Photocurable resin composition containing self-crosslinking polymer
A photocurable resin composition with self-crosslinking polymers forms a protective film on semiconductor substrates, addressing metal contamination issues by enhancing etching resistance and improving yield.
Patent Information
- Application Number
- JP2023567875
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-22
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2043-02-21
AI Technical Summary
Existing methods for forming protective films on semiconductor substrates fail to adequately prevent metal contamination at the edges of wafers during manufacturing, leading to cross-contamination and reduced yield due to insufficient etching resistance.
A photocurable resin composition containing a self-crosslinking polymer with aryl ketone residues and aliphatic hydrocarbon or aromatic ring residues, which forms a protective film with high etching resistance without the need for a polymerization initiator, effectively covering the wafer edges.
The protective film provides sufficient etching resistance, preventing metal contamination and improving the yield of non-defective semiconductor devices by ensuring complete coverage of the wafer edges during manufacturing.
Smart Images

Figure 0007559977000001 
Figure 0007559977000002 
Figure 0007559977000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocurable resin composition containing a crosslinkable polymer; and further relates to a protective film for an end face of a substrate (wafer) for semiconductor production in a semiconductor device production process, a protective film-forming composition for forming the protective film, a wafer for semiconductor production produced using the protective film, and a method for producing the wafer for semiconductor production and a semiconductor device. [Background technology]
[0002] In the manufacture of semiconductor devices, as the manufacturing process becomes more complicated, a method of applying a chemical solution containing a metal to a wafer is being considered for the purpose of, for example, improving the etching selectivity. Furthermore, for example, in the case of performing exposure using extreme ultraviolet (EUV), the resolution of the resist pattern is increased, and since the resist has high etching resistance, it is being considered to form a resist film using a resist containing an inorganic metal. Meanwhile, adhesion of metal to unintended portions of a wafer in the manufacturing process of a semiconductor device greatly affects the electrical characteristics of the semiconductor device. However, when forming a coating film containing a metal as described above, there is a concern that the chemical solution supplied to the surface of the wafer will wrap around the peripheral edge and backside edge of the wafer, and the coating film will be formed on these unintended peripheral edge and backside edge portions, resulting in metal contamination of these portions. In addition, when the contaminated portion of the wafer comes into contact with a wafer processing device such as an exposure device or an etching device, or a wafer transport mechanism, the wafers transported and processed after the wafer will also be metal contaminated, that is, cross contamination may occur.
[0003] In order to address such problems, a technique has been disclosed in which, when forming a coating film on the surface of a substrate, a protective film is formed on at least the peripheral edge and backside peripheral edge of the substrate, thereby forming the coating film so that the peripheral edge and backside peripheral edge of the substrate, which are the peripheral edges of the substrate, do not come into contact with the coating film (Patent Document 1).In addition, a method for manufacturing a semiconductor device has been disclosed in which a simple additional process (forming a second mask to cover the first mask on the bevel portion so that the first mask on the bevel portion does not collapse) is provided, thereby suppressing peeling of the film from the bevel portion of the substrate (Patent Document 2).
[0004] However, the film material that functions as the protective film for the substrate edge is required to have a high degree of etching resistance, and further improvement is desired. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-098333 A [Patent Document 2] JP 2011-228340 A Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, the problem that the present invention aims to solve is to provide a resin material capable of forming a protective film having sufficient etching resistance required to protect the edge of a substrate (wafer) used for semiconductor manufacturing in the manufacture of semiconductor devices. Furthermore, the problem to be solved by the present invention also includes providing a protective film capable of completely covering the edge of a substrate (wafer) for semiconductor manufacturing in a simple manner by application in the manufacture of a semiconductor device, a protective film-forming composition for forming the protective film, a wafer for semiconductor manufacturing manufactured using the protective film, and a method for manufacturing the wafer for semiconductor manufacturing and the semiconductor device. [Means for solving the problem]
[0007] The present invention encompasses the following: [1] (a) a first monomer unit comprising an aryl ketone residue in a side chain; and (b) In the side chain, (b-1) an aliphatic hydrocarbon residue containing a carbon atom that is susceptible to hydrogen abstraction reactions; and / or (b-2) a second monomer unit containing an aromatic ring residue; A photocurable resin composition comprising a self-crosslinking polymer (A) and a solvent (B). [1―1] The self-crosslinking polymer (A) (b-1) an aliphatic hydrocarbon residue containing a carbon atom that is susceptible to hydrogen abstraction reactions; and (b-2) a second monomer unit containing an aromatic ring residue; The photocurable resin composition according to [1], [2] The photocurable resin composition according to [1], further comprising a crosslinkable polymer or a crosslinkable compound (C) other than the self-crosslinkable polymer (A). [3] The photocurable resin composition according to [2], wherein the crosslinkable group in the crosslinkable polymer or the crosslinkable compound (C) is selected from the group consisting of an epoxy group, a (meth)acrylic group, a vinyl group, a carboxylic acid group, a thiol group, a silanol group, a cinnamoyl group, and a hydroxyl group. [4] The photocurable resin composition according to any one of [1] to [3], having a viscosity of 100 cps or less at 25° C. [5] A composition for forming a wafer edge protection film for use in semiconductor production, comprising the photocurable resin composition according to any one of [1] to [4]. [6] A protective film which is a cured product of a coating film made of the composition for forming a wafer edge protective film for semiconductor manufacturing according to [5]. [7] The protective film according to [6], having a thickness of 1 to 500 nm. [8] A protective film according to [6] or [7] for preventing metal contamination of a wafer edge. [9] The protective film according to any one of [6] to [8], which is cured by light having a wavelength of 170 to 800 nm.
[10] A wafer for semiconductor manufacturing having a protected wafer edge, the wafer for semiconductor manufacturing being formed by applying the composition for forming a wafer edge protection film for semiconductor manufacturing described in [5] to the edge of a wafer precursor.
[11] (A) forming a resist film on a semiconductor substrate; (B) forming a resist pattern by irradiating the resist film with light or an electron beam and then developing it; (C) etching the semiconductor substrate; A method for manufacturing a semiconductor device comprising: A method for manufacturing a semiconductor device, comprising a step (X) of forming a protective film from the composition for forming a protective film for semiconductor manufacturing wafer edge described in [5] on a front surface edge and, optionally, a bevel portion and / or a back surface edge of a wafer for semiconductor manufacturing.
[12] The method for manufacturing a semiconductor device according to
[11] , further comprising a step (X) prior to the step (A).
[13] The method for manufacturing a semiconductor device according to
[11] , further comprising a step (X) between the steps (A) and (B).
[14] The method for manufacturing a semiconductor device according to
[11] , further comprising a step (X) after the step (B) or the step (C).
[15] The method for producing a semiconductor device according to any one of
[11] to
[14] , further comprising, after the step (X), a step (Y) of removing the resist film on the protective film.
[16] The method for producing a semiconductor device according to any one of
[11] to
[14] , further comprising, after the step (X), a step (Z) of removing the protective film.
[17] The method for manufacturing a semiconductor device according to
[15] , further comprising, after the step (Y), a step (Z) of removing the protective film.
[18] The method for producing a semiconductor device according to any one of
[11] to
[17] , wherein the resist film contains a metal.
[19] The method for producing a semiconductor device according to any one of
[11] to
[18] , in the step (X), the composition for forming a wafer edge protection film for semiconductor production according to [5] is applied, and a predetermined region is exposed and developed.
[20] The method for producing a semiconductor device according to
[16] or
[17] , wherein the step (Z) is carried out by ashing or a treatment with hydrofluoric acid, an organic solvent, an alkaline developer, or a semiconductor cleaning solution. [twenty one] A method for manufacturing a wafer for semiconductor manufacturing, comprising the steps of: A method for producing a wafer for semiconductor production, comprising the step of applying the composition for forming a wafer edge protection film for semiconductor production described in [5] to an edge of a wafer precursor, and producing a wafer having the edge protected. [twenty two] The aryl ketone residue is acetophenone, benzophenone, anthraquinone, anthrone, or a compound represented by the following structural formula: [ka] and substituted derivatives thereof; The photocurable resin composition according to any one of [1] to [4], wherein X is O, S or NR, and R is a hydrogen atom, a hydrocarbon group or an acyl group. [twenty three] The photocurable resin composition according to any one of [1] to [4], wherein the carbon atom in the hydrocarbon chain (b-1) that is susceptible to a hydrogen abstraction reaction is selected from the group consisting of a tertiary carbon atom; a secondary carbon atom; and a methyl group, a methylene group, or a methine group directly bonded to an aromatic ring. [twenty four] The photocurable resin composition according to any one of [1] to [4], wherein the aromatic ring (b-2) is an aromatic ring having 6 to 40 carbon atoms which may be substituted. [twenty five] The photocurable resin composition according to any one of [1] to [4], wherein a ratio of the repeat number of the first monomer unit to the repeat number of monomer units other than the first monomer unit, including the second monomer unit, is selected so that when a film having a thickness of 300 nm is formed, the film has a transmittance at a wavelength of 300 nm of 0.01% or more, preferably 0.1% or more, and more preferably 1% or more.
[26] (a) a first monomer unit comprising an aryl ketone residue in a side chain; and (b) In the side chain, (b-1) an aliphatic hydrocarbon residue containing a carbon atom that is susceptible to hydrogen abstraction reactions; and / or (b-2) a second monomer unit containing an aromatic ring residue; A self-crosslinking polymer (A) comprising: Effect of the Invention
[0008] By using the photocurable resin composition according to one embodiment of the present invention, a protective film having sufficient etching resistance, particularly a protective film for an edge of a wafer used in semiconductor manufacturing, can be formed without using a polymerization initiator. Furthermore, in the manufacture of a semiconductor device, which is one embodiment of the present invention, a protective film that can completely cover the edge of a substrate (wafer) for semiconductor manufacture by a simple method of application can prevent cross-contamination due to metal contamination in the subsequent semiconductor device manufacturing process, thereby improving the yield of non-defective semiconductor manufacturing equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <1. Photocurable resin composition [1] / Wafer edge protection film forming composition for semiconductor manufacturing [5]> (1-1) The photocurable resin composition according to one embodiment of the present invention contains a self-crosslinking polymer (A) and a solvent (B). The photocurable resin composition may further contain a crosslinkable polymer or a crosslinkable compound (C) other than the self-crosslinkable polymer (A). In addition, the photocurable resin composition can be preferably used as a protective film-forming composition used to protect the surface edge of a wafer for semiconductor production (wafer edge protective film-forming composition for semiconductor production, hereinafter sometimes abbreviated as "protective film-forming composition").
[0010] [1-2; Self-crosslinking polymer (A)] (1-2-1) The self-crosslinking polymer (A) is (a) a first monomer unit comprising an aryl ketone residue in a side chain; and (b) In the side chain, (b-1) an aliphatic hydrocarbon residue containing a carbon atom that is susceptible to hydrogen abstraction reactions; and / or (b-2) a second monomer unit containing an aromatic ring residue; It is a polymer comprising: The self-crosslinking polymer may optionally contain monomer units other than the above-mentioned first and second monomer units, as long as the effects of the present invention are not impaired.
