Printed Wiring Boards

By controlling the void density and side etching at the interface between the electroless and electrolytic copper plating layers, the printed wiring board design prevents pattern peeling, enhancing the structural integrity of the conductive pattern.

JP7566214B2Active Publication Date: 2024-10-11SUMITOMO ELECTRIC INDUSTRIES LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024528753
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-14
Filing Date
2023-06-07
Publication Date
2024-10-11
Estimated Expiration
2043-06-07

AI Technical Summary

Technical Problem

The issue in existing printed wiring boards is the excessive void density at the interface between the electroless copper plating layer and the electrolytic copper plating layer, leading to side etching and peeling of the conductive pattern from the base film.

Method used

The printed wiring board design includes a conductive pattern with a base conductive layer and an electrolytic copper plating layer, where the void density at their interface is controlled to be between 0.01 μm²/μm and 5.5 μm²/μm, limiting side etching and preventing pattern peeling by maintaining a T×VL/L value of 0.39 or less.

Benefits of technology

This approach effectively suppresses the peeling of the conductive pattern from the base film by managing the void density and side etching, ensuring the integrity of the conductive pattern.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566214000002
    Figure 0007566214000002
  • Figure 0007566214000003
    Figure 0007566214000003
  • Figure 0007566214000004
    Figure 0007566214000004
Patent Text Reader

Abstract

This printed wiring board comprises a base film that has a main surface, and a conductive pattern that is disposed on the main surface. The conductive pattern has a base conductive layer that is disposed directly or indirectly on the main surface, and an electrolytic copper plating layer that is disposed on the base conductive layer. At the interface between the base conductive layer and the electrolytic copper plating layer, the void density, which is the value of the total surface area of voids within the range of a prescribed observation length divided by the observation length, is greater than 0.01μm2 / μm and not more than 5.5μm2 / μm. The value of T×VL / L within the observation length is 0.39 or less, where T is the thickness (μm) of the base conductive layer, L is the observation length (μm) at the interface and VL is the total length (μm) of voids existing at the interface within the range of the observation length.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a printed wiring board. This application claims priority based on Japanese Patent Application No. 2022-095739 filed on June 14, 2022. All contents of the Japanese patent application are incorporated herein by reference. [Background technology]

[0002] Japanese Patent Laid-Open Publication No. 2019-197851 (Patent Document 1) describes a printed wiring board. The printed wiring board described in Patent Document 1 has a base film and a conductive pattern.

[0003] The base film has a main surface. The conductive pattern is disposed on the main surface. The conductive pattern has a seed layer, an electroless copper plating layer, and an electrolytic copper plating layer. The seed layer is disposed on the main surface. The electroless copper plating layer is disposed on the seed layer. The electrolytic copper plating layer is disposed on the electroless copper plating layer. The electroless copper plating layer and the electrolytic copper plating layer are formed of copper. That is, the conductive pattern is formed using a semi-additive method.

[0004] In the printed wiring board of Patent Document 1, the void density at the interface between the electroless copper plating layer and the electrolytic copper plating layer is 0.01 μm 2 The void density at the interface between the electroless copper plating layer and the electrolytic copper plating layer is the sum of the areas of voids present at the interface between the electroless copper plating layer and the electrolytic copper plating layer within a predetermined observation length in a cross-sectional view, divided by the observation length.

[0005] In the printed wiring board described in Patent Document 1, the void density at the interface between the electroless copper plating layer and the electrolytic copper plating layer is set to 0.01 μm 2 By making the thickness of the conductive pattern less than 1 μm, peeling of the conductive pattern from the base film is suppressed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-197851 A Summary of the Invention

