Molding material for radio wave absorbing components and radio wave absorber
By using a molding material with magnetic iron oxide and a controlled hysteresis curve, the solution maintains consistent radio wave absorption characteristics, addressing the instability issue in high-frequency absorbers.
Patent Information
- Application Number
- JP2020063073
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing radio wave absorbers experience changes in absorption characteristics due to mechanical shearing forces during processes like molding, leading to unstable performance in absorbing high-frequency radio waves.
A molding material for radio wave absorbers using magnetic iron oxide, such as hexagonal ferrite, with a hysteresis curve differentiated twice to ensure P2/P1 is 0.15 or less, maintaining consistent absorption characteristics before and after processing.
The solution ensures minimal change in radio wave absorption characteristics, allowing for stable production of absorbers that effectively absorb high-frequency radio waves within a predetermined frequency range.
Smart Images

Figure 0007566482000002 
Figure 0007566482000003 
Figure 0007566482000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a molding material for radio wave absorbing components that absorbs radio waves, and a radio wave absorber produced using this material, and in particular to a molding material for radio wave absorbing components and a radio wave absorber that include magnetic iron oxide powder as a radio wave absorbing component and are capable of absorbing high-frequency radio waves from several tens of gigahertz to the millimeter wave band. [Background technology]
[0002] Radio wave absorbers are used to absorb radio waves, in order to avoid the effects of leaked radio waves emitted to the outside from electric circuits, etc., and undesired reflected radio waves. Radio wave absorbers are formed by molding or coating materials with radio wave absorbing properties according to the application, such as in a block or sheet shape.
[0003] In recent years, research has been progressing on technologies that utilize centimeter waves, which have a frequency band of several gigahertz (GHz), millimeter waves, which have frequencies from 30 gigahertz to 300 gigahertz, and even radio waves with a frequency of 1 terahertz (THz), which is a high-frequency band exceeding the millimeter wave band, for use in mobile communications such as mobile phones, wireless LAN, and automated toll collection systems (ETC).
[0004] In response to this technological trend toward utilizing radio waves of higher frequencies, there is an increasing demand for radio wave absorbers that can absorb high-frequency radio waves from several tens of gigahertz to the millimeter wave band, as radio wave absorbers that absorb unwanted radio waves.
[0005] As a radio wave absorber capable of absorbing such high frequency radio waves, a radio wave absorber has been proposed in which the particle size distribution of hexagonal ferrite powder is regulated to use a powder with a high proportion of particles close to primary particles, thereby enabling the absorption of radio waves of 1 GHz or above with a sheet thickness thinner than conventional ones (see Patent Document 1).
[0006] In addition, a sintered body of hexagonal ferrite in which the orientation degree of ferrite crystal grains is limited and a manufacturing method thereof have been proposed as a radio wave absorber having high absorption characteristics for radio waves in the GHz band and no anisotropy in radio wave absorption properties (see Patent Document 2). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2012-216865 A [Patent Document 2] JP 2018-154541 A Summary of the Invention [Problem to be solved by the invention]
[0008] By including magnetic iron oxide as a radio wave absorber, it is possible to absorb high frequency radio waves by the magnetic resonance of the magnetic iron oxide. As such magnetic iron oxide, hexagonal ferrite and epsilon iron oxide, which were also used in the above-mentioned conventional techniques, have already been put to practical use.
[0009] A radio wave absorber containing hexagonal ferrite as a radio wave absorbing material is prepared by preparing a composition, which is a molding material, by mixing a powder of sintered particles of hexagonal ferrite into an organic binder, and molding the composition by injection molding, extrusion molding, or the like, or by applying and drying the composition by a coater method or the like, and then forming the composition into a sheet of a predetermined thickness by an appropriate calendaring process, or the like, to produce a radio wave absorber of a desired shape.
[0010] The inventors have confirmed that when the composition, which is the molding material, is molded or when it is subjected to a stirring process using a kneader or the like, the radio wave absorbing characteristics of the processed radio wave absorber differ from those previously understood at the time of the molding material, and more specifically, undesirable situations arise such as a shift in the frequency of the absorbed radio waves and a decrease in the radio wave absorbing ability at a specific frequency. In this way, when the designed absorption frequency differs from the actual absorption frequency of the processed radio wave absorber, it is not possible to stably manufacture a radio wave absorber having the desired radio wave absorbing characteristics.
[0011] The present disclosure has an object to solve the above-mentioned conventional problems and to provide a molding material for radio wave absorbing members that does not significantly change the radio wave absorbing properties that it had as a molding material even after undergoing a process in which a radio wave absorbing composition is subjected to a high mechanical shear force, such as a molding process or a kneading process, and to provide a radio wave absorber produced using this molding material for radio wave absorbing members. [Means for solving the problem]
[0012] In order to solve the above-mentioned problems, the present application discloses a molding member for a radio wave absorbing material, which comprises a magnetic iron oxide that undergoes magnetic resonance by radio waves with a frequency of 20 GHz to 300 GHz and an organic binder, and is molded into a predetermined shape, wherein the magnetic iron oxide is hexagonal ferrite, and when a point A in a hysteresis curve is magnetized by applying a positive magnetic field of +10 kOe or more and +15 k or less, and a point B is magnetized by reducing the applied magnetic field strength from point A and applying a negative magnetic field of -10 kOe or more and -15 kOe or less, the hysteresis curve from point A to point B is differentiated twice, the apex of the maximum peak in the positive direction is P1 in a curve in the range of an applied magnetic field of 0 to -10 kOe, and the apex of the peak having the next extreme value in the positive direction is P2, the value of P2 / P1 is 0.15 or less.
