Optical layer, optical member and optical device

The optical layer design with alternating thin film layers addresses stress-related cracking and peeling issues, ensuring durability and maintaining optical performance by managing stress and interference conditions.

JP7560264B2Active Publication Date: 2024-10-02CANON DENSHI KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020064151
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-31
Publication Date
2024-10-02
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Optical multilayer films experience stress issues leading to cracking and peeling due to large stress in thin films, which affects the optical properties and durability.

Method used

An optical layer design with alternating thin film layers having opposite internal stresses and controlled thicknesses to manage stress, ensuring optical interference conditions are met without significant optical property changes.

Benefits of technology

Reduces stress in the optical layer, minimizing cracking and peeling while maintaining optical performance, enhancing durability and reducing defects in optical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560264000002
    Figure 0007560264000002
  • Figure 0007560264000003
    Figure 0007560264000003
  • Figure 0007560264000004
    Figure 0007560264000004
Patent Text Reader

Abstract

To provide an optical layer that has satisfactory durability against cracks and peeling and an optical film that is a laminate of the optical layers, an optical member including the same, and an optical device that has the optical member arranged therein.SOLUTION: An optical layer 2 is an optical layer in which an optical film thickness as a whole satisfies an interference condition for a predetermined wavelength. The optical layer 2 has a first thin film layer 3 that mainly contributes as the refractive index of the optical layer 2, and a second thin film layer 4 that is provided adjacent to the first thin film layer 3 and has an internal stress opposite to the internal stress of the first thin film layer 3. The optical film thickness of the second thin film layer 3 is an optical film thickness at which light interference is not developed for the predetermined wavelength.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical layer that utilizes light interference conditions to prevent reflection or cut off a specific wavelength range, an optical filter having an optical layer formed thereon, an optical member such as a lens, and an optical device such as a camera that captures light transmitted through the optical member. [Background technology]

[0002] Conventionally, optical films that utilize the optical interference of thin films to provide functions such as anti-reflection and infrared cut have been known for optical components such as optical filters and lenses. Optical devices such as cameras that include image sensors incorporate optical components with these optical films formed on substrates such as lenses, and the optical components suppress ghosts and flares caused by reflections that occur within the optical device, as well as image degradation caused by unnecessary light entering the image sensor.

[0003] It is known that when forming an optical film on a lens substrate or a synthetic resin substrate having a curvature, a film with good shape conformability and high gas barrier properties can be formed by using atomic layer deposition (ALD). Patent Document 1 discloses a technology in which molecular layers with different physical property values ​​related to optical characteristics are laminated by ALD to produce a thin film with complex optical characteristics, and this is further laminated to form an optical multilayer film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-176081 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the optical multilayer film described in Patent Document 1, the stress in the thin film becomes large, and there is a possibility that cracks or peeling occurs. [Means for solving the problem]

[0006] In order to solve the above problems, the optical layer of the present invention is an optical layer whose overall optical thickness satisfies an interference condition for a predetermined wavelength, and the optical layer mainly contributes to the refractive index of the optical layer. Physical thickness is 4nm or less The optical element comprises a first thin film layer and a second thin film layer disposed adjacent to the first thin film layer and having an internal stress opposite to that of the first thin film layer, the optical film thickness of the second thin film layer is an optical film thickness at which no optical interference occurs for the specified wavelength, the refractive index difference between the optical layer and the first thin film layer is ±3% or less, and the optical layer is composed of a repeated set of the first thin film layer and the second thin film layer according to a specified film thickness ratio. Effect of the Invention

[0007] According to the present invention, it is possible to relieve the stress in the first thin film layer, which mainly contributes to the refractive index of the optical layer, and reduce the possibility of cracking or peeling without significantly affecting the optical film design or optical properties. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view of an optical layer and an optical member according to the present invention. [Diagram 2] Configuration examples of optical layers according to the present invention [Diagram 3] Configuration examples of optical layers according to the present invention [Figure 4] 1 is a cross-sectional view of an optical layer and an optical member according to Example 1. [Diagram 5] 1 is a cross-sectional view of an optical layer and an optical member according to Example 2. [Figure 6] 1 is a cross-sectional view of an optical film and an optical member according to a third embodiment. [Figure 7] 1 is a cross-sectional view of an optical film and an optical member according to a fourth embodiment. [Figure 8] Optical device according to the present invention DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An embodiment of the present invention will be described with reference to the drawings.

[0010] FIG. 1 shows a cross-sectional view of the optical layer and optical member according to the present invention cut along a plane passing through the optical axis. FIG. 1(b) shows a partially enlarged view of the optical layer 2 in FIG. 1(a). The optical layer 2 of the present invention is configured by laminating a main material thin film (first thin film layer) 3 that mainly contributes to the refractive index of the optical layer 2 and a molecular layer (second thin film layer) 4 having a stress opposite to that of the main material thin film, and the optical layer has a thickness that causes optical interference. Here, the molecular layer 4 is formed to a thickness that does not cause optical interference, and optical interference does not occur between the main material thin film 3 and the molecular layer 4. The optical member of the present invention is configured such that one or more optical layers 2 are formed on a substrate.

[0011] In FIG. 1, the optical member 6 is one optical layer, but the optical film may be formed by laminating another optical layer having a different refractive index from the optical layer 2. Here, the other optical layer may be a layer made of a single material. That is, in the optical film of the present invention, at least one optical layer is configured by laminating a main material thin film (first thin film layer) 3 and a molecular layer (second thin film layer) 4 having a stress opposite to that of the main material thin film. In addition, the optical film may have a plurality of optical layers made of the same combination of materials, or may have optical layers made of different combinations of materials.