[0011] (1-2-2) First Monomer Unit (1-2-2-1) The aryl ketone residue in the first monomer unit is a residue of a compound (monoaryl ketone or diaryl ketone) in which one or two aryl groups are directly bonded to a carbonyl group [—C(═O)—]. This aryl ketone residue acts as a photoreactive group and can be activated by light of a specific wavelength, such as ultraviolet light, to cause a crosslinking reaction. In this specification, the term "residue" of a compound refers to an organic group in which a hydrogen atom bonded to a carbon atom or a heteroatom (such as a nitrogen atom, oxygen atom, or sulfur atom) constituting the compound is replaced with a bond for covalent bonding. The aryl ketone residue constitutes the side chain of the self-crosslinking polymer, which is one embodiment of the present invention, via a suitable linking group, such as an ester bond or an amide bond. In this specification, the term "side chain" broadly includes a chemical group that is covalently bonded to a main chain and hangs down to the side, and is used synonymously with a so-called pendant group. Specific examples of aryl ketone residues include acetophenone, benzophenone, anthraquinone, anthrone, and the following structural formula: [ka] and heteroatom-substituted anthrone analogues and substituted derivatives thereof, wherein X is O, S or NR, and R is a hydrogen atom, a hydrocarbon group (preferably having 1 to 4 carbon atoms) or an acyl group (preferably having 1 to 4 carbon atoms). The aromatic rings of these aryl ketone residues have substituents such as hydroxyl, amino or carboxyl groups, or the side chains of the self-crosslinking polymer are formed by forming covalent bonds such as ester bonds (-O-CO- or -CO-O-), amide bonds (-NH-CO- or -CO-NH-), urethane bonds (-NH-CO-O- or -O-CO-NH-), carbonate bonds (-O-CO-O-), urea bonds (-NH-CO-NH-), etc. between the X of the nitrogen atom-substituted anthrone analogue (X=NH) and a functional group such as a carboxyl group, hydroxyl group or amino group of the polymer that constitutes the main chain. Two covalent bonds such as an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate bond (-O-CO-O-), or a urea bond (-NH-CO-NH-) may be combined and linked to each other by a divalent linking group L, for example, a hydrocarbon chain which may be interrupted by a heteroatom (such as an oxygen atom). Examples include -CO-OLO-CO- and -CO-NH-L-NH-CO-.
[0012] (1-2-2―2) Among these aryl ketone residues, residues of benzophenone or substituted derivatives thereof (hereinafter referred to as "benzophenone compounds") are preferred in view of the relatively long lifetime of the lowest excited triplet and the ease with which photochemical reactions can occur. Examples of such benzophenone compounds include 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxydisulfobenzophenone disodium, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',3,4-tetrahydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'3,4,4'-pentahydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,3,3'4,4',5'-hexahydroxybenzophenone, Hydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, 2,3,4-trihydroxybenzophenone, 2,4,4'-trihydroxybenzophenone, 2,4,5-trihydroxybenzophenone, 2,4,6-trihydroxybenzophenone, 2,4-dihydroxy-4'-diethylaminobenzophenone, 2,4-dihydroxy-4'-dimethylaminobenzophenone, 2,4-dihydroxybenzophenone, 4,4'-dihydroxybenzophenone, 2-hydroxy-4-(2-hydroxy-3- methacryloxy)propoxybenzophenone, 2-hydroxy-4'-dimethylaminobenzophenone, 2-hydroxy-4-i-octyloxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-acetoxyethoxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy Examples of the benzophenone include hydroxy-4-methoxy-5-sulfobenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxybenzophenone, 4,4'-dihydroxybenzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, 4',6-dihydroxy-2-naphthobenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-hydroxybenzophenone, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone, etc. Optionally substituted vinylbenzophenones are also included. Other examples of structures capable of abstracting hydrogen radicals upon irradiation with ultraviolet light include a benzyl group, an o-benzoylbenzoate group, a thioxanthone group, a 3-ketocoumarin group, a 2-ethylanthraquinone group, and a camphorquinone group, etc. Compounds having these structures may be used as compounds that derive the first monomer unit.
[0013] (1-2-2-3) The monomer constituting the main chain portion of the first monomer unit may be any polymerizable monomer having an aryl ketone residue and a functional group (such as a carboxyl group, a hydroxyl group, or an amino group) that can form a covalent bond, such as an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate bond (-O-CO-O-), or a urea bond (-NH-CO-NH-).
[0014] (1-2-2-4) Specific examples of the first monomer unit that can be suitably used, in which the aryl ketone residue is a residue of a benzophenone compound, include the following: benzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and the like.
[0015] (1-2-3) Second Monomer Unit (1-2-3-1) The aliphatic hydrocarbon residue containing a carbon atom that is susceptible to hydrogen abstraction reaction in the second monomer unit refers to an aliphatic hydrocarbon residue (preferably a monovalent hydrocarbon residue) containing a carbon atom that undergoes a hydrogen abstraction reaction and contributes to a crosslinking reaction by a photochemical reaction caused by an aryl ketone residue in the side chain. For example, it is an aliphatic hydrocarbon chain containing a carbon atom selected from the group consisting of a tertiary carbon atom; a secondary carbon atom, preferably a secondary carbon atom having a hydroxyl group; and a methyl group, methylene group, or methine group directly bonded to an unsaturated organic group [such as an aromatic ring or an ethylene group]; and a methylene group or methine group directly bonded to an oxygen atom of a hydroxyl group. It may be optionally substituted with a substituent such as a hydroxyl group, an alkoxy group, or an aryl group. The aliphatic hydrocarbon residue referred to here is interpreted as meaning that it may be substituted with an aromatic ring so that an abstraction reaction of a hydrogen atom bonded to a carbon atom in the residue occurs easily, or that the chain of the aliphatic hydrocarbon residue may be interrupted midway by an aromatic ring (for example, -R-Ar-R when R is an aliphatic hydrocarbon chain and Ar is an aromatic ring). The aliphatic hydrocarbon residue in the side chain may be directly covalently bonded to the main chain, or may form a side chain via a covalent bond such as an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate bond (-O-CO-O-), or a urea bond (-NH-CO-NH-) between the side chain and a functional group such as a carboxyl group, a hydroxyl group or an amino group of the polymer constituting the main chain. Covalent bonds such as an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate bond (-O-CO-O-), and a urea bond (-NH-CO-NH-) may be combined in two and linked to each other by a divalent linking group L, for example, a hydrocarbon chain which may be interrupted by a heteroatom (such as an oxygen atom). Examples include -CO-OLO-CO- and -CO-NH-L-NH-CO-. The aliphatic hydrocarbon residue preferably has 1 to 18 carbon atoms. From the viewpoint of improving the adhesion of the self-crosslinking polymer to the coating surface, it is preferable that a hydrophilic substituent such as a hydroxyl group is bonded to a carbon atom that is likely to undergo a hydrogen abstraction reaction. For example, —CH(OH)— is an example of an aliphatic hydrocarbon residue containing such a carbon atom. 3 CH(OH)CH 2 - etc. can be mentioned as preferred examples.
[0016] (1-2-3-2) Specific examples of the second monomer containing an aliphatic hydrocarbon residue in the side chain include the following: As the alkyl (meth)acrylate, an acrylate monomer having a branched or cyclic alkyl chain having 1 to 22 carbon atoms, such as 2-ethylhexyl (meth)acrylate, isobutyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, or dicyclopentanyl (meth)acrylate monomer; Hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 1-glycerol (meth)acrylate, 2-hydroxyethyl (meth)acrylamide, N-hydroxypropyl (meth)acrylamide, and allyl alcohol; It is.
[0017] (1-2-3-3) The aromatic ring residue in the second monomer unit may be any residue that undergoes a hydrogen abstraction reaction due to a photochemical reaction caused by an aryl ketone residue in a side chain and contributes to a crosslinking reaction, but is different from the side chain of the first monomer unit containing the above-mentioned aryl ketone residue. More specifically, examples of the aromatic ring include residues having an aromatic ring structure having 6 to 40 carbon atoms which may be substituted. Specific examples of the aromatic ring include benzene, naphthalene, anthracene, acenaphthene, fluorene, triphenylene, phenalene, phenanthrene, indene, indane, indacene, pyrene, chrysene, perylene, naphthacene, pentacene, coronene, heptacene, benzo[a]anthracene, dibenzophenanthrene, and dibenzo[a,j]anthracene. The aromatic ring residue may optionally have a substituent. Examples of such a substituent include a hydroxy group, a halogen atom, a carboxyl group, a nitro group, a cyano group, a methylenedioxy group, an acetoxy group, a methylthio group, an amino group, or an alkoxy group having 1 to 9 carbon atoms in place of some or all of the hydrogen atoms present in the aromatic ring structure having 6 to 40 carbon atoms. Examples of the alkoxy group having 1 to 9 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentoxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, an n-hexyloxy group, a 1-methyl-n-pentyloxy group, a 2-methyl-n-pentyloxy group, a 3-methyl-n-pentyloxy group, a 4- Examples of the alkyl group include a methyl-n-pentyloxy group, a 1,1-dimethyl-n-butoxy group, a 1,2-dimethyl-n-butoxy group, a 1,3-dimethyl-n-butoxy group, a 2,2-dimethyl-n-butoxy group, a 2,3-dimethyl-n-butoxy group, a 3,3-dimethyl-n-butoxy group, a 1-ethyl-n-butoxy group, a 2-ethyl-n-butoxy group, a 1,1,2-trimethyl-n-propoxy group, a 1,2,2-trimethyl-n-propoxy group, a 1-ethyl-1-methyl-n-propoxy group, a 1-ethyl-2-methyl-n-propoxy group, a n-heptyloxy group, a n-octyloxy group, and a n-nonyloxy group.
[0018] (1-2-3-4) The monomer constituting the main chain portion of the second monomer unit may be any polymerizable monomer having a functional group (such as a carboxyl group, a hydroxyl group, or an amino group) capable of forming a covalent bond such as an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate bond (-O-CO-O-), or a urea bond (-NH-CO-NH-), with an aliphatic hydrocarbon residue containing a carbon atom that is susceptible to hydrogen abstraction reaction, or an aromatic ring residue. Specific examples include vinyl monomers such as styrene, as well as the main chain portions of the exemplary monomers in (1-2-3-2) above. Here, the aliphatic hydrocarbon residue may form a covalent bond with a functional group (such as a carboxyl group, a hydroxyl group, or an amino group) of a monomer constituting the main chain portion as an aliphatic hydrocarbon moiety constituting a functional group such as an alkoxy group or an alkylamino group. The aromatic ring residue may also have a substituent, such as a hydroxyl group, an amino group, or a carboxyl group, present on the aromatic ring, which may form a covalent bond with a functional group, such as a carboxyl group, a hydroxyl group, or an amino group, of the polymer constituting the main chain. These covalent bonds include ester bonds (-O-CO- or -CO-O-), amide bonds (-NH-CO- or -CO-NH-), urethane bonds (-NH-CO-O- or -O-CO-NH-), carbonate bonds (-O-CO-O-), urea bonds (-NH-CO-NH-), etc. In addition, two covalent bonds such as an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate ester bond (-O-CO-O-), or a urea bond (-NH-CO-NH-) may be combined and linked to each other by a divalent linking group L, for example, a hydrocarbon chain which may be interrupted by a heteroatom (such as an oxygen atom). Examples include -CO-OLO-CO- and -CO-NH-L-NH-CO-.
