Preparation method of black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material

Through the aramid nanofiber aerogel material carrying black phosphorus, the problem of insufficient mechanical properties and stability of existing electromagnetic shielding materials is solved by using two solvent exchange and vacuum freeze-drying processes, and the efficient electromagnetic shielding performance improvement is achieved and Material performance optimization.

CN118994714APending Publication Date: 2024-11-22CHAMBROAD CHEM IND RES INST CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411259308.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The mechanical properties and stability of existing electromagnetic shielding materials are poor, which limits their application in microelectronics, communications and other fields.

Method used

Aramid nanofiber aerogel material carrying black phosphorus was used to prepare aramid nanofiber hydrogel by stirring in a potassium hydroxide/DMSO/water mixing system, and two solvent exchanges and vacuum freeze-drying to form excellent mechanics. Composite material with performance and electromagnetic shielding capability.

Benefits of technology

It significantly improves the electromagnetic shielding performance of aramid nanofiber aerogel, with a porosity of 98.9%, and reduces material density and improves flexibility and strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994714A_ABST
    Figure CN118994714A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, which comprises the following specific steps: stirring para-aramid fibers in a potassium hydroxide and DMSO mixed system to obtain aramid nanofiber hydrogel, carrying out suction filtration, placing the aramid nanofiber hydrogel in a tert-butyl alcohol aqueous solution for two times of solvent exchange, and drying to obtain the black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material. Adding the black phosphorus dispersion liquid into the aramid nanofiber hydrogel, stirring to obtain black phosphorus / aramid nanofiber mixed hydrogel, and finally performing vacuum freeze drying to obtain black phosphorus / aramid nanofiber aerogel; when the aerogel is prepared, a tert-butyl alcohol aqueous solution with a certain volume fraction is adopted for solvent replacement, so that the pore size of the aerogel is regulated and controlled; the obtained aerogel has excellent mechanical properties and certain electromagnetic shielding capability, the porosity of the shielding material reaches 98.9%, and the electromagnetic shielding performance of the aramid nanofiber aerogel is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to functional porous materials and preparation methods thereof, and in particular relates to a preparation method of black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material. Background Art

[0002] With the development of modern science and technology, and the human society's requirements for high-efficiency electronic instruments, electronic and electrical equipment are gradually transitioning towards high integration, miniaturization and light weight. The electromagnetic radiation generated by various instruments will cause harm to the normal production and life of society. It is estimated that electrical and electronic equipment around the world will cause equipment failures due to electromagnetic radiation, causing inestimable economic losses every year. Long-term exposure to electromagnetic radiation can even cause great harm to the body. Therefore, alleviating or blocking the pollution caused by electromagnetic radiation has become an important research direction in the field of materials science. Traditional electromagnetic shielding materials involve metals such as silver, copper, aluminum alloy, stainless acid-resistant steel, etc. Although metals have excellent shielding effects on electromagnetic radiation, due to factors such as difficult processing, easy corrosion and high density, their application in microelectronics, communications and other fields is limited to a certain extent.

[0003] Aramid fiber, the full name of which is "aromatic polyamide fiber", was successfully developed and commercialized by DuPont in the United States. Aramid fiber is a long chain formed by at least 85% of amide groups directly connected to two aromatic rings. It has excellent properties such as ultra-high strength, ultra-high modulus, ultra-high temperature resistance, acid and alkali resistance and light weight. At a temperature of 550°C, it does not decompose or melt, so it can work normally under high temperature conditions. It also has good insulation and anti-aging properties, has a long life cycle, and is widely used in aerospace, bulletproof materials, automotive industry, ships, sports equipment and other fields. Aramid nanofiber aerogel prepared with aramid as raw material theoretically has excellent mechanical properties, good thermal stability, high porosity, low density and high specific surface area. Aramid nanofibers are light, non-toxic and pollution-free, have strong environmental adaptability and strong molecular designability. They are ideal matrix materials in many fields including paper products, electronic and electrical and functional materials. At present, the application of aramid nanofibers is mainly concentrated in filtration, adsorption, supercapacitors, insulation materials, electromagnetic shielding and energy storage materials. Summary of the invention