[0012] (optical layer) The optical layer 2 will be described. The optical layer 2 of the present invention is composed of a main material thin film 3 and a molecular layer 4 having a stress opposite to that of the main material thin film, and has an optically significant film thickness. The optically significant film thickness refers to a film thickness at which optical interference occurs at the target wavelength. The molecular layer 4 forming the optical layer 2 is controlled to a film thickness at which optical interference does not occur, and is formed by ALD. In order to provide the optical component 6 with functions such as anti-reflection and infrared cut, it is preferable that the optical layer 2 has a lower or higher refractive index. For example, when providing an AR function with a single layer, it is preferable that the optical layer 2 has a refractive index as low as possible.

[0013] In addition, in an optical film including an optical layer described below, it is preferable to laminate layers having a large difference in refractive index, that is, a laminate of a low refractive index layer and a high refractive index layer. In other words, when an optical layer is used as a low refractive index layer or a high refractive index layer, it is preferable to provide the molecular layer 4 with a thickness that does not significantly increase or decrease the refractive index of the main material thin film 2. For this reason, it is preferable that the refractive indexes of the main material thin film 3 and the molecular layer 4 that form the optical layer 2 are as close as possible, for example, 0.5 or less, and more preferably 0.2 or less.

[0014] Here, the refractive index n of the optical layer 2 can be considered to be a value represented by the following formula (1) when the thickness of the optical layer 2 is D, the refractive index and total thickness of the main material thin film 3 are nM and ΣdM, respectively, and the refractive index and total thickness of the molecular layer 4 are nA and ΣdA, respectively. At this time, it is preferable that the difference in refractive index between the main material thin film 3 and the optical layer 2 is within the range represented by formula (2). If the difference in refractive index between the main material thin film 3 and the optical layer 2 is at a level that satisfies formula (2), the stress of the optical layer 2 can be alleviated without significantly affecting the optical design. In the present invention, the refractive index is a value at a light wavelength of 550 nm unless otherwise specified.

[0015]

number

[0016] -3% ≦ 100×(n - nM) / nM ≦ 3% (2)

[0017] The thickness of the molecular layer 4 is the thickness of one molecule, and depends on the material, but is preferably, for example, 0.05 nm or more. In order not to cause optical interference and to ensure that the optical properties of the optical layer 2 do not deviate significantly from the optical properties of the main material thin film 3, the thickness of the molecular layer 4 in the optical layer 2 is preferably 1 / 3 or less, and more preferably 1 / 5 or less.

[0018] The optical layer 2 is composed of a plurality of main material thin films 3 and molecular layers 4, and the thicknesses of the main material thin films 3 arranged at different positions in the thickness direction may be the same or different, and the thicknesses of the molecular layers 4 arranged at different positions may be the same or different. Considering the stress during the formation of the optical layer, it is preferable that the main material thin film 3 does not have an extremely thick layer, and it is more preferable that at least the main material thin film 3 is composed of a substantially uniform thickness. In other words, when a combination of the thickness dM per layer of the main material thin film 3 forming the optical layer 2 and the thickness dA of the molecular layer 4 is set as one set, it is preferable to repeatedly mold this set multiple times so that the optical layer has a desired thickness. At this time, the material of the optical layer 2 that is initially formed on the substrate 1 may be formed from the main material thin film 3 or the molecular layer 4.

[0019] On the other hand, as described below, when forming an optical film by combining with other optical layers or other optical layers, the film thickness balance between the main material thin film 3 and the molecular layer 4 of the optical layer 2 may be adjusted in consideration of the stress balance until the entire optical film or optical layers are formed.

[0020] For example, if another optical layer having an internal stress opposite to the film stress of the main material thin film 3 is formed before the optical layer is formed, the main material thin film 3 (compressive stress) of the optical layer 2 to be formed may have a region in which the thickness of the main material thin film 3 becomes thinner continuously or stepwise as it moves away from the optical layer directly below or from the optical layer, as shown in Figure 2.

[0021] FIG. 2(a) shows a partially enlarged view of the optical layer 2, and FIG. 2(b) shows the film thickness corresponding to each layer. The vertical axis of FIG. 2(b) shows the film thickness of each layer stacked up to that point, and when the main material thin film 3 with a thickness of dMn is formed on the outermost surface of the optical layer 2, the film thickness becomes D. That is, in the initial stage of film formation of the optical layer 2, the film may be formed so as to relieve the stress of the optical layer or the optical layer 2 directly below as much as possible. At this time, the thickness of the molecular layer 4 forming the optical layer 2 may be uniform, or may become thinner as it moves away from the optical layer or the optical layer directly below, like the main material thin film 3, or may become thicker as long as optical interference does not occur.

[0022] Also, the optical layer 2 may have a region in which the thickness increases continuously or stepwise with increasing distance from the optical layer directly below or from the optical layer. Fig. 3(a) shows an enlarged view of a portion of the optical layer 2, and Fig. 3(b) shows the thickness of each layer. The vertical axis of Fig. 3(b) shows the thickness of the layers stacked up to each layer, and when a main material thin film 3 with a thickness of dMn is formed on the outermost surface of the optical layer 2, the thickness of the optical layer 2 becomes D.

[0023] As shown in Figure 3, by combining regions in which the thickness of the main material thin film 3 decreases continuously or stepwise with regions in which the thickness increases with distance from the optical layer directly below or from the optical layer, the stress of the optical layer directly below can be alleviated in the early stages of the optical layer, while the stress of the optical layer 2 due to the stress of the main material thin film 3 does not suddenly increase in the later stages of molding of the optical layer 2.

