Method for manufacturing a polarizing plate with a retardation layer
By humidifying and storing an intermediate laminate with a water-absorbing film, the method addresses warping issues in thin polarizing plates with retardation layers, ensuring their suitability for flexible image display devices.
Patent Information
- Application Number
- JP2020187767
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-11
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-11-11
AI Technical Summary
Thin polarizing plates with retardation layers are prone to warping, particularly those with a protective layer on one side and a liquid crystal alignment solidified layer on the other, which complicates their use in flexible image display devices.
A manufacturing method involving humidification and storage of an intermediate laminate with a water-absorbing film temporarily attached to the retardation layer side, followed by peeling off the film, to control moisture content and reduce warping.
The method effectively suppresses warping in polarizing plates with retardation layers, enabling their use in curved, bent, or wound applications without significant deformation.
Smart Images

Figure 00000015_0000 
Figure 00000015_0001 
Figure 00000015_0002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polarizing plate with a retardation layer. [Background technology]
[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (for example, organic EL display devices and inorganic EL display devices), are rapidly becoming widespread. In image display devices, a polarizing plate and a retardation plate are typically used. In practice, a retardation layer-attached polarizing plate in which a polarizing plate and a retardation plate are integrated is widely used (for example, Patent Document 1). In recent years, the possibility of bending, bending, folding, and rolling up image display devices has been considered, and there is a demand for thinner image display devices. Accordingly, there is also a demand for thinner retardation layer-attached polarizing plates. However, there is a problem that thin retardation layer-attached polarizing plates are prone to warping. In particular, the problem of warping is prominent in a retardation layer-attached polarizing plate that has a protective layer with low moisture permeability only on one side of the polarizer and includes a retardation layer that is an oriented and solidified layer of a liquid crystal compound. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3325560 Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide a simple and efficient method for producing a retardation layer-attached polarizing plate in which warping is suppressed. [Means for solving the problem]
[0005] According to an embodiment of the present invention, there is provided a method for producing a polarizing plate with a retardation layer, the polarizing plate having a polarizer, a protective layer disposed on one side of the polarizer, and a retardation layer disposed on the other side of the polarizer. The method includes: humidifying an intermediate laminate having a water-absorbing film temporarily attached to the retardation layer side of the polarizing plate with a retardation layer while transporting it with a roll; storing the humidified intermediate laminate for 12 hours or more; and setting the moisture permeability of the protective layer at 40° C. and 92% RH to 100 g / m 2 24h or less, and the retardation layer is a layer in which a liquid crystal compound is aligned and solidified. In one embodiment, the water-absorbent film has a water absorption rate of 2% or more. In one embodiment, the water-absorbent film is a triacetyl cellulose film. In one embodiment, the water-absorbent film has a thickness of 40 μm or more. In one embodiment, the water-absorbent film has a moisture permeability of 300 g / m at 40° C. and 92% RH. 2 -24 hours or more. In one embodiment, the humidification treatment is performed at a temperature of 34° C. or less and a water vapor amount of 13.8 g / m 3 The humidification is carried out under the above-mentioned environment. In one embodiment, the humidification time in the humidification treatment is 5 minutes or more. In one embodiment, the storage time of the humidified intermediate laminate is 24 hours or more. In one embodiment, the storage of the humidified intermediate laminate is performed in an environment at a temperature of 34° C. or lower. In one embodiment, the manufacturing method further comprises peeling and removing the water-absorbent film from the intermediate laminate after the storage. In one embodiment, the retardation layer has a moisture permeability of 300 g / m at 40° C. and 92% RH. 2 -24 hours or more. In one embodiment, the retardation layer is a single layer, the retardation layer has Re(550) of 100 nm to 190 nm, the retardation layer has Re(450) / Re(550) of 0.8 or more and less than 1, and the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is 40° to 50°. In one embodiment, the retardation layer-attached polarizing plate further has another retardation layer on the outer side of the retardation layer, and the refractive index characteristics of the another retardation layer satisfy the relationship nz>nx=ny. In one embodiment, the retardation layer has a laminated structure of a first liquid crystal compound alignment layer and a second liquid crystal compound alignment layer; the first liquid crystal compound alignment layer has a Re(550) of 200 nm to 300 nm, and the angle between the slow axis and the absorption axis of the polarizer is 10° to 20°; the second liquid crystal compound alignment layer has a Re(550) of 100 nm to 190 nm, and the angle between the slow axis and the absorption axis of the polarizer is 70° to 80°. In one embodiment, the retardation layer-attached polarizing plate has a total thickness of 45 μm or less. Effect of the Invention
[0006] According to an embodiment of the present invention, in a method for manufacturing a polarizing plate with a retardation layer, an intermediate laminate to which a predetermined water-absorbent film is temporarily attached is subjected to a predetermined humidification treatment, and the humidified intermediate laminate is stored for a predetermined period of time, thereby making it possible to simply and efficiently manufacture a polarizing plate with a retardation layer having reduced warping. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view showing an example of a retardation layer-attached polarizing plate obtained by a production method according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing another example of a retardation layer-attached polarizing plate obtained by a manufacturing method according to an embodiment of the present invention. [Diagram 3] 1 is a conceptual diagram for explaining a manufacturing method according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°.
