Sustainable nonwoven laminates for structural applications
A nonwoven laminate using melt-bonded polyester and copolyester fibers addresses the challenges of cost, recyclability, and structural irregularities, providing high mechanical stability and sound absorption for automotive underbody shields.
Patent Information
- Application Number
- JP2023036474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-10
- Filing Date
- 2023-03-09
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-03-09
AI Technical Summary
Existing nonwoven laminates for automotive underbody shields face issues such as high cost, non-uniformity, poor recyclability, low heat resistance, flammability, and structural irregularities due to the use of polyolefins and spunbond fibers, which affect mechanical stability and sound absorption.
A nonwoven laminate composed of multicomponent and monocomponent polyester and copolyester fibers, bonded by melt bonding, with a needled short fiber core layer and optional adhesive layers, ensuring high mechanical stability, low heat shrinkage, and uniformity, without needling, to enhance recyclability and reduce complexity.
The laminate achieves high tensile and tear strength, low heat shrinkage, and excellent sound absorption, while being cost-effective and recyclable, with improved dimensional stability and aesthetic appeal, suitable for molded articles.
Smart Images

Figure 0007562734000005 
Figure 0007562734000006 
Figure 0007562734000007
Abstract
Description
[Technical field]
[0001] The present invention relates to nonwoven laminates, shaped articles comprising such nonwoven laminates, their uses, products and methods for making them. [Background technology]
[0002] Nonwoven fabrics and nonwoven laminates are used in various technical applications, such as underbody shielding materials for automotive applications. Such underbody shielding can be manufactured by heating and molding fibrous precursor materials. Underbody shielding must meet stringent performance specifications, especially with respect to high mechanical stability, low water absorption and high sound absorption. To meet such specifications, various underbody shielding materials have generally been proposed in the art.
[0003] WO 2016 / 183079 discloses a composite article having a porous core layer containing a plurality of reinforcing fibers and a lofting agent. However, the reinforcing fibers may reduce the processability of the core layer. Furthermore, the lofting agent may cause dimensional instability when the article is heated and molded. The reinforcing fibers and / or the lofting agent may further increase the cost of the composite article.
[0004] EP 3489008 A1 describes a substrate nonwoven fabric having a two-layer structure of a long fiber nonwoven fabric layer and a short fiber nonwoven fabric layer. Both nonwoven fabric layers contain polyester fibers. A polypropylene layer is located at the interface between the two nonwoven fabric layers. However, the use of polyolefins in such composite materials has various disadvantages. In general, it is difficult to recycle products containing a combination of polyolefins and polyester. In addition, polypropylene has a melting point of about 160°C, so the heat resistance and flame resistance of the product are relatively low. In addition, polyester fibers and polypropylene have different properties, such as elongation, tensile strength, etc., so the product is not uniform. Therefore, the simultaneous use of polyester and polypropylene may cause problems in adjusting the properties of the final product.
[0005] Some nonwoven laminates in the art include a combination of a specific staple fiber layer and a spunbond layer. A common problem with such laminates is that the staple fiber layer can be shrunk when heated, whereas the spunbond layer usually does not. This can result in undesirable structural irregularities, which can lead to poor stability and poor aesthetics (the so-called elephant skin phenomenon). Another problem is that spunbond nonwovens are relatively expensive.
[0006] US 2016 / 0288451 describes a laminate with a needled staple fiber core layer suitable for vehicle underbody applications. At least one spunbond polyester layer is mechanically bonded to the core layer by needling. However, lamination by needling can have undesirable effects on the overall layer structure. For example, needled staple fibers from the core layer can penetrate the outer spunbond polyester layer. Such structural irregularities can adversely affect stability and function.
[0007] EP 3769954 A1 discloses a laminate comprising a spunbonded nonwoven layer and a central staple fiber nonwoven layer. This product is suitable as an underbody shield and can have mechanical stability, low water absorption and good sound absorption. Since the laminate is not needled, the disadvantages of needling construction can be avoided. However, spunbonded nonwovens are very expensive. The combination of a spunbonded fiber layer with a staple fiber needled heat-set core layer can result in a non-uniform product that may have different properties. In addition, there may be room for further improvement in performance and mechanical properties.
[0008] US 2018 / 0251924 A1 relates to nonwoven composites with hydrophobic and sound absorbing properties. Typically, the composites include a surface water-resistant layer from polyolefin and polyester fibers hydrophobized with polyalkylsiloxanes or perfluorinated compounds, and a B surface sound absorbing layer comprising hollow multilobal fibers. Various assemblies and manufacturing methods are suggested throughout the specification, including a laminate with a membrane inserted between both layers. However, no practical examples are disclosed that may provide guidance for specific embodiments, as well as whether and how advantageous properties can be achieved. A common problem with such composites is that they are complex and expensive to manufacture, and very difficult to recycle, since they are based on a variety of different components. Moreover, the lack of practical examples places a heavy burden on providing functional products from the various potential components, structures, and materials proposed. Overall, such composites and methods may be open to further improvement.
[0009] There is a general desire in the art to provide improved textiles, particularly for underbody shield applications, that overcome the problems discussed above. Summary of the Invention [Problem to be solved by the invention]
[0010] It is an object of the present invention to provide a textile product, use, method and products obtained therefrom that overcomes the drawbacks faced in the art. It is an object of the present invention to provide a textile product that can be heated and shaped into a desired configuration and, in particular, is dimensionally stable when heated and shaped.
[0011] In particular, the objective is to provide a textile product with high mechanical stability, especially with respect to tensile strength, flexural strength and tear strength, as well as low heat shrinkage properties. The product is required to be available at a relatively low cost and with a relatively simple and convenient manufacturing process. The product is required to be uniform, highly recyclable, highly heat-resistant and non-flammable, lightweight and with high sound absorption properties. [Means for solving the problem]
[0012] Surprisingly, it has been found that the problem underlying the present invention is solved by the nonwoven laminates, shaped articles, uses and methods as claimed. Further embodiments of the present invention are outlined throughout this specification.
[0013] The subject of the present invention is a nonwoven laminate comprising: - a nonwoven layer (A) containing multicomponent staple fibers; - optionally a nonwoven layer (B) comprising multicomponent staple fibers or monocomponent staple fibers, - a needled nonwoven layer (C) comprising monocomponent staple fibers (c1) and multicomponent staple fibers (c2); - an optional nonwoven layer (D) containing multicomponent staple fibers or monocomponent staple fibers; - optionally a nonwoven layer (E) comprising multicomponent staple fibers; Equipped with The layers are arranged in the order of (A) to (E). the layers are bonded together by melt bonding rather than by needling; The multicomponent fiber comprises a polyester component and a copolyester component; The monocomponent fibers in layer (C) are polyester fibers; the monocomponent fibers in layers (B) and (D) are copolyester fibers; the content of copolyester in optional nonwoven layers (B) and (D) is higher than that in nonwoven layer (A) and optional layer (E); all of the fibers in the nonwoven laminate are polyester and / or copolyester fibers; Layer (C) has a coating density of 500 to 2000 g / m2 determined according to DIN EN 29073-1:1992-08. 2 and The nonwoven laminate has a bending force of at least 6 N determined in accordance with ISO 178:2019 for a deflection of 2 mm; It is a nonwoven fabric laminate.