[0024] In this embodiment, the main material thin film 3 forming the optical layer 2 can be made of various known materials such as MgF2, SiO2, Al2O3, MgO, HfO2, ZrO2, La2Ti2O7 (LaTiO3), Si3N4, Ta2O5, Nb2O5, TiO2, etc. The molecular layer 4 can be appropriately selected from known materials that can be formed by ALD, such as MgF2, SiO2, Al2O3, MgO, HfO2, ZrO2, Si3N4, Ta2O5, Nb2O5, TiO2, etc., according to the main material thin film 3. If some light absorption is acceptable as an optical film, metal atoms such as Al, Mg, Si, and Ti may be used as the molecular layer 4. Compared to its oxide / nitride layer, the metal atomic layer is preferable in terms of ductility and stress relaxation. The metal compound layer and the atomic layer of a metal element having a thickness similar to that of the molecular layer may be mixed to form the molecular layer.

[0025] In the present invention, the main material thin film 3 constituting the optical layer 2 can be formed by using a known film formation technique, for example, a physical vapor deposition technique such as vacuum deposition, an ion-assisted method, an ion plating method, or a sputtering method, or a chemical vapor deposition technique such as CVD (Chemical Vapor Deposition), PECVD (Plasma Enhanced Chemical Vapor Deposition), thermal ALD, or PEALD (Plasma Enhanced Atomic Layer Deposition). However, as described above, considering that the molecular layer 4 is formed by the ALD method, it is preferable in terms of the manufacturing process to select a chemical vapor deposition method.

[0026] (optical film) In the present invention, the optical film is a film having an optical function, which is composed of multiple layers including at least the optical layer 2. The film having an optical function refers to, for example, a cut film such as a multi-AR film, an infrared cut film, a bandpass film, a mirror film, etc. These films obtain the desired spectral characteristics by the optical interference of optical layers having different refractive indices.

[0027] For example, an optical film will be described in the case of a multi-AR film. In the multi-AR film, low reflection is realized in a desired wavelength region by alternately stacking low refractive index layers and high refractive index layers. When stacking optical layers like a multi-AR film, MgF2, SiO2, Al2O3, MgO, HfO2, ZrO2, La2Ti2O7 (LaTiO3), Si3N4, Ta2O5, Nb2O5, TiO2, etc. can be used, but it is preferable to select materials with stresses in different directions for the low refractive index layer and the high refractive index layer so that the stress of the entire optical film is as small as possible. For example, it is preferable to select SiO2 with compressive stress as the low refractive index material and TiO2 with tensile stress as the high refractive index material, because they have opposing stresses and a large refractive index difference. If the refractive index difference is large, the number of layers (film thickness) required to obtain the desired spectral characteristics can be reduced, which contributes to crack suppression.

[0028] For example, when a multi-AR film is formed on a synthetic resin lens as a substrate, it is preferably made of 4 to 12 layers, and more preferably made of 6 to 10 layers. A laminate such as a multi-AR film tends to have higher gas barrier performance as the number of layers increases.

[0029] This is because, even if there is a defect in the layer forming the laminate, if there is no defect in the same region between the laminated layers, gases such as oxygen and water vapor will not easily reach the synthetic resin substrate. In other words, the more the number of layers, the easier it is to suppress deterioration such as yellowing of the synthetic resin even if a minute film defect occurs in the layer forming the multi-AR film. On the other hand, if the number of layers is increased too much, the multi-AR film is likely to crack due to film stress, especially when a synthetic resin lens substrate is used. The number of layers here refers to the optical layer or the number of layers of the optical layer that exhibits optical interference. The film thickness of the multi-AR film is preferably about 200 nm or more and 600 nm or less, and more preferably 250 nm or more and 500 nm or less. If the film thickness is too thin, it becomes difficult to sufficiently reduce reflection due to the interference effect of the thin film, and the gas barrier effect of the multi-AR film becomes small. On the other hand, if the film thickness is too thick, cracks are likely to occur. Furthermore, the optical layer or optical layer is preferably 80 nm or less, and more preferably 50 nm or less, except for the outermost layer. If each layer is too thick, the stress in that layer becomes too large, and there is a risk of cracking or peeling, especially when the layer is formed on a synthetic resin lens substrate. On the other hand, the outermost layer is formed so that its optical thickness is approximately λ / 4 at the target wavelength λ in order to prevent reflection.

[0030] Here, the preferred conditions for forming a multi-AR film on a synthetic resin lens substrate are described, but suitable conditions may be selected according to the optical film. For example, when forming an optical film that requires multiple layers and film thickness to obtain optical properties such as an infrared cut film on a glass substrate (including lenses) or a synthetic resin substrate that does not have a curved surface, the number of layers and film thickness should be appropriately determined so that cracks do not occur.

[0031] (substrate) The optical layer and optical film according to the present invention can be formed on a substrate 1 to form an optical member 6. As the substrate 1, for example, a substrate made of an inorganic material such as glass or quartz, or various synthetic resin substrates such as polyester, olefin, polyether, acrylic, styrene, PET (polyethylene terephthalate), PES (polyethersulfone), polysulfone, PEN (polyethylene naphthalate), PC (polycarbonate), and polyimide can be used. Furthermore, a substrate made of an organic-inorganic hybrid material, for example, a substrate having a silsesquioxane skeleton, may be used. In addition, a lens can be used as the substrate 1 as necessary. Various materials such as glass and synthetic resin can be used for the lens. As a synthetic resin lens, olefin, PC, acrylic, styrene, polyester, polyurethane, etc. can be suitably used from the viewpoint of moldability and refractive index characteristics. In addition, a thermo- or photo-curable resin such as a multifunctional reactive polymer having an aromatic dendrimer-like multi-branched structure may be used. A synthetic resin substrate is flexible, light, and has good processability compared to glass, but is prone to deformation and deterioration due to heat. For this reason, the synthetic resin substrate should have high heat resistance (high glass transition temperature Tg), for example, the glass transition temperature Tg is preferably 120°C or higher, more preferably 140°C or higher. Furthermore, in consideration of deformation of the synthetic resin substrate due to water absorption, olefin-based, particularly cycloolefin-based materials are preferred. In addition, for lenses, etc., materials with high refractive index and small Abbe number are sometimes required. In this case, for example, PC-based or fluorene-containing polyester resins can be preferably used.