[0019] (1-2-3-5) The second monomer unit undergoes a photochemical reaction caused by the aryl ketone residue of the first monomer unit, and hardens through crosslinking. Here, "self-crosslinking" means that hardening through a crosslinking reaction can be performed without the need for the addition of a polymerization initiator. The ratio of the repeat number of the first monomer unit to the repeat number of the second monomer unit can be determined taking into consideration the film thickness to be formed by photocuring of the self-crosslinking polymer and the light absorption by the aryl ketone residue. This is because, in order to allow the light for curing to reach the bottom of the film to be formed sufficiently, it is necessary to consider the ratio of the first monomer unit, which is a measure of the degree of light absorption, and the film thickness, which corresponds to the distance for the light to reach. The ratio of the repeat number of the first monomer unit to the repeat number of the monomer unit other than the first monomer unit (including the second monomer unit) may be adjusted so that when a film having a thickness of 300 nm is formed, the transmittance of the film at a wavelength of 300 nm is 0.01% or more, preferably 0.1% or more, and more preferably 1% or more.
[0020] (1-2-3-6) When the self-crosslinking polymer contains an additional monomer unit different from the first and second monomers, the above (1-2-3-5) is applied by replacing the number of repeats of the first monomer unit with the number of repeats of monomer units other than the first monomer unit, including the second monomer unit.
[0021] (1-2-3-7) The self-crosslinking polymer according to one embodiment of the present invention contains, as a monomer unit, a first monomer unit having an aryl ketone residue in a side chain, and therefore can self-crosslink without adding a polymerization initiator, and can improve etching resistance by reducing the oxygen atom content.
[0022] (1-3: Solvent (B)) Examples of the solvent contained in the photocurable resin composition according to one embodiment of the present invention include water, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, and cyclopentene. Examples of the solvent include cyclopentanone, cyclohexanone, cycloheptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents can be used alone or in combination of two or more. The solvent may be added so that the photocurable resin composition according to one embodiment of the present invention has an appropriate viscosity. In general, the amount of the solvent is preferably about 100 to 3,000 parts by mass per 100 parts by mass of the total amount of the self-crosslinking polymer (A) and the optionally contained crosslinking polymer or compound (C).
[0023] (1-4: Crosslinkable polymer or crosslinkable compound (C)) (1-4-1) The photocurable resin composition according to one embodiment of the present invention may further contain a crosslinkable polymer or a crosslinkable compound (C). The crosslinkable polymer or crosslinkable compound (C) refers to a polymer or compound having a crosslinkable group, other than the self-crosslinkable polymer (A). Here, the crosslinkable group means a group capable of forming a crosslinked structure by the action of light, an electron beam, other electromagnetic waves, radicals, acids, heat, water, oxygen, etc. Examples of the crosslinkable group include, but are not limited to, an epoxy group, an acrylic group, a vinyl group, a carboxylic acid group, a thiol group, a silanol group, a cinnamoyl group, a hydroxyl group (including a phenolic hydroxyl group), etc. Examples of the crosslinkable polymer or crosslinkable compound (C) include, but are not limited to, the following. Epoxy (meth)acrylate, Cinnamic acid grafted epoxy novolac, Phenoplasts, which are thermosetting materials obtained by polycondensation of phenols and aldehydes with the elimination of water and the formation of three-dimensional networks; For example, melamine resins such as trimethylol melamine and hexamethylol melamine, urea resins such as dimethylol propylene urea, dimethylol ethylene urea, and dimethylol hydroxyl urea, and amino blast resins such as dimethylol uron resin, (Blocked) isocyanates, Vinyl ethers, Polysiloxane resin with (meth)acrylic groups Epoxy resin.
[0024] (1-4-2) The crosslinkable polymer or crosslinkable compound (C) is a partial structure (I) represented by the following formulas (1-1) to (1-7) described in WO 2018 / 190380: [ka] (In the formula, R 1 , R 1a , R 3 , R 5a , and R 6aeach independently represents an alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 40 carbon atoms (the alkylene group and the arylene group may be optionally substituted with one or more amide groups or amino groups), an oxygen atom, a carbonyl group, a sulfur atom, -C(O)-NR a -, -NR b - or a divalent group consisting of a combination thereof, R 5 each independently represents a nitrogen atom, or a nitrogen atom and an alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 40 carbon atoms (the alkylene group and the arylene group may be optionally substituted with one or more amido groups or amino groups), an oxygen atom, a carbonyl group, a sulfur atom, -C(O)-NR a - and -NR b - represents a trivalent group consisting of a combination of at least one group selected from the group consisting of R 2 , R 2a , R 4 , and R 6 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a hydrogen atom and an alkylene group having 1 to 10 carbon atoms, an oxygen atom, a carbonyl group, or -C(O)-NR a - and -NR b - represents a monovalent group consisting of a combination of at least one group selected from the group consisting of R a represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, R b represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkylcarbonyl group having 1 to 10 carbon atoms, n represents the number of repeating units from 1 to 10; and The dotted lines represent chemical bonds to adjacent atoms.) The crosslinkable compound may be a compound containing at least one, preferably at least two, partial structures selected from the following: The entire disclosure of WO 2018 / 190380 is incorporated by reference into this application.
[0025] (1-4-3) The crosslinkable polymer or crosslinkable compound (C) may be a combination of a multifunctional epoxy (meth)acrylate compound and a multifunctional thiol compound as described in JP2016-003160A. Such a combination can be suitably crosslinked by a radical polymerization initiator. The polyfunctional epoxy (meth)acrylate compound may have a molecular weight of 300 to 20,000. The polyfunctional epoxy (meth)acrylate compound may be a bisphenol-type polyfunctional epoxy (meth)acrylate compound. The polyfunctional thiol compound may be in a liquid state at 25°C. In addition to the above combination, a polymerization inhibitor may be contained. The entire disclosure of JP 2016-003160 A is incorporated by reference into this application.
[0026] (1-4-4) The crosslinkable polymer or crosslinkable compound (C) may be a photopolymerizable substance as described in WO 2009 / 104643. The photopolymerizable substance may be a compound having at least one reactive group capable of cationic polymerization, or may be a compound having at least one reactive group capable of radical polymerization. The photopolymerizable compound may be a sugar compound. The sugar compound may be a monosaccharide or a disaccharide compound. The sugar compound has the formula (10): [ka] (However, G 1 represents a sugar skeleton, T represents a divalent linking group, R 1 represents a vinyl group or a glycidyl group, R 2 represents a hydrogen atom or a hydroxyl group. n and L each represent an integer of 0 or 1, and p is an integer that is the total number of hydroxyl groups in the sugar. m is an integer that satisfies 1≦m≦(pm), preferably 2≦m≦(pm). The photopolymerizable compound may be an alicyclic epoxy compound or an alicyclic oxetane compound. The alicyclic epoxy compound may be a cycloalkylene oxide derivative. The alicyclic epoxy compound is represented by formula (2) or (3): [ka] (However, G 2 represents a monovalent to pentavalent linking group having an alkylene group, a carbonyloxy group, a heterocycle, an aromatic ring, or a combination thereof; G 3 represents an organic group having an alkyl group, an alkylcarbonyl group, a heterocycle, an aromatic ring, or a combination thereof, and n and m each represent an integer of 1 to 5, preferably m represents an integer of 2 to 5. The entire disclosure of WO 2009 / 104643 is incorporated herein by reference.
[0027] (1-5: Resin composition) The method for preparing the photocurable resin composition is not particularly limited. That is, the self-crosslinking polymer (A), the solvent (B), the optional crosslinking polymer or crosslinking compound (C), and other components may be mixed in any ratio and in any order to prepare a homogeneous solution. The photocurable resin composition in the solution state thus prepared is preferably used after filtering using a filter having a pore size of about 0.2 μm. When a cured film having a thickness of about 300 nm is produced by a spin coating method, the photocurable resin composition preferably has a viscosity of about 100 cps or less at 25° C. In the present invention, the viscosity is a value measured using an E-type viscometer.
[0028] (1-6: Protective film forming composition) The photocurable resin composition according to one embodiment of the present invention has excellent etching resistance, and therefore can be preferably used as a protective film-forming composition used to protect the edge of a surface of a wafer for semiconductor production (wafer edge protective film-forming composition for semiconductor production, hereinafter sometimes abbreviated as "protective film-forming composition"). The properties of the protective film covering the edge of a substrate (wafer) for semiconductor manufacturing desirably satisfy, in addition to the function of preventing metal contamination described above, dry etching resistance, phosphoric acid resistance, tetramethylammonium hydroxide (TMAH) resistance, HF removability, scratch resistance, good embedding ability for uneven substrates, low amount of sublimation, affinity for hydrophobic substrates, no crater foreign matter or the like left on the side of the wafer, good edge shape, and the function of suppressing inner humps (a phenomenon in which a film-forming composition remains in a lump shape directly below the nozzle injection hole). The protective film forming composition according to one embodiment of the present invention is photosensitive. For example, it may be a negative solvent-developable type. After applying the photosensitive protective film forming composition (negative type) to the front surface end and, optionally, the bevel portion and / or the back surface end of the substrate, the bevel portion can be accurately covered with the protective film by exposing and developing the portion where the film is to be cured. The photosensitivity of the protective film has the advantages of facilitating film thickness control at the wafer end surface of the protective film, making it possible to remove inner humps, improving the edge shape, and correcting the deviation of the center position during spin coating.
[0029] (1-7: Polysiloxane) (1-7-1) The photocurable resin composition according to one embodiment of the present invention may optionally contain a polysiloxane. The polysiloxane may be a modified polysiloxane in which a portion of the silanol groups has been modified, for example, a polysiloxane modified product in which a portion of the silanol groups has been alcohol-modified or acetal-protected. The polysiloxane may be, for example, a hydrolysis condensation product of a hydrolysis condensation product, or a modified product in which at least a portion of the silanol groups of the hydrolysis condensation product have been alcohol-modified or acetal-protected (hereinafter, sometimes referred to as a "modification product of the hydrolysis condensation product"). The hydrolysis silane related to the hydrolysis condensation product may contain one or more hydrolysis silanes. The polysiloxane may have any of a cage type, ladder type, straight chain type, and branched type main chain structure. Furthermore, commercially available polysiloxanes may be used. In addition, the "hydrolysis condensate" of hydrolyzable silane, that is, the product of hydrolysis condensation, includes not only polyorganosiloxane polymers that are condensates in which condensation is completely completed, but also polyorganosiloxane polymers that are partial hydrolysis condensates in which condensation is not completely completed.Similar to the condensates in which condensation is completely completed, such partial hydrolysis condensates are also polymers obtained by hydrolysis and condensation of hydrolyzable silane, but they are only partially hydrolyzed and not condensed, and therefore Si-OH groups remain. Examples of the polysiloxane include hydrolysis condensates of hydrolyzable silanes containing at least one hydrolyzable silane represented by the following formula (1) or modified products thereof. [ka] In formula (1), R 1 are groups bonded to silicon atoms and independently represent an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted aralkyl group, an optionally substituted halogenated alkyl group, an optionally substituted halogenated aryl group, an optionally substituted halogenated aralkyl group, an optionally substituted alkoxyalkyl group, an optionally substituted alkoxyaryl group, an optionally substituted alkoxyaralkyl group, or an optionally substituted alkenyl group, or represent an organic group having an epoxy group, an organic group having an acryloyl group, an organic group having a methacryloyl group, an organic group having a mercapto group, an organic group having an amino group, an organic group having an alkoxy group, an organic group having a sulfonyl group, or an organic group having a cyano group, or a combination of two or more thereof. Also R 2 are groups or atoms bonded to a silicon atom, and each independently represents an alkoxy group, an aralkyloxy group, an acyloxy group, or a halogen atom. a represents an integer of 0 to 3.