[0007] The printed wiring board of the present disclosure includes a base film having a main surface and a conductive pattern disposed on the main surface. The conductive pattern includes an underlying conductive layer disposed directly or indirectly on the main surface, and an electrolytic copper plating layer disposed on the underlying conductive layer. The void density, which is the value obtained by dividing the total area of ​​voids within a range of a predetermined observation length at the interface between the underlying conductive layer and the electrolytic copper plating layer by the observation length, is 0.01 μm 2 / μm more than 5.5μm 2 When the thickness of the underlying conductive layer is T (μm), the observation length is L (μm), and the total length of voids present at the interface within the observation length is VL (μm), the value of T × VL / L is 0.39 or less within the observation length. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a plan view of a printed wiring board 100. FIG. [Diagram 2] FIG. 2 is a bottom view of the printed wiring board 100. FIG. [Diagram 3] FIG. 3 is a cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 4 is an enlarged view of IV in FIG. [Diagram 5] FIG. 5 is a schematic enlarged cross-sectional view of the interface between electrolessly plated layer 25 and electrolytic copper plated layer 26. As shown in FIG. [Figure 6] FIG. 6 is a manufacturing process diagram of the printed wiring board 100. [Figure 7] FIG. 7 is a cross-sectional view illustrating the preparation step S1. [Figure 8] FIG. 8 is a cross-sectional view illustrating the electroless plating step S2. [Figure 9]FIG. 9 is a cross-sectional view illustrating the resist pattern forming step S3. [Figure 10] FIG. 10 is a cross-sectional view illustrating the electrolytic plating step S4. [Figure 11] FIG. 11 is a cross-sectional view of a printed wiring board 100 according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Problem that this disclosure aims to solve] When forming a conductive pattern by the semi-additive method, first, an electroless copper plating layer is formed on a seed layer. Second, a resist pattern is formed on the electroless copper plating layer. Third, an electrolytic copper plating layer is formed on the electroless copper plating layer exposed from the openings of the resist pattern. Fourth, the resist pattern is removed. Fifth, the electroless copper plating layer and the seed layer exposed between adjacent portions of the electrolytic copper plating layer are removed by etching.

[0010] When the void density at the interface between the electroless copper plating layer and the electrolytic copper plating layer becomes large, side etching is likely to progress at the interface between the electroless copper plating layer and the electrolytic copper plating layer due to etching for removing the electroless copper plating layer and the seed layer exposed between the adjacent electrolytic copper plating layers. If such side etching progresses excessively, it may cause a part of the conductive pattern to peel off from the base film.

[0011] For example, when a resist pattern is formed, an adhesion assistant treatment is performed to ensure adhesion between the resist pattern and the electroless copper plating layer, or a thick resist pattern is used to ensure the thickness of the electrolytic copper plating layer. In such cases, the void density at the interface between the electroless copper plating layer and the electrolytic copper plating layer may be reduced to 0.01 μm due to the influence of contamination remaining on the surface of the electroless copper plating layer. 2 It can be difficult to achieve a thickness of less than / μm.

[0012] [Effects of this disclosure] According to the printed wiring board of the present disclosure, even if the void density at the interface between the underlying conductive layer and the electrolytic copper plating layer becomes large, peeling of a portion of the conductive pattern from the base film due to side etching at the interface between the underlying conductive layer and the electrolytic copper plating layer can be suppressed.

[0013] The present disclosure has been made in consideration of the above-mentioned problems of the conventional techniques. More specifically, the present inventors have discovered that the void density, which is the value obtained by dividing the total area of ​​voids within a range of a predetermined observation length at the interface between a base conductive layer and an electrolytic copper plating layer, is 0.01 μm 2 / μm more than 5.5μm 2 / μm or less, peeling of a part of the conductive pattern from the base film can be suppressed. Furthermore, the present inventors have found that peeling of the conductive pattern is caused by side etching at the interface between the underlying conductive layer and the electrolytic copper plating layer, and that the amount of side etching is correlated with the thickness of the electroless copper plating layer and the underlying conductive layer. The present disclosure provides a printed wiring board capable of suppressing peeling of a part of the conductive pattern from the base film.

[0014] [Description of the embodiments of the present disclosure] First, embodiments of the present disclosure will be listed and described.