[0014] The nonwoven layers (A)-(E) are nonwoven fabrics. In the art, a nonwoven fabric is defined as a fiber mat that is consolidated mechanically, thermally (by melting the fiber polymer and bonding the fibers together) or chemically (with adhesives). In contrast, a mere fiber assembly or pile that is not consolidated is not a nonwoven fabric. A nonwoven fabric is not a woven or knitted fabric or a paper. Generally, a nonwoven fabric is a textile fabric as defined in DIN EN ISO 9092:2018. Typically, nonwoven fibers are randomly arranged and not aligned.
[0015] The layers (A)-(E) are arranged in the order (A)-(E). When all layers are present, layers (B), (C) and (D) are embedded between layers (A) and (E). Preferably, layers (A) and (E) shield the inner layer (C) from the environment. Preferably, optional layers (B) and (D) are adhesive layers that enhance the bond strength between layers (A) and (C) and between layers (C) and (E). Preferably, the nonwoven composite does not include additional layers. Preferably, the nonwoven composite is composed of layers (A), (C) and (E), and optionally layers (B) and (D).
[0016] The nonwoven laminate is characterized by a relatively high stiffness and mechanical stability. According to the invention, these properties can be adjusted in particular by the basis weight and thickness of the layer (C) and can be further adjusted by thermal bonding. Overall, the composite material is very stable, but due to the fibrous nonwoven structure, it is significantly lighter than comparable plastic materials. This is advantageous in many technical applications that require a lightweight and highly stable material, which can be easily transformed into molded parts.
[0017] The nonwoven laminate has a bending force of at least 6N determined according to ISO 178:2019 for a deflection of 2 mm. Preferably, the bending force is at least 10N or at least 15N. Preferably, the bending force is between 6N and 40N, or between 10N and 30N. For example, the bending force can be adjusted by increasing the basis weight or thickness and / or consolidation of layer C. In this case, consolidation is preferably performed by calendaring the laminate so that one or more outer layers are bonded to layer (C). A high bending force means that the material is difficult to bend. The nonwoven laminate is plate-like and has low flexibility and high stiffness, resembling a hard plastic material.
[0018] The needled short fiber nonwoven layer (C) has a fiber density of 500 to 2000 g / m2, determined according to DIN EN 29073-1:1992-08. 2 More preferably, the basis weight is 800 to 1800 g / m 2 , particularly preferably 900 to 1600 g / m 2 For standard passenger car applications, the recommended load is 800-1500g / m 2 , more preferably 1000 to 1400 g / m 2 , and most preferably about 1200 g / m 2 For applications in off-road vehicles, layer (C) may have a basis weight of 1500 to 1700 g / m 2 , more preferably 1550 to 1650 g / m 2A high basis weight is advantageous because the nonwoven fabric can have high mechanical stability and good barrier function. Preferably, the bending force is 1000 to 1700 g / m 2 The basis weight is 10N~30N.
[0019] Preferably, the nonwoven layers (A) and / or (E) each have a density of 20 to 200 g / m according to DIN EN 29073-1:1992-08. 2 , more preferably 25 to 150 g / m 2 , or 30 to 100 g / m 2 The sheet has a basis weight of 1.0 g.
[0020] Typically, the basis weight of layers (A) and / or (E) is significantly lower than that of layer (C). Preferably, the basis weight of layer (C) is at least three or five times that of layers (A) and / or (E), respectively. This is advantageous because the outer layers (A) and (E) can shield layer (C). For example, the outer layers can be relatively compact and mechanically stable, whereas layer (C) can have a lower density. Thus, a relatively light nonwoven laminate can be obtained that is effectively shielded and stabilized by the outer layers.
[0021] Preferably, the optional layer (B) and / or layer (D) has a coating weight of 5 to 100 g / m according to DIN EN 29073-1:1992-08. 2 , preferably 5 to 50 g / m 2 , more preferably 10 to 20 g / m 2 These layers, when having a relatively low basis weight, can function as adhesive layers and impart high stability and peel strength to the laminate. Preferably, the basis weight of each of layers (A) and / or (E) is at least twice, preferably at least three times, that of each of layers (B) and / or (D).
[0022] The nonwoven laminate has the following characteristics: - Tensile strength of ≥ 800N according to ASTM 5034:2009, and / or - Tear strength ≥ 100N according to DIN EN 29073-3:1992-08 It is preferable to have at least one of the following:
[0023] These properties can provide the nonwoven laminate with high abrasion resistance and sound absorption.
[0024] The nonwoven fabric laminate more preferably has a tensile strength of ≧800 N, preferably ≧1000 N, more preferably ≧1050 N. By improving the tensile strength, the mechanical properties such as stiffness, abrasion resistance and sound absorption of the nonwoven fabric laminate can be further increased.
[0025] The nonwoven fabric laminate more preferably has a tear strength of ≧100 N, preferably ≧120 N, more preferably ≧140 N. By improving the tear strength, the mechanical properties such as stiffness, abrasion resistance, and sound absorption of the nonwoven fabric laminate can be further increased.
[0026] Preferably, the nonwoven laminate has a thickness, preferably determined according to DIN EN ISO 9073-2 (method A), of 1 mm to 10 mm, preferably 1.5 to 8 mm, particularly preferably 2 to 6 mm. Particularly preferred is a thickness of at least 1.5 mm or at least 2 mm. Preferably, the thickness of the outer layer (A) and / or (E) in the nonwoven laminate is 0.2 to 1 mm, preferably 0.3 to 0.8 mm.
[0027] The nonwoven fabric laminate is characterized in that all of the fibers in layers (A) to (E) are staple fibers. Staple fibers are fibers of discontinuous length. The staple fibers have an average fiber length called the staple length. Preferably, the nonwoven fabric does not contain any fibers other than the staple fibers.
[0028] On the other hand, spunbond nonwoven fabrics are formed by continuously laying "endless" fibers drawn from molten fiber raw material onto a fiber felt. Spunbond fibers are not cut to a predetermined length. Layers (A)-(E) are not spunbond nonwoven fabrics and do not contain spunbond fibers. Preferably, the nonwoven fabric laminate does not contain spunbond fibers and / or spunbond nonwoven fabrics.
