Zirconium-containing nitride powder and black ultraviolet-curable organic composition
A zirconium-containing nitride powder with optimized composition and particle size addresses the challenge of achieving high-definition black patterns by enhancing ultraviolet light transmittance and visible light shielding, suitable for color filters and CMOS camera modules.
Patent Information
- Application Number
- JP2022559266
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-02
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing insulating black pigments used in displays and CMOS camera modules face challenges in achieving high-definition black patterns with improved ultraviolet light transmittance and visible light shielding properties, as enhancing ultraviolet light transmittance often compromises visible light shielding.
A zirconium-containing nitride powder with a specific composition and particle size range (10 nm to 70 nm) is developed, featuring a general formula (Zr,X,Y)(N,O), where X represents certain Group 3 elements and Y is yttrium, optimizing the wavelength range for visible light extinction and improving ultraviolet light transmittance and visible light shielding.
The zirconium-containing nitride powder achieves balanced ultraviolet light transmittance and visible light shielding, enabling the formation of high-definition black patterns suitable for color filters and CMOS camera modules.
Smart Images

Figure 0007563476000002 
Figure 0007563476000003 
Figure 0007563476000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a zirconium-containing nitride powder and a black ultraviolet-curable organic composition. This application claims priority based on Japanese Patent Application No. 2020-183603, filed on November 2, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] The insulating black pigment is used, for example, as a material for a black pattern constituting a black matrix of a color filter for a display or a light-shielding material in a CMOS camera module. As a method for forming a black pattern, a photolithography method using a black photosensitive composition containing an ultraviolet-curable organic material and an insulating black pigment is known. In the photolithography method, a black photosensitive composition is applied to a substrate to form a photoresist film. Then, the photoresist film is exposed to ultraviolet light in a pattern to form a pattern consisting of exposed and cured hardened parts and unexposed uncured parts. Then, the uncured parts are removed to form a black pattern. The insulating black pigment used when forming a black pattern by this photolithography method needs to transmit ultraviolet light that hardens the photoresist film, that is, to have ultraviolet light transmittance.
[0003] Zirconium nitride powder is known as an insulating black pigment having ultraviolet light transmittance. In order to improve the ultraviolet light transmittance of the zirconium nitride powder, the addition of magnesium and / or aluminum to zirconium nitride has been considered (Patent Document 1).
[0004] In recent years, the increasing resolution of displays and the miniaturization of CMOS camera modules have led to a demand for high-definition black patterns. In order to form high-definition black patterns using photolithography, it is effective to improve the ultraviolet light transmittance of the black pigment, particularly to improve the transmittance of ultraviolet light (i-line) with a wavelength of 365 nm that is generally used in ultraviolet light exposure devices. However, improving the ultraviolet light transmittance of the black pigment may reduce the ability to block visible light. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-112275 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a powder that is excellent in transmittance of ultraviolet light and in blocking visible light. [Means for solving the problem]
[0007] In order to solve the above problems, the zirconium-containing nitride powder according to the first aspect of the present invention comprises: A zirconium-containing nitride powder used as an insulating black pigment having ultraviolet light transmittance, The composition is represented by the following general formula (I): At the same time, the average particle size is within the range of 10 nm to 70 nm. Zirconium-containing nitride powder. (Zr,X,Y)(N,O)···(I) In the above general formula (I), X represents at least one element selected from the group consisting of Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb and Tm, and Y represents the element symbol for yttrium, and The content of X is within the range of 0.05 moles or more and 0.30 moles or less, The content of Y is 0 moles or more, N represents nitrogen, O represents oxygen, and the content of oxygen is 0 moles or more per mole of the total content of nitrogen and oxygen.
[0008] The zirconium-containing nitride powder having the above-mentioned composition has a composition represented by the above-mentioned general formula (I), and therefore the wavelength showing the maximum peak of the extinction coefficient in the visible light region can be set within the range of 540 nm to 600 nm. Therefore, it is possible to block visible light from the short wavelength side (e.g., wavelength 400 nm) to the long wavelength side (e.g., wavelength 800 nm). Therefore, the zirconium-containing nitride powder having the above-mentioned composition has excellent ultraviolet light transmittance and visible light blocking properties.
[0009] Here, in the zirconium-containing nitride powder according to the first aspect of the present invention, the average particle size is preferably within the range of 10 nm or more and 70 nm or less. In this case, the zirconium-containing nitride powder has a fine average particle size within the above range, so that the plasma oscillation of the zirconium-containing nitride particles due to visible light is not easily attenuated. This improves the shielding ability of visible light. In addition, the particle size is sufficiently small compared to the wavelength of light, so that light scattering is not easily caused, improving the transmittance of ultraviolet light with a wavelength of 365 nm.
[0010] In addition, in the zirconium-containing nitride powder related to the first aspect of the present invention, the ratio of the extinction coefficient of visible light having a wavelength of 550 nm to the extinction coefficient of ultraviolet light having a wavelength of 365 nm, measured by the following method, is preferably in the range of 1.4 or more and 100 or less. (Method of measuring extinction coefficient) A dispersion liquid containing zirconium-containing nitride powder at a mass concentration of 50 ppm is placed in a cell with an optical path length d (unit: m). Light is irradiated onto the cell containing the dispersion liquid, and the transmitted light intensity of the light that passes through the cell is measured. The optical path length d, the incident light intensity I0 of the light irradiated onto the cell, and the transmitted light intensity I of the light that passes through the cell are substituted into the following equation (1) to calculate α as the extinction coefficient of the light irradiated onto the cell. I = I0exp(-α × d) (1) In this case, the ratio of the extinction coefficient of visible light having a wavelength of 550 nm to the extinction coefficient of ultraviolet light having a wavelength of 365 nm is within the range of 1.4 to 100, so that the transmittance of ultraviolet light and the shielding property of visible light are improved in a well-balanced manner. Therefore, by using the zirconium-containing nitride powder having the above-mentioned configuration, a high-definition black pattern having excellent shielding property of visible light can be formed.
[0011] In addition, in the zirconium-containing nitride powder according to the first aspect of the present invention, the extinction coefficient of visible light having a wavelength of 550 nm is 600m -1 More preferably, it is equal to or greater than this. In this case, the extinction coefficient of visible light with a wavelength of 550 nm is 600m -1 For the above reasons, the visible light shielding property is further improved. Therefore, a black pattern formed using the zirconium-containing nitride powder having the above-mentioned configuration is useful as a black matrix of a color filter of a display or a light shielding material in a CMOS camera module.