[0013] The radio wave absorber disclosed in the present application is characterized in that it is produced by molding any one of the molding materials for radio wave absorbers disclosed in the present application. Effect of the Invention
[0014] In the molding material for radio wave absorbing members disclosed in the present application, when the apexes of two peaks in a curve obtained by differentiating a hysteresis curve twice are P1 and P2, the value of P2 / P1 is 0.15 or less. By using such a molding material for radio wave absorbing members, the change in the radio wave absorbing characteristics before and after molding is suppressed within a predetermined range, and a radio wave absorber that is suitable for use in applications where radio waves of a specific frequency are used can be produced. [Brief description of the drawings]
[0015] [Figure 1] 1 is a cross-sectional view illustrating the configuration of a radio wave absorbing sheet, which is a radio wave absorber produced from a molding material for radio wave absorbing members according to this embodiment. [Diagram 2] FIG. 2 is a diagram illustrating a hysteresis loop of a first molding material for an electromagnetic wave absorbing member according to the present embodiment. [Diagram 3] FIG. 3 is a diagram showing a curve obtained by differentiating a hysteresis curve of a first molding material for an electromagnetic wave absorbing member according to the present embodiment. [Figure 4] FIG. 2 is a diagram showing a curve obtained by differentiating twice the hysteresis curve of the first molding material for radio wave absorbing member according to the present embodiment. [Diagram 5] FIG. 2 is a diagram showing the radio wave absorbing characteristics before and after molding of a first molding material for radio wave absorbing member according to the present embodiment. [Figure 6] FIG. 4 is a diagram showing a curve obtained by differentiating twice the hysteresis curve of the second molding material for radio wave absorbing member according to the present embodiment. [Figure 7] FIG. 4 is a diagram showing the radio wave absorbing characteristics before and after molding of the second molding material for radio wave absorbing member according to the present embodiment. [Figure 8] FIG. 11 is a diagram illustrating a hysteresis loop of a fourth molding material for an electromagnetic wave absorbing member according to the present embodiment. [Figure 9] FIG. 11 is a diagram showing a curve obtained by differentiating twice the hysteresis curve of the fourth molding material for radio wave absorbing member according to the present embodiment. [Figure 10] FIG. 11 is a diagram showing the radio wave absorbing characteristics before and after molding of a fourth molding material for radio wave absorbing member according to the present embodiment. [Figure 11] FIG. 2 is a diagram illustrating a hysteresis loop of a molding material for an electromagnetic wave absorbing member of a first comparative example. [Figure 12] FIG. 2 is a diagram showing a curve obtained by differentiating twice the hysteresis curve of the molding material for radio wave absorbing member of the first comparative example. [Figure 13] FIG. 4 is a diagram showing the radio wave absorbing characteristics before and after molding of the molding material for radio wave absorbing members of the first comparative example. [Figure 14] FIG. 11 is a diagram showing a curve obtained by differentiating twice the hysteresis curve of the molding material for radio wave absorbing members of the second comparative example. [Figure 15] FIG. 11 is a diagram showing the radio wave absorption characteristics before and after molding of a molding material for radio wave absorbing members of a second comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The molding material for radio wave absorbing members disclosed in the present application comprises magnetic iron oxide which undergoes magnetic resonance when exposed to radio waves with a frequency of 20 GHz to 300 GHz, and an organic binder, and is molded into a predetermined shape, wherein the magnetic iron oxide is hexagonal ferrite, and when a point A in a hysteresis curve is magnetized by application of a positive magnetic field of +10 kOe or more and +15 k or less, and a point B is magnetized by reducing the applied magnetic field strength from point A and applying a negative magnetic field of -10 kOe or more and -15 kOe or less, the hysteresis curve from point A to point B is differentiated twice, the apex of the maximum peak in the positive direction in a curve in the applied magnetic field range of 0 to -10 kOe is defined as P1, and the apex of the peak having the next extreme value in the positive direction is defined as P2, and the value of P2 / P1 is 0.15 or less.
[0017] In this way, the molding material for radio wave absorbing members disclosed in the present application can suppress the change in radio wave absorbing properties before and after molding within a predetermined range, making it possible to produce a radio wave absorber that suitably absorbs undesired radio waves from devices used in specific fields where the range of frequencies used is regulated.
[0018] In the molding material for radio wave absorbing members disclosed in the present application, the magnetic iron oxide is preferably strontium ferrite.
[0019] The molding material for radio wave absorbing members disclosed in the present application may be one in which a part of the Fe sites of the magnetic iron oxide is substituted with a trivalent metal atom.
[0020] Furthermore, in the molding material for radio wave absorbing members disclosed in the present application, the binder may be any one of a thermosetting rubber, a thermoplastic elastomer, and a thermoplastic resin.
[0021] The radio wave absorber disclosed in the present application is produced by molding any one of the molding materials for radio wave absorbing members disclosed in the present application.
[0022] By using the molding material for radio wave absorbing members disclosed in the present application, the change in radio wave absorbing characteristics before and after molding can be suppressed within a predetermined range, and therefore the radio wave absorbing characteristics of the radio wave absorber after molding can be sufficiently controlled at the molding material stage. Therefore, there is no large difference between the designed absorption frequency and the absorption frequency of the molded body after processing, and it is possible to easily manufacture a radio wave absorber that can be used in electronic devices in specific fields where the range of frequencies used is regulated to prevent undesired radio waves from being emitted or entering the electronic device.
[0023] Hereinafter, the molding material for radio wave absorbing members disclosed in the present application and the radio wave absorber produced by molding this molding material will be described with reference to the drawings.
[0024] (Embodiment) [Radio wave absorber] First, as one embodiment of the radio wave absorber disclosed in the present application, a radio wave absorbing sheet, which is a radio wave absorber, will be described, which is constituted by a radio wave absorbing layer containing particulate magnetic iron oxide and an organic binder.
[0025] FIG. 1 is a cross-sectional view showing the structure of a radio wave absorbing sheet which is a radio wave absorber explained in this embodiment.
[0026] FIG. 1 shows an electromagnetic wave absorbing sheet 1 formed by applying an electromagnetic wave absorbing composition onto a resin sheet 2 serving as a substrate and drying it.
[0027] Note that FIG. 1 is a diagram provided to facilitate understanding of the configuration of the electromagnetic wave absorbing sheet according to this embodiment, and the sizes and thicknesses of the components shown in the diagram are not depicted based on reality.
[0028] The electromagnetic wave absorbing sheet 1 exemplified in this embodiment is formed as an electromagnetic wave absorbing layer containing strontium ferrite powder 1a as magnetic iron oxide powder and a resin binder 1b.