[0029] The nonwoven laminate is not produced by needling layers together. However, layer (C) is mechanically needled. A needled nonwoven layer comprises a plurality of fibers that are intermingled and consolidated using mechanical needles. Needled nonwovens are characterized by localized areas where the needles pass vertically through the nonwoven, thereby stretching the fibers and fiber bundles along with them in the vertical direction. Needled nonwovens include localized areas of low fiber density or even voids surrounded by areas of densified fibers.
[0030] Prior to assembling the nonwoven laminate, the nonwoven layer (C) was needled. In a preferred embodiment, the layers (A) and (B) were also mechanically needled prior to assembling the nonwoven laminate. It has been found that the needling structure of the layers can impart advantageous mechanical properties to the nonwoven laminate.
[0031] Overall, the nonwoven laminate comprises, and preferably is composed of, multicomponent and monocomponent staple fibers. The multicomponent fibers comprise a polyester component and a copolyester component. The monocomponent fibers in layer (C) are polyester fibers. The monocomponent fibers in optional layers (B) and (D) are copolyester fibers. Typically, the copolyester and polyester are thermoplastic polymers.
[0032] A polyester is a polymer that contains an ester functionality in every repeat unit of the polymer backbone. A copolyester is a polymer of a first diacid monomer and a first diol monomer, and also contains at least one second different diacid monomer and / or at least one second different diol monomer. Thus, a copolyester is a specific type of polyester. Although the term polyester includes polymers from at least two different monomers, a copolyester is formed from three or more different monomers. Preferably, the polyester in the fiber is formed from two monomers. Typically, the diacid monomer is a dicarboxylic acid monomer.
[0033] The nonwoven layers are bonded together by melt bonding (thermal bonding). Melt bonding is a technique for bonding thermoplastic fibers by applying energy to at least one of the materials, thereby softening or melting the fibers and bringing them into intimate contact, followed by cooling. Typically, pressure is applied so that the fibers and / or layers are in intimate contact and bonded. The nonwoven laminate of the present invention is obtained by laminating in the order (A)-(E) and then melt bonding the layers. Each layer contains at least one component that contributes to melt bonding. Preferably, the bonding component in all layers is a copolyester, which is preferably the same copolyester in all layers. Typically, all copolyesters in the nonwoven fabric are thermoplastic polymers. Melt bonding the layers together is advantageous because it can result in high uniformity in the heat shrink properties of the nonwoven laminate. This high uniformity can reduce the formation of elephant skin during molding, which allows the nonwoven laminate to have attractive aesthetics and high bending strength after molding. Melt bonding of the layers to one another can also impart high dimensional stability to the nonwoven laminate when heated and molded.
[0034] It has been found that nonwoven laminates can be very stable when consolidated only by melt bonding. The nonwoven laminate is preferably not chemically bonded. This means that no additional binder, for example in the form of particles or liquid, is used for bonding. Using only melt bonding has the advantage that the manufacturing process can be kept relatively simple and the number of components can be kept low. In contrast, adhesive binders for chemical bonding can cause various problems, such as recycling problems or undesirable deterioration, wear and peeling of microparticles or nanoparticles.
[0035] Preferably, the multicomponent fibers are bicomponent fibers. Thus, they are composed of a polyester component and a copolyester component. The multicomponent fibers act as binder fibers in the nonwoven laminate. The copolyester is the binder component, so it is present at least on the surface of the binder fiber. The melting point and / or softening point of the copolyester is lower than the melting point and / or softening point of the polyester. Preferably, the difference is at least 10°C or at least 20°C. During melt bonding, the nonwoven is heated to a temperature where only the copolymer melts or softens, and the polyester component does not melt or soften. Thus, the polyester fibers or components maintain their structure and shape in the melt bonding process.
[0036] The polyester component of the multicomponent and monocomponent fibers in layer (C) may be any known polyester. It is highly preferred that the polyester is polyethylene terephthalate (PET). PET is a copolymer of terephthalic acid and ethane-1,2-diol (also called ethylene glycol). PET is mechanically stable, has a relatively high melting point, can be conveniently spun into fibers, and is available at low cost. In another embodiment, another polyester is used, such as polycarbonate, polylactide (PLA), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), or polytrimethyl terephthalate (PTT), or copolymers or mixtures thereof.
[0037] Preferably, the polyester in all layers is PET. The PET may be virgin PET (not recycled), recycled PET (r-PET) or a mixture thereof. Virgin PET may allow for more precise setting of the mechanical properties of the nonwoven laminate. Recycled PET may allow for cost reduction of the nonwoven laminate. Recycled PET may contain small amounts of other polymers such as polyolefins.
[0038] The use of PET for all nonwoven layers has various advantages. PET can impart high uniformity of mechanical properties to the nonwoven laminate. This can increase the uniformity of the elongation and tensile strength of the nonwoven laminate in particular. The nonwoven laminate can thereby be easily heated and molded to provide a desired configuration. The nonwoven laminate can thereby be dimensionally stable when heated and molded. Furthermore, PET can provide a relatively low basis weight for the layers and the entire laminate, respectively. This is advantageous because in automotive or other applications low weight is generally desired to reduce energy costs. Furthermore, PET has a relatively high melting point of about 260°C. This allows the nonwoven laminate to have high heat resistance and non-flammability properties. The melting point is determined herein, preferably according to DIN ISO 11357-3:2013. PET is also relatively inexpensive. This allows the nonwoven laminate to contribute to a reduction in the cost of the article containing the nonwoven laminate.
[0039] All layers of the nonwoven laminate include a copolyester. The copolyester may be an amorphous copolyester, a crystalline copolyester, or a mixture of amorphous and crystalline copolyesters. The copolyester is preferably a copolymer of polyethylene terephthalate. The copolymer of polyethylene terephthalate includes the monomers terephthalic acid, ethane-1,2-diol, and at least one additional different dicarboxylic acid monomer and / or at least one additional different diol monomer. A preferred additional dicarboxylic acid monomer is adipic acid. Another preferred additional dicarboxylic acid monomer is isophthalic acid. A preferred additional diol monomer is cyclohexanedimethanol. The copolymer of polyethylene terephthalate can facilitate the recyclability of the nonwoven laminate. The copolymer of polyethylene terephthalate can increase the peel strength within the nonwoven laminate. The copolymer of polyethylene terephthalate can reduce the cost of raw materials for the nonwoven laminate.