[0012] In addition, the zirconium-containing nitride powder according to the second aspect of the present invention has an average particle size in the range of 10 nm or more and 70 nm or less, and in the extinction coefficient measured by the following method, the ratio of the extinction coefficient of visible light having a wavelength of 550 nm to the extinction coefficient of ultraviolet light having a wavelength of 365 nm is in the range of 1.4 or more and 100 or less. (Method of measuring extinction coefficient) A dispersion liquid containing zirconium-containing nitride powder at a mass concentration of 50 ppm is placed in a cell with an optical path length d (unit: m). Light is irradiated onto the cell containing the dispersion liquid, and the transmitted light intensity of the light that passes through the cell is measured. The optical path length d, the incident light intensity I0 of the light irradiated onto the cell, and the transmitted light intensity I of the light that passes through the cell are substituted into the following equation (1) to calculate α as the extinction coefficient of the light irradiated onto the cell. I = I0exp(-α × d) (1)
[0013] According to the zirconium-containing nitride powder having the above-mentioned configuration, the average particle size is within the above-mentioned range and is fine, so that the plasma vibration of the zirconium-containing nitride particles caused by visible light is not easily attenuated. Therefore, the shielding property of visible light is improved. In addition, since the particle size is sufficiently small compared to the wavelength of light, light scattering is not easily caused, so that the transmittance of ultraviolet light having a wavelength of 365 nm is improved. Furthermore, since the ratio of the extinction coefficient of visible light having a wavelength of 550 nm to the extinction coefficient of ultraviolet light having a wavelength of 365 nm measured by the above-mentioned method is within the range of 1.4 to 100, the transmittance of ultraviolet light and the shielding property of visible light are improved in a well-balanced manner. Therefore, by using the zirconium-containing nitride powder having the above-mentioned configuration, a black pattern that is highly precise and has excellent shielding property of visible light can be formed.
[0014] A black ultraviolet-curable organic composition according to a third aspect of the present invention includes an ultraviolet-curable organic material and a black pigment dispersed in the ultraviolet-curable organic material, and the black pigment is the zirconium-containing nitride powder according to the first and second aspects of the present invention.
[0015] In the black ultraviolet-curable organic composition according to the third aspect of the present invention, the ultraviolet-curable organic material is preferably at least one organic material selected from the group consisting of acrylic monomers, acrylic oligomers, epoxy monomers, and epoxy oligomers. Effect of the Invention
[0016] According to the first and second aspects of the present invention, it is possible to provide a powder that is excellent in ultraviolet light transmittance and visible light shielding properties. According to the third aspect of the present invention, it is possible to provide a black ultraviolet-curable organic composition that is excellent in ultraviolet light transmittance and visible light blocking properties. [Brief description of the drawings]
[0017] [Figure 1] 1 shows wavelength-extinction coefficient curves for five types of zirconium nitride powders having average particle sizes of 20 nm, 40 nm, 60 nm, 80 nm, and 100 nm calculated in Test Example 1. [Diagram 2] 1 shows a wavelength-extinction coefficient curve of a zirconium-containing nitride powder substituted with Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb, Tm, or Y+Dy, calculated in Test Example 2. [Diagram 3] This is a graph showing the relationship between particle size and the ratio (α550 / α365) of the extinction coefficient α550 of visible light having a wavelength of 550 nm to the extinction coefficient α365 of ultraviolet light having a wavelength of 365 nm in the zirconium nitride powder assumed in Test Example 1 and the zirconium-containing nitride powder substituted with Dy, Er, Ho, Tb, Tm or Y+Dy assumed in Test Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] A zirconium-containing nitride powder according to one embodiment of the present invention will be described below. The zirconium-containing nitride powder according to the present embodiment is a black powder used as a material for a black pattern constituting, for example, a black matrix of a color filter of a display or a light-shielding material in a CMOS camera module. The black pattern is formed, for example, by a photolithography method using a black ultraviolet-curable organic composition containing the zirconium-containing nitride powder according to the present embodiment and an ultraviolet-curable organic material.
[0019] (Zirconium-containing nitride powder) The zirconium-containing nitride powder of this embodiment has an average particle size in the range of 10 nm to 70 nm. Since the zirconium-containing nitride powder has an average particle size in this range and is fine, the plasma vibration of the zirconium-containing nitride particles due to visible light is not easily attenuated. This improves the shielding ability of visible light. In addition, since the particle size is sufficiently small compared to the wavelength of light, light scattering is unlikely to occur, so that the transmittance of ultraviolet light (i-line) with a wavelength of 365 nm, which is generally used in ultraviolet light exposure devices, is increased. However, if the average particle size of the zirconium-containing nitride powder becomes too small, the wavelength of the plasmon resonance becomes too short, and the position of the extinction coefficient peak in the visible light region may shift excessively to the short wavelength side. If the position of the extinction coefficient peak in the visible light region shifts excessively to the short wavelength side, the extinction coefficient of the visible light on the long wavelength side may decrease, and the shielding ability of the visible light on the long wavelength side may decrease. For this reason, the zirconium-containing nitride powder of this embodiment has an average particle size in the range of 10 nm to 70 nm. The zirconium-containing nitride powder preferably has an average particle size in the range of 20 nm to 70 nm, and particularly preferably in the range of 30 nm to 60 nm.
[0020] The average particle size of the zirconium-containing nitride powder is a BET diameter, and is measured by the following method. Nitrogen molecules are adsorbed onto the particle surface of the zirconium-containing nitride powder at the temperature of liquid nitrogen, and the adsorption isotherm (amount of adsorption) is measured. A BET plot is created, and the amount of nitrogen molecules adsorbed in a monolayer is calculated using the BET equation. The specific surface area of the zirconium-containing nitride powder particles is then calculated from the amount of nitrogen molecules adsorbed in a monolayer. Assuming that the particles of the zirconium-containing nitride powder are spherical, the BET diameter is calculated from the specific surface area (BET specific surface area) measured by the BET single-point method using the following equation. BET diameter = 6 / (density x BET specific surface area) The BET diameter in this specification was measured using Macsorb HM model-1210 manufactured by Mountech Co., Ltd.
[0021] The zirconium-containing nitride powder of the present embodiment has a composition represented by the following general formula (I). (Zr,X,Y)(N,O)···(I) In the above general formula (I), X represents at least one element selected from the group consisting of Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb and Tm. Y represents the element symbol of yttrium, and the content of Y is 0 moles or more per mole of the total content of Zr, X, and Y. N represents nitrogen. O represents oxygen, and the content of oxygen is 0 moles or more per mole of the total content of nitrogen and oxygen. In 1 mole of the zirconium-containing nitride powder, the total number of moles of Zr, X, and Y is the same as the total number of moles of N and O. General formula (I) represents the overall composition of the zirconium-containing nitride powder, which may be a single phase of nitride or oxynitride, or a mixture of nitride and oxide, oxynitride and oxide, nitride and oxynitride, or a mixture of nitride, oxynitride and oxide.