[0030] (1-7-2: Specific examples of hydrolyzable silanes represented by formula (1)) Specific examples of hydrolyzable silanes represented by formula (1) include tetramethoxysilane, tetrachlorosilane, tetraacetoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, methyltrimethoxysilane, methyltrichlorosilane, methyltriacetoxysilane, methyltriethoxysilane, methyltripoxysilane, methyltributoxysilane, methyltriamyloxysilane, methyltriphenoxysilane, methyltribenzyloxysilane, and methyltriphenoxysilane. Netyloxysilane, glycidoxymethyltrimethoxysilane, glycidoxymethyltriethoxysilane, α-glycidoxyethyltrimethoxysilane, α-glycidoxyethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, α-glycidoxypropyltrimethoxysilane, α-glycidoxypropyltriethoxysilane, β-glycidoxypropyltrimethoxysilane, β-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane Glycidoxypropyltriethoxysilane, γ-glycidoxypropyltripropoxysilane, γ-glycidoxypropyltributoxysilane, γ-glycidoxypropyltriphenoxysilane, α-glycidoxybutyltrimethoxysilane, α-glycidoxybutyltriethoxysilane, β-glycidoxybutyltriethoxysilane, γ-glycidoxybutyltrimethoxysilane, γ-glycidoxybutyltriethoxysilane, δ-glycidoxybutyltrimethoxysilane, δ-glycidoxybutyltriethoxysilane, (3,4-epoxysilane cyclohexyl)methyltrimethoxysilane, (3,4-epoxycyclohexyl)methyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltripropoxysilane, β-(3,4-epoxycyclohexyl)ethyltributoxysilane, β-(3,4-epoxycyclohexyl)ethyltriphenoxysilane, γ-(3,4-epoxycyclohexyl)propyltrimethoxysilane,γ-(3,4-epoxycyclohexyl)propyltriethoxysilane, δ-(3,4-epoxycyclohexyl)butyltrimethoxysilane, δ-(3,4-epoxycyclohexyl)butyltriethoxysilane, glycidoxymethylmethyldimethoxysilane, glycidoxymethylmethyldiethoxysilane, α-glycidoxyethylmethyldimethoxysilane, α-glycidoxyethylmethyldiethoxysilane, β-glycidoxyethylmethyldimethoxysilane, β-glycidoxyethylethyldimethoxysilane, α-glycidoxypropylmethyldimethoxysilane Silane, α-glycidoxypropyl methyl diethoxysilane, β-glycidoxypropyl methyl dimethoxysilane, β-glycidoxypropyl ethyl dimethoxysilane, γ-glycidoxypropyl methyl dimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-glycidoxypropyl methyl dipropoxysilane, γ-glycidoxypropyl methyl dibutoxysilane, γ-glycidoxypropyl methyl diphenoxysilane, γ-glycidoxypropyl ethyl dimethoxysilane, γ-glycidoxypropyl ethyl diethoxysilane, γ-glycidoxypropyl methyl diphenoxysilane Glycidoxypropylvinyldimethoxysilane, γ-glycidoxypropylvinyldiethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrichlorosilane, vinyltriacetoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, methylvinyldichlorosilane, methylvinyldiacetoxysilane, dimethylvinylmethoxysilane, dimethylvinylethoxysilane, dimethylvinylchlorosilane, dimethylvinylacetoxysilane, divinyldimeth silane, divinyldiethoxysilane, divinyldichlorosilane, divinyldiacetoxysilane, gamma-glycidoxypropylvinyldimethoxysilane, gamma-glycidoxypropylvinyldiethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, allyltrichlorosilane, allyltriacetoxysilane, allylmethyldimethoxysilane, allylmethyldiethoxysilane, allylmethyldichlorosilane, allylmethyldiacetoxysilane, allyldimethylmethoxysilane, allyldimethylethoxysilane, allyldimethylchlorosilane,Allyldimethylacetoxysilane, diallyldimethoxysilane, diallyldiethoxysilane, diallyldichlorosilane, diallyldiacetoxysilane, 3-allylaminopropyltrimethoxysilane, 3-allylaminopropyltriethoxysilane, p-styryltrimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenyltrichlorosilane, phenyltriacetoxysilane, phenylmethyldimethoxysilane, phenylmethyldiethoxysilane, phenylmethyldichlorosilane, phenylmethyldiacetoxysilane , Phenyldimethylmethoxysilane, Phenyldimethylethoxysilane, Phenyldimethylchlorosilane, Phenyldimethylacetoxysilane, Diphenylmethylmethoxysilane, Diphenylmethylethoxysilane, Diphenylmethylchlorosilane, Diphenylmethylacetoxysilane, Diphenyldimethoxysilane, Diphenyldiethoxysilane, Diphenyldichlorosilane, Diphenyldiacetoxysilane, Triphenylmethoxysilane, Triphenylethoxysilane, Triphenylacetoxysilane, Triphenylchlorosilane, 3-Phenyl aminopropyltrimethoxysilane, 3-phenylaminopropyltriethoxysilane, dimethoxymethyl-3-(3-phenoxypropylthiopropyl)silane, triethoxy((2-methoxy-4-(methoxymethyl)phenoxy)methyl)silane, benzyltrimethoxysilane, benzyltriethoxysilane, benzylmethyldimethoxysilane, benzylmethyldiethoxysilane, benzyldimethylmethoxysilane, benzyldimethylethoxysilane, benzyldimethylchlorosilane, phenethyltrimethoxysilane, phenethyltriethoxysilane Silane, phenethyltrichlorosilane, phenethyltriacetoxysilane, phenethylmethyldimethoxysilane, phenethylmethyldiethoxysilane, phenethylmethyldichlorosilane, phenethylmethyldiacetoxysilane, methoxyphenyltrimethoxysilane, methoxyphenyltriethoxysilane, methoxyphenyltriacetoxysilane, methoxyphenyltrichlorosilane, methoxybenzyltrimethoxysilane, methoxybenzyltriethoxysilane, methoxybenzyltriacetoxysilane, methoxybenzyltrichlorosilane,Methoxyphenethyltrimethoxysilane, Methoxyphenethyltriethoxysilane, Methoxyphenethyltriacetoxysilane, Methoxyphenethyltrichlorosilane, Ethoxyphenyltrimethoxysilane, Ethoxyphenyltriethoxysilane, Ethoxyphenyltriacetoxysilane, Ethoxyphenyltrichlorosilane, Ethoxybenzyltrimethoxysilane, Ethoxybenzyltriethoxysilane, Ethoxybenzyltriacetoxysilane, Ethoxybenzyltrichlorosilane, i-Propoxyphenyltrimethoxysilane, i-Propoxy i-Propoxyphenyltriethoxysilane, i-Propoxyphenyltriacetoxysilane, i-Propoxyphenyltrichlorosilane, i-Propoxybenzyltrimethoxysilane, i-Propoxybenzyltriethoxysilane, i-Propoxybenzyltriacetoxysilane, i-Propoxybenzyltrichlorosilane, t-Butoxyphenyltrimethoxysilane, t-Butoxyphenyltriethoxysilane, t-Butoxyphenyltriacetoxysilane, t-Butoxyphenyltrichlorosilane, t-Butoxybenzyltrimethoxysilane, t-Butoxy Benzyltriethoxysilane, t-butoxybenzyltriacetoxysilane, t-butoxybenzyltrichlorosilane, methoxynaphthyltrimethoxysilane, methoxynaphthyltriethoxysilane, methoxynaphthyltriacetoxysilane, methoxynaphthyltrichlorosilane, ethoxynaphthyltrimethoxysilane, ethoxynaphthyltriethoxysilane, ethoxynaphthyltriacetoxysilane, ethoxynaphthyltrichlorosilane, γ-chloropropyltrimethoxysilane, γ-chloropropyltriethoxysilane, γ-chloropropyltrichlorosilane Triacetoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, β-cyanoethyltriethoxysilane, thiocyanatepropyltriethoxysilane, chloromethyltrimethoxysilane, chloromethyltriethoxysilane, triethoxysilylpropyldiallylisocyanurate, bicyclo[2,2,1]heptenyltriethoxysilane, benzenesulfonylpropyltriethoxysilane,Examples of the silane include, but are not limited to, benzenesulfonamidopropyltriethoxysilane, dimethylaminopropyltrimethoxysilane, dimethyldimethoxysilane, phenylmethyldimethoxysilane, dimethyldiethoxysilane, phenylmethyldiethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropylmethyldiethoxysilane, dimethyldiacetoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptomethyldiethoxysilane, methylvinyldimethoxysilane, and methylvinyldiethoxysilane.
[0031] (1-8: Other optional ingredients) Furthermore, the photocurable resin composition according to one embodiment of the present invention may contain, as necessary, a radical polymerization initiator (such as a photopolymerization initiator), an acid (catalyst), a thermal acid generator, a photoacid generator, a base (catalyst), a thermal base generator, a photobase generator, an antioxidant, a polymerization inhibitor, a crosslinking agent (such as a polyfunctional acrylic), an adhesion improver, an adhesion aid (a silane coupling agent), a surfactant, an antifoaming agent, a rheology adjuster, a pigment, a dye, a storage stabilizer, a dissolution promoter such as a polyhydric phenol or a polyvalent carboxylic acid, a sensitizer, or the like. However, since the self-crosslinking polymer (A) contained in the photocurable resin composition according to one embodiment of the present invention is self-crosslinkable, it is not essential to add a photopolymerization initiator at least for curing the self-crosslinking polymer (A).