[0040] The melting point of the copolyester is preferably ≦240° C. More preferably, the copolyester, especially the copolyester in layers (B), (C) and (D), has a melting point of ≦220° C., more preferably ≦210° C., even more preferably ≦200° C., even more preferably ≦190° C., especially 180° C. This allows the copolyester to reduce the energy required for melt bonding between the fiber layers, and further reduce the energy required for the production of the fiber layers. At a low melting point, the energy reduction can be continuously increased. Copolymers with such melting points are particularly suitable binder components when the polymer is PET.
[0041] It is preferred that the copolyester in all layers has a melting point in the range of 100-240° C., more preferably in the range of 110-230° C., even more preferably in the range of 140-225° C., and even more preferably in the range of 160-220° C. Copolyesters having a melting point in this range can reduce the energy required to melt bond the layers together, especially when the polymer is PET, and can increase the bond strength between the layers after melt bonding.
[0042] In a preferred embodiment, the copolyester in layers (A) and / or (E) has a melting point higher than the copolyester in layer (C), preferably ≥ 20°C higher, more preferably ≥ 30°C higher, even more preferably ≥ 35°C higher, in this way a stronger bond between the layers after melt bonding can be achieved.
[0043] It is preferred that the copolyester in all layers has a melting point of ≧120° C., more preferably ≧140° C., and even more preferably ≧160° C., which can increase the bond strength between the layers during melt bonding and impart thermal stability to the nonwoven fabric.
[0044] The nonwoven laminate may include one or both of layers (B) and (D). The copolyester content in the nonwoven layers (B) and (D) is higher than the copolyester content in the nonwoven layers (A) and (E). Thus, layers (B) and (D) can function as a binder (adhesive) layer that increases the bond strength (peel strength) between layers (A) and (C) and / or layers (C) and (E).
[0045] The nonwoven fabric laminate is -Layers (A), (B), (C), (D) and (E) -Layers (A), (B), (C) and (E) -Layers (A), (C) and (E) - layers (A), (B) and (C), or -Layers (A) and (C) It may comprise or consist of:
[0046] Layers (A) and (C) are always included. However, it is highly preferred that at least layers (A), (C) and (E) are included. In this embodiment, the central layer (C) is embedded between two outer layers that can provide protection and shielding. To increase the peel strength, a nonwoven laminate that includes all layers (A), (B), (C), (D) and (E) may be preferred. From the viewpoint of simplifying production and cost efficiency, a nonwoven laminate composed of layers (A), (C) and (E) may be preferred. A laminate composed of layers (A) and (C) may be preferred from cost / benefit considerations when shielding from one side or properties such as water absorption or acoustics are not very important. In a laminate, an assembly of only layers (A) and (C) is equivalent to an assembly of only layers (C) and (E).
[0047] When layer (E) is present, layers (A) and (E) may be the same or different from each other. When layers (B) and (D) are present, they may be the same or different from each other. It is preferred that layers (A) and (E) are the same and / or layers (B) and (D) are the same. This has the advantage that fewer components are required to manufacture the nonwoven laminate, reducing complexity and cost.
[0048] In a preferred embodiment, the nonwoven laminate does not include any additional layers disposed between layers (A)-(E). More preferably, the nonwoven laminate is composed of layers (A), (C) and optionally layers (B), (D) and (E). Preferably, the nonwoven laminate does not include any additional layers that are not nonwoven layers, such as woven layers, membranes or polymer films. Thus, the nonwoven laminate can have a relatively simple structure, which is advantageous for manufacturing and cost reasons.
[0049] In another embodiment, the nonwoven composite may include one or more additional layers different from layers (A)-(E). For example, it is possible to include at least one further intermediate layer and / or outer protective layer. The intermediate layer may be configured as layer (C), but with a different fiber ratio, composition, type, etc. For example, a gradient of structure and properties may be provided. However, this is less preferred, as it makes the laminate more complex and expensive.
[0050] In a preferred embodiment, nonwoven layer (A) and / or nonwoven layer (E), if present, are composed of multicomponent staple fibers, preferably bicomponent staple fibers, which is advantageous since the production of layer (A) or (E) from a single fiber type is simple and the layer is very uniform.
[0051] The nonwoven laminate layers are not bonded to each other by needling, so that none of the layers is needled to another layer. Typically, they are not mechanically bonded to each other, so that there is no mechanical bond between adjacent layers. Generally, nonwovens can be mechanically bonded by needling or hydroentanglement (fluid jet processing). These methods result in the penetration of fibers or fiber bundles from one layer to another. Typically, the fibers of the nonwoven laminate of the present invention do not penetrate adjacent layers and / or there is no fiber entanglement between layers. This has the advantage that molded articles can be produced from the nonwoven laminate that are flat, in particular without wrinkles or wavy structures, and have high bending strength.
[0052] In a preferred embodiment, at least one nonwoven layer is thermally bonded (melt bonded) prior to combining the laminate layers (i.e. individually). Preferably, the layers are thermally bonded by calendaring. In this embodiment, the layers are pressed between calendar rolls heated to a temperature above the softening point of the fibrous material. Preferably, layers (A), (C) and (E), or all layers, are thermally bonded individually. This has the advantage that each layer can be provided in a stable form before the laminate is formed. The layers can be subsequently combined and melt bonded together. Typically, the thermal bonding of the individual layers and the subsequent thermal bonding of the laminate are achieved by the same means, i.e. melting and bonding of the copolyester.
[0053] Preferably, the nonwoven layers (C) are individually thermally bonded by heat setting and / or heat shrinking. In the heat setting process, the individual layers are subjected to heat, for example by a calendar roll, without applying significant pressure. Typically, the nonwoven is heat set in an oven. This can be advantageous when the layers (C) can be relatively thick, since thermal bonding by calendaring can be inefficient. Furthermore, heat setting can have the advantage that the layers (C) are heat shrunk. Preferably, the needled fibers are heat shrunk in both the longitudinal and transverse directions. The heat shrunk needled staple fibers are dimensionally stable, which is advantageous for subsequent lamination and molding. Typically, the basis weight is increased during heat shrinking. This can avoid the undesirable formation of elephant skin during the subsequent molding process. Heat setting is also advantageous because the material is not compressed and can have a relatively light weight.
[0054] In a preferred embodiment, the nonwoven layers (A) and / or (E) are thermally bonded by calendering before assembly of the laminate. In such a method, the substrate is compressed under heat to obtain a tight bond. This is advantageous because it allows the outer nonwoven layers (A) and / or (E) to be provided in a relatively compact and stable form, effectively shielding layer (C) from the environment in the nonwoven laminate.
[0055] Preferably, the nonwoven layers (A) and / or (E) are needled before assembly of the laminate, which is advantageous since the needled outer layer can have high mechanical stability and thus protect layer (C) from the environment.