[0010] A. Outline of the structure of a retardation layer-attached polarizing plate obtained by the manufacturing method according to an embodiment of the present invention FIG. 1 is a schematic cross-sectional view showing an example of a retardation layer-attached polarizing plate obtained by a manufacturing method according to an embodiment of the present invention. The retardation layer-attached polarizing plate 100 in the illustrated example has a polarizer 11, a protective layer 12 arranged on one side (typically, the viewing side) of the polarizer 11, and a retardation layer 20 arranged on the other side of the polarizer 11. That is, the retardation layer-attached polarizing plate 100 has the protective layer 12 only on the viewing side (opposite side to the retardation layer 20) of the polarizer 11. In such a retardation layer-attached polarizing plate, the effect according to the embodiment of the present invention (described later) can be remarkable. For practical purposes, a pressure-sensitive adhesive layer (not shown) is provided on the opposite side of the retardation layer 20 to the polarizer 11 (i.e., as the outermost layer on the opposite side to the viewing side), so that the retardation layer-attached polarizing plate can be attached to an image display panel. Furthermore, it is preferable that a release film (not shown) is temporarily attached to the surface of the pressure-sensitive adhesive layer until the retardation layer-attached polarizing plate is used. By temporarily attaching the release film, the pressure-sensitive adhesive layer is protected and the retardation layer-attached polarizing plate can be rolled. In this specification, a laminate of a polarizer and a protective layer may be referred to as a polarizing plate.
[0011] In the embodiment of the present invention, the moisture permeability of the protective layer 12 at 40° C. and 92% RH (hereinafter simply referred to as moisture permeability) is 100 g / m 2 In a retardation layer-attached polarizing plate having such a moisture-permeable protective layer on only one side of a polarizer, the effects of the embodiment of the present invention (described later) can be remarkable. The moisture permeability of the protective layer is preferably 80 g / m 2 - 24h or less, preferably 60g / m 2 The lower limit of the moisture permeability is, for example, 5 g / m 2 · It can be 24h.
[0012] In the embodiment of the present invention, the retardation layer 20 is an alignment solidified layer of a liquid crystal compound (liquid crystal alignment solidified layer). By using a liquid crystal compound, the difference between nx and ny of the obtained retardation layer can be significantly increased compared to non-liquid crystal materials, so that the thickness of the retardation layer for obtaining a desired in-plane retardation can be significantly reduced. Therefore, a remarkable thinning of the retardation layer-attached polarizing plate can be realized. In such a retardation layer-attached polarizing plate, the effect of the embodiment of the present invention (described later) can be remarkable. In this specification, the "alignment solidified layer" refers to a layer in which the liquid crystal compound is aligned in a predetermined direction in the layer and the alignment state is fixed. Note that the "alignment solidified layer" is a concept that includes an alignment solidified layer obtained by hardening a liquid crystal monomer as described later. In the retardation layer 20, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the retardation layer (homogeneous alignment). The retardation layer 20 may be a single layer as shown in FIG. 1, or may have a laminated structure of two or more layers as shown in FIG. 2.
[0013] The moisture permeability of the retardation layer is preferably 300 g / m 2 - 24h or more, preferably 300g / m 2 24h~1000g / m 2 24h, and more preferably 400g / m 2 24h~800g / m 2 The difference between the moisture permeability of the protective layer and the moisture permeability of the retardation layer is preferably 200 g / m 2 - 24h or more, preferably 250g / m 2 24h~750g / m 2 -24 hours.
[0014] The total thickness of the retardation layer-attached polarizing plate (the total thickness of the polarizer, protective layer, retardation layer, and adhesive layer for laminating these) is preferably 45 μm or less, more preferably 40 μm or less, and even more preferably 35 μm or less. The total thickness of the retardation layer-attached polarizing plate can be, for example, 25 μm or more. Furthermore, in the retardation layer-attached polarizing plate, the ratio of the thickness of the polarizing plate (polarizer and protective layer) to the thickness of the retardation layer (polarizing plate / retardation layer: hereinafter, sometimes simply referred to as "thickness ratio") is preferably 5 or more, more preferably 5 to 16, and even more preferably 5 to 14. Such a thickness ratio can be realized by having a protective layer only on one side of the polarizer, the retardation layer being an alignment solidification layer of a liquid crystal compound, and the polarizer being thin as described later.
[0015] The retardation layer-attached polarizing plate may further include other optical functional layers. The type, characteristics, number, combination, arrangement position, etc. of the optical functional layers that can be provided in the retardation layer-attached polarizing plate may be appropriately set according to the purpose. For example, the retardation layer-attached polarizing plate may further have a conductive layer or a conductive layer-attached isotropic substrate (both are not shown). The conductive layer or the conductive layer-attached isotropic substrate is typically provided on the outside of the retardation layer 20 (opposite side to the polarizing plate 10). The conductive layer or the conductive layer-attached isotropic substrate is typically an arbitrary layer that is provided as necessary, and may be omitted. In addition, when the conductive layer or the conductive layer-attached isotropic substrate is provided, the retardation layer-attached polarizing plate may be applied to a so-called inner touch panel type input display device in which a touch sensor is incorporated between an image display cell (for example, an organic EL cell) and a polarizing plate. In addition, for example, the retardation layer-attached polarizing plate may further include other retardation layers. Other optical properties of the retardation layer (e.g., refractive index properties, in-plane retardation, Nz coefficient, photoelastic coefficient), thickness, arrangement position, etc. may be appropriately set depending on the purpose. Additionally / alternatively, a layer (typically, a λ / 4 plate imparting (elliptical) polarizing function, an ultra-high retardation layer) that improves visibility when viewed through polarized sunglasses may be provided on the surface of the protective layer 12 as necessary. With such a configuration, excellent visibility can be achieved even when the display screen is viewed through polarized lenses such as polarized sunglasses. Therefore, the polarizing plate with a retardation layer can be suitably applied to image display devices that can be used outdoors.