[0032] When the optical member 6 of the present invention is used as a lens in a wide range of temperatures, such as an in-vehicle camera or a security camera, it is preferable that the synthetic resin substrate has a small change in refractive index due to temperature. For example, the difference between the refractive index at 0°C and the refractive index at 80°C in e-line is preferably 0.8% or less, more preferably 0.6% or less. In addition, it is preferable that the change in optical properties due to high temperatures, that is, yellowing (ΔYI), is small, and for example, the value of ΔYI, which is the difference between the yellowing index (YI: yellow index) at 120°C for 1500 hours and the initial YI, is preferably 10 or less, more preferably 8 or less. In addition, the transmittance of the synthetic resin substrate is 80% or more at visible light wavelengths (400-700 nm), and it is preferable that the transmittance at visible light wavelengths at 120°C for 1500 hours is 60% or more.

[0033] When a plurality of substrates are used in the same optical device, such as a lens unit, a plurality of substrates 1 with different refractive indices or Abbe numbers can be used in order to adjust optical characteristics such as aberration.

[0034] When the substrate 1 is a resin lens, it can be molded by, for example, injection molding. Specifically, a cavity including the lens section, outer periphery, gate section, etc., formed by butting the fixed mirror piece and the movable mirror piece together, is filled with resin material through the gate section, and when the resin has solidified, the mold is opened and the substrate is removed. Finally, the gate section is cut off. With this method, aspheric lenses and high curvature lenses, which are difficult to process with glass, can be made relatively easily. Note that the molding of the substrate is not limited to injection molding, and various other known methods such as injection compression molding and cast polymerization can be used.

[0035] When a synthetic resin substrate is used, it is preferable to perform an annealing treatment before forming the optical layer and optical film in order to release internal stress due to molding and to remove moisture absorbed by the substrate. The annealing treatment is suitably performed at a temperature of about 80° C. to the Tg of the substrate, preferably about 15° C. below the Tg of the substrate, for about 0.5 to 24 hours, more preferably about 1 to 12 hours.

[0036] (Manufacturing method) The optical layers and optical films of the present embodiment can be fabricated, for example, by an ALD process.

[0037] Here we will explain ALD. ALD is a vapor phase thin film formation method similar to CVD. In CVD, two types of precursors are introduced simultaneously into the reaction chamber, and the reaction products are deposited on the substrate, whereas in ALD, only one type of precursor is introduced simultaneously into the reaction chamber, and the precursors other than the one adsorbed on the substrate 1 do not chemically react with other precursors, and the reaction products are formed only on the surface of the substrate 1. For this reason, ALD can form a conformal layer even on a substrate 1 with a complex shape.

[0038] The ALD film formation process will be described. First, a site, such as an OH group, to which a first precursor described later can be adsorbed is provided on a substrate or a surface on which an ALD film is to be formed. To provide the OH group, for example, plasma or UV / O3 may be used, or, for example, water molecules may be used as a precursor to adsorb the OH group on the substrate. Next, the first precursor, which is a source gas of the molecular layer 3 to be formed, is chemically adsorbed on the substrate. At this time, since chemical adsorption can be performed on the exposed OH group of the substrate, the adsorbed first precursor forms a monolayer on the film formation surface regardless of the shape of the substrate. Next, the excess first precursor that could not be adsorbed on the film formation surface and the gas generated when the first precursor is adsorbed on the film formation surface are purged (removed).

[0039] Then, a molecular layer of metal oxide, metal, metal nitride, etc. is obtained by using a second precursor or radical ozone plasma that oxidizes, reduces, and nitrides the first precursor adsorbed on the film formation surface. This process can be repeated to form a layer with the desired thickness. N2, Ar, etc. can be used as a carrier gas when introducing each precursor. Since ALD proceeds with film formation by adsorption of a monomolecular layer on the film formation surface, it is possible to form a film with a uniform thickness without being affected by the shape of the substrate, and is suitable for film formation on, for example, high curvature or aspheric lenses. Furthermore, since the layer formed is a monomolecular layer, precise film thickness control is possible. Furthermore, unlike physical vapor deposition, ALD forms a layer even with a monomolecular level thickness, so a layer with few film defects and high gas barrier properties is formed. For this reason, when a synthetic resin is used for the substrate, it is expected to have the effect of suppressing yellowing due to oxidation of the resin, and expansion and hydrolysis due to moisture.

[0040] The molecular layer formation process by ALD using an Al2O3 layer will be described in detail. First, the deposition surface is irradiated with plasma to provide OH groups. Next, TMA (trimethylaluminum) is supplied into the deposition chamber as the first precursor. At this time, the reaction shown in formula (1) or (2) occurs. Next, excess TMA and the generated CH4 are removed by purging. Inert gases such as N2 and Ar are preferably used for purging. Next, water molecules are supplied into the deposition chamber as the second precursor. At this time, the reaction shown in formula (3) or (4) occurs. Furthermore, excess water molecules and the generated CH4 are removed by purging. These steps constitute one cycle, and the number of cycles is repeated to obtain the desired film thickness. In the case of Al2O3, one cycle results in a film thickness of approximately 1 Å.