[0032] (1-8-1: Radical polymerization initiator) The radical polymerization initiator may be any one capable of releasing a substance that initiates radical polymerization by irradiation with light and / or heating. Examples of the photoradical polymerization initiator include benzophenone derivatives, imidazole derivatives, bisimidazole derivatives, N-arylglycine derivatives, organic azide compounds, titanocene compounds, aluminate complexes, organic peroxides, N-alkoxypyridinium salts, and thioxanthone derivatives. More specifically, examples of the compounds include benzophenone, 1,3-di(tert-butyldioxycarbonyl)benzophenone, 3,3',4,4'-tetrakis(tert-butyldioxycarbonyl)benzophenone, 3-phenyl-5-isoxazolone, 2-mercaptobenzimidazole, bis(2,4,5-triphenyl)imidazole, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, bis(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium), and the like. As the photoradical polymerization initiator, commercially available products can be used, for example, IRGACURE (registered trademark) 651, 184, 369, 784 manufactured by BASF. In addition, commercially available products other than the above can also be used, specifically, IRGACURE (registered trademark) 500, 907, 379, 819, 127, 500, 754, 250, 1800, 1870, OXE01, DAROCUR (registered trademark) TPO, 1173 manufactured by BASF; Speedcure (registered trademark) MBB, PBZ, ITX, CTX, EDB manufactured by Lambson; Esacure (registered trademark) ONE, KIP150, KTO46 manufactured by Lamberti; KAYACURE (registered trademark) DETX-S, CTX, BMS, DMBI manufactured by Nippon Kayaku Co., Ltd. Examples of the thermal radical polymerization initiator include peroxides such as acetyl peroxide, benzoyl peroxide, methyl ethyl ketone peroxide, cyclohexanone peroxide, hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, tert-butyl peroxyacetate, tert-butyl peroxypivalate, and tert-butylperoxy-2-ethylhexanoate; 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and (1-phenylethyl) Examples of the azo-based compounds include azodiphenylmethane, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl-2,2'-azobisisobutyrate, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(1-cyclohexanecarbonitrile), 2-(carbamoylazo)isobutyronitrile, 2,2'-azobis(2,4,4-trimethylpentane), 2-phenylazo-2,4-dimethyl-4-methoxyvaleronitrile, and 2,2'-azobis(2-methylpropane); and persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate, but are not limited to these. Examples of commercially available thermal radical polymerization initiators include Perloil (registered trademark) IB, NPP, IPP, SBP, TCP, OPP, SA, 355, L, Perbutyl (registered trademark) ND, NHP, MA, PV, 355, A, C, D, E, L, I, O, P, Z, Perhexyl (registered trademark) ND, PV, D, I, O, Z, Perocta (registered trademark) ND, Niper (registered trademark) PMB, BMT, BW, Pertetra (registered trademark) A, Perhexa (registered trademark) MC, TMH, HC, 250, 25B, C, 25Z, 22, V, Perocta (registered trademark) O, Percumyl (registered trademark) ND, D, Permenta (registered trademark) H, and Nofumar (registered trademark) BC, all of which are manufactured by NOF Corporation; and V-70, V-65, V-59, V-40, V-30, and V, all of which are manufactured by Wako Pure Chemical Industries, Ltd. Examples of the acrylic resins include, but are not limited to, A-044, VA-046B, VA-061, V-50, VA-057, VA-086, VF-096, VAm-110, V-601, and V-501; BASF's IRGACURE (registered trademark) 184, 369, 651, 500, 819, 907, 784, 2959, CGI1700, CGI1750, CGI1850, CG24-61, DAROCUR (registered trademark) 1116, 1173, and LUCIRIN (registered trademark) TPO; Cytec Surface Specialties' UVECRYL (registered trademark) P36; and Lamberti's Esacure (registered trademark) KIP150, KIP65LT, KIP100F, KT37, KT55, KTO46, and KIP75 / B. The radical polymerization initiator may be used alone or in combination of two or more. The content of the radical polymerization initiator is preferably 1 part by mass or more, 2 parts by mass or more, 3 parts by mass or more, and 50 parts by mass or less, 20 parts by mass or less, or 10 parts by mass or less, based on 100 parts by mass of the polymer or compound having a crosslinkable group.
[0033] (1-8-2: Polymerization inhibitor) As the polymerization inhibitor, a hindered phenol compound may be used, specifically, 2,6-diisobutylphenol, 3,5-di-t-butylphenol, 3,5-di-t-butylcresol, hydroquinone, hydroquinone monomethyl ether, N-nitroso-N-phenylhydroxylamine aluminum, pyrogallol, t-butylcatechol, 4-methoxy-1-naphthol, 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)- ... 1,6-Hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butylphenol), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] 〕, 2,2-thio-diethylenebis〔3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate〕, N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), pentaerythrityl-tetrakis〔3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate〕, tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanate anurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-Triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl) benzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3- 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, etc. can be mentioned. Among the hindered phenol compounds, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione is preferred. As the polymerization inhibitor, a commercially available product may be used, and a specific example thereof is Irganox-3114 (manufactured by BASF Japan Ltd.). The polymerization inhibitor may be used alone or in combination of two or more. The content of the polymerization inhibitor is preferably 0.01 to 1 part by mass, more preferably 0.01 to 0.5 parts by mass, based on 100 parts by mass of the total amount of the self-crosslinking polymer (A) and the optionally contained crosslinking polymer or crosslinking compound (C).
[0034] (1-8-3: Surfactant) Examples of surfactants include polyoxyethylene alkyl ether compounds such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl allyl ether compounds such as polyoxyethylene octyl phenol ether and polyoxyethylene nonyl phenol ether; polyoxyethylene-polyoxypropylene block copolymer compounds; sorbitan fatty acid ester compounds such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan trioleate, and sorbitan tristearate; and polyoxyethylene sorbitan fatty acid ester compounds such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, and polyoxyethylene sorbitan tristearate. Other examples include fluorine-based surfactants such as F-TOP EF301, EF303, and EF352 (manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, R-08, and R-30 (manufactured by Dainippon Ink Co., Ltd.), Fluorad FC430 and FC431 (manufactured by Sumitomo 3M Limited), and Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by Asahi Glass Co., Ltd.), and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The surfactant may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 parts by mass or more, 0.5 parts by mass or more, 5 parts by mass or less, and 2 parts by mass or less, based on 100 parts by mass of the total amount of the self-crosslinking polymer (A) and the crosslinking polymer or crosslinking compound optionally contained.
[0035] (1-8-4: Other components such as acid-base catalysts) As the acid catalyst or base catalyst, an acidic compound, a basic compound, or various compounds that generate an acid or a base by heat or light can be used. As the acidic compound, a sulfonic acid compound or a carboxylic acid compound can be used. Examples of the sulfonic acid compound or carboxylic acid compound include p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium trifluoromethanesulfonate (=pyridinium trifluoromethanesulfonic acid), pyridinium-p-toluenesulfonate, pyridinium-4-hydroxybenzenesulfonate, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-phenolsulfonic acid, pyridinium-4-phenolsulfonate, benzenedisulfonic acid, 1-naphthalenesulfonic acid, 4-nitrobenzenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid. As the basic compound, an amine compound or an ammonium hydroxide compound can be used, and as the compound that generates a base by heat, urea can be used. Examples of the amine compound include tertiary amines such as triethanolamine, tributanolamine, trimethylamine, triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, tri-tert-butylamine, tri-n-octylamine, triisopropanolamine, phenyldiethanolamine, stearyldiethanolamine, and diazabicyclooctane, and aromatic amines such as pyridine and 4-dimethylaminopyridine. Other examples of the amine compound include primary amines such as benzylamine and n-butylamine, and secondary amines such as diethylamine and di-n-butylamine. Examples of ammonium hydroxide compounds include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, benzyltriethylammonium hydroxide, cetyltrimethylammonium hydroxide, phenyltrimethylammonium hydroxide, and phenyltriethylammonium hydroxide. As the acid generator, either a thermal acid generator or a photoacid generator can be used. Examples of the thermal acid generator include sulfonic acid compounds and carboxylic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate (pyridinium p-toluenesulfonic acid), pyridinium p-hydroxybenzenesulfonic acid (pyridinium p-phenolsulfonic acid salt), pyridinium trifluoromethanesulfonic acid, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid. Examples of commercially available products include K-PURE (registered trademark) CXC-1612, CXC-1614, TAG-2172, TAG-2179, TAG-2678, and TAG2689 (all manufactured by King Industries), and SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (all manufactured by Sanshin Chemical Industry Co., Ltd.). Examples of photoacid generators include sulfonium salts, iodonium salts, sulfonyldiazomethane, N-sulfonyloxyimide, benzoin sulfonate-type photoacid generators, pyrogallol trisulfonate-type photoacid generators, sulfone-type photoacid generators, glyoxime derivative-type photoacid generators, oxime-O-sulfonate-type acid generators, bisoxime sulfonate-type acid generators, etc. Examples include bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, phenyl-bis(trichloromethyl)-s-triazine, benzoin tosylate, and N-hydroxysuccinimide trifluoromethanesulfonate. Examples of the thermal base generator include carbamates such as 1-methyl-1-(4-biphenylyl)ethyl carbamate and 2-cyano-1,1-dimethylethyl carbamate; ureas such as urea and N,N-dimethyl-N'-methylurea; guanidines such as guanidine trichloroacetate, guanidine phenylsulfonylacetate, and guanidine phenylpropiolate; dihydropyridines such as 1,4-dihydronicotinamide; dimethylpiperidines such as N-(isopropoxycarbonyl)-2,6-dimethylpiperidine, N-(tert-butoxycarbonyl)-2,6-dimethylpiperidine, and N-(benzyloxycarbonyl)-2,6-dimethylpiperidine; quaternary ammonium salts such as tetramethylammonium phenylsulfonylacetate and tetramethylammonium phenylpropiolate; and dicyandiamide. Further examples include U-CAT (registered trademark) SA810, SA831, SA841, and SA851 (all manufactured by San-Apro Ltd.), which are salts of 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU). Examples of the photobase generator include alkylamine-based photobase generators such as 9-anthrylmethyl-N,N-diethylcarbamate; cycloalkylamine-based photobase generators such as 9-anthryl-N,N-dicyclohexylcarbamate, 1-(9,10-anthraquinone-2-yl)ethyl-N,N-dicyclohexylcarbamate, dicyclohexylammonium-2-(3-benzoylphenyl)propionate, 9-anthryl-N-cyclohexylcarbamate, 1-(9,10-anthraquinone-2-yl)ethyl-N-cyclohexylcarbamate, cyclohexylammonium-2-(3-benzoylphenyl)propionate, and (E)-N-cyclohexyl-3-(2-hydroxyphenyl)acrylamide; and 9-anthrylmethyl=piperidine-1-carboxylate and (E)-1-piperidino-3-(2-hydroxyphenyl)-2-propene. -1-one, (2-nitrophenyl)methyl-4-hydroxypiperidine-1-carboxylate, (2-nitrophenyl)methyl-4-(methacryloyloxy)piperidine-1-carboxylate and other piperidine-based photobase generators; guanidinium = 2-(3-benzoylphenyl)propionate, 1,2-diisopropyl-3-(bis(dimethylamino)methylene)guanidinium = 2-(3-benzoylphenyl)propionate, guanidine-based photobase generators such as 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidium-n-butyltriphenylborate and 1,5,7-triazabicyclo[4.4.0]dec-5-enium-2-(9-oxoxanthen-2-yl)propionate; and imidazole-based photobase generators such as 1-(9,10-anthraquinone-2-yl)ethyl-imidazole-1-carboxylate. The above components can be used alone or in combination of two or more kinds. In that case, they are used in an amount of usually 10 mass % or less, preferably 3 mass % or less, based on the solid content of the photocurable resin composition of the present application.