[0029] In FIG. 1, a radio wave absorbing sheet is shown as an example of the radio wave absorber disclosed in the present application, but the radio wave absorber disclosed in the present application can be produced in any shape, such as a block shape or a shape corresponding to the shape of the location where it is to be placed, by injection molding or extrusion molding a molding material for a radio wave absorbing component using a predetermined mold (die).
[0030] The radio wave absorbing sheet 1 exemplified in this embodiment contains, in a binder 1b made of an organic material, strontium ferrite magnetic iron oxide 1a as magnetic iron oxide that magnetically resonates with radio waves of 20 GHz to 300 GHz.
[0031] [Magnetic iron oxide] In the radio wave absorbing sheet 1 according to this embodiment, strontium ferrite is used as the particulate magnetic iron oxide 1a.
[0032] Strontium ferrite is SrFe 12 O 19 By adding Al to the system, the resonance frequency can be increased to 60 GHz to 80 GHz, and a radio wave absorber compatible with 60 GHz band wireless LAN can be fabricated. By adding Al, the frequency at which radio wave absorption is observed shifts to the high frequency side, but this is due to the anisotropic magnetic field (H A This is thought to correspond to an increase in the value of
[0033] In addition, barium ferrite magnetic powder can be used as the hexagonal ferrite magnetic powder used in the radio wave absorbing sheet disclosed in the present application. In M-type (magnetoplumbite type) ferrites containing barium ferrite, the imaginary part (μr'') of the complex permeability related to radio wave absorption becomes high at the frequency at which resonance occurs when the magnetic material is magnetized at high frequency, so the magnetic resonance frequency f is determined by the anisotropic magnetic field (H A ), so the anisotropy magnetic field (H A The higher the magnetic resonance frequency f, the higher the material's magnetic field. 12 O 19 The magnetic resonance frequency f of the H A The value of is calculated to be 1.35MA / m to 48GHz, and it can absorb radio waves in the high GHz band. 3+ Part of (TiMn) 3+ Or Al 3+ By replacing it with A ) can be controlled to control the magnetic resonance frequency f in the range of 5 GHz to 150 GHz.
[0034] [binder] The radio wave absorbing sheet 1 of this embodiment has overall flexibility due to the magnetic iron oxide particles 1a being dispersed in the organic binder 1b.
[0035] As the organic binder 1b used in the molding material for the radio wave absorbing member from which the radio wave absorbing sheet 1 is produced, a thermosetting plastic, a thermoplastic plastic, or an elastomer can be used.
[0036] As thermosetting plastics, phenolic resin (PF), urea resin (UF), melamine resin (MF), unsaturated polyester (UP), epoxy resin (EP), silicone resin (SI), and polyurethane (PUR) can be used.
[0037] Thermoplastics include general-purpose plastics, engineering plastics, and super engineering plastics. General-purpose plastics include polyvinyl chloride (PVC), polyethylene (PE), polypropylene (PP), polystyrene (PS), acrylonitrile-butadiene-styrene (ABS), acrylonitrile-styrene (AS), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyvinylidene chloride (PVDC), and polyethylene terephthalate (PET).
[0038] As the engineering plastic, polyamide (PA), polyacetal (POM), polycarbonate (PC), polyolefin ether (PPE), polybutylene terephthalate (PBT), ultra-high molecular weight polyethylene (U-EP), and polyvinylidene fluoride (PVDF) can be used.
[0039] Examples of super engineering plastics that can be used include polysulfone (PSU), polyethersulfone (PES), polyphenylene sulfide (PPS), polyarylate (PAR), polyamide-imide (PAI), polyetherimide (PEI), polyetheretherketone (PEEK), polyimide (PI), liquid crystal polymer (LCP), and polytetrafluoroethylene (PTFE).
[0040] Elastomers also include thermosetting rubber (vulcanized rubber) and thermoplastic elastomers. Thermosetting rubber (vulcanized rubber) can be styrene butadiene rubber (SBR), nitrile rubber (NBR), butadiene rubber (BR), chloroprene rubber (CR), ethylene propylene diene rubber (EPDM), butyl rubber (IIR), isobutylene rubber (IR), acrylic rubber (ACM), and silicone rubber (Q).
[0041] Examples of thermoplastic elastomers that can be used include softened polyvinyl chloride, heat-resistant polyvinyl chloride, ethylene-vinyl acetate copolymer (EVA), ethylene propylene rubber (EPR), styrene-based TPE (TPS), olefin-based TPE (TPO), urethane-based TPE (TPU), polyester-based (TPPE), and chlorinated polyethylene.
[0042] From the viewpoint of environmental consideration, it is preferable to use an organic material that does not contain halogen as the binder. These resin materials are commonly used as binder materials for resin sheets and are therefore easily available.
[0043] Here, in this specification, having flexibility indicates a state in which the radio wave absorbing sheet 1 can be curved to a certain degree, that is, a state in which the radio wave absorbing sheet 1 returns to its original shape without plastic deformation such as breakage when it is returned to its original shape after being curved. Also, in the case where the radio wave absorber is not in a sheet shape but is a block body having a certain thickness or more, for example, when an external force is applied while holding both ends of the radio wave absorber, the radio wave absorber will bend, and when this external force is released, the radio wave absorber can easily return to its original shape.
[0044] As a molding material for radio wave absorbing members for forming the radio wave absorber 10, it is important to disperse the magnetic iron oxide powder well in the binder made of an organic material. For this reason, the binder 2 may contain, as a dispersant, arylsulfonic acids such as phenylphosphonic acid and phenylphosphonic acid dichloride, alkylphosphonic acids such as methylphosphonic acid, ethylphosphonic acid, octylphosphonic acid, and propylphosphonic acid, or polyfunctional phosphonic acids such as hydroxyethanediphosphonic acid and nitrotrismethylenephosphonic acid. These phosphoric acid compounds have flame retardancy and function as dispersants for the magnetic iron oxide powder, so that the magnetic iron oxide in the binder can be dispersed well.