[0056] All fibers of the nonwoven laminate are polyester fibers, especially PET fibers, and copolyester fibers. Thus, all fibers are either monocomponent polyester or monocomponent copolyester fibers, or multicomponent fibers including polyester and copolyester components. This is advantageous because it allows the nonwoven laminate to have a relatively low cost, relatively low weight, and relatively high peel strength. This allows the nonwoven laminate to be recycled more easily. This allows for increased heat resistance and flame resistance properties. This also allows for improved mechanical properties of the nonwoven laminate, especially the uniformity of its elongation and tensile strength. This allows for easier adjustment of the properties of products including the nonwoven laminate.
[0057] Since all fibers are polyester and copolyester fibers, the nonwoven laminate does not contain polyolefin fibers, especially polypropylene and / or polyethylene fibers. However, the fibers may contain unavoidable impurities of other polymers, such as small amounts of polyethylene or polypropylene, especially when recycled polyester fibers are included. For example, it is known in the art that r-PET may contain small amounts of polyolefins that are difficult to remove in standard recycling processes.
[0058] The nonwoven laminate preferably does not contain further polymers, e.g. as binders, that are not polyesters or copolyesters, such as polypropylene and / or polyethylene. It is advantageous for manufacturing and recycling that the only polymers in the nonwoven laminate are polyesters and copolyesters.
[0059] Preferably, the fibers of the nonwoven laminate do not contain hydrophobizing agents, such as silicon or fluorine based compounds, such as polyalkylsiloxanes and fluorinated compounds, which are disadvantageous because such additives make the nonwoven laminate more complex, expensive and difficult to recycle.
[0060] Preferably, the nonwoven laminate does not contain hollow and / or multilobal fibers. Preferably, the fibers have a circular (or elliptical) diameter and / or are blocky (non-hollow). Such round blocky fibers are readily available at low cost and can provide the advantageous properties outlined herein.
[0061] The nonwoven laminate preferably does not contain inorganic reinforcement, especially glass fiber. The absence of inorganic reinforcement, especially glass fiber, can facilitate the processability of the nonwoven laminate and reduce costs. The nonwoven laminate preferably does not contain any lofting agent. The absence of lofting agent can increase the dimensional instability of the nonwoven laminate when it is heated and molded, and can reduce costs.
[0062] To impart even higher abrasion resistance and increased sound absorption to the nonwoven laminate, it is particularly preferred that the nonwoven laminate has a flexural strength of ≧150 MPa and / or a tensile strength of ≧800 N. It is most preferred that the nonwoven laminate has a tear strength of ≧100 N. High flexural and tensile strengths mean that the product is rigid, which is relevant for structural parts such as underbody shields. High tear and tensile strengths also mean that the product has high stability against mechanical stress or strain, which is also relevant for use in structural parts such as underbody shields. These properties mean that the nonwoven laminate can replace traditional molded thermoplastic parts used in the art for such applications. Furthermore, the nonwoven laminate and products derived therefrom are advantageous because the fibrous structure is lightweight, can have high sound absorption, and is surprisingly stable.
[0063] The nonwoven fabric laminate preferably has a flexural strength of ≧150 MPa, preferably ≧300 MPa, more preferably ≧350 MPa. When the thickness is relatively large, for example, greater than 3 mm, the flexural strength is preferably ≧350 MPa, more preferably ≧500 MPa. By improving the bonding strength, the abrasion resistance and sound absorption of the nonwoven fabric laminate can be further increased.
[0064] The copolyester in all layers, especially in layers (A) and (E), has a viscosity of 1.1 to 1.6 g / cm 3 , more preferably 1.2 to 1.5 g / cm 3 , and even more preferably 1.3 to 1.4 g / cm 3 It is preferred that the laminate has a density of 0.1 to 0.5 mm. The density is determined in accordance with DIN EN ISO 1183-1:2019-09. Such a density can result in a laminate of adequate strength while avoiding excessive costs.
[0065] Preferably, the bicomponent fibers in layers (A), (C) and / or (E) contain at least 20% copolyester, preferably 5% to 70% copolyester and 30% to 95% polyester. Preferably, layers (A), (C) and (E), especially when layers (B) and (D) are not present, contain 20% to 80%, preferably 30 to 70% copolyester, particularly preferably at least 40% copolyester, at least 50% copolyester, at least 60% copolyester, or at least 70% copolyester. Such a copolyester content can provide efficient bonding and thereby avoid wavy structures in the laminate. Such a copolyester content can further improve the bending strength of the laminate. In this specification, "%" means weight % unless otherwise defined. In this specification, the residual is the polyester component.
[0066] When layers (B) and (D) are present, it may be preferred that layers (A) and / or (E) contain 2% to 30% copolyester, more preferably 5 to 25% copolyester. The bond is then supported by adhesive layers (B) and (D). When layers (A) and / or (E) contain at least 30%, more preferably at least 40%, at least 50%, at least 60% or at least 70% copolyester, the laminate without layers (B) and (D) can have a high peel strength. That is, neither layers (B) nor layers (D) are required to increase the peel strength. This can simplify the manufacture of the laminate.
[0067] The layer (C) is preferably composed of 10-90% monocomponent fibers (c1) and 10-90% multicomponent fibers (c2), more preferably 20-80% monocomponent fibers (c1) and 20-80% multicomponent fibers (c2), even more preferably 30-70% monocomponent fibers (c1) and 30-70% multicomponent fibers (c2), even more preferably 40-60% monocomponent fibers (c1) and 40-60% multicomponent fibers (c2). The monocomponent fibers do not melt during thermal bonding. Thus, the basic structure of the layer can be maintained during thermal bonding. Thus, the layer and the entire laminate can remain mechanically stable but on the other hand be relatively lightweight.
[0068] Specifically, when layer (C) is composed of 10-90% monocomponent staple fiber (c1) and 10-90% multicomponent staple fiber (c2), it can be more easily needled. Furthermore, the use of PET as the polyester in layer (C) can reduce the total weight of the nonwoven fabric laminate, can bring about high heat resistance and nonflammability properties of the nonwoven fabric laminate, and can reduce the cost of the nonwoven fabric laminate.
[0069] Preferably, in layer (C), the monocomponent fibers are PET fibers and the multicomponent fibers are bicomponent fibers comprising PET as a first component and CoPET as a second component.