[0016] Hereinafter, a method for producing the above-mentioned polarizing plate with a retardation layer according to an embodiment of the present invention will be described, and then components of the polarizing plate with a retardation layer will be described.
[0017] B. Method for manufacturing a polarizing plate with a retardation layer The method for producing a polarizing plate with a retardation layer according to an embodiment of the present invention includes: humidifying an intermediate laminate having a water-absorbing film temporarily attached to the retardation layer side of the polarizing plate with a retardation layer while transporting it by a roll; and storing the humidified intermediate laminate for 12 hours or more. Each step in the method for producing a polarizing plate with a retardation layer will be described below in order.
[0018] B-1. Preparation of polarizing plate The polarizing plate may be produced by any suitable method. Specifically, the polarizing plate may include a polarizer produced from a single-layer resin film, or may include a polarizer produced using a laminate of two or more layers.
[0019] B-1-1. Preparation of a polarizing plate using a polarizer obtained from a single layer of resin film The method for producing a polarizer from a single-layer resin film typically includes subjecting the resin film to a dyeing treatment using a dichroic substance such as iodine or a dichroic dye, and a stretching treatment. Examples of the resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA)-based films, partially formalized PVA-based films, and partially saponified ethylene-vinyl acetate copolymer-based films. The method may further include an insolubilization treatment, a swelling treatment, a crosslinking treatment, and the like. A polarizing plate can be obtained by laminating a protective layer (protective film) on at least one side of the obtained polarizer. Such a production method is well known and commonly used in the art, and therefore a detailed description thereof will be omitted.
[0020] B-1-2. Preparation of a polarizing plate using a polarizer obtained from a laminate When a laminate is used to manufacture a polarizer, the laminate may be a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. As an example, a method for manufacturing a polarizer using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate will be described. The manufacturing method typically includes: applying a PVA-based resin solution to a resin substrate and drying the substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; and stretching and dyeing the laminate to make the PVA-based resin layer into a polarizer. In such a manufacturing method, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch the laminate. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (e.g., 95°C or higher) before stretching in the aqueous boric acid solution. In addition, in such a manufacturing method, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, the manufacturing method includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of the PVA, and to achieve high optical properties. At the same time, by increasing the orientation of the PVA in advance, problems such as a decrease in the orientation or dissolution of the PVA when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and the decrease in the orientation of the polyvinyl alcohol molecules can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained through a treatment process in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction by the drying shrinkage treatment.The obtained laminate of resin substrate / polarizer may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the laminate of resin substrate / polarizer, and any suitable protective layer may be laminated on the peeled surface depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.
[0021] B-2. Formation of retardation layer A method for forming a retardation layer (liquid crystal alignment solidified layer) will be briefly described. The liquid crystal alignment solidified layer can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. Any appropriate alignment treatment can be adopted as the alignment treatment. Specifically, mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment can be mentioned. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique deposition method and photoalignment treatment. As the treatment conditions of various alignment treatments, any appropriate conditions can be adopted according to the purpose.
[0022] The alignment of the liquid crystal compound is performed by treating the liquid crystal compound at a temperature at which the liquid crystal compound exhibits a liquid crystal phase according to the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compound takes on a liquid crystal state and is aligned according to the alignment treatment direction of the substrate surface.
[0023] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is a polymerizable monomer or a crosslinkable monomer, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.
[0024] Specific examples of the liquid crystal compound and details of the method for forming the alignment solidified layer are described in JP-A-2006-163343, the disclosure of which is incorporated herein by reference.
[0025] In this manner, a liquid crystal alignment and solidification layer is formed on the substrate.
[0026] B-3. Preparation of polarizing plate with retardation layer A polarizing plate with a retardation layer can be obtained by laminating the polarizing plate and the retardation layer obtained above. The polarizing plate and the retardation layer are typically laminated while being transported by rolls (that is, by so-called roll-to-roll). The lamination can typically be performed by transferring a liquid crystal alignment solidified layer formed on a substrate. When the retardation layer has a laminated structure, each retardation layer may be laminated (transferred) sequentially onto the polarizing plate, or a laminate of the retardation layers may be laminated (transferred) onto the polarizing plate. The transfer is typically performed via an active energy ray curable adhesive. The thickness of the active energy ray curable adhesive after curing is preferably 0.4 μm or more, more preferably 0.4 μm to 3.0 μm, and even more preferably 0.6 μm to 1.5 μm.
[0027] When the retardation layer-attached polarizing plate further includes other optically functional layers (for example, a conductive layer, another retardation layer), these optically functional layers can be laminated or formed at predetermined positions by any appropriate method.
[0028] The production (lamination) of a polarizing plate with a retardation layer is typically performed at a water vapor concentration of 11.5 g / m 3 The lamination is carried out under the following conditions: The amount of water vapor during lamination is preferably 6.0 g / m 3 ~11.5g / m 3 and more preferably 8.0 g / m 3 ~11.5g / m 3By performing lamination under an environment in which the amount of water vapor is in this range, the effect of the humidification treatment described below becomes significant. Such an amount of water vapor in lamination can be realized, for example, by changing the relative humidity according to the temperature in the range of 18°C to 25°C. For example, when the temperature is 18°C, the amount of water vapor can be realized by setting the relative humidity to 65% RH or less; for example, when the temperature is 20°C, the amount of water vapor can be realized by setting the relative humidity to 55% RH or less; and for example, when the temperature is 23°C, the amount of water vapor can be realized by setting the relative humidity to 45% RH or less. The lower limit of the relative humidity can be, for example, 30% RH.