[0022] In the above general formula (I), all of the elements represented by X are group 3 elements. The element represented by X has the effect of shifting the wavelength showing the maximum peak of the extinction coefficient in the visible light region of the zirconium-containing nitride powder to the long wavelength side. The element represented by X may be used alone or in combination of two or more. Among the elements represented by X, Dy, Er, Ho, and Tm are preferred. The content of the element represented by X is preferably in the range of 0.05 mol to 0.30 mol, assuming that the total content of zirconium, the element represented by X, and yttrium is 1 mol. By the content of the element represented by X being within this range, the wavelength showing the maximum peak of the extinction coefficient in the visible light region can be maintained within the range of 540 nm to 600 nm. The content of the element represented by X is more preferably in the range of 0.07 mol to 0.25 mol, and particularly preferably in the range of 0.10 mol to 0.20 mol.
[0023] When the zirconium-containing nitride powder of the present embodiment does not contain yttrium, the composition is preferably represented by the following general formula (II). Zr1-a X a N 1-c O c (II) In the above general formula (II), X is the same as in the above general formula (I). a represents a number in the range of 0.05 to 0.30. a is more preferably in the range of 0.07 to 0.25, and particularly preferably in the range of 0.10 to 0.20. c is preferably in the range of 0 to 0.5, more preferably in the range of 0 to 0.45, and particularly preferably in the range of 0 to 0.4. The amount of metal elements (including Y, which will be described later) in the zirconium-containing nitride powder is measured by X-ray photoelectron spectroscopy. The amount of nitrogen in the zirconium-containing nitride powder is measured by an inert gas fusion-thermal conductivity method. The amount of oxygen in the zirconium-containing nitride powder (c in general formula (II)) is measured by a method conforming to JIS Z2613 "General rules for the determination of oxygen in metallic materials."
[0024] The zirconium-containing nitride powder of the present embodiment may further contain yttrium (Y). In this case, the composition of the zirconium-containing nitride powder is preferably represented by the following general formula (III). Zr 1-a-b X a Y b N 1-c O c (III) The total content of zirconium, the element represented by X, and Y is taken as 1 mole, and the content of Y (b in general formula (III)) is preferably in the range of 0.05 moles to 0.30 moles, more preferably in the range of 0.07 moles to 0.25 moles, and particularly preferably in the range of 0.10 moles to 0.20 moles. The numerical ranges of a and c in general formula (III) are the same as the numerical ranges of a and c in general formula (II).
[0025] The zirconium-containing nitride powder of this embodiment has an extinction coefficient α 365The extinction coefficient α of visible light with a wavelength of 550 nm 550 The ratio (α 550 / α 365 ) is set to be in the range of 1.4 to 100. 550 / α 365 By keeping the ratio (α) within this range, the transmittance of ultraviolet light and the shielding property of visible light are improved in a well-balanced manner. 550 / α 365 ) is more preferably in the range of 2 or more and 80 or less, and particularly preferably in the range of 2.5 or more and 60 or less.
[0026] Extinction coefficient α of visible light with a wavelength of 550 nm 550 is 600m -1 More than 700m is preferable. -1 More preferably, 750m or more. -1 It is particularly preferable that the dissipation coefficient α is equal to or greater than α. 550 is 1000m -1 It may be the following.
[0027] Extinction coefficient α of ultraviolet light with a wavelength of 365 nm 365 is 300m -1 Preferably less than 250m -1 It is more preferable that it is less than 200m. -1 It is particularly preferable that the extinction coefficient α 365 is 1m -1 It may be more than that.
[0028] The extinction coefficient is the rate at which the intensity of light passing through a dispersion containing a zirconium-containing nitride powder attenuates with distance due to scattering and absorption by zirconium-containing nitride particles in the dispersion. In this embodiment, the extinction coefficient of the zirconium-containing nitride powder is a value measured by the following method. A dispersion liquid containing zirconium-containing nitride powder at a mass concentration of 50 ppm is placed in a cell with an optical path length d (unit: m). Light is irradiated onto the cell containing this dispersion liquid, and the transmitted light intensity of the light that passes through the cell is measured. The optical path length d, the incident light intensity I0 of the light irradiated onto the cell, and the transmitted light intensity I of the light that passes through the cell are substituted into the following formula (1) to calculate α as the extinction coefficient of the light irradiated onto the cell. I = I0exp(-α × d) (1)
[0029] The zirconium-containing nitride powder of the present embodiment can be produced, for example, by the following first production method and second production method. <First manufacturing method> First, zirconium dioxide powder (raw oxide powder) containing an oxide of the X element (X element) represented by X in the general formula (I), an oxide powder of yttrium, and a zirconium dioxide (ZrO2) powder and an oxide of Y is prepared. As the zirconium dioxide powder, for example, powders such as monoclinic zirconium dioxide, cubic zirconium dioxide, and yttrium-stabilized zirconium dioxide can be used. Among these zirconium dioxide powders, monoclinic zirconium dioxide powder is preferred from the viewpoint of increasing the production rate of zirconium nitride powder. The zirconium dioxide powder preferably has an average primary particle size in the range of 10 nm to 500 nm. The reason why the average primary particle size of the zirconium dioxide powder is set to the above range is as follows. If it is less than 10 nm, the particle size of the zirconium-containing nitride obtained by the reaction may be too small, which may reduce the shielding ability of visible light. On the other hand, if it exceeds 500 nm, the particle size of the zirconium-containing nitride obtained by the reaction may be too large, which may reduce the shielding ability of visible light.
[0030] The X element oxide powder preferably has an average primary particle size of 10 nm or more and 500 nm or less. The reason why the average primary particle size of the X element oxide powder is set within the above range is as follows. If it is less than 10 nm, the particle size of the zirconium-containing nitride obtained by the reaction may be too small, which may reduce the visible light shielding ability. On the other hand, if it exceeds 500 nm, the particle size of the zirconium-containing nitride obtained by the reaction may be too large, which may reduce the visible light shielding ability. As the yttrium oxide powder, yttrium-stabilized zirconium dioxide and yttrium oxide (Y2O3) powder can be used. Yttrium-stabilized zirconium dioxide is also the zirconium dioxide powder mentioned above. The average primary particle size of the yttrium oxide powder is preferably 1000 nm or less, and more preferably 10 nm or more and 500 nm or less in terms of ease of handling of the powder. When producing a zirconium-containing nitride that does not contain yttrium, no yttrium oxide powder is added. The average primary particle size of the zirconium dioxide powder, the X element oxide powder, and the yttrium oxide powder is a converted value (BET diameter) calculated by converting the measured value of the specific surface area measured by the BET method into a spherical shape.