[0045] More specifically, examples of dispersants that can be used include phenylphosphonic acid (PPA) manufactured by Wako Pure Chemical Industries, Ltd. or Nissan Chemical Industries, Ltd., and oxidized phosphoric acid ester "JP-502" (product name) manufactured by Johoku Chemical Industry Co., Ltd.
[0046] As an example of the composition of the molding material for radio wave absorbing members, the content of the organic binder is 2 to 50 parts and the content of the phosphate compound is 0.1 to 15 parts per 100 parts of magnetic iron oxide powder. If the content of the organic binder is less than 2 parts, the magnetic iron oxide cannot be dispersed well. In addition, the specified shape of the radio wave absorber cannot be maintained. If the content is more than 50 parts, the volume content of the magnetic iron oxide in the radio wave absorber becomes small, and the magnetic permeability becomes low, resulting in a reduced radio wave absorption effect.
[0047] If the content of the phosphate compound is less than 0.1 parts, the magnetic iron oxide cannot be dispersed well using a resin binder. If it is more than 15 parts, the effect of dispersing the magnetic iron oxide well is saturated. The volume content of the magnetic iron oxide in the radio wave absorbing layer is reduced, and the magnetic permeability is reduced, resulting in a reduced radio wave absorption effect.
[0048] [Method of manufacturing radio wave absorber] Here, an example of a method for manufacturing the radio wave absorber according to this embodiment will be described.
[0049] The molding material for radio wave absorbing members according to this embodiment is prepared as a magnetic compound containing magnetic iron oxide powder, a binder made of an organic material such as rubber, and an appropriate filler, etc. The magnetic compound can be obtained by kneading the magnetic iron oxide powder and the binder, mixing the obtained kneaded product with a crosslinking agent, and adjusting the viscosity.
[0050] As shown in FIG. 1, a radio wave absorbing sheet 1 serving as a radio wave absorber can be produced by applying a magnetic compound to a predetermined thickness, drying it, and then performing a calendar treatment.
[0051] When preparing the electromagnetic wave absorbing sheet 1, the magnetic compound prepared above is applied onto a resin sheet 2 as shown in FIG. 1. As an example of the resin sheet 2, a polyethylene terephthalate (PET) sheet having a thickness of 38 μm, the surface of which is subjected to a release treatment by a silicone coat, can be used. The magnetic compound is applied onto the resin sheet 2 by a coating method such as a table coater method or a bar coater method. Thereafter, the wet magnetic compound is dried and further subjected to a calendaring treatment. The thickness of the electromagnetic wave absorbing sheet 1 can be controlled by the coating thickness, the conditions of the calendaring treatment, and the like. The electromagnetic wave absorbing sheet 1 after the calendaring treatment is peeled off from the resin sheet 2 to obtain an electromagnetic wave absorbing sheet 1 having a desired thickness. The calendaring treatment may be performed as necessary, and if the volume content of the magnetic iron oxide powder is within a predetermined range in the dried state of the magnetic compound, the calendaring treatment may not be performed.
[0052] In addition, when the formed radio wave absorbing sheet 1 is too thin to obtain a predetermined strength required for the radio wave absorbing sheet 1, the resin sheet 2 used as the base material can be used as a base film, and the radio wave absorbing sheet 1 can be laminated on the resin base film 2. When the resin sheet 2 is used as the base film, in addition to various resin films such as the above-mentioned PET film, rubber and paper materials such as Japanese paper can be used. Since the material and thickness of the base film do not affect the radio wave absorbing characteristics of the radio wave absorbing sheet 1, a base film made of an appropriate material and having an appropriate thickness can be selected from the practical viewpoint of the strength of the radio wave absorbing sheet, ease of handling, etc.
[0053] Next, a method for producing a radio wave absorber having a desired shape will be described.
[0054] As an example, when using a rubber binder, 80 parts by weight of strontium ferrite as the magnetic iron oxide powder and 18 parts by weight of silicone rubber KE-510-U (product name: manufactured by Shin-Etsu Chemical Co., Ltd.) as the rubber binder are kneaded in a batch kneader with pressure. 2 parts by weight of 2.5 dimethyl-2.5 bishexane C-8A (product name: manufactured by Shin-Etsu Chemical Co., Ltd.) as the crosslinking agent are mixed into this kneaded mixture.
[0055] The molding material for radio wave absorbing members thus obtained is vulcanized and molded using a press molding machine into a desired shape such as a sheet, an O-ring (packing), etc. As described above, the radio wave absorber disclosed in the present application is based on silicone rubber, and therefore has the deformability to curve as a whole and absorb unevenness to a certain degree, and for example, by arranging it so as to cover a specific circuit component that is mounted on a circuit board and becomes a noise source, it is possible to wrap around the noise source electronic component without any gaps and improve the shielding performance against undesired leaked radio waves.
[0056] When preparing a radio wave absorber in a block shape such as a rectangular parallelepiped, the magnetic compound, which is the molding material for radio wave absorbing members, is crosslinked and molded into a sheet shape at a temperature of 150°C, for example, using a hydraulic press. After that, a secondary crosslinking process is performed in a thermostatic chamber at a temperature of, for example, 170°C, to form a radio wave absorber of a predetermined shape. In this way, when a rubber-based binder is used, the absorber can be prepared by direct molding using heat vulcanization by pressing.
[0057] When a thermoplastic resin is used as the binder, 80 parts by weight of strontium ferrite as the magnetic iron oxide powder and 20 parts by weight of nylon 6 1013B (product name: manufactured by Ube Industries, Ltd.) as the thermoplastic resin are kneaded in a pressurized batch kneader.
[0058] The molding material for radio wave absorbing members thus obtained is injection molded using an injection molding machine to be molded into a desired shape such as a bracket, cover, etc. As described above, the radio wave absorber disclosed in the present application is based on nylon 6, and therefore has overall toughness and strength. For this reason, it is suitably used as a radio wave absorber to be disposed in, for example, an in-vehicle millimeter wave radar for collision prevention that is accompanied by vibration, and can absorb and suppress unwanted radio waves that are diffusely reflected among the radio waves irradiated from the radar.