[0029] B-4. Preparation of intermediate laminate Next, as shown in Fig. 3, a water-absorbing film 150 is temporarily attached to the retardation layer side of the retardation layer-attached polarizing plate obtained above to prepare an intermediate laminate 200. The intermediate laminate is prepared by roll-to-roll method as described above. The retardation layer-attached polarizing plate at the time of preparing the intermediate laminate has the same layer structure as the retardation layer-attached polarizing plate finally obtained, but is essentially an intermediate body. In Fig. 3, the intermediate body corresponding to the retardation layer-attached polarizing plate 100 in Fig. 1 is indicated by reference numeral 100', and the intermediate body corresponding to the retardation layer-attached polarizing plate 101 in Fig. 2 is indicated by reference numeral 101'.
[0030] The water absorption rate of the water-absorbing film is preferably 2% or more, more preferably 2% to 20%, and further preferably 2% to 10%. If the water absorption rate of the water-absorbing film is in such a range, the amount of moisture that can reach the polarizer can be adjusted to an appropriate range by the humidification treatment and storage after the humidification treatment (both described later). More specifically, the water-absorbing film can absorb an appropriate amount of moisture by the humidification treatment and retain a predetermined amount of the absorbed moisture. The moisture retained in the water-absorbing film can transfer to the polarizer during storage. Therefore, the moisture amount of the polarizer can be set to an appropriate range by appropriately setting the conditions of the humidification treatment to adjust the amount of moisture absorbed and retained in the water-absorbing film, and appropriately adjusting the storage conditions to adjust the amount of moisture transferred from the water-absorbing film to the polarizer. As a result, the warping of the retardation layer-attached polarizing plate can be significantly suppressed. If the water absorption rate is too low, the suppression of warping may be insufficient. If the water absorption rate is too high, warping may occur in the reverse direction and / or in a direction perpendicular to the initial direction in the plane. More specifically, if the humidification treatment is not performed, the polarizing plate with a retardation layer typically has a convex warp on the protective layer side. On the other hand, if the humidification treatment is performed, a convex warp is generated on the retardation layer side. As a result, the warps in the opposite directions are offset, and the warp can be suppressed in the obtained polarizing plate with a retardation layer. Therefore, if the water absorption rate is too high, the convex warp on the retardation layer side becomes too large, and the obtained polarizing plate with a retardation layer may have a warp in the opposite direction (convex on the protective layer side) and / or in a direction perpendicular to the initial direction in the plane.
[0031] The water-absorbent film may be made of any suitable material as long as it has the desired water absorption rate. Examples of materials constituting the water-absorbent film include triacetyl cellulose (TAC) and acrylic resins. TAC is preferred.
[0032] The thickness of the water-absorbing film is preferably 40 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more. The upper limit of the thickness of the water-absorbing film can be, for example, 200 μm. If the thickness of the water-absorbing film is in this range, the amount of moisture that can reach the polarizer during the humidification treatment can be adjusted to an appropriate range due to the synergistic effect with the effect of setting the water absorption rate within a predetermined range, and therefore, the moisture amount of the polarizer can be set to an appropriate range by storage after the humidification treatment. As a result, the warping of the retardation layer-attached polarizing plate can be significantly suppressed.
[0033] The moisture permeability of the water-absorbent film is preferably 300 g / m 2 - 24h or more, preferably 300g / m 2 24h~1000g / m 2 24h, and more preferably 300g / m 2 24h~800g / m 2 24h. If the moisture permeability of the water-absorbing film is within this range, an appropriate amount of the moisture absorbed in the water-absorbing film by the humidification treatment and retained in the water-absorbing film can be transferred to the polarizer by storage after the humidification treatment. Therefore, the moisture content of the polarizer can be set to an appropriate range by storage after the humidification treatment. As a result, warping of the retardation layer-attached polarizing plate can be significantly suppressed.
[0034] The preparation (lamination) of the intermediate laminate can be typically carried out under the same environment as that for the preparation (lamination) of a retardation layer-attached polarizing plate.
[0035] B-5. Humidification treatment The intermediate laminate 200 obtained above is subjected to a humidification treatment, as shown in Fig. 3. The humidification treatment is typically performed while the intermediate laminate is being transported with rolls. The humidification treatment is typically performed at a temperature of 34°C or less and a water vapor amount of 13.8 g / m 3 The humidification treatment is carried out under the above-mentioned conditions. The temperature in the humidification treatment is preferably 18°C to 34°C. The amount of water vapor in the humidification treatment is preferably 13.8 g / m 3 ~30g / m 3 and more preferably 13.8 g / m3 ~24g / m 3 Such a water vapor amount in the humidification treatment can be realized, for example, when the temperature is 20°C, by setting the relative humidity to 80%RH or more; for example, when the temperature is 23°C, by setting the relative humidity to 70%RH or more; for example, when the temperature is 25°C, by setting the relative humidity to 60%RH or more; for example, when the temperature is 28°C, by setting the relative humidity to be greater than 50%RH. The upper limit of the relative humidity can be, for example, 100%RH. By carrying out the humidification treatment under such conditions, an appropriate amount of moisture is given to the retardation layer-attached polarizing plate, and the warping of the retardation layer-attached polarizing plate can be suppressed by the synergistic effect with the effect of temporarily attaching the water-absorbing film.