[0041] Al(CH3)3+ :OH → :O-Al(CH3)2+ CH4(3) Al(CH3)3+ 2:OH → :O-Al(CH3) + 2CH4(4)

[0042] :O-Al(CH3)2+ 2H2O → :Al-O-Al(OH)2+ 2CH4(5) :O-Al(CH3) + H2O → :Al-O-Al(OH) + CH4(6)

[0043] The fabrication of the optical layer 2, which is made of the main material SiO2 and the molecular layer Al2O3 having the stress in the opposite direction to the main material, as described in the above embodiment, will be described. First, the substrate is set on the deposition holder and introduced into the reaction chamber. The reaction chamber is evacuated by a vacuum pump, and the substrate 1 is heated by a heater. When the pressure in the reaction chamber and the substrate temperature reach the desired values, deposition begins. First, the main material SiO2 is deposited. The SiO2 layer is formed by a deposition process that is approximately the same as that described for the Al2O3 molecular layer described above, using TDMAS (trisdimethylaminosilane) as the first precursor and water molecules as the second precursor. At this time, the film thickness per cycle is approximately 0.8 Å. The SiO2 molecular layer forming cycle is repeated the number of cycles required to form the desired film thickness.

[0044] Next, a monolayer of Al2O3 is formed by the above process using TMA as the first precursor and water molecules as the second precursor. At this time, the number of cycles is limited so that the thickness of the Al2O3 film is within a thickness that does not cause optical interference. After the desired number of cycles of the Al2O3 molecular layer are repeated, a SiO2 layer is further formed. This process is repeated to form a composite film of SiO2 and Al2O3 to a desired thickness. Here, TDMAS is used as the first precursor of SiO2, but it is not limited to this and other aminosilanes may be used, or TEOS (tetraethoxysilane) or silicon tetrachloride may also be used. In particular, in the formation of the SiO2 molecular layer, the reaction can be promoted by introducing a catalytic gas such as pyridine into the reaction chamber after the first and second precursors are introduced.

[0045] For example, when obtaining an optical film in which multiple optical layers with different refractive indices are formed, such as a multi-AR film, a TiO2 layer (high refractive index layer) with a different refractive index is provided from the optical layer 2 made of SiO2 and Al2O3 described above. When forming a TiO2 film by ALD, for example, TDMAT (tetrakisdimethylaminotitanium) can be used as the first precursor and water molecules can be used as the second precursor. In this case, the film thickness is approximately 0.6 Å per cycle described above. This is repeated the number of cycles required to reach the desired film thickness. As the first precursor of TiO2, other aminotitaniums, titanium tetrachloride, etc. can be used in addition to TDMAT, and a catalyst gas can be introduced to promote the reaction as necessary.

[0046] After the TiO2 layer is formed, a low refractive index layer made of SiO2 or SiO2 and Al2O3 is formed. This is stacked as many times as necessary to obtain the desired optical characteristics. Naturally, the high refractive index layer may also be an optical layer that combines a main material and a molecular layer having the opposite stress to the main material. In this case, for example, the main material can be TiO2, and the molecular layer having the opposite stress to the main material can be Si3N4. Note that the same first precursor as SiO2 can be used to form the Si3N4 molecular layer, and ammonia gas or nitrogen gas can be used as the second precursor.

[0047] Although the method of using ALD to form the optical layer 2 has been described so far, a film formation process combining CVD and ALD can also be used. For example, when the main material is SiO2 and the molecular layer is Al2O3, the main material SiO2 can be formed by CVD, and the molecular layer Al2O3 can be formed by ALD. The molecular layer Al2O3 needs to be controlled to a film thickness that does not cause optical interference, while the main material SiO2 does not necessarily need to be controlled at the molecular layer level. Therefore, by forming the main material SiO2 by CVD, the film formation rate can be improved compared to forming the optical layer only by the ALD process, and productivity is improved. When forming an optical film, which is a laminate of optical layers including an optical layer, CVD and ALD may be combined within the optical layer in a specific optical layer, or the layers may be formed by switching between them for each optical layer, for example, some layers of the low refractive index layer are formed by ALD and other layers are formed by CVD.

[0048] Although the ALD has been explained using thermal ALD, PEALD, which uses plasma to promote chemical reactions, can also be used. In particular, when a synthetic resin substrate is used as the substrate 1, PEALD is more suitable since it allows for a lower film formation temperature. In this case, in order to avoid damage to the substrate 1 by the plasma, it is preferable to use a process in which, for example, the plasma is generated outside the reaction chamber, and only the excited OH radicals reach the reaction chamber. Similarly, the use of PECVD for film formation by CVD is particularly suitable when forming a film on a synthetic resin substrate.

[0049] Example 1 Fig. 4 shows a cross-sectional view of the optical layer and optical member according to Example 1, cut by a plane passing through the optical axis. Fig. 4(b) shows a partially enlarged view of the optical layer 2 in Fig. 4(a). The optical member 6 of Example 1 uses a cycloolefin resin lens as the substrate 1, and one optical layer 2 is formed on the resin lens. The optical layer 2 is made of a SiO2 thin film having compressive stress as the main material thin film 3, and a molecular layer 4 made of Al2O3 having tensile stress, and has a physical film thickness d M The main material thin film 3 and physical thickness d AThe optical layer 2 has a physical thickness D determined so that the optical thickness at wavelength λ is about λ / 4. In other words, the optical layer 2 has an AR function at wavelength λ. In Example 1, the main material thin film 3 (SiO2) and the molecular layer 4 (Al2O3) are both formed by PEALD, and an optical layer having the same thickness as the main surface, that is, approximately the physical thickness D, is formed on the edge of the resin lens. Here, the main surface refers to the effective surface of the optical member 6, and in the case of a lens, for example, refers to a surface having a curvature.