[0031] The zirconium dioxide powder (raw oxide powder) containing the above-mentioned X element oxide and Y oxide can be obtained, for example, by mixing an X element oxide powder, an yttrium oxide powder, and a zirconium dioxide powder. The zirconium dioxide powder containing the X element oxide and Y oxide can also be obtained by the following method. An aqueous solution containing an inorganic or organic salt of zirconium, an inorganic or organic salt of X element, and an inorganic or organic salt of yttrium is made alkaline to coprecipitate the hydroxide of X element, yttrium hydroxide, and zirconium hydroxide. The obtained coprecipitated product is collected, dried, and calcined.
[0032] Next, in a nitrogen-containing gas atmosphere, the zirconium dioxide powder (raw oxide powder) containing the above-mentioned X element oxide and Y oxide, magnesium oxide powder or magnesium nitride powder, or both, and metallic magnesium powder are mixed to prepare a mixed powder. As the nitrogen-containing gas, for example, N2 gas, a mixed gas of N2 and Ar, a mixed gas of N2 and H2, or a mixed gas of N2 and NH3 can be used.
[0033] Magnesium oxide powder and magnesium nitride powder have the effect of preventing sintering of zirconium nitride produced by firing the mixed powder. The average primary particle size of the magnesium oxide powder and magnesium nitride powder is preferably 1000 nm or less, and particularly preferably 500 nm or less and 10 nm or more from the viewpoint of ease of handling of the powder. The average primary particle size is a converted value calculated by converting the measured value of the specific surface area measured by the BET method into a spherical shape. The total amount of magnesium atoms in magnesium oxide and magnesium nitride is preferably in the range of 0.3 times mol to 3.0 times mol, more preferably in the range of 0.4 times mol to 2.0 times mol, relative to 1 mole of the total of zirconium, X element, and yttrium. The reason why the preferable amount of magnesium oxide and magnesium nitride to be added is within the above range is as follows. If it is less than 0.3 times mol, the effect of preventing sintering of the zirconium nitride powder may be insufficient. On the other hand, if it exceeds 3.0 times mol, the amount of acid solution required for acid washing after firing may increase.
[0034] The metallic magnesium powder has the effect of accelerating the reduction of the X element oxide, the yttrium oxide, and the zirconium dioxide, and facilitating the production of zirconium-containing nitride. If the metallic magnesium powder has a too small particle size, the reaction will proceed rapidly, increasing the danger of operation. For this reason, the metallic magnesium powder is preferably granular with a particle size of 100 μm to 1000 μm when passed through a sieve mesh, and particularly preferably granular with a particle size of 200 μm to 500 μm. However, the particle size of the metallic magnesium does not have to be within the above range, as long as 80% by mass or more, particularly 90% by mass or more of the particles are within the above range. If the amount of metallic magnesium added is too small, there is a risk that the reduction will be insufficient and the desired zirconium nitride powder will be difficult to obtain. On the other hand, if the amount is too large, the reaction temperature will rise rapidly due to the excess metallic magnesium, which may cause the powder grain growth and is uneconomical. The amount of metallic magnesium powder added is preferably 2.0 to 6.0 times the molar amount, more preferably 3.0 to 5.0 times the molar amount, relative to 1 mole of the total of zirconium, X element, and yttrium. The reason why the amount of metallic magnesium added is within the above range is as follows. If the amount is less than 2.0 times the molar amount, the reducing power of zirconium dioxide may be insufficient. On the other hand, if the amount is more than 6.0 times the molar amount, the reaction temperature may rise rapidly due to the excess metallic magnesium, which may cause grain growth of the powder and may be uneconomical.
[0035] Next, the mixed powder is fired in a nitrogen-containing gas atmosphere to reduce the X element oxide, the yttrium oxide, and the zirconium dioxide, thereby causing a nitriding reaction, thereby producing a zirconium-containing nitride powder. As the nitrogen-containing gas, for example, N2 gas, a mixed gas of N2 and Ar, a mixed gas of N2 and H2, or a mixed gas of N2 and NH3 can be used. N2 gas has a role of reacting with X element oxide, yttrium oxide, and zirconium dioxide to generate zirconium-containing nitride powder, and a role of preventing contact between metallic magnesium and zirconium-containing nitride powder and oxygen, thereby suppressing their oxidation. In addition, H2 gas or NH3 gas has a role of reducing zirconium dioxide together with metallic magnesium. The concentration of H2 gas in the mixed gas of N2 and H2 is preferably in the range of more than 0 volume% and less than 40 volume%, more preferably in the range of 10 volume% to 30 volume%. In addition, the concentration of NH3 gas in the mixed gas of N2 and NH3 is preferably in the range of more than 0 volume% and less than 50 volume%, more preferably in the range of 0 volume% to 40 volume%. By using this nitrogen-containing gas with reducing power, it is possible to produce zirconium nitride powder (zirconium-containing nitride) that does not contain low-order zirconium oxide or low-order zirconium oxynitride. On the other hand, if the concentration of H2 gas in the mixed gas of N2 and H2 and the concentration of NH3 gas in the mixed gas of N2 and NH3 become too high, the reduction proceeds but the nitrogen source becomes less, so there is a risk of low-order zirconium oxide or low-order zirconium oxynitride being produced. In addition, the maximum concentration (upper limit of the preferred concentration range) of NH3 gas is higher than that of H2 gas because NH3 gas contains nitrogen and has a higher ability to convert X element oxide and zirconium dioxide into nitrides than H2 gas.
[0036] The sintering temperature of the mixed powder is preferably in the range of 650°C to 900°C, more preferably in the range of 700°C to 800°C. The reason why the sintering temperature of the mixed powder is set to the above range is as follows. Since 650°C is the melting temperature of metallic magnesium, if the sintering temperature is lower than 650°C, the reduction of the X element oxide, the yttrium oxide, and the zirconium dioxide may not occur sufficiently. On the other hand, even if the sintering temperature is higher than 900°C, the effect is not increased, and there is a risk of wasting heat energy and of sintering of the generated zirconium-containing nitride particles proceeding. The sintering time of the mixed powder is preferably in the range of 30 minutes to 90 minutes, more preferably in the range of 30 minutes to 60 minutes. The reaction vessel for sintering the mixed powder is preferably one with a lid so that the raw materials and products do not scatter during the reaction. This is because when the melting of the metallic magnesium starts, the reduction of the X element oxide, the yttrium oxide, and the zirconium dioxide proceeds rapidly, and the temperature rises accordingly, causing the gas inside the vessel to expand, which may cause the contents inside the vessel to scatter to the outside.