[0036] The humidification time in the humidification treatment is preferably 5 minutes or more, more preferably 5 to 30 minutes, even more preferably 5 to 20 minutes, and particularly preferably 5 to 15 minutes. If the humidification time is 5 minutes or more, the desired amount of water absorption can be achieved. Even if the humidification time is excessively long, the effect will not change, so the upper limit of the humidification time can be determined by balancing the desired amount of water absorption and production efficiency.
[0037] The humidification treatment is carried out so that the weight per unit volume of the retardation layer-attached polarizing plate increases by, for example, 0.2% or more. The weight increase per unit volume of the retardation layer-attached polarizing plate in the humidification treatment is preferably 0.2% to 2.5%, more preferably 0.3% to 2.0%, and even more preferably 0.3% to 1.0%. The weight increase in the humidification treatment means that the retardation layer-attached polarizing plate has absorbed moisture, so by setting the weight increase amount within this range, the polarizer can absorb a desired amount of moisture. As a result, the warping of the retardation layer-attached polarizing plate can be suppressed.
[0038] B-6.Storage The intermediate laminate subjected to the humidification treatment is stored as shown in FIG. 3. Typically, the intermediate laminate is wound into a roll and stored in the rolled state. By storing in this manner, the moisture imparted to the intermediate laminate (substantially a water-absorbing film) by the humidification treatment can be transferred well to the polarizer. This increases the moisture content of the polarizer, and as a result, the warping of the retardation layer-attached polarizing plate can be suppressed. The storage time is 12 hours or more as described above, preferably 16 hours or more, more preferably 24 hours or more, and even more preferably 30 hours or more. Since the effect does not change even if the storage time is excessively long, the upper limit of the storage time can be determined by balancing the desired amount of moisture absorption and production efficiency.
[0039] Typically, storage is performed at around room temperature. The storage temperature is typically 34° C. or lower, preferably 30° C. or lower, more preferably 20° C. to 30° C., and further preferably 23° C. to 27° C. If the storage temperature is too high, moisture imparted (absorbed) to the retardation layer-attached polarizing plate by the humidification treatment evaporates to the outside, and may not be transferred well to the polarizer.
[0040] Storage is typically at a water vapor content of 11.5 g / m 3 The storage is performed under the following environment. In other words, the storage is performed without substantially humidifying the intermediate laminate. By storing in such an environment, moisture can be effectively transferred from the water-absorbing film to the polarizer.
[0041] After storage, the water-absorbing film is peeled off and removed from the intermediate laminate, as shown in Fig. 3. In this manner, a polarizing plate with a retardation layer can be obtained.
[0042] C. Polarizing plate C-1.Polarizer As is clear from the above manufacturing method, the polarizer 11 is typically a resin film containing a dichroic material (e.g., iodine). As described above, examples of the resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA)-based films, partially formalized PVA-based films, and partially saponified ethylene-vinyl acetate copolymer-based films.
[0043] The thickness of the polarizer is preferably 15 μm or less, more preferably 1 μm to 12 μm, and further preferably 3 μm to 12 μm. When the thickness of the polarizer is within this range, the desired amount of moisture can be absorbed satisfactorily by the above-mentioned humidification treatment.
[0044] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is, for example, 41.5% to 46.0%, preferably 42.0% to 46.0%, and preferably 44.5% to 46.0%. The degree of polarization of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.
[0045] C-2.Protective layer The protective layer 12 is formed of any appropriate film that can be used as a protective layer for a polarizer as long as it has the moisture permeability described above. Specific examples of materials that are the main components of the film include transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, cyclic olefins (e.g., polynorbornene), polyolefins, (meth)acrylics, and acetates. Preferably, the protective layer 12 can be composed of a cyclic olefin (e.g., polynorbornene) resin film.
[0046] The retardation layer-attached polarizing plate obtained by the manufacturing method according to the embodiment of the present invention is typically disposed on the viewing side of an image display device, and the protective layer 12 is disposed on the viewing side. Therefore, the protective layer 12 may be subjected to surface treatment such as hard coat treatment, anti-reflection treatment, anti-sticking treatment, and anti-glare treatment, as necessary.
[0047] The thickness of the protective layer 12 is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 15 μm to 35 μm. When a surface treatment is applied, the thickness of the protective layer 12 includes the thickness of the surface treatment layer.
[0048] D. Retardation layer As described above, the retardation layer 20 may be a single layer or may have a laminated structure of two or more layers.
[0049] When the retardation layer 20 is a single layer, the retardation layer may function as a λ / 4 plate in one embodiment. Specifically, the Re(550) of the retardation layer is preferably 100 nm to 180 nm, more preferably 110 nm to 170 nm, and further preferably 110 nm to 160 nm. The thickness of the retardation layer may be adjusted so as to obtain a desired in-plane retardation of the λ / 4 plate. The thickness of the retardation layer may be, for example, 1.0 μm to 2.5 μm. In this embodiment, the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is preferably 40° to 50°, more preferably 42° to 48°, and further preferably 44° to 46°. When the retardation layer is a single layer, the retardation layer preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. In this embodiment, the retardation layer-attached polarizing plate may further have another retardation layer (not shown) exhibiting refractive index characteristics of nz>nx=ny on the outer side of the retardation layer 20 (opposite side to the polarizer).