[0059] [Adhesive layer] Although not shown in Fig. 1, an adhesive layer can be formed on at least a part of the surface of the radio wave absorber so that the radio wave absorber according to this embodiment can be easily fixed to a predetermined position. In particular, in the case of a thin block-shaped radio wave absorber, by providing an adhesive layer on at least one of its main surfaces, the radio wave absorber can be easily attached to a desired position on the inner surface of a housing that houses an electric circuit or on the inner or outer surface of an electric device. In particular, since the radio wave absorber according to this embodiment has elasticity due to the use of a rubber binder, the adhesive layer 2 can easily attach the radio wave absorber to a curved surface, improving the ease of handling of the radio wave absorber.
[0060] The adhesive layer may be a known material used as an adhesive layer for adhesive tapes, an acrylic adhesive, a rubber adhesive, a silicon adhesive, or the like. A tackifier or a crosslinking agent may also be used to adjust the adhesive strength to the adherend and reduce adhesive residue. The adhesive strength to the adherend is preferably 5N / 10mm to 12N / 10mm. If the adhesive strength is less than 5N / 10mm, the radio wave absorber may easily peel off or shift from the adherend. If the adhesive strength is more than 12N / 10mm, the radio wave absorber may be difficult to peel off from the adherend.
[0061] The thickness of the adhesive layer is also preferably a predetermined thickness, for example, about 20 μm to 1 mm or more, so that the radio wave absorber does not easily peel off. When the radio wave absorber is reattached as appropriate, it is necessary to consider the adhesive strength and thickness of the adhesive layer so that the adherend is not damaged when peeled off from the adherend, the radio wave absorber is not damaged, and glue residue is not left behind.
[0062] Furthermore, when adhering the radio wave absorber to a predetermined surface, even if the radio wave absorber does not have an adhesive layer, it is possible to attach the radio wave absorber by providing adhesiveness to the surface of the member on which the radio wave absorber is to be placed. Also, by using double-sided tape or adhesive, the radio wave absorber can be attached to a predetermined portion. In this respect, it is clear that the adhesive layer is not an essential component of the radio wave absorber shown in this embodiment.
[0063] [Radio wave absorption characteristics] The magnetic properties stipulated for the molding material for radio wave absorbing members disclosed in the present application will be specifically described below.
[0064] In measuring the magnetic properties, a radio wave absorber containing a specified magnetic iron oxide was cut to prepare a disk-shaped sample with a diameter of 8 mmφ and a thickness of 0.1 mm to 10 mm, and the applied magnetic field was measured in the range of -15 kOe to +15 kOe using a vibration sample magnetometer VSM-P7 (product name) manufactured by Toei Industry Co., Ltd. The measurement time constant Tc was 0.03 sec, the drawing step was 40 bits, and the wait time was 0.2 sec.
[0065] The average particle size of the magnetic iron oxide was measured as follows.
[0066] Using a Hitachi scanning electron microscope (SEM) "S-4800 (product name)", photographs were taken with an accelerating voltage of 2 kV, magnification of 10,000 times, and observation conditions of U-LA100. The maximum diameter of 100 particles of iron oxide powder in one field of view was measured, and the simple average of the measured particle diameters was taken as the average particle diameter.
[0067] FIG. 2 is a graph showing a magnetization curve of the first molding material for radio wave absorption member according to this embodiment.
[0068] The first molding material for radio wave absorbing members (hereinafter, appropriately referred to as "molding material of Example 1") used 79 parts by weight of strontium ferrite as magnetic iron oxide powder, 17 parts by weight of nylon 6 (1013B (product name) manufactured by Ube Industries, Ltd.) as a binder, and 4 parts by weight of a low-volatile carboxylic acid derivative as a dispersant. The average particle diameter of the strontium ferrite was 3.6. μ It was m.
[0069] The magnetic iron oxide powder, binder material, and dispersant were stirred in a tumbler, and then continuously mixed in a twin-screw extruder (15 nmφ, L / D=45) at a temperature of 235°C to 270°C and a screw rotation speed of 100 rpm. The strand-like mixture extruded from the nozzle was cooled with water and cut into 3 mm lengths using a pelletizer to prepare molding materials, and molded bodies measuring 120 mm square and 2 mm thick were produced using an injection molding machine.
[0070] From this molded body, a disk-shaped sample of Example 1 having a diameter of 8 mm and a thickness of 1 mm was prepared.
[0071] As shown in Figure 2, the magnetization curve, which indicates the strength of magnetization remaining in magnetic iron oxide when an external magnetic field of varying strength is applied, draws a so-called hysteresis curve.
[0072] Anisotropic magnetic field (H A The relationship shown in the following formula (1) holds between the value of φ ) and the magnetic resonance frequency fr of the magnetic material.
[0073] fr=ν / 2π*H A (1) Here, ν is the gyromagnetic constant, and its value is determined depending on the type of magnetic material.
[0074] Thus, in the gyromagnetic resonance type magnetic material, the anisotropic magnetic field (H A ) is proportional to the magnetic resonance frequency fr.
[0075] For example, different anisotropy fields (H A ), magnetic resonance occurs at different frequencies, converting radio waves of the corresponding frequencies into heat and attenuating them. As a result, radio waves of a specific different frequency can be absorbed. In addition, the anisotropic magnetic field (H A It is known that the size of the magnetic iron oxide varies depending on its particle size. Therefore, by analyzing the hysteresis curve of magnetic iron oxide, it is possible to understand the particle size distribution of magnetic iron oxide contained in a sample.
[0076] Fig. 3 is a diagram showing a curve (SFD: Switching Field Distribution) obtained by differentiating the hysteresis curve of the molding material of Example 1 shown in Fig. 2 from point A where the applied magnetic field is +15 kOe to point B where the applied magnetic field is -15 kOe. Note that Fig. 3 shows the SFD curve for applied magnetic fields from 0 kOe to -10 kOe.
[0077] More specifically, in the measurement device described in this embodiment, since the hysteresis curve shown in FIG. 2 is drawn from point A to point B using 637 pieces of data, linear least-squares approximation was performed for the 11th to 627th measurement points, including 10 points before and after the 11th measurement point, for a total of 21 points, and the slope of the obtained approximation equation was taken as the differential value at that measurement point (the value obtained by first differentiation).