[0037] Next, the zirconium-containing nitride powder obtained by the nitriding reaction is washed with an acid solution and then neutralized. Specifically, the zirconium-containing nitride powder obtained by the nitriding reaction is taken out of the reaction vessel and finally cooled to room temperature. Next, it is washed with an acid solution such as an aqueous hydrochloric acid solution. This removes magnesium oxide generated by oxidation of metallic magnesium, and magnesium oxide and magnesium nitride contained from the beginning of the reaction to prevent sintering of the product. This acid washing is preferably performed under conditions where the pH of the acid solution is 0.5 or more, particularly pH 1.0 or more, and the temperature of the acid solution is 90°C or less. This is because if the acidity of the acid solution becomes too strong or the liquid temperature becomes too high, zirconium, X element, and even yttrium in the zirconium-containing nitride powder may be eluted. After the acid washing, the pH is adjusted to 5 to 6 with ammonia water or the like to obtain a black slurry. Furthermore, the solid content is separated from this black slurry and dried to obtain a black material. Specifically, the black slurry is filtered or centrifuged to separate the solid content. The solid is dried and then pulverized to obtain a black material (black pigment, zirconium-containing nitride powder).
[0038] <Second manufacturing method> This manufacturing method is a method for manufacturing zirconium-containing nitride powder (black material) by a thermal plasma method. As an apparatus for carrying out the above-mentioned thermal plasma method, for example, a thermal plasma apparatus such as a high-frequency induction thermal plasma nanoparticle synthesis apparatus (manufactured by JEOL Ltd., TP40020NPS) can be mentioned. This thermal plasma apparatus is equipped with a raw material supplying machine that supplies raw materials to a plasma torch, a plasma torch that is connected to the raw material supplying machine and causes the raw materials to be subjected to a synthetic nitriding reaction by a thermal plasma method, an induction coil wound around the outer periphery of the plasma torch, a high-frequency power source that is electrically connected to the induction coil and supplies high-frequency power to the induction coil, a chamber connected to the plasma torch and through which a cooling gas such as N2 gas or Ar gas flows, and a bag filter connected to the chamber for collecting the zirconium-containing nitride powder.
[0039] To produce zirconium-containing nitride powder using the thermal plasma device, first, raw material metal powders including metallic zirconium powder, metallic powder of X element, and metallic yttrium powder are supplied to a raw material supplying device. When producing a zirconium-containing nitride that does not contain yttrium, a raw metal powder that does not contain metallic yttrium powder is used. The metal zirconium powder preferably has a purity of 98% or more and an average primary particle size of 30 μm or less. The reason why the average primary particle size of the metal zirconium powder is set to 30 μm or less is that it is easy to obtain a zirconium-containing nitride powder with high purity. On the other hand, if the average primary particle size exceeds 30 μm, the dissolution and gasification of the metal zirconium powder becomes insufficient, and the metal zirconium powder is recovered as a non-nitrided metal zirconium powder, and there is a risk that a zirconium-containing nitride powder exhibiting sufficient properties cannot be obtained.
[0040] The metal powder of the X element preferably has a purity of 98% or more and an average primary particle size of 1000 μm or less. The reason why the purity of the metal powder of the X element is set to 98% or more is that if the purity is less than 98%, the purity of the zirconium-containing nitride obtained may decrease and sufficient characteristics may not be obtained. The reason why the metal powder of the X element preferably has an average primary particle size of 1000 μm or less is that if the average primary particle size exceeds 1000 μm, it may be difficult to obtain a zirconium-containing nitride powder with a uniform composition. The metal yttrium powder preferably has a purity of 98% or more and an average primary particle size of 1 μm to 1000 μm. If the average primary particle size of the metal yttrium powder exceeds 1000 μm, it may be difficult to obtain a zirconium-containing nitride powder with a uniform composition. The average primary particle size of the metallic zirconium powder, the metallic powder of the X element, and the metallic yttrium powder is a particle size (volume-based median diameter (D50)) measured using a laser diffraction / scattering type particle size distribution measuring device (LA-950, manufactured by Horiba, Ltd.), and is the volume-based average primary particle size.
[0041] Next, the raw metal powder supplied to the raw material supplying machine is introduced into a plasma torch together with a carrier gas such as N2 gas or Ar gas. The inside of the plasma torch may be an N2 gas atmosphere, a mixed gas atmosphere of N2 and H2, a mixed gas atmosphere of N2 and Ar, or a mixed gas atmosphere of N2 and NH3. These N2-containing gases generate thermal plasma of N2 gas, thermal plasma of mixed gas of N2 and H2, thermal plasma of mixed gas of N2 and Ar, or thermal plasma (plasma flame) of mixed gas of N2 and NH3 by supplying high-frequency power from a high-frequency power source to an induction coil. Then, the raw metal powder introduced into the plasma torch is volatilized and gasified by the thermal plasma of high-temperature N2 gas of several thousand degrees generated in the plasma torch. That is, a synthetic nitriding reaction occurs by the thermal plasma method. Next, the gasified raw metal is quenched in a chamber where a cooling gas such as N2 gas or Ar gas flows. That is, it is instantly cooled and condensed by a cooling gas such as N2 gas or Ar gas in a chamber below the plasma torch. This produces zirconium-containing nitride powder. The produced zirconium-containing nitride powder is collected by a bag filter. In this way, the zirconium-containing nitride powder is obtained. The zirconium-containing nitride powder obtained as described above may be a nano-sized black material having an average primary particle size in the range of 10 nm to 50 nm. The average primary particle size of the black material (black pigment, zirconium-containing nitride powder) is a converted value (BET diameter) calculated by converting the measured value of the specific surface area measured by the BET method into a spherical shape.
[0042] According to the zirconium-containing nitride powder of the present embodiment configured as described above, since it has a composition represented by the above general formula (I) and contains a specific Group 3 element represented by X, the wavelength showing the maximum peak of the extinction coefficient in the visible light region can be set to a range of 540 nm to 600 nm. Therefore, it is possible to block visible light from the short wavelength side (for example, wavelength 400 nm) to the long wavelength side (for example, wavelength 800 nm). Therefore, the zirconium-containing nitride powder of the present embodiment has excellent ultraviolet light transmittance and visible light shielding properties. In addition, in the zirconium-containing nitride powder of the present embodiment, when the average particle size is in the range of 10 nm to 70 nm, the plasma oscillation of the zirconium-containing nitride particles due to visible light is unlikely to attenuate. Therefore, the visible light shielding properties are further improved. In addition, since the particle size is sufficiently small compared to the wavelength of light, light scattering is unlikely to occur, and therefore the transmittance of ultraviolet light with a wavelength of 365 nm is improved.