[0050] When the retardation layer 20 has a laminated structure, the retardation layer typically has a two-layer structure of an H layer 21 and a Q layer 22 in this order from the polarizing plate side, as shown in FIG. 2. The H layer typically functions as a λ / 2 plate, and the Q layer typically functions as a λ / 4 plate. Specifically, the Re(550) of the H layer is preferably 200 nm to 300 nm, more preferably 220 nm to 290 nm, and further preferably 230 nm to 280 nm; the Re(550) of the Q layer is preferably 100 nm to 180 nm, more preferably 110 nm to 170 nm, and further preferably 110 nm to 150 nm. The thickness of the H layer can be adjusted so that a desired in-plane retardation of the λ / 2 plate is obtained. The thickness of the H layer can be, for example, 2.0 μm to 4.0 μm. The thickness of the Q layer can be adjusted so that a desired in-plane retardation of the λ / 4 plate is obtained. The thickness of the Q layer can be, for example, 1.0 μm to 2.5 μm. In this embodiment, the angle between the slow axis of the H layer and the absorption axis of the polarizer is preferably 10° to 20°, more preferably 12° to 18°, and even more preferably 12° to 16°; the angle between the slow axis of the Q layer and the absorption axis of the polarizer is preferably 70° to 80°, more preferably 72° to 78°, and even more preferably 72° to 76°. The order of arrangement of the H layer and the Q layer may be reversed, and the angle between the slow axis of the H layer and the absorption axis of the polarizer and the angle between the slow axis of the Q layer and the absorption axis of the polarizer may be reversed. When the retardation layer has a laminated structure, each layer (for example, the H layer and the Q layer) may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes depending on the wavelength of the measurement light.
[0051] The retardation layer (each layer in the case of having a laminated structure) typically exhibits a refractive index characteristic of nx > ny = nz. Note that "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny > nz or ny < nz may occur. The Nz coefficient of the retardation layer is preferably 0.9 to 1.5, more preferably 0.9 to 1.3.
[0052] The retardation layer is a liquid crystal alignment solidified layer as described above. Examples of the liquid crystal compound include liquid crystal compounds (nematic liquid crystals) in which the liquid crystal phase is a nematic phase. As such liquid crystal compounds, for example, liquid crystal polymers and liquid crystal monomers can be used. The mechanism for the manifestation of liquid crystallinity of the liquid crystal compound may be either lyotropic or thermotropic. The liquid crystal polymer and the liquid crystal monomer may be used alone or in combination.
[0053] When the liquid crystal compound is a liquid crystal monomer, the liquid crystal monomer is preferably a polymerizable monomer and a crosslinkable monomer. This is because the alignment state of the liquid crystal monomer can be fixed by polymerizing or crosslinking (i.e., curing) the liquid crystal monomer. After the liquid crystal monomer is aligned, for example, if the liquid crystal monomers are polymerized or crosslinked with each other, the alignment state can be fixed thereby. Here, a polymer is formed by polymerization, and a three-dimensional network structure is formed by crosslinking, but these are non-liquid crystalline. Therefore, in the formed retardation layer, for example, a transition from a liquid crystal phase, a glass phase, or a crystal phase due to a temperature change peculiar to the liquid crystalline compound does not occur. As a result, the retardation layer becomes an extremely stable retardation layer that is not affected by temperature changes.
[0054] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on its type. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.
[0055] Any suitable liquid crystal monomer can be used as the liquid crystal monomer. For example, the polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445 can be used. Specific examples of such polymerizable mesogen compounds include BASF's product name LC242, Merck's product name E7, and Wacker-Chem's product name LC-Sillicon-CC3767. For example, nematic liquid crystal monomers are preferred as the liquid crystal monomer. EXAMPLES
[0056] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified. (1) Warpage The retardation layer-attached polarizing plates obtained in the Examples and Comparative Examples were cut into a size of 140 mm x 70 mm before humidification (before preparation of intermediate laminate) and after humidification and storage (after peeling off the TAC film). At this time, the polarizing plates were cut so that the absorption axis direction of the polarizer was the long side direction. When the cut retardation layer-attached polarizing plate was placed on a flat surface, the height of the highest part from the flat surface was taken as the warpage. Next, the amount of warping of the retardation layer-attached polarizing plate cut out after storage was measured in the same manner as above, and the change in the amount of warping before and after humidification and storage was evaluated according to the following criteria. ○: Change in warpage is ±25mm or less ×: The change in the amount of warping is greater than ±25 mm. In addition, when the warp is convex toward the stationary surface, it is expressed as "positive (+)", and when it is convex toward the opposite side to the stationary surface, it is expressed as "negative (-)". The stationary surface side is the retardation layer (Q layer) side.
[0057] [Example 1] 1. Preparation of Polarizing Plates As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the finally obtained polarizer would be the desired value (dyeing treatment). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, the film was dried in an oven maintained at about 90° C. while being brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment). In this manner, a polarizer having a thickness of about 5 μm was formed on the resin substrate, and a polarizing plate having a resin substrate / polarizer structure was obtained.
[0058] Furthermore, an HC-COP film was attached as a viewing-side protective layer to the surface of the obtained polarizer (the surface opposite to the resin substrate) via an ultraviolet-curable adhesive. The HC-COP film is a film in which an HC layer (thickness 2 μm) is formed on a cycloolefin resin (COP) film (thickness 25 μm), and the COP film was attached to the polarizer side. Next, the resin substrate was peeled off to obtain a polarizing plate having a configuration of HC-COP film (viewing-side protective layer) / polarizer. The moisture permeability of the viewing-side protective layer was 100 g / m 2 -It was 24 hours.