[0070] Preferably, the multicomponent fibers in the nonwoven laminate are bicomponent fibers having a sheath-core, island-in-the-sea, pie-segment or side-by-side structure, preferably a sheath-core structure. The copolyester binder component is present at least on the surface of the bicomponent fibers. The staple fibers (c2) have the following characteristics: - a fineness determined according to DIN EN ISO 1973:2020-05 of 2 to 9 dtex, more preferably 3 to 7 dtex, even more preferably 4 to 6 dtex - Fiber length of 30 to 100 mm, more preferably 40 to 70 mm, and even more preferably 45 to 55 mm a strength determined according to DIN EN 13844:2003-04 of 1 to 6 g / de, more preferably 2 to 5 g / de, even more preferably 3 to 4 g / de An elongation determined according to DIN EN ISO 5079:2020-01 of 20-60%, more preferably 30-50%, even more preferably 35-55%. A crimp amount determined according to JIS L-1074 of 4 to 10 EA / inch, more preferably 5 to 9 EA / inch, and even more preferably 6 to 8 EA / inch A heat shrinkage of 3-7%, more preferably 4-6%, even more preferably 3.5-4.5% at 75°C for 15 min, determined according to DIN EN 13844:2003-04 It is preferable that the compound has at least one of the above, more preferably two or more of the above, and most preferably all of the above.
[0071] When the staple fibers (c2) have at least one, more preferably two or more, and most preferably all of the above characteristics, the needled staple fiber nonwoven fabric layer (C) can simultaneously impart strength and rigidity to the nonwoven fabric laminate.
[0072] The nonwoven laminate has the following features: the copolyester in all layers is a copolymer of polyethylene terephthalate (CoPET) having a melting point between 160 and 240°C; - comprising a layer (B) and a layer (D), both made of copolyester and having a coating weight of 5 to 30 g / m2 according to DIN EN 29073-1:1992-08 2 having a basis weight of - layer (C) is composed of 30-70% monocomponent short fibers (c1) and 30-70% multicomponent short fibers (c2); is preferred.
[0073] Such preferred nonwoven laminates can be easily heated and molded to provide a desired configuration and can be dimensionally stable when heated and molded. They can be particularly suitable as underbody shielding materials. By having layers (B) and (D), peel strength and heat resistance can be increased.
[0074] In another embodiment, the nonwoven laminate comprises: does not include layers (B) and (D), the copolyester in layers (A), (C) and (E) is a copolymer of polyethylene terephthalate, the copolymer having a melting point between 160 and 240°C; - layer (C) is composed of 30-70% monocomponent short fibers (c1) and 30-70% multicomponent short fibers (c2); is preferred.
[0075] Such nonwoven laminates can be easily heated and shaped to provide a desired configuration and can be dimensionally stable when heated and shaped. Such preferred nonwoven laminates can be particularly suitable for use as underbody shielding materials. The absence of layers (B) and (D) can reduce the cost of the nonwoven laminate and simplify manufacturing.
[0076] The subject of the present invention is also a molded article (molded body, molded part) comprising the nonwoven laminate of the present invention. This article can be obtained by molding the nonwoven laminate into a desired shape. The shape can be a flat sheet or have defined dimensions and can include edges or bend areas. Advantageously, such molded articles can be lightweight and homogeneous. The molded articles are easy and inexpensive to manufacture, since they contain only staple fibers and can be entirely based on polyesters and copolyesters, without the need for spunbond materials.
[0077] The subject of the present invention is also a method for producing a molded article, comprising the steps of: providing a nonwoven laminate of the present invention, heating the nonwoven laminate to a temperature at which the copolyester softens or melts; forming the nonwoven laminate into a shaped article; The method includes:
[0078] Preferably, at least one of the nonwoven layers is thermally bonded by calendaring before combining the layers. Preferably, layer (C) is thermally bonded by heat setting and / or heat shrinking before combining the layers, and / or layer (A) and / or layer (E) are thermally bonded by calendaring before combining the layers.
[0079] Preferably, the molded article is cold molded. In the cold molding process, the nonwoven laminate is preheated in an oven for 1-5 minutes, for example at a temperature range of 180°C to 220°C, depending on the basis weight, to activate the low melting copolyester, which acts as a binder. The binder softens or melts and can bond the PET fibers to each other. After heat activation, the nonwoven laminate is placed in a compression mold. The compression mold can compress all or part of the nonwoven laminate with a tonnage of 50 tons to 200 tons. Typically, the nonwoven laminate can remain in the mold for up to 60 seconds. The compressed nonwoven laminate is allowed to cool inside or outside the mold to allow the copolyester to cool below its melting point. The nonwoven laminate can then be converted to its final shape. The final thickness of the material can be 2mm to 6mm, depending on the requirements of the intended application. The nonwoven laminate can then be trimmed as needed, which can be achieved by mechanical cutting, thermal cutting, or water jet cutting.
[0080] In another embodiment, the molded article is thermoformed. In this process, the nonwoven laminate is placed between a pair of hot compression mold plates. The plates can then be brought closer to the desired thickness, which is less than the thickness of the material. For example, if the nonwoven laminate is 6 mm thick, the thickness between the plates is 2 mm to 5 mm. The mold plates are heated to a temperature ranging from 180°C to 220°C. The nonwoven laminate is then compressed for 1 to 3 minutes, depending on the basis weight, to activate the low melting point copolyester (or binder). The nonwoven laminate can then be transformed into its final shape. Typically, the final thickness of the material is 2 mm to 6 mm, depending on the requirements of the intended application.
[0081] The nonwoven laminates and / or molded articles can be used in various technical applications where high stability, low weight, sound absorption and / or low cost are required. The subject of the invention is underbody shields, wheel arch liners, roof pillars, structural parts for luggage or luggage compartments, covering or paneling materials or other structural parts, in particular for automotive applications.
[0082] The subject of the present invention is also the use of the nonwoven laminate of the present invention or the molded part of the present invention as an underbody shield, wheel arch liner, roof pillar, structural part for luggage or luggage compartment, covering or panel material or other structural part, in particular for automotive applications, in which the advantages of improved abrasion resistance and high heat resistance and non-flammability properties, and the advantages associated therewith, are particularly prominent.
[0083] The present invention also provides a method for producing the nonwoven laminate of the present invention, comprising the steps of: - preparing a stable nonwoven layer (C) by needling; - providing a layer (A) and optionally layers (B), (D) and (E); - melt bonding the layers together; The present invention relates to a method comprising the steps of:
[0084] This method is advantageous due to the benefits of easy joining of layers by melt bonding which can result in high peel strength and stability in associated technical applications.
[0085] Exemplary embodiments of the invention and aspects of the invention are illustrated in the figures. [Brief description of the drawings]
[0086] [Figure 1] FIG. 1 illustrates in schematic and exemplary form the individual layers of a preferred five-layer nonwoven laminate according to the present invention. [Diagram 2] FIG. 1 illustrates in schematic and exemplary form the individual layers of a preferred three-layer nonwoven laminate according to the present invention. [Diagram 3] FIG. 13 shows the results of acoustic measurements according to a practical example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0087] A preferred five-layer nonwoven laminate 1 according to the present invention is shown in Figure 1. The five-layer nonwoven laminate 1 comprises a first outer layer 2 corresponding to layer (A), a first adhesive layer 3 corresponding to layer (B), a core layer 4 corresponding to layer (C), a second adhesive layer 5 corresponding to layer (D), and a second outer layer 6 corresponding to layer (E). The layers of this laminate are not mechanically bonded to each other, but are exclusively melt bonded to each other.