[0036] <2. Protective film [6] / Semiconductor manufacturing wafer
[10] > (2-1:Protective film [6]) The protective film [6] according to one embodiment of the present invention is a cured product of a coating film made of a composition for forming a protective film for a wafer edge in semiconductor manufacturing [5]. The protective film has excellent etching resistance and is therefore useful for preventing metal contamination of the wafer edge in semiconductor manufacturing. The thickness of the protective film can be, for example, 1 to 500 nm, and light with a wavelength of, for example, 170 to 800 nm can be used for photocuring.
[0037] (2-2: Wafers for semiconductor manufacturing
[10] ) The semiconductor manufacturing wafer of one embodiment of the present invention is a semiconductor manufacturing wafer having a protected wafer edge, which is formed by applying a protective film forming composition [5] of one embodiment of the present invention (see <1. Photocurable resin composition [1] / Wafer edge protective film forming composition [5] for semiconductor manufacturing> above) to the wafer edge.
[0038] <3. Semiconductor device manufacturing method
[11] > A method for manufacturing a semiconductor device according to one aspect of the present invention includes the steps of: (A) forming a resist film on a semiconductor substrate; (B) forming a resist pattern by irradiating the resist film with light or an electron beam and then developing it; (C) processing the semiconductor substrate by etching, or processing the semiconductor substrate by etching through the patterned resist; A method for manufacturing a semiconductor device comprising: A step (X) of forming a protective film from the protective film forming composition according to [5] of one embodiment of the present invention on the front surface edge and, optionally, the bevel portion and / or the back surface edge of the wafer for semiconductor manufacturing. The present invention relates to a method for manufacturing a semiconductor device. The following explains each in order.
[0039] (3-1: (A) A step of forming a resist film on a semiconductor substrate) A resist film is formed on a semiconductor substrate. The semiconductor substrate is a wafer used for manufacturing semiconductor elements and the like, and in addition to commonly used silicon wafers and germanium wafers, compound semiconductor wafers formed by combining two or more elements, such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride, can be used. These are usually disk-shaped and have sizes of, for example, 4, 6, 8, or 12 inches. Commercially available products may be used. When using a semiconductor substrate having an inorganic film formed on its surface, the inorganic film is formed by, for example, ALD (atomic layer deposition), CVD (chemical vapor deposition), reactive sputtering, ion plating, vacuum deposition, or spin-coating (spin-on glass: SOG). Examples of the inorganic film include polysilicon film, silicon oxide film, silicon nitride film, BPSG (Boro-Phospho Silicate Glass) film, titanium nitride film, titanium nitride oxide film, tungsten film, gallium nitride film, and gallium arsenide film. On such a semiconductor substrate, a resist underlayer film, a resist film, etc., of a predetermined thickness are formed by an appropriate coating method such as spray, spinner, coater, etc. In general, in the case of a spin coating method, the resist underlayer film forming composition, the resist film forming composition, etc. are each supplied from above the center of a rotating disk-shaped substrate through a nozzle, etc. Usually, these films are baked using a heating means such as a hot plate. The photoresist used to form the resist film is not particularly limited as long as it is sensitive to the light used for exposure. Both negative photoresists and positive photoresists can be used. There are positive photoresists made of novolac resin and 1,2-naphthoquinone diazide sulfonic acid ester, chemically amplified photoresists made of a binder having a group that decomposes with acid to increase the alkaline dissolution rate and a photoacid generator, chemically amplified photoresists made of a low molecular compound that decomposes with acid to increase the alkaline dissolution rate of the photoresist, an alkali-soluble binder, and a photoacid generator, chemically amplified photoresists made of a binder having a group that decomposes with acid to increase the alkaline dissolution rate of the photoresist, a low molecular compound that decomposes with acid to increase the alkaline dissolution rate of the photoresist, and a photoacid generator, resists containing metal elements, and the like. For example, there are V146G (trade name) manufactured by JSR Corporation, APEX-E (trade name) manufactured by Shipley Co., Ltd., PAR710 (trade name) manufactured by Sumitomo Chemical Co., Ltd., and AR2772 and SEPR430 (trade names) manufactured by Shin-Etsu Chemical Co., Ltd. Further, for example, fluorine-containing polymer photoresists such as those described in Proc. SPIE, Vol. 3999, 330-334 (2000), Proc. SPIE, Vol. 3999, 357-364 (2000), and Proc. SPIE, Vol. 3999, 365-374 (2000) can be used. Negative photoresists are preferred. The resist film forming composition used for forming the resist film can contain one or more metals. The form of the metal can be a simple metal, a metal salt, a metal complex, or other metal-containing compounds. The metal species is not particularly limited, and examples thereof include tin, indium, antimony, bismuth, gallium, germanium, aluminum, zirconium, hafnium, cerium, lanthanum, and cesium. The bake conditions for the resist film are appropriately selected from a bake temperature of 70° C. to 400° C. and a bake time of 0.3 to 60 minutes, preferably a bake temperature of 80° C. to 350° C. and a bake time of 0.5 to 30 minutes, and more preferably a bake temperature of 90° C. to 300° C. and a bake time of 0.8 to 10 minutes. The lower limit of the average thickness of the resist film is preferably 1 nm, more preferably 3 nm, 5 nm, or 10 nm.The upper limit of the average thickness of the resist film is 5,000 nm, 3,000 nm, or 2,000 nm, preferably 1,000 nm, more preferably 200 nm, and more preferably 50 nm.
[0040] (3-2: Step (X) of forming a protective film, and optional steps (Y) and (Z)) (3-2-1: Process X) Step (X) of forming a protective film from the protective film-forming composition according to one embodiment of the present invention [5] on the front surface edge and, optionally, on the bevel portion and / or back surface edge of a semiconductor manufacturing wafer is carried out at any time. In step (X), a preferred procedure is to apply the protective film-forming composition, and then expose and develop a predetermined area. Step (X) may be carried out before step (A), between step (A) and step (B), or after step (B) or step (C). In this specification, the surface of the substrate on which a device portion such as a resist film is provided is referred to as the front surface, and the opposite surface is referred to as the back surface. The front surface edge refers to a region that is usually 1 to 10 mm wide from the edge of the device portion provided on the substrate to the bevel portion, the bevel portion refers to a curved region that connects the front surface edge and the back surface edge, and the back surface edge refers to a region that corresponds to the front surface edge on the back surface of the substrate. First, the protective film forming composition according to one embodiment of the present invention [5] (see <1. Photocurable resin composition [1] / Wafer edge protective film forming composition for semiconductor manufacturing [5]>) is applied to a semiconductor substrate on which a resist film or the like is formed. The method for applying the protective film forming composition is not particularly limited, and for example, known means such as a spin coating method or a spray method can be adopted. For example, when the spin coating method is adopted, the protective film forming composition is supplied through a nozzle from above or near the front edge of the rotating disk-shaped substrate while rotating the semiconductor substrate on which a resist film or the like is formed at a predetermined rotation speed. Preferably, the protective film forming composition is also supplied through a nozzle from the vicinity of the bevel portion and / or back edge of the substrate. The spin-coating conditions can be appropriately selected and are not limited in any way. Typical conditions are as follows: Viscosity of protective film-forming composition: Approximately 100 cps or less Wafer rotation speed: ·When supplying the protective film forming composition: 50~500rpm When shaking off the dry air: 700 to 2,000 rpm Protective film thickness: 300nm Next, the protective film-forming composition is exposed to light. The exposure can be performed by irradiating the protective film-forming composition with ultraviolet light, visible light, radiation, or other actinic rays (including i-rays, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet), and EB (electron beam)) through or without a mask. Note that soft baking (SB) may be performed before exposure, and post-exposure baking (PEB) may be performed after exposure and before development. The post-exposure baking temperature is preferably 50°C to 150°C, and the post-exposure baking time is preferably 1 minute to 10 minutes. Next, the protective film-forming composition after exposure is developed. The development can be carried out by removing the exposed portion of the protective film-forming composition after exposure with a developer, and the development temperature is appropriately selected from 5° C. to 50° C., and the development time is appropriately selected from 10 seconds to 300 seconds. Examples of the organic solvent contained in the developer include alcohol-based solvents, ether-based solvents, ketone-based solvents, amide-based solvents, ester-based solvents, and hydrocarbon-based solvents. The organic solvent in the developer is preferably an ester-based solvent, a ketone-based solvent, or a combination thereof. The developer may contain one organic solvent alone or two or more organic solvents. Examples of the alcohol solvent include aliphatic monoalcohol solvents having 1 to 18 carbon atoms, such as 4-methyl-2-pentanol and n-hexanol; alicyclic monoalcohol solvents having 3 to 18 carbon atoms, such as cyclohexanol; and polyhydric alcohol partial ether solvents having 3 to 19 carbon atoms, such as propylene glycol monomethyl ether. Examples of ether solvents include dialkyl ether solvents such as diethyl ether, dipropyl ether, dibutyl ether, dipentyl ether, diisoamyl ether, dihexyl ether, and diheptyl ether; cyclic ether solvents such as tetrahydrofuran and tetrahydropyran; and aromatic ring-containing ether solvents such as diphenyl ether and anisole. Examples of ketone solvents include chain ketone solvents such as acetone, methyl ethyl ketone, methyl-n-propyl ketone, methyl-n-butyl ketone, diethyl ketone, methyl-iso-butyl ketone, 2-heptanone, ethyl-n-butyl ketone, methyl-n-hexyl ketone, di-iso-butyl ketone, and trimethylnonanone; cyclic ketone solvents such as cyclopentanone, cyclohexanone, cycloheptanone, cyclooctanone, and methylcyclohexanone; 2,4-pentanedione, acetonylacetone, and acetophenone. Examples of the amide solvents include cyclic amide solvents such as N,N'-dimethylimidazolidinone and N-methylpyrrolidone; and chain amide solvents such as N-methylformamide, N,N-dimethylformamide, N,N-diethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, and N-methylpropionamide. Examples of ester-based solvents include monocarboxylic acid ester-based solvents such as n-butyl acetate and ethyl lactate; polyhydric alcohol carboxylate-based solvents such as propylene glycol acetate; polyhydric alcohol partial ether carboxylate-based solvents such as propylene glycol monomethyl ether acetate; polyvalent carboxylic acid diester-based solvents such as diethyl oxalate; and carbonate-based solvents such as dimethyl carbonate and diethyl carbonate. Examples of the hydrocarbon solvent include aliphatic hydrocarbon solvents having 5 to 12 carbon atoms, such as n-pentane and n-hexane; and aromatic hydrocarbon solvents having 6 to 16 carbon atoms, such as toluene and xylene. Among these, ester solvents, ketone solvents, ether solvents and combinations thereof are preferred, and ester solvents, ketone solvents and combinations thereof are more preferred. As the ester solvent, propylene glycol monomethyl ether acetate is preferred. As the ketone solvent, cyclohexanone is preferred. As the ether solvent, propylene glycol monomethyl ether is preferred. The lower limit of the content of the organic solvent in the developer is preferably 80% by mass, more preferably 90% by mass, even more preferably 99% by mass, and particularly preferably 100% by mass.By setting the content of the organic solvent in the developer within the above range, the dissolution contrast between the exposed part and the unexposed part can be improved, and as a result, a resist pattern with better lithography performance can be formed.Examples of components other than the organic solvent include water, silicone oil, etc. The developer may contain a nitrogen-containing compound. When the developer contains a nitrogen-containing compound, film loss in the formed resist pattern can be further reduced. The developer may be an aqueous developer instead of the organic solvent developer. Specifically, the developer may be an aqueous alkali solution such as sodium hydroxide, potassium hydroxide, sodium silicate, ammonia, monoethylamine, diethylamine, triethylamine, triethanolamine, or tetramethylammonium hydroxide. The base concentration of these aqueous solutions is not particularly limited, but may be, for example, 0.1 to 10% by weight. The developer may also be used by adding alcohols or surfactants. These may each be blended in an amount of preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, per 100 parts by weight of the developer. Examples of surfactants include ionic and nonionic fluorine-based surfactants and silicon-based surfactants. Development methods include, for example, a method in which the substrate is immersed in a tank filled with developer for a certain period of time (dip method), a method in which the developer is piled up on the substrate surface by surface tension and left to stand for a certain period of time (paddle method), a method in which the developer is sprayed onto the substrate surface (spray method), and a method in which the developer is continuously dispensed by scanning a developer dispensing nozzle at a constant speed over a substrate rotating at a constant speed (dynamic dispense method). Next, the protective film-forming composition after development is baked. By baking the pattern obtained after development, a desired pattern can be formed. The heating temperature in the heat treatment is usually 150° C. or more and 350° C. or less, preferably in the range of 200 to 300° C. The heat treatment time is the time until the protective film-forming composition is cured, and is preferably approximately less than 30 minutes in consideration of productivity. The lower limit of the average thickness of the protective film is preferably 1 nm, more preferably 3 nm, and the upper limit of the average thickness of the protective film is preferably 500 nm, more preferably 300 nm.