[0004] In order to solve the problem that the existing electromagnetic shielding materials have poor mechanical properties and stability, the present invention provides a method for preparing black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding materials with different pores, wherein para-aramid fibers are placed in a potassium hydroxide / DMSO / water mixed system and stirred to obtain aramid nanofiber hydrogel, and after filtration, the aramid nanofiber hydrogel is placed in a tert-butyl alcohol aqueous solution for two solvent exchanges, and then a black phosphorus dispersion is added to the aramid nanofiber hydrogel and stirred to obtain a black phosphorus / aramid nanofiber mixed hydrogel, and the filter cake after vacuum-assisted filtration is subjected to supercritical drying and vacuum freeze drying to obtain a black phosphorus / aramid nanofiber aerogel; when preparing the aerogel, a tert-butyl alcohol aqueous solution with a certain volume fraction is used for solvent replacement to adjust the pore size of the aerogel; the obtained aerogel has excellent mechanical properties and a certain electromagnetic shielding ability, and the porosity of the shielding material reaches 98.9%, which greatly improves the electromagnetic shielding performance of the aramid nanofiber aerogel.

[0005] The present invention provides a method for preparing a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, the specific steps of which are as follows:

[0006] (1) preparing an aramid nanofiber dispersion in a mixed system of an organic solvent and an alkali, then uniformly mixing the aramid nanofiber dispersion with deionized water, and filtering to obtain an aramid nanofiber hydrogel;

[0007] (2) taking an appropriate amount of black phosphorus powder and ultrasonically dispersing it in deionized water for 0.5-1 h to obtain a black phosphorus dispersion;

[0008] (3) emulsifying and stirring the aramid nanofiber hydrogel and the black phosphorus dispersion for 40-60 minutes to make them evenly mixed, and then vacuum filtering for standby use to obtain a black phosphorus / aramid nanofiber mixed hydrogel;

[0009] (4) placing the black phosphorus / aramid nanofiber hybrid hydrogel in a tert-butyl alcohol aqueous solution and performing two solvent exchanges;

[0010] (5) subjecting the solvent-exchanged hydrogel to vacuum-assisted filtration to obtain a block hydrogel;

[0011] (6) The block hydrogel is subjected to supercritical drying and vacuum freeze drying to obtain aramid nanofiber / black phosphorus aerogel.

[0012] In step (1), the aramid nanofiber is a para-aramid nanofiber, and the diameter of the para-aramid nanofiber is preferably 10 to 100 nm, and most preferably 40 to 60 nm; the length of the para-aramid nanofiber is 100 nm to 1000 μm, more preferably 100 to 200 μm, and most preferably 140 to 160 μm.

[0013] Specifically, the aramid fiber is added to a mixed system of an organic solvent and an alkali and stirred twice to make the two mixed more evenly and to ensure that the organic solvent can fully enter the fiber to form a porous structure, thereby obtaining an aramid nanofiber dispersion.

[0014] The usage ratio of the aramid fiber, the alkali, and the organic solvent is preferably (1-20):(1-10):450, wherein the aramid fiber and the alkali are measured in grams, and the organic solvent is measured in milliliters;

[0015] The base used is solid potassium hydroxide, and the organic solvent is dimethyl sulfoxide.

[0016] After obtaining the aramid nanofiber dispersion, the aramid nanofiber dispersion is mixed evenly with deionized water in a volume ratio of 1:(2-3) to remove the organic solvent, and the aramid nanofiber hydrogel is obtained by filtering.

[0017] Preferably, in step (2), the black phosphorus solid content is 0.5-2wt%, preferably 1wt%, and the ultrasonic time is preferably 1h.

[0018] Preferably, in step (3), the volume ratio of the black phosphorus dispersion to the aramid nanofiber hydrogel is 1:(2-4), and the preferred mixing volume ratio is 1:4. The stirring time is preferably 40 minutes. The emulsifying disperser is specifically selected to complete the process, and the speed is controlled to be not less than 30,000 r / min, so as to achieve a better shearing and refining effect.

[0019] Preferably, in step (4), during the first solvent replacement, the volume ratio of tert-butanol to deionized water is 1:(1-3), preferably 1:3, and the first replacement time is 12-24 h, preferably 12 h; during the second solvent replacement, the volume ratio of tert-butanol to deionized water is 1:(1-2), preferably 1:1, and the second replacement time is 8-24 h, preferably 8 h.

[0020] The vacuum-assisted filtration in step (5) uses a circulating water vacuum pump for filtration.