[0078] Fig. 4 is a diagram showing a curve obtained by differentiating twice from point A, where the applied magnetic field is +15 kOe, to point B, where the applied magnetic field is -15 kOe, of the hysteresis curve of the molding material of Example 1 shown in Fig. 2. Fig. 4 also shows a twice-differentiated curve from an applied magnetic field of 0 kOe to -10 kOe.
[0079] Specifically, the differential values at each of the measurement points from the 11th to the 627th points on the hysteresis curve shown in Figure 2 were again subjected to least squares approximation of the differential values at the measurement points from the 21st to the 617th points, as well as the differential values at the measurement points 10 points before and after each of the measurement points, for a total of 21 measurement points, to determine the slope of a straight line, and this value was taken as the second derivative value (the value obtained by differentiating twice) of the hysteresis curve at that measurement point.
[0080] In the molding material of Example 1 of this embodiment, as shown in FIG. 4, the first positive peak P1 (3.12×10 -6 ), and a second positive peak P2 (4.33×10 -7 ) appears. From these P1 and P2, we can calculate P2 / P1 to be 0.14.
[0081] FIG. 5 shows the radio wave absorbing characteristics of the molding material of Example 1 and the radio wave absorbing characteristics of the first radio wave absorber obtained by injection molding the molding material of Example 1.
[0082] As for the radio wave absorption characteristics, the amount of radio wave absorption (amount of radio wave attenuation) was measured using the free space method. Specifically, using Anritsu Corporation's millimeter wave network analyzer ME7838A (product name), an input wave (millimeter wave) of a specific frequency was irradiated from a transmitting antenna through a dielectric lens to each of sample 1 or the radio wave absorber made from sample 1, and the transmitted radio wave was measured by a receiving antenna placed on the back side. The strength of the irradiated radio wave and the strength of the transmitted radio wave were grasped as voltage values, and the amount of radio wave attenuation was calculated in dB from the difference in strength.
[0083] As shown in FIG. 5, the difference in absorption peak frequency between the radio wave absorption characteristics of the molding material of Example 1 (reference symbol 5a) and the radio wave absorption characteristics of the radio wave absorber molded using the molding material of Example 1 (reference symbol 5b) is small at 0.1 GHz, and the curves showing the two radio wave absorption characteristics almost overlap, confirming that the change in the radio wave absorption characteristics before and after the molding process was small.
[0084] Next, a molding material for a radio wave absorbing member of Example 2 was prepared using strontium ferrite as the magnetic iron oxide, and a molding material for a radio wave absorbing member of Example 3 was prepared using strontium ferrite as the magnetic iron oxide.
[0085] Furthermore, a molding material for a radio wave absorbing member of Example 4 using barium ferrite as the magnetic iron oxide and a molding material for a radio wave absorbing member of Example 5 using barium ferrite as the magnetic iron oxide were prepared. Details of the molding materials of Examples 2 to 5 are as follows.
[0086] [Example 2] As magnetic iron oxide powder, the average particle size is 4.1 μ The same procedure was followed as in Example 1, except that strontium ferrite of 0.1 m was used.
[0087] [Example 3] Magnetic iron oxide powder with an average particle size of 2.3 μ The same procedure was followed as in Example 1, except that strontium ferrite of 0.1 m was used.
[0088] [Example 4] As magnetic iron oxide powder, the average particle size is 4.8 μ m Barium ferrite The same procedure was followed as in Example 1, except that the following was used:
[0089] [Example 5] Magnetic iron oxide powder with an average particle size of 5.0 μ m Barium ferrite The same procedure was followed as in Example 1, except that the following was used:
[0090] Furthermore, as comparative examples, Comparative Example 1 and Comparative Example 2, which are molding materials for radio wave absorbing members using strontium ferrite as the magnetic iron oxide, and Comparative Example 3, which uses barium ferrite as the magnetic iron oxide, were prepared. Details of the molding materials for radio wave absorbing members of Comparative Example 1, Comparative Example 2, and Comparative Example 3 are as follows.
[0091] [Comparative Example 1] Magnetic iron oxide powder with an average particle size of 4.1 μ The composition was the same as in Example 1 except that strontium ferrite of 0.01 m was used, magnetic iron oxide powder was 82 parts by weight, nylon 6 was 18 parts by weight, and no low-volatile carboxylic acid derivative was used.
[0092] [Comparative Example 2] As magnetic iron oxide powder, the average particle size is 49.4 μ The same procedure was followed as in Example 1, except that strontium ferrite of 0.1 m was used.
[0093] [Comparative Example 3] As magnetic iron oxide powder, the average particle size is 5.5 μ m Barium ferrite The same procedure was followed as in Example 1, except that the following was used:
[0094] For the molding materials of Examples 2 and 4, and further for the molding materials of Comparative Examples 1 and 2, the magnetic properties as a molding material for a radio wave absorbing component were measured in the same manner as for the molding material of Example 1 described above, and the obtained hysteresis curve was differentiated twice from point A to point B.
[0095] FIG. 6 shows a curve obtained by differentiating the hysteresis curve of the molding material of Example 2 twice.
[0096] FIG. 7 is a diagram showing the radio wave absorbing characteristics of the molding material of Example 2 in a state where it is used as a molding material for a radio wave absorbing member, and the radio wave absorbing characteristics of a radio wave absorber obtained by injection molding the molding material.
[0097] As shown in FIG. 6, the curve obtained by differentiating the hysteresis curve twice shows the first positive peak P1 (3.99×10 -6 ), and a second positive peak P2 (6.02×10 -7 ) appears. From these P1 and P2, we can calculate P2 / P1 to be 0.15.
[0098] Moreover, when comparing the radio wave absorption characteristics of the molded member of Example 2 (reference symbol 7a) shown in Fig. 7 with the radio wave absorption characteristics of a radio wave absorber molded using the molded member of Example 2 (reference symbol 7b), it can be confirmed that by molding into a radio wave absorber, the absorption curve is shifted to the lower frequency side compared to before molding. However, the respective peak absorption frequencies are 77 GHz and 76 GHz, and the shift in the absorption peak frequency is only 0.9 GHz. In addition, it can be confirmed that the transmission attenuation, which indicates the absorption capacity, is about 14.5 dB, and almost the same absorption characteristics are obtained for both.