[0041] (3-2-2:Process Y,Z) After step (X), in step (Y), the resist film on the protective film can be removed by a remover. At this time, similar to step (X), it is preferable to apply the remover to the front end of the semiconductor manufacturing wafer and, optionally, the bevel and / or back end. Examples of the resist remover include propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, water, butyl acetate, tetramethylammonium aqueous solution, or a mixture of these. Among these, propylene glycol monomethyl ether acetate and water are preferable from the viewpoint of removability of the resist film. After step (X) or step (Y), in step (Z), the protective film can be removed by ashing or treatment with hydrofluoric acid, an organic solvent, an alkaline developer, or a semiconductor cleaning solution, and then preferably washed with any solvent or a conventional semiconductor cleaning solution. Steps (X), (Y), and (Z) can be performed simultaneously with steps (A), (B), and (C), or at any time before or after each step. For example, when step (X) is included before step (A), step (Y) of removing the resist film on the protective film can be performed between steps (A) and (B), and step (Z) of removing the protective film can be performed between steps (Y) and (B). In addition, when step (X) is included between step (A) and step (B) or step (C), step (Z) of removing the protective film can also be performed between step (X) and step (B) or step (C).
[0042] (3-3: (B) a step of forming a resist pattern by irradiating a resist film with light or an electron beam and then developing it, and (C) a step of processing a semiconductor substrate by etching) (3-3-1: Exposure in step (B)) The resist film is exposed through a mask (reticle) for forming a predetermined pattern, and for example, i-line, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet) or EB (electron beam) is used. A soft bake (SB) may be performed before exposure, and a post-exposure bake (PEB) may be performed after exposure and before development. The post-exposure bake temperature is preferably 50°C to 150°C, and the post-exposure bake time is preferably 1 minute to 10 minutes.
[0043] (3-3-2: Development of step (B)) An alkaline developer is used for development, and the development temperature is appropriately selected from 5°C to 50°C, and the development time is appropriately selected from 10 seconds to 300 seconds. As the alkaline developer, for example, an aqueous solution of an alkaline such as inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and ammonia water, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-butylamine, tertiary amines such as triethylamine and methyldiethylamine, alcohol amines such as dimethylethanolamine and triethanolamine, quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline, and cyclic amines such as pyrrole and piperidine can be used. The base concentration of these aqueous solutions is not particularly limited, but can be, for example, 0.1 to 10% by weight. Furthermore, the aqueous solution of the above alkalis may be used by adding an appropriate amount of alcohols such as isopropyl alcohol, or a nonionic surfactant. Each of these may be blended in an amount of preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, per 100 parts by weight of the developer. Among these, preferred developers are quaternary ammonium salts, more preferably tetramethylammonium hydroxide and choline. Furthermore, surfactants may be added to these developers. Alternatively, instead of using an alkaline developer, development may be performed using a polyhydric alcohol solvent having 2 to 18 carbon atoms, such as 1,2-propylene glycol, or an organic solvent, such as butyl acetate, to develop the portions of the photoresist where the alkaline dissolution rate is not improved.
[0044] (3-3-3: Baking process (B)) Step (B) may include a step of baking the semiconductor substrate that has been exposed and developed as described above. The baking means is not particularly limited, but for example, a proximity bake furnace that uses multiple substrate support pins to ensure a gap between the substrate and a hot plate is preferably used. The baking temperature is usually 40° C. to 300° C., preferably 200 to 300° C. for 1 to 30 minutes, but may be set to 90° C. or lower when it is necessary to avoid damage to the resist pattern. Baking may be performed on the semiconductor substrate after exposure and before development. The baking means and conditions are as described above, but the temperature may be set to 90° C. or less if it is necessary to avoid damage to the resist pattern.
[0045] (3-3-4: Etching in step (C)) Next, the resist underlayer film is etched, preferably dry etched, using the formed resist pattern as a mask to form a patterned resist. In this case, if the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed, and if the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed. After that, the semiconductor substrate is processed by a method known per se (such as a dry etching method) using the patterned resist. The etching for processing the semiconductor substrate may be a known method. For example, when the semiconductor substrate is a silicon substrate, the etching method includes a process of processing the shape by dry etching using a fluorine-based gas such as carbon tetrafluoride, as well as a surface treatment process such as removing a silicon nitride film present on the surface of the semiconductor substrate with hot phosphoric acid.
[0046] <4. Manufacturing method of semiconductor wafers
[21] > (4-1) A method for manufacturing a semiconductor manufacturing wafer, which is one aspect of the present invention, includes a step of applying (or coating) a composition for forming a protective film for a semiconductor manufacturing wafer according to
[10] , which is one aspect of the present invention, to a front edge and, optionally, a bevel portion and / or a back edge of a semiconductor manufacturing wafer precursor, in the method for manufacturing a semiconductor device as described above, to produce a semiconductor manufacturing wafer with a protective film. Here, the wafer precursor for semiconductor manufacturing refers to a material obtained by subjecting a semiconductor substrate to at least one step of a method for manufacturing a semiconductor device. For example, in the above-mentioned method for manufacturing a semiconductor device, the material may be a material that has undergone a step of forming an inorganic film, a resist underlayer film, a resist film, etc. on a semiconductor substrate, and is not yet subjected to a step of forming a resist pattern by irradiating the resist film with light or an electron beam and then developing it.
[0047] (4-2: Specific aspects of the method for manufacturing wafers for semiconductor manufacturing) A composition for forming a protective film for a semiconductor manufacturing wafer according to one embodiment of the present invention [5] is applied by spin coating to the front edge and, optionally, the bevel and / or back edge of a semiconductor manufacturing wafer precursor obtained by one or more steps of a semiconductor device manufacturing process. Thereafter, the semiconductor substrate may be baked. In this case, the baking means is not particularly limited, but for example, a proximity bake furnace in which a gap is secured between the substrate and a hot plate using a plurality of substrate support pins is preferably used. The baking temperature is usually 40°C to 300°C, preferably 200°C to 300°C, for 1 to 30 minutes. After the protective film-forming composition is applied, the end face of the protective film may be subjected to known treatments in the semiconductor manufacturing process, such as edge bead removal and back rinsing. EXAMPLES
[0048] <Synthesis Example 1> 1 g of 4-benzoylphenyl methacrylate, 10.3 g of 2-hydroxypropyl methacrylate, and 0.2 g of 2,2'-azobis(methyl isobutyrate) were dissolved in 29.5 g of ethyl lactate and 12.6 g of propylene glycol monomethyl ether acetate, and the mixture was heated to 80°C and reacted for 24 hours to obtain the compounds represented by the following formulas (I) and (II): [ka] A solution of a copolymer of 4-benzoylphenyl methacrylate and 2-hydroxypropyl methacrylate having the repeating unit of the formula was obtained. GPC analysis of the copolymer was performed and the weight average molecular weight was 35,000 in terms of standard polystyrene.
[0049] <Synthesis Example 2> 1.5 g of 4-benzoylphenyl methacrylate, 1.6 g of 2-hydroxypropyl methacrylate, 10 g of styrene, and 0.3 g of 2,2'-azobis(methyl isobutyrate) were dissolved in 37.5 g of ethyl lactate and 16.1 g of propylene glycol monomethyl ether acetate, and the mixture was heated to 80°C and reacted for 24 hours to obtain the following compounds (I) to (III): [ka] A solution of a copolymer polymer compound of 4-benzoylphenyl methacrylate, 2-hydroxypropyl methacrylate, and styrene having the repeating unit was obtained. The obtained polymer solution was reprecipitated in methanol and then dried in a vacuum oven to obtain a white polymer compound. When the obtained polymer compound was subjected to GPC analysis, the weight average molecular weight was 34,000 in terms of standard polystyrene.
[0050] <Synthesis Example 3> 10 g of 2-hydroxypropyl methacrylate and 0.2 g of 2,2'-azobis(methyl isobutyrate) were dissolved in 28.9 g of ethyl lactate and 12.2 g of propylene glycol monomethyl ether acetate, and the mixture was heated to 80°C and reacted for 24 hours to obtain the compound represented by the formula (II):
[0051] [ka] A solution of a 2-hydroxypropyl methacrylate polymer compound having the repeating unit of the following formula was obtained. When the obtained copolymer polymer compound was subjected to GPC analysis, it was found that the weight average molecular weight was 35,000 in terms of standard polystyrene.
[0052] <Synthesis Example 4> 30.00 g of an epoxy group-containing novolak resin (product name: EPPN-201, epoxy value: 192 g / eq., manufactured by Nippon Kayaku Co., Ltd.), 11.26 g of acrylic acid, 1.99 g of tetrabutylphosphonium bromide, and 0.09 g of hydroquinone were added to 101.11 g of propylene glycol monomethyl ether acetate, and the mixture was heated and stirred at 100 °C for 18 hours under a nitrogen atmosphere. 43 g of an anion exchange resin (product name: AMBERJET® ESG4002(OH), manufactured by Organo Corporation) and 43 g of a cation exchange resin (product name: Amberlite® 15JWET, manufactured by Organo Corporation) were added to the obtained solution, and the ion exchange treatment was carried out at room temperature for 4 hours. After separating the ion exchange resin, a compound solution was obtained. The obtained compound corresponded to a polymer compound having a repeating unit of the formula (XX):
Chemical formula
[0053] <b. Preparation of Composition> <Composition 1> After adding 4.5 g of ethyl lactate and 1.9 g of propylene glycol monomethyl ether acetate to 8 g of the reaction product obtained in Synthesis Example 1, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a photocurable resin composition solution.