[0021] Preferably, in step (6), the supercritical drying temperature is 50°C, the critical pressure is 20 MPa, and the supercritical drying time is 12-24 h; the vacuum drying temperature is preferably -55°C, the air pressure is 5 Pa, and the time is 24 to 72 h.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The aramid nanofiber hydrogel is replaced twice in a tert-butyl alcohol aqueous solution and then mixed with a black phosphorus dispersion. The aerogel is formed with a developed reticular structure by changing the replacement time with the tert-butyl alcohol aqueous solution and drying to sublimate the tert-butyl alcohol, so that most electromagnetic waves can enter the material, and multiple reflections and polarization losses are enhanced. At the same time, the ice nucleus growth and ice crystal size are adjusted to regulate the pores inside the aramid nanofiber aerogel, so that the preparation of aramid nanofiber / black phosphorus composite aerogels with different pore sizes is possible. The present invention adopts a new replacement solvent and combines a new freezing method to develop and produce a composite material with excellent mechanical properties and a certain electromagnetic shielding ability. The porosity of the shielding material reaches 98.9%, which greatly improves the electromagnetic shielding performance of the aramid nanofiber aerogel, and the material density is greatly reduced, while the flexibility and strength of the material are also improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM image of the aerogel structure prepared in Example 1 of the present invention.

[0025] Figure 2 This is a SEM image of the aerogel structure prepared in Example 2 of the present invention.

[0026] Figure 3 This is a SEM image of the aerogel structure prepared in Example 3 of the present invention.

[0027] Figure 4 This is a SEM image of the aerogel structure prepared in Example 4 of the present invention.

[0028] Figure 5 This is a SEM image of the aerogel structure prepared in Example 5 of the present invention;

[0029] It can be seen from the above electron microscope scanning images that the aerogel finally obtained in the embodiment shows a rich porous structure, and most of the black phosphorus is evenly attached to the fibers;

[0030] Figure 6 This is the thermal stability curve of the aramid nanofiber aerogel prepared in Example 1;

[0031] This shows that aramid nanofiber aerogel can remain stable even at 600°C. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described below in conjunction with specific examples. These examples are only used to illustrate the technical solution of the present invention in more detail and should not be construed as limiting the scope of protection of the present invention. The following percentages of solid content and other percentages are all mass percentages.

[0033] Example 1

[0034] A method for preparing a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, the specific steps are as follows:

[0035] First, 5 g of para-aramid nanofibers with a diameter of 40 to 60 nm and a length of 140 to 160 μm, 450 ml of dimethyl sulfoxide (DMSO), and 1 g of KOH were added to a reaction container and mechanically stirred at room temperature for 1 hour; then, it was dispersed in 1000 ml of water to obtain an aramid nanofiber hydrogel dispersion.

[0036] The black phosphorus dispersion with a solid content of 2% was added to the aramid nanofiber hydrogel dispersion at a volume ratio of 1:2.5 after ultrasonication for 30 minutes, and the mixture was mechanically stirred for about 40 minutes to be evenly mixed and then vacuum filtered to obtain the black phosphorus / aramid nanofiber mixed hydrogel.

[0037] Then, the black phosphorus / aramid nanofiber hybrid hydrogel was placed in a mixed solution of tert-butanol and ultrapure water in a volume ratio of 25%:75% (1:3) (the mixed solution was in excess) for the first solvent exchange, and the duration of the solvent exchange was 12 hours to obtain a single exchange hydrogel; then, the single exchange hydrogel filter cake was vacuum filtered and placed in a mixed solution of tert-butanol and ultrapure water in a volume ratio of 50%:50% (1:1) for a second solvent exchange, and the duration of the second solvent exchange was 8 hours to obtain a second exchange hydrogel.

[0038] The secondary exchange hydrogel was filtered using a circulating water vacuum pump, and the filter cake was supercritically dried at a temperature of 50°C and a pressure of 20 MPa for 12 hours, then placed in a freeze dryer and freeze-dried for 48 hours at a temperature of -55°C and a vacuum of 5 Pa to obtain a composite aramid nanofiber aerogel with electromagnetic shielding capability.

[0039] The aerogel prepared above was observed by scanning electron microscopy to be an electromagnetic shielding aerogel material with a porous structure and a specific surface area of ​​248 m 2 / g, conductivity is 2.37S / m, tensile stress is 1.37MPa, and shielding effectiveness is 24.3dB.