[0015] (1) A printed wiring board according to an embodiment includes a base film having a principal surface, and a conductive pattern disposed on the principal surface. The conductive pattern includes an underlying conductive layer disposed directly or indirectly on the principal surface, and an electrolytic copper plating layer disposed on the underlying conductive layer. The void density, which is the sum of the areas of voids within a given observation length at the interface between the underlying conductive layer and the electrolytic copper plating layer divided by the observation length, is 0.01 μm 2 / μm more than 5.5μm 2 / μm or less. When the thickness of the conductive underlayer is T (μm), the observation length is L (μm), and the total length of voids present at the interface within the observation length is VL (μm), the value of T×VL / L is 0.39 or less within the observation length. Note that "the conductive underlayer is directly disposed on the main surface" means that the main surface and the conductive underlayer are in contact with each other, and "the conductive underlayer is indirectly disposed on the main surface" means that at least one layer (for example, a seed layer, which will be described later) is disposed between the main surface and the conductive underlayer.

[0016] According to the printed wiring board of (1) above, even if the void density at the interface between the underlying conductive layer and the electrolytic copper plating layer becomes large, peeling of a part of the conductive pattern from the base film due to side etching at the interface between the underlying conductive layer and the electrolytic copper plating layer can be suppressed.

[0017] (2) In the printed wiring board of (1) above, the conductive pattern may further include a seed layer disposed on a main surface thereof. The underlying conductive layer may include an underlayer disposed on the seed layer and an electroless plating layer disposed on the underlayer.

[0018] (3) In the printed wiring board of (2) above, the underlayer and the electroless plating layer may be made of copper.

[0019] (4) In the printed wiring boards according to (1) to (3) above, the conductive pattern may have a thickness of 5 μm or more and 150 μm or less.

[0020] (5) In the printed wiring boards according to any one of (1) to (4) above, the amount of side etching at the interface may be 0.33 times or less the width of the conductive pattern.

[0021] (6) In the printed wiring boards according to any one of (1) to (5), the conductive pattern may have a plurality of adjacent wiring portions, and the distance between adjacent ones of the plurality of wiring portions may be 5 μm or more and 100 μm or less.

[0022] [Details of the embodiment of the present disclosure] The details of the embodiment of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are given the same reference characters, and duplicated explanations will not be repeated. The printed wiring board according to the embodiment is referred to as a printed wiring board 100.

[0023] (Configuration of printed wiring board 100) The configuration of the printed wiring board 100 will be described below.

[0024] FIG 1 is a plan view of printed wiring board 100. FIG 2 is a bottom view of printed wiring board 100. FIG 2 shows printed wiring board 100 as viewed from the opposite side to that of FIG 1. FIG 3 is a cross-sectional view taken along line III-III in FIG 1. FIG 4 is an enlarged view taken along line IV in FIG 3. As shown in FIG 1 to FIG 4, printed wiring board 100 has a base film 10, and conductive patterns 21 and 22.

[0025] The base film 10 has a main surface 10a and a main surface 10b. The main surface 10a and the main surface 10b are end surfaces in the thickness direction of the base film 10. The main surface 10b is the opposite surface to the main surface 10a. The base film 10 is made of a flexible, electrically insulating material. The base film 10 is made of, for example, polyimide or liquid crystal polymer.

[0026] The conductive pattern 21 is disposed on the main surface 10a. The conductive pattern 21 is wound in a spiral shape in a plan view. The conductive pattern 21 has a plurality of wiring portions 21a adjacent to each other.

[0027] The conductive pattern 22 is disposed on the main surface 10b. The conductive pattern 22 is wound in a spiral shape in a plan view. The conductive pattern 22 has a plurality of wiring portions 22a adjacent to each other.

[0028] The conductive pattern 21 has a land 21b at one end and a land 21c at the other end. The lands 21b and 21c are located at the outermost and innermost circumferences of the conductive pattern 21, respectively. The conductive pattern 22 has a land 22b at one end and a land 22c at the other end. The lands 22b and 22c are located at the innermost and outermost circumferences of the conductive pattern 22, respectively. The land 21c and the land 22b overlap each other in a plan view.