[0099] FIG. 8 is a diagram showing a hysteresis curve of the molded member of Example 4.
[0100] Since the magnetic iron oxide of the molded part of Example 4 is barium ferrite, it is clear that the shape of the hysteresis curve is different from that of the molding material for radio wave absorption parts of Example 1, which uses strontium ferrite as the magnetic iron oxide shown in Figure 2.
[0101] In this case as well, as shown in FIG. 8, a curve is obtained by differentiating twice from point A where the applied magnetic field is +15 kOe to point B where the applied magnetic field is -15 kOe.
[0102] Fig. 9 is a diagram showing a curve obtained by differentiating the hysteresis curve of the molded member of Example 4 twice from point A to point B. Note that Fig. 9 also shows a second-order differential curve for an applied magnetic field from 0 kOe to -10 kOe, similar to Figs. 4 and 6.
[0103] As shown in FIG. 9, the curve obtained by differentiating the hysteresis curve twice has a first positive peak P1 (1.33×10 -5 ), and a second positive peak P2 (5.84×10 -7 ) appears. From these P1 and P2, we can calculate P2 / P1 to be 0.04.
[0104] Furthermore, when comparing the radio wave absorption characteristics of the molded member of Example 4 shown in FIG. 10 (reference symbol 10a) with the radio wave absorption characteristics of the radio wave absorber molded using the molded member of Example 4 (reference symbol 10b), it is found that the shift in the absorption peak frequency before and after molding is approximately 0 GHz, and the radio wave absorption characteristics are almost unchanged.
[0105] Next, the case of a molding material for radio wave absorbing members as a comparative example will be considered.
[0106] FIG. 11 shows a hysteresis curve of the molding material of Comparative Example 1, which is a molding material for radio wave absorbing members, which is a sample prepared as a comparative example.
[0107] Fig. 12 is a diagram showing a curve obtained by differentiating the hysteresis curve of the molding material of Comparative Example 1 twice from point A to point B. Note that Fig. 12 also shows a second-order differential curve from an applied magnetic field of 0 kOe to -10 kOe, similar to Figs. 4, 6, and 9.
[0108] As shown in FIG. 12, the curve obtained by differentiating the hysteresis curve of the molding material of Comparative Example 2 twice has a first positive peak P1 (3.54×10 -6 ), and a second positive peak P2 (6.14×10 -7 ) appears. From these P1 and P2, we can calculate P2 / P1 to be 0.17.
[0109] FIG. 13 is a diagram showing the radio wave absorbing characteristics of the molded member of Comparative Example 1 in a state as a molding material for a radio wave absorbing member, and the radio wave absorbing characteristics of the radio wave absorber after injection molding.
[0110] When comparing the radio wave absorption characteristics (reference symbol 13a) of the molding material of Comparative Example 1 shown in Fig. 13 with the radio wave absorption characteristics (reference symbol 13b) of the radio wave absorber after molding, it can be confirmed that by molding into a radio wave absorber, the absorption characteristics are shifted to the lower frequency side compared to before molding. As shown in Fig. 13, the peak absorption frequency in the radio wave absorption characteristics (reference symbol 13a) of the molded member of Comparative Example 1 is about 77.3 GHz, whereas the peak absorption frequency in the radio wave absorption characteristics (reference symbol 13b) of the radio wave absorber molded using the molded member of Comparative Example 1 is about 76.1 GHz, indicating a shift in the absorption peak frequency of about 1.2 GHz.
[0111] Fig. 14 is a diagram showing a curve obtained by differentiating the hysteresis curve of the molding material of Comparative Example 2 twice from point A to point B. Note that Fig. 14 also shows a second-order differential curve from an applied magnetic field of 0 kOe to -10 kOe, similar to Figs. 4, 6, 9, and 12.
[0112] As shown in FIG. 14, the curve obtained by differentiating the hysteresis curve twice has a first positive peak P1 (3.44×10 -6 ), and a second positive peak P2 (11.16×10 -6 ) appears. From these P1 and P2, we can calculate P2 / P1 to be 0.34.
[0113] FIG. 15 is a diagram showing the radio wave absorbing properties of the molding material of Comparative Example 2 in a state as a molding material for radio wave absorbing members, and the radio wave absorbing properties of the radio wave absorber after injection molding.
[0114] When comparing the radio wave absorption characteristics (symbol 15a) of the molding material of Comparative Example 2 shown in FIG. 15 with the radio wave absorption characteristics (symbol 15b) of the radio wave absorber after molding using Comparative Example 2, it can be seen that by molding into a radio wave absorber, the peak absorption frequency of the radio wave absorption characteristics (symbol 15a) of the molding material is approximately 77.5 GHz, while the peak absorption frequency of the radio wave absorption characteristics (symbol 15b) of the radio wave absorber molded using Comparative Example 2 is approximately 75.6 GHz, resulting in a shift of approximately 1.9 GHz in the absorption peak frequencies.
[0115] The above measurement results, as well as the measurement results of the P1, P2, P2 / P1 values and the peak frequency deviation amounts for the molded parts of Example 3, Example 5, and Comparative Example 3, are summarized in Table 1 below.
[0116] [Table 1]
[0117] The reason why the shift in the absorption peak frequency was larger in the molding material of Comparative Example 3 than in the molding materials of Examples 4 and 5, which also used barium ferrite magnetic powder as the magnetic iron oxide, is that, like the molding material of Comparative Example 2 described above, the average particle diameter of the barium ferrite magnetic powder was large, so the particle diameter changed due to the shear force applied to the particles in the injection molding process, resulting in a difference in the effective average particle diameter before and after injection molding, and the anisotropic magnetic field (H A ) is thought to be the cause.