[0043] In addition, in the zirconium-containing nitride powder of this embodiment, the extinction coefficient α of ultraviolet light having a wavelength of 365 nm measured by the above method is 365 The extinction coefficient α of visible light with a wavelength of 550 nm 550 The ratio (α 550 / α 365 ) is in the range of 1.4 or more and 100 or less, the transmittance of ultraviolet light and the shielding ability of visible light are improved in a well-balanced manner. Therefore, by using the zirconium-containing nitride powder of this embodiment, a high-definition black pattern with excellent shielding ability of visible light can be formed. Furthermore, in the zirconium-containing nitride powder of this embodiment, the extinction coefficient of visible light at a wavelength of 550 nm is 600m -1 In the case where the zirconium-containing nitride powder is more than 100%, the visible light shielding property is further improved. Therefore, the black pattern formed by using the zirconium-containing nitride powder of the present embodiment is useful as a black matrix of a color filter of a display or a light shielding material in a CMOS camera module.
[0044] In the zirconium-containing nitride powder of this embodiment, the above ratio (α 550 / α 365) is within the range of 1.4 or more and 100 or less, the composition does not necessarily have to be the composition represented by the above general formula (I).
[0045] (Black UV curable organic composition) For example, black patterns are used as black matrices of image forming devices or light shielding materials in CMOS camera modules. The zirconium-containing nitride powder described above can be used as a raw material for the black ultraviolet-curable organic composition for forming the black patterns. The black ultraviolet-curable organic composition contains an ultraviolet-curable organic material and a black pigment dispersed in the ultraviolet-curable organic material. The zirconium-containing nitride powder is used as the black pigment. Examples of the ultraviolet-curing organic material that can be used include acrylic acid esters, methacrylic acid esters, glycidyl ethers, glycidyl amines, and glycidyl esters. Examples of the ultraviolet-curing organic material that can be used include monomers or oligomers that polymerize to form polymers when irradiated with ultraviolet light. Examples of these include acrylic monomers, acrylic oligomers, epoxy monomers, and epoxy oligomers. These organic materials may be used alone or in combination of two or more.
[0046] The acrylic monomer is a monomer having a (meth)acryloyl group. The (meth)acryloyl group includes an acryloyl group and a methacryloyl group. The acrylic monomer may be a monofunctional acrylic monomer having one (meth)acryl group in one molecule, or a polyfunctional acrylic monomer having two or more (meth)acryl groups in one molecule. Examples of monofunctional (meth)acrylic monomers include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, isoamyl acrylate, tetrahydrofurfuryl (meth)acrylate, and isobornyl (meth)acrylate. Examples of the difunctional (meth)acrylic monomer include 1,6 hexanediol di(meth)acrylate, 1,9 nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, ethylene oxide modified bisphenol A di(meth)acrylate, neopentyl triethylene glycol di(meth)acrylate, etc. Examples of the polyfunctional (meth)acrylic monomer include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.
[0047] The acrylic oligomer is a low molecular weight polymer obtained by polymerization of an acrylic monomer, and examples thereof include acrylic acrylate, urethane acrylate, epoxy acrylate, and polyester acrylate. The molecular weight of the acrylic oligomer may be, for example, within the range of 1000 to 10000 in number average molecular weight. These (meth)acrylate monomers and oligomers can be used alone or in combination of two or more. In addition, the (meth)acrylic monomers and oligomers are not limited to those described above, and generally available (meth)acrylic monomers and oligomers can be used.
[0048] The epoxy monomer has an epoxy group. The epoxy monomer may be a monofunctional epoxy monomer having one epoxy group in one molecule, or a multifunctional epoxy monomer having two or more epoxy groups in one molecule. Examples of the epoxy monomer include glycidyl ether and alicyclic epoxy.
[0049] The epoxy oligomer is a low molecular weight polymer formed by polymerization of an epoxy monomer. The molecular weight of the epoxy oligomer may be, for example, in the range of 1,000 to 10,000 in terms of number average molecular weight.
[0050] The black ultraviolet-curable organic composition may contain other ultraviolet-curable organic substances. Examples of the other ultraviolet-curable organic substances that can be used include styrene-based monomers, vinyl-based monomers, and cationic curable monomers. Examples of the styrene-based monomers include styrene, vinyl toluene, and divinyl benzene. Examples of the vinyl-based monomers include vinyl chloride and vinyl acetate. Examples of the cationic curable monomers include oxetane.
[0051] The black ultraviolet-curable organic composition may contain a photopolymerization initiator. The photopolymerization initiator is preferably a compound that can absorb ultraviolet light, specifically light with a wavelength of 100 to 400 nm, and initiate a polymerization reaction. As the photopolymerization initiator, for example, benzophenone, azobisisobutylether, benzoyl peroxide, bis(4-tert-butylphenyl)iodonium hexafluorophosphate, triphenylsulfonium tetrafluoroborate, tri-p-tolylsulfonium trifluoromethanesulfonate, etc. can be used.
[0052] The content of the ultraviolet-curable organic material is preferably in the range of 50% by mass to 90% by mass based on the solid content of the black ultraviolet-curable organic composition. By having the content of the ultraviolet-curable organic material in this range, the shielding property of the obtained black pattern tends to be improved. The content of the ultraviolet-curable organic material is more preferably in the range of 55% by mass to 85% by mass, and particularly preferably in the range of 60% by mass to 80% by mass. The content of the photopolymerization initiator is preferably within the range of 0.5% by mass to 15% by mass with respect to the ultraviolet-curable organic material. The content of the zirconium-containing nitride powder is preferably in the range of 0.1% by mass or more and 50% by mass or less based on the solid content of the black ultraviolet-curable organic composition. By having the content of the zirconium-containing nitride powder in this range, it is possible to improve the visible light shielding property and the ultraviolet light transmittance in a well-balanced manner. The lower limit of the content of the zirconium-containing nitride powder is preferably 5% by mass or more, preferably 10% by mass or more, and particularly preferably 20% by mass or more. The upper limit of the content of the zirconium-containing nitride powder is preferably 45% by mass or less, more preferably 40% by mass or less.
[0053] The black ultraviolet-curable organic composition may contain a solvent. Examples of the solvent that can be used include propylene glycol monomethyl ether acetate (PGM-Ac), ethanol, toluene, and water. The content of the solvent is preferably in the range of 0% by mass to 60% by mass with respect to the black ultraviolet-curable organic composition. When the content of the solvent is in this range, the coating property of the black ultraviolet-curable organic composition is improved, and the thickness of the photoresist film formed on the substrate tends to be uniform. The content of the solvent is more preferably in the range of 5% by mass to 50% by mass, and particularly preferably in the range of 10% by mass to 40% by mass.