[0059] 2. Preparation of polarizing plate with retardation layer 2-1. Preparation of retardation layer A liquid crystal composition (coating liquid) was prepared by dissolving 10 g of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: product name "Paliocolor LC242", represented by the following formula) and 3 g of a photopolymerization initiator for the polymerizable liquid crystal compound (manufactured by BASF: product name "Irgacure 907") in 40 g of toluene. [ka] The surface of a polyethylene terephthalate (PET) film (thickness 38 μm) was rubbed with a rubbing cloth and subjected to an alignment treatment. The direction of the alignment treatment was set to be 15° from the viewing side with respect to the direction of the absorption axis of the polarizer when it was attached to the polarizing plate. The above liquid crystal coating liquid was applied to this alignment-treated surface with a bar coater, and the liquid crystal compound was aligned by heating and drying at 90°C for 2 minutes. The liquid crystal layer thus formed was then irradiated with 1 mJ / cm using a metal halide lamp. 2The liquid crystal layer was cured by irradiating the liquid crystal with light, forming a liquid crystal alignment solidified layer A on the PET film. The liquid crystal alignment solidified layer A had a thickness of 2.0 μm and an in-plane retardation Re(550) of 270 nm. Furthermore, the liquid crystal alignment solidified layer A exhibited a refractive index characteristic of nx>ny=nz. The liquid crystal alignment solidified layer A was used as the H layer. A liquid crystal alignment layer B was formed on a PET film in the same manner as above, except that the coating thickness was changed and the orientation treatment direction was set to be 75° from the viewing side relative to the absorption axis direction of the polarizer. The liquid crystal alignment layer B had a thickness of 1.0 μm and an in-plane retardation Re(550) of 140 nm. Furthermore, the liquid crystal alignment layer B showed a refractive index characteristic of nx>ny=nz. The liquid crystal alignment layer B was used as the Q layer.
[0060] 2-2. Preparation of polarizing plate with retardation layer The liquid crystal alignment solidified layer A (H layer) and the liquid crystal alignment solidified layer B (Q layer) obtained in 2-1 above were transferred in this order onto the polarizer surface of the polarizing plate obtained in 1 above. At this time, the transfer (lamination) was performed so that the angle between the absorption axis of the polarizer and the slow axis of the alignment solidified layer A was 15°, and the angle between the absorption axis of the polarizer and the slow axis of the alignment solidified layer B was 75°. Note that each transfer (lamination) was performed via an ultraviolet-curing adhesive (thickness 1.0 μm). In this way, a retardation layer-attached polarizing plate having a configuration of protective layer / adhesive / polarizer / adhesive / retardation layer (H layer) / adhesive / retardation layer (Q layer) was obtained. The total thickness of the retardation layer-attached polarizing plate was 38 μm. Note that the transfer (lamination) was performed while being transported by rolls.
[0061] 3. Preparation of Intermediate Laminate A TAC film (thickness 70 μm) was temporarily attached to the surface of the Q layer of the retardation layer-attached polarizing plate obtained in 2 above via an acrylic adhesive to prepare an intermediate laminate. The intermediate laminate was prepared while being transported by rolls. The water absorption rate of the TAC film was 5% and the moisture permeability was 400 g / m 2 -It was 24 hours.
[0062] 4. Humidification and storage The intermediate laminate obtained in the above step 3 was subjected to a humidification treatment while being transported by rolls. The humidification treatment was performed at 23°C and 70% RH (water vapor amount of 14.4 g / m 3 The humidified polarizing plate with a retardation layer was wound into a roll, and the roll was immersed in a 23°C, 55% RH (water vapor amount: 11.3 g / m 3 The retardation layer-attached polarizing plates before and after the humidification treatment were subjected to the evaluation in the above (1). The results are shown in Table 1.
[0063] [Example 2] Humidification was performed at 20°C and 80% RH (water vapor volume was 13.8 / m 3 ) for 10 minutes, a polarizing plate with a retardation layer was obtained in the same manner as in Example 1. The polarizing plates with a retardation layer before the humidification treatment and after the roll storage were each subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0064] [Comparative Example 1] A polarizing plate with a retardation layer was obtained in the same manner as in Example 1, except that the humidification treatment and roll storage were performed without laminating a TAC film. The polarizing plates with a retardation layer before the humidification treatment and after the roll storage were each subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0065] [Comparative Example 2] A polarizing plate with a retardation layer (before preparing an intermediate laminate) was obtained in the same manner as in Example 1. This polarizing plate with a retardation layer was stored in a roll as is (i.e., without preparing an intermediate laminate or subjecting it to a humidification treatment) in the same manner as in Example 1. The polarizing plates with a retardation layer after roll storage were each subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0066] [Reference example 1] A long roll of a PVA-based resin film having a thickness of 30 μm was uniaxially stretched in the longitudinal direction by a roll stretching machine so that the total stretching ratio was 6.0 times, while simultaneously undergoing swelling, dyeing, crosslinking and washing treatments, and finally drying treatment to produce a polarizer having a thickness of 12 μm. An HC-COP film was attached to one surface of the obtained polarizer as a viewing side protective layer in the same manner as in Example 1. Furthermore, a TAC film (thickness 25 μm) was attached to the other surface of the polarizer via a PVA-based adhesive to obtain a polarizing plate having a configuration of protective layer (HC-COP film) / polarizer / protective layer (TAC film). The following procedure was performed in the same manner as in Example 1 to obtain a retardation layer-attached polarizing plate having a configuration of protective layer (HC-COP film) / adhesive / polarizer / adhesive / protective layer (TAC film) / adhesive / retardation layer (H layer) / adhesive / retardation layer (Q layer). The total thickness of the retardation layer-attached polarizing plate was 71 μm.