[0054] <Composition 2> After adding 16 g of propylene glycol monomethyl ether acetate to 4 g of the reaction product obtained in Synthesis Example 2, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a photocurable resin composition solution.
[0055] <Comparative Example 1> To 8 g of the reaction product obtained in Synthesis Example 3, 4.5 g of ethyl lactate and 1.9 g of propylene glycol monomethyl ether acetate were added, and then the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a photocurable resin composition solution.
[0056] <Comparative Example 2> To 11.72 g of the resin solution (solid content: 23.73% by mass) obtained in Synthesis Example 4, 0.28 g of Irgacure Oxe01 (manufactured by BASF Japan Ltd.) as a photopolymerization initiator, 0.008 g of Megafac R-30 (manufactured by Dainippon Ink and Chemicals, Inc.) as a surfactant, 0.042 g of Irganox 3114 (manufactured by BASF Japan Ltd.) as an antioxidant, 0.042 g of KBM-5103 (manufactured by Shin-Etsu Chemical Co., Ltd.) as an adhesion improver, and 17.91 g of propylene glycol monomethyl ether acetate were added, and the mixture was filtered to prepare a photocurable resin composition solution.
[0057] <c. Elution test in a photoresist solvent> The photocurable resin composition solutions prepared in Composition Examples 1 to 2 and Comparative Example 1 were applied onto a silicon wafer using a spinner. They were baked on a hot plate at 80°C for 1 minute, and then irradiated with 254 nm light at 300 mJ / cm 2 to form a photocured film (film thickness: 0.10 μm). This photocured film was immersed in cyclohexanone, which is a solvent used for the photoresist. It was confirmed that the films in Composition Examples 1 to 2 were insoluble in the solvent, while the film in Comparative Example 1 was dissolved by the solvent.
[0058] <d. Solvent resistance test in edge exposure> The photocurable resin composition solutions prepared in Composition Examples 1 to 2 and Comparative Example 1 were applied onto a 12-inch silicon wafer using a spinner. They were baked on a hot plate at 80°C for 1 minute, and then the wafer edge was irradiated with 50 mJ / cm 2A photocured film (film thickness 0.30 μm) was formed by irradiating the photocured film with light. The photocured film was immersed in OK73 thinner, a solvent used for photoresists. It was confirmed that Composition Examples 1 and 2 were insoluble in the solvent, but the film in Comparative Example 1 was dissolved by the solvent.
[0059] <Measurement of dry etching rate> The photocurable resin composition solutions prepared in Composition Example 2 and Comparative Example 2 were applied onto a silicon wafer using a spinner. Then, 254 nm light was applied at 300 mJ / cm using an aligner (PLA-501, Canon Inc.). 2 A photocured film (film thickness 0.10 μm) was formed by irradiating with 1000 uV of fluorine. A Samco RIE system (RIE-10NR) was used, and CF was used as the dry etching gas. 4 The dry etching rate (amount of film thickness reduction per unit time) was measured under the conditions using the above. The dry etching rates of the photocurable resins formed from Composition Example 2 and Comparative Example 2 were compared. The results are shown in Table 1. In Table 1, the etching rate is shown when the dry etching rate of Comparative Example 2 is set to 1.00.
[0060] [Table 1] Table 1 ---------------------------------- Selectivity ---------------------------------- Composition Example 2 0.69 Comparative Example 2 1.00 ---------------------------------- This shows that the photocured film obtained from the photocurable resin-forming composition of one embodiment of the present invention has greater dry etching resistance than Comparative Example 2.
Claims
1. A wafer edge protected semiconductor manufacturing wafer, comprising: (a) A first monomer unit containing only an aryl ketone residue as a crosslinkable group in a side chain, the aryl ketone residue being acetophenone, benzophenone, anthraquinone, anthrone, or a monomer having the following structural formula: 【Chemistry 1】 and substituted derivatives thereof; A first monomeric unit in which X is O, S, or N-R, and R is a hydrogen atom, a hydrocarbon group, or an acyl group; and (b) In the side chain, (b-1) an aliphatic hydrocarbon residue containing a tertiary carbon atom; a secondary carbon atom having a hydroxyl group; and a carbon atom selected from the group consisting of a methyl group, a methylene group, or a methine group directly bonded to an aromatic ring; and / or (b-2) a second monomer unit containing an aromatic ring residue; Including, A wafer for semiconductor manufacturing formed by applying a composition for forming a wafer edge protection film for semiconductor manufacturing, the composition comprising a photocurable resin composition including: a self-crosslinking polymer (A) in which the aromatic ring of the first monomer unit is bonded to a main chain via an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate ester bond (-O-CO-O-), or a urea bond (-NH-CO-NH-); and a solvent (B).
2. (A) forming a resist film on a semiconductor substrate; (B) forming a resist pattern by irradiating the resist film with light or an electron beam and then developing it; (C) etching the semiconductor substrate; A method for manufacturing a semiconductor device comprising: At least the front edge and, optionally, the bevel and / or back edge of a semiconductor manufacturing wafer, (a) A first monomer unit containing only an aryl ketone residue as a crosslinkable group in a side chain, the aryl ketone residue being acetophenone, benzophenone, anthraquinone, anthrone, or a monomer having the following structural formula: 【Chemistry 1】 and substituted derivatives thereof; A first monomeric unit in which X is O, S, or N-R, and R is a hydrogen atom, a hydrocarbon group, or an acyl group; and (b) In the side chain, (b-1) an aliphatic hydrocarbon residue containing a tertiary carbon atom; a secondary carbon atom having a hydroxyl group; and a carbon atom selected from the group consisting of a methyl group, a methylene group, or a methine group directly bonded to an aromatic ring; and / or (b-2) a second monomer unit containing an aromatic ring residue; Including, A method for manufacturing a semiconductor device, comprising: a step (X) of forming a protective film from a wafer edge protective film forming composition for semiconductor manufacturing, the photocurable resin composition including (A) a self-crosslinking polymer in which an aromatic ring of the first monomer unit is bonded to a main chain via an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate ester bond (-O-CO-O-), or a urea bond (-NH-CO-NH-), and a solvent (B).
3. A method for manufacturing a wafer for semiconductor manufacturing, comprising the steps of: At least an edge of the wafer precursor is (a) A first monomer unit containing only an aryl ketone residue as a crosslinkable group in a side chain, the aryl ketone residue being acetophenone, benzophenone, anthraquinone, anthrone, or a monomer having the following structural formula: 【Chemistry 1】 and substituted derivatives thereof; A first monomeric unit in which X is O, S, or N-R, and R is a hydrogen atom, a hydrocarbon group, or an acyl group; and (b) In the side chain, (b-1) an aliphatic hydrocarbon residue containing a tertiary carbon atom; a secondary carbon atom having a hydroxyl group; and a carbon atom selected from the group consisting of a methyl group, a methylene group, or a methine group directly bonded to an aromatic ring; and / or (b-2) a second monomer unit containing an aromatic ring residue; Including, A method for producing a wafer for semiconductor production, comprising the steps of: applying a composition for forming a wafer edge protection film for semiconductor production, the composition comprising a photocurable resin composition containing a self-crosslinking polymer (A) in which the aromatic ring of the first monomer unit is bonded to a main chain via an ester bond (-O-CO- or -CO-O-), an amide bond (-NH-CO- or -CO-NH-), a urethane bond (-NH-CO-O- or -O-CO-NH-), a carbonate ester bond (-O-CO-O-), or a urea bond (-NH-CO-NH-), and a solvent (B), to produce a wafer having the edge protected.
4. The wafer for semiconductor production according to claim 1 , wherein the photocurable resin composition further contains a crosslinkable polymer or a crosslinkable compound (C) other than the self-crosslinkable polymer (A).
5. 5. The wafer for semiconductor manufacturing according to claim 4, wherein the crosslinkable group in the crosslinkable polymer or the crosslinkable compound (C) is selected from the group consisting of an epoxy group, a (meth)acrylic group, a vinyl group, a carboxylic acid group, a thiol group, a silanol group, a cinnamoyl group, and a hydroxyl group.
6. 6. The wafer for semiconductor manufacturing according to claim 1, 4 or 5, wherein the photocurable resin composition has a viscosity of 100 cps or less at 25°C.
7. 3. The method for manufacturing a semiconductor device according to claim 2, wherein the protective film is a cured product of a coating film made of the composition for forming a wafer edge protective film for semiconductor manufacturing.
8. 8. The method for manufacturing a semiconductor device according to claim 7, wherein the protective film has a thickness of 1 to 500 nm.
9. 8. The method for manufacturing a semiconductor device according to claim 7, wherein the protective film is for preventing metal contamination of an edge of a wafer.
10. 10. The method for manufacturing a semiconductor device according to claim 7, wherein the protective film is cured by light having a wavelength of 170 to 800 nm.
11. The method for manufacturing a semiconductor device according to claim 2 , further comprising the step (X) prior to the step (A).
12. The method for manufacturing a semiconductor device according to claim 2 , further comprising a step (X) between the steps (A) and (B).
13. The method for manufacturing a semiconductor device according to claim 2 , further comprising a step (X) after the step (B) or the step (C).
14. 14. The method for manufacturing a semiconductor device according to claim 2, further comprising, after the step (X), a step (Y) of removing the resist film from a portion above the protective film.
15. 14. The method for manufacturing a semiconductor device according to claim 2, further comprising, after the step (X), a step (Z) of removing the protective film.
16. The method for manufacturing a semiconductor device according to claim 14, further comprising the step (Z) of removing the protective film after the step (Y).
17. The method for manufacturing a semiconductor device according to any one of claims 2 and 11 to 16, wherein the resist film contains a metal.
18. The method for producing a semiconductor device according to any one of claims 2 and 11 to 17, wherein in the step (X), the composition for forming a wafer edge protection film for semiconductor production is applied, and a predetermined area is exposed and developed.
19. 16. The method for producing a semiconductor device according to claim 15, wherein the step (Z) is carried out by ashing or a treatment with hydrofluoric acid, an organic solvent, an alkaline developer, or a cleaning liquid for semiconductors.
20. The semiconductor manufacturing wafer according to claim 1, 4 or 5, wherein the aliphatic hydrocarbon residue (b-1) is an aliphatic hydrocarbon residue containing a secondary carbon atom having a hydroxyl group.
21. A wafer for semiconductor production described in claim 1, 4 or 5, wherein the aromatic ring residue (b-2) is an aromatic ring residue having 6 to 40 carbon atoms which may be substituted.
22. A wafer for semiconductor manufacturing as described in claim 1, 4 or 5, wherein the ratio of the number of repetitions of the first monomer unit to the number of repetitions of monomer units other than the first monomer unit including the second monomer unit is selected so that when a film having a thickness of 300 nm is formed, the transmittance of the film at a wavelength of 300 nm is 0.01% or more.
Citation Information
Patent Citations
Electroconductive pattern material and method for forming electroconductive pattern
JP2005101554A
Semiconductor device manufacturing method
JP2011228340A
Substrate processing method
JP2017098333A
Polymer for forming anti-reflective coating layer
US20060199108A1