[0054] The black ultraviolet-curable organic composition can be prepared, for example, by mixing a zirconium-containing nitride powder, an ultraviolet-curable organic material, and a solvent. The order of mixing may be to simultaneously mix the zirconium-containing nitride powder, the ultraviolet-curable organic material, and the solvent, to add the solvent to the mixture of the zirconium-containing nitride powder and the ultraviolet-curable organic material, to add the ultraviolet-curable organic material to the mixture of the zirconium-containing nitride powder and the solvent, or to add the zirconium-containing nitride powder to the mixture of the ultraviolet-curable organic material and the solvent and mix.
[0055] The black ultraviolet-curable organic composition having the above-mentioned structure contains the zirconium-containing nitride powder of the present embodiment, and therefore has excellent ultraviolet light transmittance and visible light shielding properties. Therefore, by using the above-mentioned black ultraviolet-curable organic composition, it is possible to form a high-definition black pattern by a photolithography method using ultraviolet light. The obtained black pattern has excellent visible light shielding properties.
[0056] (Method of forming black pattern) As a method for forming a black pattern using the above-mentioned black ultraviolet-curable organic composition, a photolithography method using ultraviolet light can be used. The method for forming a black pattern using the photolithography method includes, for example, a coating step, an exposure step, a cleaning step, and a heating step.
[0057] The coating step is a step of coating a black ultraviolet-curable organic composition on a substrate to form a photoresist film. When the black ultraviolet-curable organic composition contains a solvent, the black ultraviolet-curable organic composition may be coated and then heated to remove the solvent. As the substrate, for example, glass, silicon, polycarbonate, polyester, aromatic polyamide, polyamideimide, polyimide, etc. may be used. In addition, the substrate may be subjected to appropriate pretreatment such as chemical treatment with a silane coupling agent, plasma treatment, ion plating, sputtering, gas phase reaction method, vacuum deposition, etc., if desired. The coating method of the black ultraviolet-curable organic composition may be a spin coating method, a casting coating method, a roll coating method, a dipping method, etc. The thickness of the photoresist film is usually in the range of 0.1 μm to 10 μm, preferably in the range of 0.2 μm to 7.0 μm, and particularly preferably in the range of 0.5 μm to 6.0 μm.
[0058] The exposure process is a process in which the photoresist film is exposed to ultraviolet light in a pattern to create a pattern consisting of exposed cured parts and unexposed uncured parts. Methods for exposing the photoresist film to ultraviolet light in a pattern can include a method using a photomask and a method of irradiating ultraviolet light in a pattern. As the ultraviolet light, ultraviolet light (i-line) with a wavelength of 365 nm can be used.
[0059] The cleaning step is a step of removing the unexposed and uncured portion using a cleaning liquid. An alkaline aqueous solution can be used as the cleaning liquid. Examples of the cleaning method include immersion, shower cleaning, spray cleaning, and ultrasonic cleaning.
[0060] The heating step is a step of heating the cured portion after the cleaning step and drying to further harden the cured portion. The heating temperature is, for example, in the range of 100° C. to 300° C. In addition, if the cured portion formed by the exposure step has sufficient hardness, the heating step may be omitted.
[0061] The method for forming a black pattern configured as described above uses a black material containing the zirconium-containing nitride powder of the present embodiment, so that it is possible to form a high-definition black pattern. The obtained black pattern has excellent visible light shielding properties. EXAMPLES
[0062] [Test Example 1] Five types of zirconium nitride (ZrN) powder samples with particle sizes of 20 nm, 40 nm, 60 nm, 80 nm, and 100 nm were assumed. First-principles calculations were performed for each assumed zirconium-containing nitride particle to calculate the dielectric constant. Using the obtained dielectric constant, Mie scattering calculations were performed for each zirconium-containing nitride particle to calculate the extinction power Q ext The wavelength-extinction coefficient curves of the dispersions containing 50 mass ppm of each zirconium-containing nitride particle were then calculated. The results are shown in FIG. 1. The extinction coefficient α 365 The extinction coefficient α of visible light with a wavelength of 550 nm 550 The ratio (α 550 / α 365 ) is shown.
[0063] [Table 1]
[0064] From the wavelength-extinction coefficient curve in Figure 1, it can be seen that as the particle size of the zirconium nitride powder decreases from 100 nm to 40 nm, the maximum extinction coefficient value in the visible light region increases, and the maximum extinction coefficient value in the visible light region is almost the same for particle sizes of 40 nm and 20 nm. It can also be seen that as the particle size decreases, the wavelength showing the maximum peak of the extinction coefficient in the visible light region becomes shorter, and the extinction coefficient of visible light on the long wavelength side decreases. This is because the wavelength of plasmon resonance becomes shorter as the particle size decreases.
[0065] [Test Example 2] Zirconium-containing nitride (ZrN) in which one-eighth of the Zr atoms are replaced by another element X 0.875 X 0.125 The element X was assumed to be Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Sc, Ti, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Tc, Re, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Hg, Al, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, Sb, Bi, S, Se, Te, Po, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. In addition, zirconium-containing nitrides (ZrN), in which some of the Zr atoms in zirconium nitride (ZrN) are replaced with Y and Dy, were also considered. 0.875 Y 0.0625 Dy 0.0625 The particle sizes of the zirconium-containing nitride particles were set to five types: 20 nm, 40 nm, 60 nm, 80 nm, and 100 nm.
[0066] For each of the assumed zirconium-containing nitride particles, the wavelength-extinction coefficient curve was calculated in the same manner as in Test Example 1. As a result, it was found that the Group 3 elements Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb, Tm, and Y+Dy have the effect of shifting the wavelength showing the maximum peak of the extinction coefficient in the visible light region to the longer wavelength side. The wavelength-extinction coefficient curve of the zirconium-containing nitride (particle size: 100 nm) in which part of Zr is replaced with Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb, Tm, or Y+Dy is shown in FIG. 2. From the wavelength-extinction coefficient curve in FIG. 2, it can be seen that the zirconium-containing nitrides in which part of Zr is replaced by Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb, Tm, or Y+Dy all have a wavelength of 580 nm or more at which the extinction coefficient shows a maximum peak in the visible light region, and that the wavelength at which the extinction coefficient shows a maximum peak in the visible light region is shifted to the longer wavelength side compared to zirconium nitride.
[0067] From the results of the above Test Examples 1 and 2, it can be seen that by reducing the average particle size of the zirconium nitride powder and further substituting a portion of the Zr with a Group 3 element such as Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb, Tm, and Y+Dy, it is possible to obtain a zirconium-containing nitride powder that has excellent ultraviolet light transmittance and visible light shielding properties.