[0029] The width of the conductive pattern 21 is width W1, and the width of the conductive pattern 22 is width W2. The width W1 and the width W2 are, for example, 5 μm or more and 50 μm or less. The thickness of the conductive pattern 21 is thickness T1. The thickness of the conductive pattern 22 is thickness T2. The thickness T1 is, for example, 5 μm or more and 150 μm or less, and may be 8 μm or more and 100 μm or less, or may be 30 μm or more and 100 μm or less. The thickness T2 is, for example, 5 μm or more and 150 μm or less, and may be 8 μm or more and 100 μm or less. The thickness T2 may be 30 μm or more and 100 μm or less. The distance between two adjacent wiring parts 21a is distance DIS1. The distance between two adjacent wiring parts 22a is distance DIS2. The distance DIS1 and the distance DIS2 are, for example, 5 μm or more and 100 μm or less. The distance DIS1 and the distance DIS2 may be not less than 5 μm and not more than 20 μm.

[0030] The thickness T1, the thickness T2, the distance DIS1, and the distance DIS2 are measured by the following method. First, a cross-sectional image is obtained using an electron microscope (SEM: Scanning Electron Microscope) in a cross section along the thickness direction of the base film 10 and perpendicular to the length direction of the conductive pattern 21 (conductive pattern 22) in a plan view. Second, in the obtained cross-sectional image, the thickness of the conductive pattern 21, the thickness of the conductive pattern 22, the distance between two adjacent wiring portions 21a, and the distance between two adjacent wiring portions 22a are measured. This measurement is performed at a position on the cross-sectional image where the width of the conductive pattern 21 (conductive pattern 22) is maximum. As a result of the above, the values ​​of the thickness T1, the thickness T2, the distance DIS1, and the distance DIS2 are obtained.

[0031] Each of the conductive patterns 21 and 22 is formed by, for example, a semi-additive method. More specifically, each of the conductive patterns 21 and 22 has a seed layer 23, a base layer 24, an electroless plating layer 25, and an electrolytic copper plating layer 26. The base layer 24 and the electroless plating layer 25 may be collectively referred to as a base conductive layer 27.

[0032] The seed layer 23 is disposed on the main surface (main surface 10a, main surface 10b) of the base film 10. The seed layer 23 is, for example, a sputtered layer (a layer formed by sputtering). The seed layer 23 is formed of, for example, a nickel-chromium alloy. The underlayer 24 is disposed on the seed layer 23. That is, the underlayer conductive layer 27 is disposed on the main surface of the base film 10 with the seed layer 23 interposed therebetween. The underlayer 24 is, for example, a sputtered layer. The underlayer 24 may be formed of copper. Note that each of the conductive patterns 21 and 22 may not have the seed layer 23. In this case, the underlayer conductive layer 27 is disposed directly on the main surface of the base film 10.

[0033] The electroless plating layer 25 is disposed on the underlayer 24. The electroless plating layer 25 is a layer formed by electroless plating. The electroless plating layer 25 may be formed of copper. The electrolytic copper plating layer 26 is disposed on the electroless plating layer 25. The electrolytic copper plating layer 26 is a layer formed by electrolytic plating. The electrolytic copper plating layer 26 is formed of copper.

[0034] Although not shown, a through hole is formed in the base film 10. The through hole of the base film 10 penetrates the base film 10 in the thickness direction. The through hole of the base film 10 overlaps with the land 21c and the land 22b in a plan view.

[0035] The electroless plating layer 25 is also disposed on the inner wall surface of the through hole of the base film 10. The electrolytic copper plating layer 26 is also embedded in the through hole of the base film 10. This electrically connects the conductive patterns 21 and 22 to each other. When a voltage is applied between the land 21b and the land 22c, a current flows in a spiral shape in the conductive patterns 21 and 22, and a magnetic field is generated by this current. In other words, the printed wiring board 100 serves as a coil device.

[0036] Fig. 5 is a schematic enlarged cross-sectional view of the interface between electroless plated layer 25 and electrolytic copper plated layer 26. As shown in Fig. 5, the thickness of base layer 24 and the thickness of electroless plated layer 25 are designated as thickness T3 and thickness T4, respectively. The sum of thickness T3 and thickness T4 is designated as T (μm). In other words, T is the thickness of base conductive layer 27. Thicknesses T3 and T4 are measured by the same method as thickness T1 (thickness T2).