[0040] Example 2

[0041] A method for preparing a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, the specific steps are as follows:

[0042] First, 4 g of para-aramid nanofibers with a diameter of 40-60 nm and a length of 140-160 μm, 450 ml of dimethyl sulfoxide (DMSO), and 1 g of KOH were added to a reaction container, mechanically stirred at room temperature for 1 hour, and dispersed in 1000 ml of water to obtain an aramid nanofiber hydrogel dispersion.

[0043] The black phosphorus dispersion with a solid content of 1.5% was added to the aramid nanofiber hydrogel dispersion at a volume ratio of 1:4 after ultrasonic treatment for 30 minutes. The mixture was mechanically stirred for about 40 minutes to make it evenly mixed and then vacuum filtered to obtain the black phosphorus / aramid nanofiber mixed hydrogel.

[0044] Then, the black phosphorus / aramid nanofiber hybrid hydrogel was placed in a mixed solution of tert-butyl alcohol and ultrapure water with a volume ratio of 25%:75% (1:3) (excess mixed solution) for the first solvent exchange, and the duration of the solvent exchange was 16 hours to obtain a first exchange hydrogel. Then, the solvent was filtered, and the obtained first exchange hydrogel was placed in a mixed solution of tert-butyl alcohol and ultrapure water with a volume ratio of 50%:50% for a second solvent exchange, and the duration of the second solvent exchange was 12 hours to obtain a second exchange hydrogel;

[0045] The secondary exchange hydrogel was filtered using a circulating water vacuum pump, and the filter cake was supercritically dried at a temperature of 50°C and a pressure of 20 MPa for 12 hours, then placed in a freeze dryer and freeze-dried for 48 hours at a temperature of -55°C and a vacuum of 5 Pa to obtain a composite aramid nanofiber aerogel with electromagnetic shielding capability.

[0046] The aerogel prepared above was observed by scanning electron microscopy to be an electromagnetic shielding aerogel material with a porous structure and a specific surface area of ​​230 m 2 / g, conductivity is 2.45S / m, tensile stress is 1.43MPa, and shielding effectiveness is 25.6dB.

[0047] Example 3

[0048] A method for preparing a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, the specific steps are as follows:

[0049] First, 3 g of para-aramid nanofibers with a diameter of 40-60 nm and a length of 140-160 μm, 450 ml of dimethyl sulfoxide (DMSO), and 1 g of KOH were added to a reaction container, mechanically stirred at room temperature for 1 hour, and dispersed in 1000 ml of water to obtain an aramid nanofiber hydrogel dispersion.

[0050] The black phosphorus dispersion with a solid content of 1% was added to the aramid nanofiber hydrogel dispersion at a volume ratio of 1:3 after ultrasonic treatment for 30 minutes. The mixture was mechanically stirred for about 40 minutes to make it evenly mixed and then vacuum filtered to obtain the black phosphorus / aramid nanofiber mixed hydrogel.

[0051] Then, the black phosphorus / aramid nanofiber hybrid hydrogel was placed in a mixed solution of tert-butyl alcohol and ultrapure water with a volume ratio of 25%:75% (1:3) (excess mixed solution) for the first solvent exchange, and the duration of the solvent exchange was 24 hours to obtain a first exchange hydrogel. Then, the solvent was filtered, and the obtained first exchange hydrogel was placed in a mixed solution of tert-butyl alcohol and ultrapure water with a volume ratio of 50%:50% for a second solvent exchange, and the duration of the second solvent exchange was 24 hours to obtain a second exchange hydrogel;

[0052] The secondary exchange hydrogel was filtered using a circulating water vacuum pump, and the filter cake was supercritically dried at a temperature of 50°C and a pressure of 20 MPa for 12 hours, then placed in a freeze dryer and freeze-dried for 48 hours at a temperature of -55°C and a vacuum of 5 Pa to obtain a composite aramid nanofiber aerogel with electromagnetic shielding capability.

[0053] The aerogel prepared above was observed by scanning electron microscopy to be an electromagnetic shielding aerogel material with a porous structure and a specific surface area of ​​224 m 2 / g, conductivity is 2.39S / m, tensile stress is 1.43MPa, and shielding effectiveness is 23.1dB.

