of the resin composition layer of the metal foil-attached resin sheet M was 2500 poise, the adhesiveness to the copper foil was 40 gf / cm, and the Vickers hardness of the resin composition layer was 0.03 HV.
[0225] [Table 1] [Table 2] *1: The content of component (d) represents the content when the non-volatile components are taken as 100% by mass. *2: The solvent content is expressed as the content when the total amount of solvent contained in the resin composition layer is taken as 100% by mass.
[0226] [Table 3]
[0227] [Table 4]
[0228] Since the resin composition layer of the metal foil-attached resin sheet L had a high Vickers hardness, the resin composition layer cracked when the metal foil-attached resin sheet L was cut with a temporary bonding device, making it impossible to laminate the metal foil-attached resin sheet L on the circuit board. Therefore, the resin bleeding property and reflow resistance of Comparative Example 5, which used the metal foil-attached resin sheet L, could not be evaluated. [Explanation of symbols]
[0229] 1 Resin sheet with metal foil 2. Metal foil 3 Resin composition layer 4 Resin sheet (resin sheet with metal foil from which the protective film has been removed) 5 Protective film 6 Circuit Board 10 Temporary attachment device (auto cutter device) 11. Rolled resin sheet with metal foil 12 Protective film take-up roll 13 Protective film removal tool 14 Cutter 15 Conveyor equipment 16, 17 Induction Roll
Claims
1. (A) a step of preparing a roll-shaped resin sheet with a metal foil, the resin sheet having a metal foil and a resin composition layer, the resin composition layer having a Vickers hardness of 0.1 HV or more and 15 HV or less and a minimum melt viscosity of 1,000 poise or more and 20,000 poise or less, the resin composition layer being wound into a roll; (B) a step of transporting a resin sheet with a metal foil from a roll-shaped resin sheet with a metal foil, arranging the resin sheet with the metal foil so that the resin composition layer of the resin sheet with the metal foil is joined to the circuit board, and attaching the resin sheet with the metal foil onto the circuit board; (C) cutting the resin sheet with the attached metal foil; and (D) heating the resin sheet with the attached metal foil while applying a pressure of 0.5 MPa or more and 1.5 MPa or less to thermally cure the resin composition layer.
2. The method for producing a circuit board according to claim 1 , wherein the resin sheet with the metal foil prepared in step (A) further comprises a protective film provided on the resin composition layer.
3. In step (B), before bonding the resin sheet with the metal foil to the circuit board, The method for producing a circuit board according to claim 2, further comprising: (A-1) a step of peeling off the protective film.
4. 2. The method for producing a circuit board according to claim 1, wherein the thickness of the metal foil of the resin sheet with the metal foil is 5 μm or less.
5. The method for producing a circuit board according to claim 1 , wherein the resin composition layer contains a thermosetting resin.
6. The method for producing a circuit board according to claim 1 , wherein the resin composition layer contains a polymer compound.
7. The method for producing a circuit board according to claim 1 , wherein the resin composition layer contains a curing accelerator.
8. The method for producing a circuit board according to claim 1 , wherein the resin composition layer contains an inorganic filler.
9. The method for producing a circuit board according to claim 6 , wherein the polymer compound includes a thermoplastic resin.
10. The method for producing a circuit board according to claim 1 , wherein the resin composition layer has a thickness of 3 μm or more and 60 μm or less.
11. The resin composition layer contains a solvent, The solvent comprises an aromatic solvent having a boiling point of less than 115° C.; The method for producing a circuit board according to claim 1, wherein the content of the aromatic solvent having a boiling point of less than 115°C is 0 mass% or more and 10 mass% or less, when the total solvent contained in the resin composition layer is 100 mass%.
12. The resin composition layer contains a solvent, The solvent includes a solvent having a boiling point of 115° C. or more and less than 200° C., 2. The method for producing a circuit board according to claim 1, wherein the content of the solvent having a boiling point of 115° C. or more and less than 200° C. is 55% by mass or more and 95% by mass or less, when the total solvent contained in the resin composition layer is taken as 100% by mass.
13. The resin composition layer contains a solvent, The solvent includes a solvent having a boiling point of 200° C. or higher, The method for producing a circuit board according to claim 1 , wherein the content of the solvent having a boiling point of 200° C. or more is 0 mass % or more and 10 mass % or less, when the total solvent contained in the resin composition layer is taken as 100 mass %.
Citation Information
Patent Citations
Metal-clad laminate sheet
JP2014208486A
Curable resin composition, dry film, copper foil with resin, cured product and electronic component
JP2022043685A
Metal base substrate, circuit board, and substrate with heat-generating body mounted thereon
WO2017086474A1
Liquid crystal polymer single-sided laminate
WO2017175649A1