[0050] In Example 1, 24 sets were formed, each set consisting of a 3 nm main material thin film (SiO2) and a 0.8 nm molecular layer (Al2O3). The refractive indices of SiO2 and Al2O3 are 1.46 and 1.62, respectively, and the refractive index of the optical layer 2 is 1.494 according to formula (1). At this time, the physical film thickness is 91.2 nm, and the optical film thickness of the optical layer 2 at a light wavelength of 550 nm approximately satisfies λ / 4.

[0051] In the first embodiment, the optical layer 2 is formed in the order of the main material thin film 3 and the molecular layer 4 from the substrate 1 side, but this is not limiting, and the molecular layer 4 may be formed first. In particular, when Al2O3 is used as the molecular layer 4, it is more preferable that the layer in contact with the substrate 1 is the molecular layer 4, taking into account the adhesion with the substrate 1.

[0052] Example 2 FIG. 5 shows a cross-sectional view of the optical layer and the optical member according to the second embodiment cut by a plane passing through the optical axis. FIG. 5(b) shows a partially enlarged view of the optical layer 2 in FIG. 5(a). The optical member 6 of the second embodiment uses a cycloolefin lens as the substrate 1 as in the first embodiment, and one optical layer 2 is formed on the substrate 1. The optical layer 2 is composed of a SiO2 thin film having compressive stress as the main material thin film 3 and an Al2O3 molecular layer 4 having tensile stress, and the physical thickness D of the optical layer 2 is determined so that the optical thickness is about λ / 4 at the wavelength λ as in the first embodiment. Here, in the second embodiment, the main material thin film 3 is formed by PECVD and the molecular layer 4 is formed by PEALD, and the physical thickness is different between the main surface and the end of the resin lens. Specifically, the main material thin film 3 and the molecular layer 4 are formed on the main surface of the resin lens with a physical thickness D, while the main material thin film is partially wrapped around, and substantially only the material of the molecular layer 4 is formed on the end, and the thickness of the thickest part is ΣdA. The physical thickness of the main surface referred to here is the thickness of at least the optically effective range of the optical member 6, and in the case of a lens, for example, it refers to at least the region having a curvature.

[0053] In Example 2, 16 sets were formed, each consisting of a 4 nm main material thin film and a 0.8 nm molecular layer. The refractive indices of SiO2 and Al2O3 are 1.46 and 1.62, respectively, and the refractive index of the optical layer is 1.487 according to formula (1). At this time, the physical film thickness is 91.2 nm, and the optical film thickness of the optical layer 2 at a light wavelength of 550 nm approximately satisfies λ / 4. The film thickness at the edge of the substrate is approximately 15.2 nm. In Example 2, similarly to Example 1, the main material thin film 3 and the molecular layer 4 may be formed first from the main material thin film 3, or first from the molecular layer 4, and the optimum conditions may be appropriately selected based on compatibility with the substrate 1.

[0054] Example 3 Fig. 6 shows a cross-sectional view of the optical film and optical member according to Example 3 cut along a plane passing through the optical axis. Fig. 6(b) shows a partially enlarged view of the optical film 5 in Fig. 6(a), Fig. 6(c) shows a partially enlarged view of the optical layer 2', and Fig. 6(d) shows a partially enlarged view of the optical layer 2. The optical film 5 is an optical multilayer film formed by alternately laminating the optical layers 2 and 2' so as to satisfy the interference conditions for a predetermined wavelength region.

[0055] Specifically, the optical member 6 of Example 3 uses a resin lens made of a fluorene-structured polyester resin as the base material 1, and a multi-AR film is formed as an optical film 5 in which low-refractive index layers and high-refractive index layers are alternately laminated on the resin lens. Here, in Example 3, both the low-refractive index layer and the high-refractive index layer are optical layers 2, 2' consisting of main material thin films 3, 3' and molecular layers 4, 4', and the low-refractive index layer uses SiO2 as the main material thin film 3 and Al2O3 as the molecular layer 4, and the high-refractive index material uses TiO2 as the main material thin film 3' and Si3N4 as the molecular layer 4', respectively. In this example, the main material thin films and molecular films of the low-refractive index layer and the high-refractive index layer are formed by PEALD. That is, the physical film thickness of the optical film 5 formed on the main surface and the end surface of the substrate 1 is approximately the same, being D. Here, the main surface refers to the effective surface of the optical member 6, and in the case of a lens, for example, refers to a surface having a curvature.

[0056] In Example 3, the low refractive index layer was formed by repeating the necessary number of sets of a main material thin film 4 nm and a molecular layer 0.8 nm as one set. At this time, the refractive indexes of the main material thin film 3 and molecular layer 4 forming the low refractive index layer were 1.46 and 1.62, respectively, and the refractive index of the low refractive index layer can be considered to be 1.487 according to formula (1). In addition, the high refractive index layer was formed by repeating the necessary number of sets of a main material thin film 4 nm and a molecular layer 0.5 nm as one set. At this time, the refractive indexes of the main material thin film 3' and molecular layer 4' forming the high refractive index layer were 2.40 and 2.00, respectively, and the refractive index of the high refractive index layer can be considered to be 2.356 according to formula (1).

[0057] In the third embodiment, all the low refractive index layers have substantially the same refractive index, but the refractive index may be different for each layer in the low refractive index layers, that is, the thickness ratio of the main material thin film 3 to the molecular layer 4 may be different, or a specific low refractive index layer may be the optical layer 2, and the other layers may be layers made of, for example, SiO2 alone. Similarly, the refractive index (thickness ratio of the main material thin film to the molecular layer) may be different for each high refractive index layer, or a specific high refractive index layer may be the optical layer 2', and the other layers may be layers made of, for example, TiO2 alone. Furthermore, at least one layer or all layers of either the low refractive index layer or the high refractive index layer forming the optical film 5 may be the optical layer 2, 2'.