[0037] Voids V exist at the interface between electroless plating layer 25 and electrolytic copper plating layer 26, i.e., the interface between underlying conductive layer 27 and electrolytic copper plating layer 26. The void density at the interface between electroless plating layer 25 and electrolytic copper plating layer 26 is 0.01 μm 2 / μm more than 5.5μm 2 / μm or less. The void density at the interface between electroless plating layer 25 and electrolytic copper plating layer 26 is the sum of the areas of voids present at the interface between electroless plating layer 25 and electrolytic copper plating layer 26 within a predetermined observation length in a cross-sectional view, divided by the observation length.

[0038] When calculating the void density at the interface between electroless plating layer 25 and electrolytic copper plating layer 26, first, a cross-sectional image is obtained using an SEM in a cross section perpendicular to the main surface of base film 10. The magnification of the cross-sectional image is set to 10,000 times or more and 50,000 times or less.

[0039] Secondly, the total area of ​​voids V within a range of a predetermined observation length (hereinafter, this observation length may be referred to as L (μm)) is measured at the interface between electroless plating layer 25 and electrolytic copper plating layer 26 in the above cross-sectional image. The direction of the observation length is parallel to the main surface of base film 10. The area of ​​voids V is obtained by binarizing the cross-sectional image using image processing software such as GNU Image Manipulation Program so that voids V are black, and calculating the proportion of black portions from a brightness histogram obtained using the image processing software. Thirdly, the calculated total area of ​​voids V is divided by the above observation length to calculate the void density at the interface between electroless plating layer 25 and electrolytic copper plating layer 26.

[0040] The total length of the voids V within the range of the observation length at the interface between electroless plating layer 25 and electrolytic copper plating layer 26 in the cross-sectional image is VL (μm). In the example shown in FIG. 5, three voids V exist at the interface between electroless plating layer 25 and electrolytic copper plating layer 26. If the lengths of these three voids V are VL1, VL2, and VL3, respectively, VL1, VL2, and VL3 are the lengths of the three voids V in the direction along the interface between electroless plating layer 25 and electrolytic copper plating layer 26. VL is the total of VL1, VL2, and VL3. The value of T×VL / L is 0.39 or less.

[0041] As shown in FIG. 4, the etching for forming the conductive pattern 21 (conductive pattern 22) has a predetermined side etching amount. The side etching amount is the depth of a notch formed at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 by the side etching in a direction along the interface. In other words, the side etching amount is a distance DIS3 between the apex of the notch in the direction along the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 and the farthest end of the underlying conductive layer 27. The distance DIS3 may be 0.33 times or less, or 0.17 times or less, of the width W1 (width W2). The distance DIS3 is measured by the same method as the distance DIS1 (distance DIS2).

[0042] (Method of Manufacturing Printed Wiring Board 100) A method for manufacturing the printed wiring board 100 will now be described.

[0043] 6 is a manufacturing process diagram of the printed wiring board 100. As shown in FIG. 6, the manufacturing method of the printed wiring board 100 includes a preparation step S1, an electroless plating step S2, a resist pattern forming step S3, an electrolytic plating step S4, and an etching step S5. The electroless plating step S2 is performed after the preparation step S1. The resist pattern forming step S3 is performed after the electroless plating step S2. The electrolytic plating step S4 is performed after the resist pattern forming step S3. The etching step S5 is performed after the electrolytic plating step S4.

[0044] Fig. 7 is a cross-sectional view illustrating the preparation step S1. As shown in Fig. 7, in the preparation step S1, a base film 10 is prepared. Note that in the base film 10 prepared in the preparation step S1, a seed layer 23 is disposed on the main surface 10a and the main surface 10b, and an underlayer 24 is disposed on the seed layer 23.

[0045] 8 is a cross-sectional view illustrating the electroless plating step S2. As shown in FIG 8, in the electroless plating step S2, electroless plating is performed to form an electroless plated layer 25 on the underlayer 24.

[0046] Although not shown, prior to the above-mentioned electroless plating, a through hole is formed by drilling the base film 10. Therefore, the above-mentioned electroless plating forms an electroless plating layer 25 on the inner wall surface of the through hole in the base film 10.