[0088] In one embodiment, an advantageous fiber preparation is carried out before the needling of the short fibers (c1) and (c2) into the core layer (C). More specifically, before the needling process, the fibers (c1) and (c2) are opened from a bale, mixed and carded. The fibers (c1) and (c2) are then cross-wrapped and passed through a needling machine. Alternatively, the fibers are prepared by an air-laying or air-laid process, and the opened fibers are collected on a suction band and needled. The core 4 is pre-shrunk by applying heat to avoid shrinkage during the subsequent molding process. The short fibers (c1) and / or (c2) preferably have a length in the range of 10 mm to 150 mm, more preferably 30 mm to 100 mm.
[0089] In one embodiment, the core layer (C) contains a mixture of 10-70% virgin or recycled PET staple fibers (c1) combined with 30-90% bicomponent fibers (c2). The bicomponent fibers have a sheath-core structure, where the sheath has a melting point lower than that of the core. The bicomponent fibers can have various geometric configurations, such as side-by-side, sheath-core, segmented pie or islands-in-the-sea.
[0090] In one embodiment, the binder polymer of the bicomponent fiber (c2) is selected based on its melting point. In a preferred sheath-core configuration, the core is preferably composed of PET and the sheath is preferably composed of a copolyester having a melting point of <200°C. One particularly preferred binder fiber has a sheath-core filament configuration. The core can be composed of PET with a melting point of >250°C, i.e., about 260°C, and the sheath can be composed of a copolyester with a lower melting point in the range of 110°C to 200°C.
[0091] FIG. 2 shows a preferred meltbonded three-layer nonwoven laminate 7 according to the present invention, with layers 2, 4 and 6 as generally described above with respect to FIG. 1, but without adhesive layers 3 and 5 corresponding to layers (B) and (D).
[0092] The nonwoven laminate, use, method and product of the present invention solve the problem underlying the present invention. The nonwoven laminate can be conveniently heated and molded into a desired shape. The nonwoven laminate is dimensionally stable, especially with respect to tensile strength, bending strength, tear strength and / or heat shrinkage. The nonwoven laminate is available at low cost and with a simple and convenient manufacturing process. There is no need to use spunbond fibers or spunbond layers. The nonwoven laminate is very uniform, since it can be obtained only from staple fibers and only from polyesters and copolyesters. Therefore, it can have good recyclability, high heat resistance and non-flammability, light weight and can provide high sound absorption. EXAMPLES
[0093] Example 1 - Preparation of nonwoven laminate A nonwoven laminate of the present invention was prepared from nonwoven layers (A), (C) and (E).
[0094] Outer layers (A) and (E): 100% bicomponent staple fiber Material: Core 50% PET, Sheath 50% PET copolyester (CoPET, T M =180℃) Length 51mm, fineness 2.1den Basis weight: 50g / m 2
[0095] Central layer (C): 50% single component short fiber (c1) / Material: r-PET / Short fiber length: 67mm / Fineness: 6.7den 50% Bicomponent Staple Fiber Material: Core 50% PET, Sheath 50% PET copolyester (CoPET, T M =180℃) Length 51mm, fineness 4.4den
[0096] For layer (C), short fibers were mixed in a 50%:50% ratio, carded, cross-lapped and needled. The needles used were 350 needles / cm 2 The needles were Groz-Beckert 36gg fine needles with a total needling strength of 1000 g / m2. The needling depth was set at 10 mm on both sides. The needled fabric was then thermally bonded in a ventilated oven heated to 200° C. so that the bicomponent fibres were activated (softened) and bonded. After cooling, the fabrics had a weight of about 1050 and about 1350 g / m2. 2 The result was a stiff nonwoven fabric having a basis weight of 1.0 g / m.
[0097] The nonwoven fabrics for use as layers (A) and (E) were produced from bicomponent staple fiber fabrics. The needling was 150 needles / cm 2 The fibers were carded, cross-lapped and needled as described above for layer (C), except that the process was carried out at 20° C. The needled nonwoven fabric was then thermally bonded by calendering at a temperature of 200° C. and a speed of 20 m / min. 2 A nonwoven fabric having a basis weight of
[0098] The nonwoven fabric for layer (C) was passed through a set of calender rollers where the outer layers (A) and (E) were introduced on both sides. The calender pressure was 25 bar on both sides at a temperature of 200° C. so that the layers were melt bonded to each other. 2 (Sample D) and about 1450 g / m 2 A nonwoven laminate was obtained having a basis weight of (Sample E) and a thickness of 4 mm or 2 mm. All layers were melt bonded (thermally bonded) to each other, but no layer was mechanically bonded to another layer. The nonwoven laminate was cut into sheets.
[0099] Approximately 1350g / m 2A comparative nonwoven fabric (Sample A) was prepared which was comprised of a single layer of bicomponent melt-bonded staple fibers having a basis weight of about 1150 g / m. A further comparative nonwoven fabric was prepared, this comparative nonwoven fabric having a basis weight of about 1150 g / m. 2 (Sample B) and 1450 g / m 2 (Sample C) basis weight, consisting of an inner needled staple fiber layer and two outer spunbond layers that were individually thermal bonded and not needled, with all three layers combined by melt bonding.
[0100] Example 2: Production of molded articles Molded articles were produced from the nonwoven laminate of Example 1 by cold molding. The sheet-cut nonwoven laminate was introduced into an oven heated to 210°C for 3 minutes (for ventilated oven) or 1 minute (for infrared oven) to soften the CoPET component. The fabric was immediately transferred to a cold press where the material was molded, bent and shaped under high pressure (50 tons or more). The molded articles are rigid and mechanically stable. The molded articles are suitable for various technical applications such as underbody shields. This result demonstrates that the nonwoven laminate of the present invention can be conveniently used to form stable molded articles of desired shapes.
[0101] Example 3: Sound absorption The acoustic properties of the nonwoven laminate of Example 1 were tested in the Alpha Cabin. Samples were placed either near a wall with a 2 mm air gap or near the ground. The absorption coefficient is measured by a series of sensors inside the cabin. The results are summarized in Table 1. Figure 3 shows the absorption coefficient α vs. acoustic frequency (horizontal axis). s The results are shown in the graph (vertical axis). Sound absorption coefficient α sThe higher the frequency, the better the acoustic performance of the sample tested. The results demonstrate that the sound absorption of the nonwoven laminate of the present invention is much better than that of Comparative Sample A, which is composed of staple fibers but does not include a defined layer. Furthermore, the performance is comparable to the comparative laminate with an outer spunbond layer. Sample E of the present invention has the best performance overall. In particular, the performance is particularly good in the 400-800 Hz range, which is particularly relevant for automotive underbody applications.