[0058] Furthermore, a functional layer may be provided in the optical film 5 to improve, for example, adhesion or gas barrier properties. An example of the functional layer is Al2O3. The Al2O3 layer may be formed to a desired thickness at the interface between the substrate 1 and the optical film 5, or may be inserted into the optical film 5. In this case, the functional layer may have a thickness at the so-called molecular layer level where no optical interference occurs, or may have a thickness at which optical interference occurs. When inserting a functional layer with a thickness at which optical interference occurs, the optical interference of the functional layer may be taken into consideration to optimally design the optical film. Of course, a plurality of functional layers may be provided, for example, at the interface between the substrate 1 and the optical film 5 and in the optical film 5.

[0059] In this embodiment, the optical film 5 is a multi-AR film, but the optical function is not limited to this.

[0060] Example 4 FIG. 7 shows a cross-sectional view of the optical film and optical member according to Example 4 cut along a plane passing through the optical axis. FIG. 7(b) shows a partially enlarged view of the optical layer 2 in FIG. 7(a), FIG. 7(c) shows a partially enlarged view of the optical layer 2', and FIG. 7(d) shows a partially enlarged view of the optical layer 2. The optical member 6 of Example 4 uses a resin lens made of a fluorene-structure polyester resin as the substrate 1, and a multi-AR film is formed thereon, which is an optical film 5 in which low-refractive index layers and high-refractive index layers are alternately laminated. Here, in Example 4, both the low-refractive index layer and the high-refractive index layer are optical layers 2, 2' made of main material thin films 3, 3' and molecular layers 4, 4', and the low-refractive index layer uses SiO2 as the main material thin film 3 and Al2O3 as the molecular layer 4, and the high-refractive index material uses TiO2 as the main material thin film 3' and Si3N4 as the molecular layer 4', respectively. In this example, the main material thin films of the low-refractive index layer and the high-refractive index layer are formed by PECVD, and the molecular films are formed by PEALD. That is, the substrate has a main surface with a physical thickness of D, and the end surface has a physical thickness of approximately ΣdA+ΣdA'. The end surface is configured by alternating low-refractive index Al2O3 molecular layers and high-refractive index Si3N4 molecular layers. Here, the Al2O3 molecular layers and Si3N4 molecular layers formed on the end surface have stresses in opposite directions.

[0061] In Example 4, similarly to Example 3, a set of 4 nm main material thin film and 0.8 nm molecular layer was formed in the low refractive index layer, and the necessary number of sets were repeatedly formed for each low refractive index layer. At this time, the refractive indexes of the main material thin film 3 and molecular layer 4 forming the low refractive index layer were 1.46 and 1.62, respectively, and the refractive index of the low refractive index layer can be considered to be 1.487 according to formula (1). In addition, a set of 4 nm main material thin film and 0.5 nm molecular layer was formed in the high refractive index layer, and the necessary number of sets were repeatedly formed for each high refractive index layer. At this time, the refractive indexes of the main material thin film and molecular layer forming the high refractive index layer were 2.40 and 2.00, respectively, and the refractive index of the high refractive index layer can be considered to be 2.356 according to formula (1).

[0062] As in Example 3, in the low refractive index layer, each layer may have a different refractive index (film thickness ratio of the main material thin film to the molecular layer), or only some of the low refractive index layers may be optical layers 2. Similarly, in the high refractive index layer, each layer may have a different refractive index (film thickness ratio of the main material thin film to the molecular layer), or only some of the low refractive index layers may be optical layers 2'. Furthermore, at least one layer or all layers of either the low refractive index layer or the high refractive index layer forming the optical film 5 may be the optical layers 2, 2'. Also, as in Example 3, a functional layer such as Al2O3 may be inserted as appropriate at any thickness and number.

[0063] In this embodiment, the optical film 5 is a multi-AR film, but the optical function is not limited to this.

[0064] FIG. 8 is a diagram showing an optical device according to the present invention. The optical device 21 according to the present invention includes a lens unit 20 consisting of a lens barrel 11, lenses 13-16, and an aperture 17, and further includes a protective filter 12, a cover glass 18, and an image sensor 19. Light incident on the lens unit is collected by a lens or the like on an image sensor 19 consisting of a CCD or CMOS sensor. The light collected on the image sensor 19 is converted into an electrical signal and imaged as necessary. At least one of the lenses 13-16 mounted on the lens unit 20 is provided with the optical member 6 described in this embodiment. That is, at least one of the lenses constituting the lens unit has an optical film 5 including at least optical layers 2, 2' formed on a substrate 1. The aperture 17 has a function of preventing unnecessary light from entering the image sensor 19, and may be provided between the lenses, or may be provided only partially between the lenses.

[0065] When used in harsh temperature conditions such as in-vehicle cameras and surveillance cameras, the aperture is preferably made of a metal substrate. As a metal aperture, for example, a metal plate blackened by anodization or a metal substrate on which a film having a light absorbing function is formed by deposition or the like can be suitably used. The protective filter 12 is a filter provided to protect the lens unit 20 from ultraviolet rays, dirt, and damage, and has functions such as UV cut, water repellency, oil repellency, hydrophilicity, and hard coating. Furthermore, the protective filter 12 may have a function of cutting off part of the visible range.