[0118] For example, the frequency of radio waves is specified depending on the intended use, such as 76.5 GHz±0.5 GHz for in-vehicle radar, etc. For this reason, if the peak absorption frequency that was grasped at the stage of the molding material for radio wave absorbing members shifts significantly in the state of the radio wave absorber after molding processing, as in the molded member of Comparative Example 1 and the molded member of Comparative Example 2, the performance as a radio wave absorber used in the originally intended technical field will be significantly reduced.
[0119] For this reason, if it is known at the stage of the molding material for radio wave absorbing components that the shift in the peak frequency of the absorbed radio waves before and after molding is small, there will be no large difference between the designed absorption frequency and the absorption frequency of the molded body after processing, making it possible to manufacture the radio wave absorber with peace of mind, and by not using a material that causes a large shift, the yield of the radio wave absorber can be improved and costs can be reduced.
[0120] In view of this, the molding material for radio wave absorbing members disclosed in the present application is specified such that, when the point A in a hysteresis curve where magnetization is achieved by applying a positive magnetic field of +10 kOe or more and +15 kOe or less is defined as point A, and the point B where magnetization is achieved by reducing the applied magnetic field strength from point A and applying a negative magnetic field of -10 kOe or more and -15 kOe or less is defined as point B, the apex of the maximum peak in the positive direction in a curve where the applied magnetic field ranges from 0 to -10 kOe obtained by differentiating the hysteresis curve from point A to point B is defined as P1, and the apex of the peak having the next extreme value in the positive direction is defined as P2, the value of P2 / P1 is specified to be 0.15 or less. By specifying in this way, the molding material for radio wave absorbing members disclosed in the present application can suppress the change in radio wave absorption characteristics before and after molding into a radio wave absorber, and can realize a radio wave absorber that satisfactorily absorbs radio waves of a predetermined frequency.
[0121] In the above measurement, the amount of shift in the absorption peak frequency before and after injection molding was measured; however, when magnetic iron oxide powder was mixed with a resin binder to prepare an electromagnetic wave absorbing paste and this was used to prepare a sheet-shaped electromagnetic wave absorbing sheet, it was confirmed that, as in the case of injection molding, the amount of shift between the absorption peak frequency in the molding material state and the absorption peak frequency after molding into a sheet could be suppressed to 1 GHz or less, as long as the P2 / P1 value was 0.15 or less.
[0122] In addition to the strontium ferrite and barium ferrite exemplified in the above embodiment, other hexagonal ferrites such as Pb ferrite are also thought to exhibit similar radio wave absorption characteristics. However, Pb ferrite is not suitable for practical use because it contains lead.
[0123] Furthermore, in the above embodiment, it has been described that the absorption frequency peak can be shifted by substituting a part of the Fe site of the hexagonal ferrite with Al. However, the metal to be substituted may be gallium, Ti-Cu-Zn, rhodium, or the like, other than aluminum.
[0124] As described above, the molding material for radio wave absorbing components disclosed in the present application and the radio wave absorber obtained by molding the same have two peak values P1 and P2 in the curve obtained by twice differentiating the hysteresis curve of the molding material, and the P2 / P1 value is 0.15 or less, so that the shift in the radio wave absorption characteristics, particularly the absorption peak frequency, before and after molding can be limited within a certain range (approximately 1 GHz).
[0125] The strength of the external magnetic field for measuring the hysteresis curve is set to 15 kOe to -15 kOe because applying an external magnetic field in at least this range will result in a good hysteresis curve. Therefore, there is no problem even if the absolute value of the applied external magnetic field is greater than 15 kOe, and it is sufficient to measure the hysteresis curve when the external magnetic field is in the range of 15 kOe to -15 kOe, and obtain the values of P1 and P2 from the second derivative curve. [Industrial Applicability]
[0126] The molding material for radio wave absorbing members disclosed in the present application is useful as a molding material that can absorb radio waves of 20 GHz to 300 GHz well and suppresses changes in radio wave absorbing properties before and after molding. In addition, a radio wave absorber molded using this molding material can be produced at low cost as a radio wave absorber in which fluctuations in the radio wave absorbing properties are suppressed within a certain range, and is therefore extremely useful in practical use. [Explanation of symbols]
[0127] 1a Magnetic iron oxide particles 1b Binder 10. Radio wave absorber
Claims
1. A molding material for a radio wave absorbing member, which comprises a magnetic iron oxide that undergoes magnetic resonance by radio waves having a frequency of 20 GHz to 300 GHz and an organic binder, and is molded into a predetermined shape, The magnetic iron oxide is a hexagonal ferrite having the same composition, A molding material for radio wave absorbing members, characterized in that, in a hysteresis curve, when a point A is magnetized by applying a positive magnetic field of +10 kOe or more and +15 kOe or less, and when a point B is magnetized by reducing the applied magnetic field strength from point A and applying a negative magnetic field of -10 kOe or more and -15 kOe or less, the applied magnetic field strength is reduced from point A, the apex of the maximum peak in the positive direction in a curve in which the applied magnetic field ranges from 0 to -10 kOe obtained by differentiating the hysteresis curve twice from point A to point B is defined as P1, and the apex of the peak having the next extreme value in the positive direction is defined as P2, the value of P2 / P1 is 0.15 or less.
2. 2. The molding material for radio wave absorbing members according to claim 1, wherein the magnetic iron oxide is strontium ferrite.
3. 3. The molding material for radio wave absorbing members according to claim 1, wherein a part of the Fe sites of the magnetic iron oxide is substituted with a trivalent metal atom.
4. 4. The molding material for radio wave absorbing members according to claim 1, wherein the binder is any one of a thermosetting rubber, a thermoplastic elastomer, and a thermoplastic resin.
5. 5. A radio wave absorber produced by molding the molding material for radio wave absorbing members according to claim 1.
Citation Information
Patent Citations
Magnetic powder for radio wave absorber and radio wave absorber
JP2012216865A
Broadband electromagnetic wave absorber and method for manufacturing the same
JP2013526775A
Radiowave absorber, method for producing the same, and high frequency module
JP2018154541A
Electromagnetic wave absorbing sheet
JP2019071426A
Magnetic material, manufacturing method thereof, and electromagnetic wave absorbing sheet
JP2019145534A