[0102] [Table 1]
[0103] Example 4: Mechanical properties The mechanical properties of the nonwoven laminate of Example 1 were investigated. The results are summarized in Table 2 for the nonwoven laminate with a thickness of 4 mm and in Table 3 for the corresponding nonwoven laminate with a thickness of 2 mm. The flexural strength was determined according to ISO 178:2019-04, the tensile strength according to ASTM 5034:2009 and the tear strength according to DIN EN 29073-3:1992-08.
[0104] The bending force is determined according to ISO 178:2019 for a bending deflection of 2 mm. The following conditions were adjusted: three-point bending test, specimen width 30 mm, preforce 0.5 N, test speed 10 mm / min, radius bending stamp 5 mm, distance (span) between probe holders 64 mm, distance between support rolls 5 mm, radius support roller 5 mm.
[0105] The results demonstrate that the nonwoven laminate of the present invention has high mechanical stability and advantageous properties. The high bending force, tensile strength and tear strength indicate that the material is stiff, robust and elastic. The stability is much higher than the comparative monolayer product. Furthermore, the performance can be similar or better than the comparative laminate with the outer spunbond layer. This is advantageous because the staple fiber nonwoven is more homogeneous and can be manufactured and processed more easily.
[0106] [Table 2]
[0107] [Table 3]
[0108] Example 5: Water absorption rate The water absorption of the nonwoven laminate according to Example 1 was investigated. The samples were immersed in water and dried. The amount of absorbed water was monitored by weighing. The results are summarized in Table 4. The results demonstrate that the water absorption of the nonwoven laminate of the present invention is much better than the comparative single-ply staple nonwoven. Overall, the water absorption is low enough to meet the requirements of technical applications such as underbody shields.
[0109] [Table 4]
Claims
1. A nonwoven fabric laminate, - a nonwoven layer (A) containing multicomponent staple fibers; - optionally a nonwoven layer (B) comprising multicomponent staple fibers or monocomponent staple fibers, - a needled nonwoven layer (C) comprising monocomponent staple fibers (c1) and multicomponent staple fibers (c2); an optional nonwoven layer (D) comprising multicomponent staple fibers or monocomponent staple fibers, - optionally a nonwoven layer (E) comprising multicomponent staple fibers; Equipped with The layers are arranged in the order of (A) to (E), the layers are bonded together by melt bonding rather than by needling; The multicomponent staple fiber comprises a polyester component and a copolyester component; the monocomponent staple fibers in layer (C) are polyester fibers; the monocomponent staple fibers in layers (B) and (D) are copolyester fibers; the content of said copolyester fibers in optional nonwoven layers (B) and (D) is higher than that in nonwoven layer (A) and optional layer (E); all of the fibers in the nonwoven laminate are polyester and / or copolyester fibers; The layer (C) has a coating density of 500 to 2000 g / m2, determined according to DIN EN 29073-1:1992-08. 2 and The nonwoven laminate has a bending force of at least 6 N determined according to ISO 178:2019 for a deflection of 2 mm. Nonwoven laminate.
2. 10. The nonwoven laminate of claim 1, wherein the layers (A) and (E) are needled prior to combining the layers.
3. 2. The nonwoven laminate of claim 1, comprising or consisting of layers (A), (C) and (E).
4. - thickness determined according to DIN EN ISO 9073-2 between 1 mm and 10 mm - a tensile strength of ≥ 800 N according to ASTM 5034:2009, and / or - Tear strength according to DIN EN 29073-3:1992-08 of ≧100 N 2. The nonwoven laminate of claim 1, having at least one of the following characteristics:
5. 10. The nonwoven laminate of claim 1, wherein the copolyester in all layers is a copolymer of polyethylene terephthalate, the copolymer having a melting point of ≦240°C.
6. 2. The nonwoven laminate of claim 1, wherein the multicomponent staple fibers in layers (A), (C) and / or (E) comprise 30% to 95% polyester and 5% to 70% copolyester.
7. Layers (A) and / or (E) each have a coating weight of 20 to 200 g / m according to DIN EN 29073-1:1992-08. 2 2. The nonwoven laminate of claim 1 having a basis weight of
8. 2. The nonwoven laminate of claim 1, wherein layer (C) is composed of 10-90% monocomponent staple fibers (c1) and 10-90% multicomponent staple fibers (c2).
9. A molded article comprising the nonwoven laminate of any one of claims 1 to 8.
10. 10. A method for producing the molded article of claim 9, comprising the steps of: - providing a nonwoven laminate according to any one of claims 1 to 8, - heating the nonwoven laminate to a temperature at which the copolyester softens or melts; - forming said nonwoven laminate into said molded part; A method comprising:
11. The method of claim 10, wherein at least one nonwoven layer is thermally bonded by calendaring prior to combining said layers.
12. 11. The method of claim 10, wherein, prior to combining the layers, layer (C) is thermally bonded by heat setting and / or heat shrinking, and / or, prior to combining the layers, layer (A) and / or layer (E) are thermally bonded by calendaring.
13. 9. Use of the nonwoven laminate of any one of claims 1 to 8 as an underbody shield, wheel arch liner, roof pillar, structural part, cover or panel material for luggage or luggage compartments, or other structural part, especially for automotive applications.
14. Use of the molded article of claim 9 as an underbody shield, wheel arch liner, roof pillar, structural part, cover or panel material for luggage or luggage compartments, or other structural part, particularly for automotive applications.
15. 9. An underbody shield, wheel arch liner, roof pillar, structural part for luggage or luggage compartment, cover or panel material, or other structural part, particularly for automotive applications, comprising the nonwoven laminate of any one of claims 1 to 8.
16. An underbody shield, wheel arch liner, roof pillar, structural part for a luggage or luggage compartment, cover or panel material, or other structural part, particularly for automotive applications, comprising the molded article of claim 9.
17. A method for producing the nonwoven laminate of any one of claims 1 to 8, comprising the steps of: - preparing layer (C) by needling; - providing a layer (A) and optionally layers (B) and (D) and (E); - melt bonding said layers together; A method comprising:
Citation Information
Patent Citations
Preparation of interior trim for vehicle
JP1994010255A
Interior material for vehicle
JP1995017315A
Nonwoven fabric laminate
JP1996156161A
Sheath material and under protector equipped with the same
JP2004359066A
Under cover of automobile body and manufacturing method of the same
JP2012218492A