[0066] When a synthetic resin material is used for the lens, light absorption may occur mainly in the short wavelength region of the visible region due to yellowing. In order to reduce the variation in the transmittance incident on the imaging element 19 before and after the yellowing of the synthetic resin substrate, the light transmission in this region may be limited in advance. For example, by cutting light wavelengths of about 450 nm or less, which are significantly affected by yellowing, the variation in the transmittance incident on the imaging element 19 before and after yellowing can be effectively reduced. Such a cutting function can be provided, for example, by laminating multiple layers of low refractive index layers and high refractive index layers alternately and utilizing the light interference effect. It is not necessary to provide the protective filter 12, and the function of the protective filter 12 may be provided to the lens 13, which is the furthest from the imaging element 19.

[0067] The cover glass 18 is provided to prevent foreign matter from adhering to the imaging element 19, and in addition to general glass materials, a quartz substrate or the like can be suitably used. The cover glass 18 may be provided with a near-infrared cut function. When imaging the light incident on the imaging element 19, the sensitivity of the imaging element 19 in the near-infrared region may cause a difference from the color visible to the human eye. In such a case, an infrared cut film or the like may be formed on the cover glass 18 in order to prevent light in the near-infrared region from being incident on the imaging element 19. The infrared cut film can be provided, for example, by laminating multiple layers of low refractive index layers and high refractive index layers alternately and utilizing the light interference effect. In addition, infrared absorbing glass in which metal ions having absorption in the near-infrared region are kneaded into the cover glass 18 as necessary may be used.

[0068] In order to suppress yellowing of the synthetic resin substrate, the lens barrel 11 may be filled with an inert gas such as nitrogen or argon, or an oxygen scavenger made of iron or the like may be placed in the lens barrel 11 so as not to be in the optical path. In this way, the synthetic resin substrate is prevented from coming into contact with oxygen, and discoloration due to oxidation, i.e., yellowing, can be suppressed. The lenses mounted on the lens unit 20 may be a combination of glass lenses and synthetic resin lenses, but it is preferable that at least the synthetic resin lenses are formed with an optical film 5 including the optical layers 2 and 2' shown in this embodiment. As described above, ALD can obtain a film with good gas barrier properties, and can coat the edge of the substrate 1, so that oxygen, which causes yellowing, is less likely to reach the synthetic resin lens. In addition, when a glass lens is used, it is preferable that the lens 13 farthest from the image sensor 19 among the lenses constituting the lens unit 20 is a glass lens. This is because the lens farthest from the image sensor 19 is most likely to come into contact with oxygen and water vapor.

[0069] In Fig. 8, a lens unit 20 of the present invention is shown configured with four lenses, but there is no limitation on the number of lenses, and it may be more or less than four. Note that, in the optical device of Fig. 8, a lens on which an optical film 5 having optical layers 2, 2' is formed has been described, but the optical layers 2, 2' or optical films of the present invention may be formed on the above-mentioned infrared cut film, UV cut film, or the like, without being limited to lenses.

[0070] As described above, according to the present invention, an optical layer having a small film stress and an optical film including the same can be obtained. By forming the optical layer or optical film of the present invention on a substrate, an optical member that is less likely to crack can be provided. In addition, an optical device including the optical member of the present invention has excellent durability and can be particularly suitably used in applications exposed to harsh environments, such as in-vehicle cameras and surveillance cameras. [Explanation of symbols]

[0071] 1 Board 2, 2´ optical layer 3, 3´ Main material thin film (first thin film layer) 4, 4´ molecular layer (second thin film layer) 5 Optical film 6 Optical Components 11 Lens barrel 12 Protective Filters 13~16 Lens 17 Aperture 18 Coverslip 19 Image sensor 20 Lens unit 21 Optical equipment

Claims

1. An optical layer having an overall optical thickness that satisfies an interference condition for a predetermined wavelength, The optical layer is a first thin film layer having a physical thickness of 4 nm or less that mainly contributes to the refractive index of the optical layer; a second thin film layer provided adjacent to the first thin film layer and having an internal stress opposite to that of the first thin film layer; the optical thickness of the second thin film layer is an optical thickness at which no optical interference occurs at the predetermined wavelength, a refractive index difference between the optical layer and the first thin film layer is ±3% or less; The optical layer is characterized in that the optical layer is formed by repeating a set of the first thin film layer and the second thin film layer according to a predetermined film thickness ratio.

2. 2. The optical layer according to claim 1, wherein the physical thickness of the second thin film layer is 0.05 nm or more, and the physical thickness of the optical layer occupied by the second thin film layer is 1 / 3 or less.

3. 3. The optical layer according to claim 1, wherein the difference in refractive index between the first thin film layer and the second thin film layer is 0.5 or less.

4. 4. The optical layer according to claim 1, wherein the second thin film layer is formed by atomic layer deposition (ALD).

5. The first thin film layer is SiO 2 , the second thin film layer is Al 2 O 3 The optical layer according to any one of claims 1 to 4,

6. 6. An optical member comprising a substrate and a plurality of optical layers according to claim 1 formed on the substrate.

7. 7. The optical member according to claim 6, wherein only the second thin film layer is formed on the end face of the substrate.

8. The optical member according to claim 6 or 7, an imaging element that captures an image of light transmitted through the optical member.

Citation Information

Patent Citations

  • Laser mirror having flat spectral characteristics in narrow wavelength band

    JP1989286476A

  • Method of producing optical multilayer film by atomic layer deposition method

    JP2004176081A

  • Films for optical applications and methods of making such films

    JP2007534007A

  • Protective coatings for organic electronic devices manufactured using atomic layer deposition and molecular layer deposition methods.

    JP2010532917A

  • Flat panel display device and method of forming passivation film in the flat panel display device

    US20030143319A1