[0047] Fig. 9 is a cross-sectional view illustrating the resist pattern forming step S3. As shown in Fig. 9, in the resist pattern forming step S3, a resist pattern 30 is formed on the electroless plating layer 25. An opening 31 is formed in the resist pattern 30. The opening 31 penetrates the resist pattern 30 in the thickness direction. In other words, the electroless plating layer 25 is exposed from the opening 31.

[0048] In the resist pattern formation step S3, first, a dry film resist is applied onto the electroless plating layer 25. At this time, in order to ensure adhesion between the dry film resist (resist pattern 30) and the electroless plating layer 25, the surface of the electroless plating layer 25 may be treated with an adhesion assistant.

[0049] Secondly, the dry film resist is exposed and developed, whereby the dry film resist is partially removed to form openings 31. In this manner, a resist pattern 30 is formed. After the resist pattern 30 is formed, the surface of the electroless plating layer 25 exposed from the openings 31 may be cleaned using plasma or the like.

[0050] Fig. 10 is a cross-sectional view illustrating the electrolytic plating step S4. As shown in Fig. 10, in the electrolytic plating step S4, electrolytic plating is performed to form an electrolytic copper plating layer 26 on the electroless plating layer 25 exposed from the opening 31. When it is desired to increase the thickness T1 (thickness T2) (to increase the thickness of the electrolytic copper plating layer 26), the resist pattern 30 is formed accordingly thick. After the electrolytic copper plating layer 26 is formed, the resist pattern 30 is removed.

[0051] In the etching step S5, the electroless plating layer 25, the underlayer 24, and the seed layer 23 exposed between adjacent electrolytic copper plating layers 26 are removed by etching. During this process, side etching may occur at the interface between the electrolytic copper plating layer 26 and the underlying electroless plating layer 25.

[0052] (Effects of the printed wiring board 100) When forming the resist pattern 30, an adhesion assistant treatment may be performed to ensure adhesion between the resist pattern 30 and the electroless plating layer 25. In addition, when a thick resist pattern 30 is used to ensure the thickness of the electrolytic copper plating layer 26, the ratio of the thickness of the resist pattern 30 to the width of the opening 31 increases, which reduces the permeability of chemicals into the opening 31 in the resist pattern formation step S3, and reduces the removability of resist components and foreign matter on the surface of the electroless plating layer 25, resulting in contamination remaining on the surface of the electroless plating layer 25. When the value obtained by dividing the thickness of the resist pattern 30 by the width of the opening 31 exceeds 0.5, the void density at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 becomes large (more specifically, the void density is increased by 0.01 μm 2 / μm more than 5.5μm 2 / μm or less).

[0053] When the thickness T3 and the thickness T4 are large, the etching amount in the etching step S5 needs to be increased, and side etching is likely to proceed. In addition, when the void density at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 is large, side etching is likely to proceed at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 due to the etching in the etching step S5. Excessive side etching causes parts of the conductive patterns 21 and 22 to peel off from the base film. However, as shown in the following evaluation results, by multiplying the sum of the thicknesses T3 and T4, which is an index for evaluating the amount of side etching, by the sum of the lengths of the voids present at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 within a predetermined observation length and dividing the result by the observation length, that is, by setting the value of T×VL / L to 0.39 or less, peeling of a part of the conductive pattern 21 (conductive pattern 22) from the base film 10 is suppressed even when the void density at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 is large.

[0054] Table 1 shows the details of Samples 1 to 9. Samples 1 to 9 were formed by carrying out the preparation step S1 to the etching step S5. When forming Samples 1 to 9, in the resist pattern formation step S3, the surface of the electroless plating layer 25 is treated with an adhesion assistant, and then the resist pattern 30 is formed on the electroless plating layer 25. As shown in Table 1, in Samples 1 to 9, the total thickness (T value) of the underlayer 24 and the electroless plating layer 25, the observation length (L value), and the total length (VL value) of the voids V present at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 within the observation length were measured. In Samples 1 to 9, the value obtained by dividing the thickness of the resist pattern 30 by the width of the opening 31 was more than 0.5, and the void density at the interface between the electroless plating layer 25 and the electrolytic copper plating layer 26 was less than 0.01 μm 2 / μm more than 5.5μm 2 / μm or less.