[0067] The following procedure was the same as in Example 1 to prepare an intermediate laminate, which was then subjected to a humidification treatment and then stored in a roll. The retardation layer-attached polarizing plates before and after the humidification treatment were each subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0068] [Table 1]
[0069] [evaluation] As is clear from Table 1, the warping of the retardation layer-attached polarizing plate obtained by the embodiment of the present invention is suppressed by subjecting the intermediate laminate with the water-absorbing film to a predetermined humidification treatment and roll storage. Furthermore, as is clear from the reference example, such warping is a problem specific to retardation layer-attached polarizing plates having a thin total thickness and a viewer-side protective layer with low moisture permeability. [Industrial Applicability]
[0070] The retardation layer-attached polarizing plate obtained by the manufacturing method of the embodiment of the present invention is used as a retardation layer-attached polarizing plate for an image display device, and can be suitably used in a curved, bent, foldable, or rollable image display device (typically, a resin substrate is used as the substrate in such an image display device). Typical examples of the image display device include a liquid crystal display device, an organic EL display device, and an inorganic EL display device. [Explanation of symbols]
[0071] 11 Polarizer 12 Protective layer 20 Retardation layer 21 Retardation layer (H layer) 22 Retardation layer (Q layer) 100 Polarizing plate with retardation layer 100' Polarizing plate with retardation layer (intermediate) 101 Polarizing plate with retardation layer 101' Polarizing plate with retardation layer (intermediate) 150 Water-absorbent film 200 Intermediate laminate
Claims
1. A method for producing a polarizing plate with a retardation layer, the polarizing plate having a polarizer, a protective layer disposed on one side of the polarizer, and a retardation layer disposed on the other side of the polarizer, comprising the steps of: humidifying an intermediate laminate having a water-absorbent film temporarily attached to the retardation layer side of the retardation layer-attached polarizing plate while transporting it with a roll; storing the humidified intermediate laminate for 12 hours or more without substantially humidifying it; Including, The moisture permeability of the protective layer at 40° C. and 92% RH is 100 g / m 2 - 24 hours or less, the retardation layer is a layer in which a liquid crystal compound is aligned and solidified, The water-absorbent film has a moisture permeability of 300 g / m 2 ·24 h or more at 40° C. and 92% RH; Manufacturing method.
2. The method for producing a polarizing plate with a retardation layer according to claim 1 , wherein the water-absorbing film has a water absorption rate of 2% or more.
3. The method for producing a polarizing plate with a retardation layer according to claim 2 , wherein the water-absorbent film is a triacetyl cellulose film.
4. The method for producing a polarizing plate with a retardation layer according to claim 3 , wherein the water-absorbing film has a thickness of 40 μm or more.
5. The humidification treatment is performed at a temperature of 34° C. or less and with a water vapor amount of 13.8 g / m 3 The method for producing a polarizing plate with a retardation layer according to claim 1 , which is carried out under the above-mentioned environment.
6. The method for producing a polarizing plate with a retardation layer according to claim 5 , wherein the humidification time in the humidification treatment is 5 minutes or more.
7. The method for producing a polarizing plate with a retardation layer according to claim 1 , wherein the humidified intermediate laminate is stored for 24 hours or more.
8. The method for producing a polarizing plate with a retardation layer according to claim 1 , wherein the humidified intermediate laminate is stored in an environment having a temperature of 34° C. or lower.
9. The method for producing a retardation layer-attached polarizing plate according to claim 1 , further comprising peeling and removing the water-absorbing film from the intermediate laminate after the storage.
10. The moisture permeability of the retardation layer at 40° C. and 92% RH is 300 g / m 2 The method for producing a polarizing plate with a retardation layer according to any one of claims 1 to 9, wherein the retardation period is 24 hours or more.
11. The retardation layer is a single layer, the retardation layer has an Re(550) of 100 nm to 190 nm, the retardation layer has an Re(450) / Re(550) of 0.8 or more and less than 1, and the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is 40° to 50°, according to any one of claims 1 to 10.
12. The method for producing a polarizing plate with a retardation layer according to claim 11, wherein the polarizing plate with a retardation layer further has another retardation layer on the outside of the retardation layer, and the refractive index characteristic of the other retardation layer shows a relationship of nz>nx=ny.
13. the retardation layer has a laminated structure of a layer having a fixed alignment of a first liquid crystal compound and a layer having a fixed alignment of a second liquid crystal compound, The Re(550) of the alignment / solidification layer of the first liquid crystal compound is 200 nm to 300 nm, and the angle between the slow axis of the layer and the absorption axis of the polarizer is 10° to 20°, the Re(550) of the alignment solidified layer of the second liquid crystal compound is 100 nm to 190 nm, and the angle between the slow axis of the layer and the absorption axis of the polarizer is 70° to 80°; A method for producing the retardation layer-attached polarizing plate according to claim 1 .
14. The method for producing a polarizing plate with a retardation layer according to claim 1 , wherein the total thickness of the polarizing plate with a retardation layer is 45 μm or less.
Citation Information
Patent Citations
Manufacturing method of polarizing element, polarizing element, and projector
JP2008015145A
Pressure-sensitive adhesive optical film and image display device
JP2009258570A
Polarizing plate with retardation layer and image display device
JP2018205663A
Circularly polarizing plate and display device
JP2020024352A
Retardation film and optical device using the same
JP3325560B2