[0068] [Test Example 3] For the zirconium-containing nitride particles (particle diameters: 20 nm, 40 nm, 60 nm, 80 nm, and 100 nm) assumed in Test Example 2, the extinction coefficient α of ultraviolet light with a wavelength of 365 nm 365 The extinction coefficient α of visible light with a wavelength of 550 nm 550 The ratio (α 550 / α 365 The particle size and ratio (α 550 / α 365 ) is shown in FIG. 3 together with the results for the zirconium nitride (ZrN) powder obtained in Test Example 1.
[0069] In the graph of FIG. 3, the horizontal axis indicates particle size, and the vertical axis indicates the ratio (α 550 / α 365 ) is shown. From the results in FIG. 3, when the particle size is 70 nm or less, the ratio (α 550 / α 365 ) is larger than that of zirconium nitride powder.
[0070] [Example 1] Zirconium dioxide powder and dysprosium oxide powder were weighed out so that the molar ratio of zirconium to dysprosium was 0.875:0.125 and the total mass was 10 g. The weighed zirconium dioxide powder and dysprosium oxide powder were mixed uniformly using a mixer. 7.86 g of the obtained dysprosium oxide-containing zirconium oxide powder, 5.83 g of metallic magnesium powder, and 3.39 g of magnesium oxide powder were mixed in a nitrogen atmosphere to prepare a mixed powder. In the obtained mixed powder, the content of the metallic magnesium powder was 4.0 times the molar amount of the metal atom in the dysprosium oxide-containing zirconium oxide powder. In addition, the content of the magnesium atom in the magnesium oxide powder was 1.4 times the molar amount of the metal atom in the dysprosium oxide-containing zirconium oxide powder. The mixed powder was fired at a temperature of 700° C. for 60 minutes in a nitrogen gas atmosphere to obtain a fired product. The obtained fired product was dispersed in 1 liter of water, and 17.5% hydrochloric acid was gradually added to keep the pH at 1 or more and the temperature at 100°C or less to wash. Then, the pH was adjusted to 7-8 with 25% ammonia water and filtered. The filtered solid was redispersed in water at 400g / liter, and once again acid washed and pH adjusted with ammonia water in the same manner as above. Then, filtered. In this manner, acid washing-pH adjustment with ammonia water was repeated twice. Next, the filtered product was dispersed in ion-exchanged water at 500g / liter in terms of solid content, heated and stirred at 60°C, and adjusted to pH 7. Next, it was filtered with a suction filter, further washed with an equal amount of ion-exchanged water, and dried in a hot air dryer set at a temperature of 120°C. The X-ray diffraction pattern of the obtained dried powder was measured, and elemental analysis was performed using X-ray photoelectron spectroscopy (XPS). The amount of oxygen was also measured by a method conforming to JIS Z2613 "General rules for the determination of oxygen in metal materials". The nitrogen content was measured by the inert gas fusion-thermal conductivity method. As a result, it was confirmed that the obtained dry powder was a zirconium-containing nitride powder containing dysprosium represented by the general formula (II). The average particle size of the obtained zirconium-containing nitride powder was 50 nm.
[0071] [Example 2] Except for using erbium oxide powder, gadolinium oxide powder, holmium oxide powder, lutetium oxide powder, neodymium oxide powder, praseodymium oxide powder, scandium oxide powder, samarium oxide powder, terbium oxide powder, and thulium oxide powder instead of dysprosium oxide powder, zirconium-containing nitride powders were produced in the same manner as in Invention Example 1. The obtained zirconium-containing nitride powders contained the Group 3 elements used, respectively. [Industrial Applicability]
[0072] The zirconium-containing nitride powder of the present embodiment has excellent ultraviolet light transmittance and visible light shielding properties, and is therefore suitable for use as a material for the black pattern constituting the black matrix of a color filter for a display or a light shielding material in a CMOS camera module.
Claims
1. A zirconium-containing nitride powder for use as an insulating black pigment having ultraviolet light transmittance, comprising: A zirconium-containing nitride powder having a composition represented by the following general formula (I) and an average particle size in the range of 10 nm to 70 nm. (Zr,X,Y)(N,O)...(I) In the above general formula (I), X represents at least one element selected from the group consisting of Dy, Er, Gd, Ho, Lu, Nd, Pr, Sc, Sm, Tb, and Tm, Y represents the atomic symbol of yttrium, the content of X is in the range of 0.05 mol or more and 0.30 mol or less per mol of the total content of Zr, X, and Y, the content of Y is 0 mol or more, N represents nitrogen, O represents oxygen, and the content of oxygen is 0 mol or more per mol of the total content of nitrogen and oxygen.
2. 2. The zirconium-containing nitride powder according to claim 1, wherein the ratio of the extinction coefficient of visible light having a wavelength of 550 nm to the extinction coefficient of ultraviolet light having a wavelength of 365 nm, as measured by the following method, is in the range of 1.4 or more and 100 or less. (Method of measuring extinction coefficient) A dispersion containing zirconium-containing nitride powder at a mass concentration of 50 ppm is placed in a cell having an optical path length d (unit: m). A cell containing a dispersion liquid is irradiated with light, and the intensity of the light transmitted through the cell is measured. The optical path length d, the incident light intensity I0 of the light irradiated to the cell, and the transmitted light intensity I of the light transmitted through the cell are substituted into the following formula (1) to calculate α as the extinction coefficient of the light irradiated to the cell. I=I 0 exp(-α×d)・・・(1)
3. The extinction coefficient of visible light with a wavelength of 550 nm is 600 m -1 The zirconium-containing nitride powder according to claim 2 .
4. The ink includes an ultraviolet-curable organic material and a black pigment dispersed in the ultraviolet-curable organic material, A black ultraviolet-curable organic composition, wherein the black pigment is the zirconium-containing nitride powder according to any one of claims 1 to 3.
5. 5. The black ultraviolet-curable organic composition according to claim 4, wherein the ultraviolet-curable organic material is at least one organic material selected from the group consisting of acrylic monomers, acrylic oligomers, epoxy monomers, and epoxy oligomers.
Citation Information
Patent Citations
Cubic zirconium nitride powder based on low-temperature reduction and preparation method of cubic zirconium nitride powder
CN107777673A
Zirconium nitride powder and manufacturing method therefor
JP2018203599A
Powder for forming black light-shielding film and manufacturing method therefor
JP2019112275A
Colored resin composition, colored film, color filter and liquid crystal display device
WO2019059359A1
Composite particles and method for producing composite particles
WO2019124100A1