[0055] In Samples 1 to 9, the presence or absence of peeling of conductive patterns 21 and 22 was observed visually or using a microscope. Samples in which peeling did not occur in conductive patterns 21 and 22 are marked as "OK" in Table 1. On the other hand, samples in which peeling occurred in part of conductive pattern 21 (conductive pattern 22) are marked as "NG" in Table 1.

[0056] [Table 1]

[0057] In Samples 1 to 6, the value of T×VL / L was 0.39 or less, and no peeling occurred in the conductive patterns 21 and 22. On the other hand, in Samples 7 to 9, the value of T×VL / L exceeded 0.39, and peeling occurred in parts of the conductive patterns 21 and 22.

[0058] From this comparison, it became clear that even when the void density at the interface between electroless plating layer 25 and electrolytic copper plating layer 26 is large, side etching at the interface between electroless plating layer 25 and electrolytic copper plating layer 26 is suppressed by setting the value of T×VL / L to 0.39 or less, and peeling of parts of conductive patterns 21 and 22 from base film 10 is suppressed.

[0059] (Modification) Fig. 11 is a cross-sectional view of a printed wiring board 100 according to a modified example. Fig. 11 shows a cross section at a position corresponding to Fig. 3. In the above, an example in which the conductive base layer 27 is composed of two layers, the base layer 24 and the electroless plating layer 25, has been shown, but the conductive base layer 27 may be composed of a single layer, as shown in Fig. 11. In this case, when calculating the value of T × VL / L, the value of T is set to the value of the thickness of the conductive base layer 27. In the example shown in Fig. 11, the conductive base layer 27 is directly disposed on the main surface of the base film 10.

[0060] The embodiments disclosed herein are illustrative in all respects and should not be considered as limiting. The scope of the present invention is defined by the claims, not the above-described embodiments, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0061] 100 printed wiring board, 10 base film, 10a, 10b main surface, 21 conductive pattern, 21a wiring portion, 21b, 21c land, 22 conductive pattern, 22a wiring portion, 22b land, 22c land, 23 seed layer, 24 underlayer, 25 electroless plating layer, 26 electrolytic copper plating layer, 27 underlayer conductive layer, 30 resist pattern, 31 opening, DIS1, DIS2, DIS3 distance, S1 preparation step, S2 electroless plating step, S3 resist pattern formation step, S4 electrolytic plating step, S5 etching step, T1, T2, T3, T4 thickness, V void, W1, W2 width.

Claims

1. A base film having a main surface; a conductive pattern disposed on the main surface, the conductive pattern has a base conductive layer disposed directly or indirectly on the main surface, and an electrolytic copper plating layer disposed on the base conductive layer, The void density, which is the value obtained by dividing the total area of ​​voids within a predetermined observation length at the interface between the underlying conductive layer and the electrolytic copper plating layer by the observation length, is less than 0.01 μm 2 / μm more than 5.5μm 2 / μm or less, A printed wiring board, wherein when the thickness of the underlying conductive layer is T (μm), the observation length is L (μm), and the total length of voids present at the interface within the observation length is VL (μm), the value of T×VL / L is 0.39 or less within the observation length.

2. the conductive pattern further comprises a seed layer disposed on the major surface; The printed wiring board according to claim 1 , wherein the underlying conductive layer includes an underlayer disposed on the seed layer, and an electroless plating layer disposed on the underlayer.

3. The printed wiring board according to claim 2 , wherein the underlayer and the electroless plating layer are made of copper.

4. 2. The printed wiring board according to claim 1, wherein the conductive pattern has a thickness of 5 μm or more and 150 μm or less.

5. The printed wiring board according to claim 1 , wherein an amount of side etching at the interface is 0.33 times or less the width of the conductive pattern.

6. the conductive pattern has a plurality of wiring portions adjacent to each other, The printed wiring board according to claim 1 , wherein a distance between two adjacent ones of the plurality of wiring portions is not less than 5 μm and not more than 100 μm.

Citation Information

Patent Citations

  • Base material for printed wiring board, and printed wiring board

    JP2019075456A

  • Printed wiring board and manufacturing method thereof

    JP2019197851A