[0054] Example 4

[0055] A method for preparing a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, the specific steps are as follows:

[0056] First, 2 g of para-aramid nanofibers with a diameter of 40-60 nm and a length of 140-160 μm, 450 ml of dimethyl sulfoxide (DMSO), and 1 g of KOH were added to a reaction container, mechanically stirred at room temperature for 1 hour, and dispersed in 1000 ml of water to obtain an aramid nanofiber hydrogel dispersion.

[0057] The black phosphorus dispersion with a solid content of 0.5% was added to the aramid nanofiber hydrogel dispersion at a volume ratio of 1:2 after ultrasonication for 30 minutes, and the mixture was mechanically stirred for about 60 minutes to be evenly mixed and then vacuum filtered to obtain the black phosphorus / aramid nanofiber mixed hydrogel.

[0058] Then, the black phosphorus / aramid nanofiber hybrid hydrogel was placed in a mixed solution of tert-butyl alcohol and ultrapure water with a volume ratio of 25%:75% (1:3) (excess mixed solution) for the first solvent exchange, and the duration of the solvent exchange was 12 hours to obtain a first exchange hydrogel. Then, the solvent was filtered, and the obtained first exchange hydrogel was placed in a mixed solution of tert-butyl alcohol and ultrapure water with a volume ratio of 50%:50% for a second solvent exchange, and the duration of the second solvent exchange was 48 hours to obtain a second exchange hydrogel;

[0059] The secondary exchange hydrogel was filtered using a circulating water vacuum pump, and the filter cake was supercritically dried at a temperature of 50°C and a pressure of 20 MPa for 6 hours. It was then placed in a freeze dryer and freeze-dried for 72 hours at a temperature of -55°C and a vacuum of 5 Pa to obtain a composite aramid nanofiber aerogel with electromagnetic shielding capability.

[0060] The aerogel prepared above was observed by scanning electron microscopy to be an electromagnetic shielding aerogel material with a porous structure and a specific surface area of ​​217 m 2 / g, conductivity is 2.42S / m, tensile stress is 1.39MPa, and shielding effectiveness is 22.0dB.

[0061] Example 5

[0062] A method for preparing a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, the specific steps are as follows:

[0063] First, add 1g of para-aramid nanofibers with a diameter of 40-60nm and a length of 140-160μm, 450ml of dimethyl sulfoxide (DMSO), and 1g of KOH into a reaction container, stir mechanically at room temperature for 0.5h, and disperse in 1000ml of water to obtain an aramid nanofiber hydrogel dispersion.

[0064] The black phosphorus dispersion with a solid content of 1.5% was added to the aramid nanofiber hydrogel dispersion at a volume ratio of 1:2 after ultrasonication for 30 minutes, and the mixture was mechanically stirred for about 60 minutes to be evenly mixed and then vacuum filtered to obtain the black phosphorus / aramid nanofiber mixed hydrogel.

[0065] Then, the black phosphorus / aramid nanofiber hybrid hydrogel was placed in a mixed solution of tert-butanol and ultrapure water in a volume ratio of 25%:75% for the first solvent exchange, and the duration of the first solvent exchange was 12 hours to obtain a first exchange hydrogel. Then, the solvent was filtered, and the first exchange hydrogel was placed in a mixed solution of tert-butanol and ultrapure water in a volume ratio of 50%:50% for a second solvent exchange, and the duration of the second solvent exchange was 8 hours to obtain a second exchange hydrogel;

[0066] The secondary exchange hydrogel was filtered using a circulating water vacuum pump, and the filter cake was supercritically dried at a temperature of 50°C and a pressure of 20 MPa for 6 hours. It was then placed in a freeze dryer and freeze-dried for 72 hours at a temperature of -55°C and a vacuum of 5 Pa to obtain a composite aramid nanofiber aerogel with electromagnetic shielding capability.

[0067] The aerogel prepared above was observed by scanning electron microscopy to be an electromagnetic shielding aerogel material with a porous structure and a specific surface area of ​​229 m 2 / g, conductivity is 2.47S / m, tensile stress is 1.41MPa, and shielding effectiveness is 21.0dB.

[0068] Comparative Example 1

[0069] Comparative Example 1 is an aerogel electromagnetic shielding material prepared according to Example 1, except that black phosphorus is not added, and the rest of the contents are the same as Example 1. The specific surface area is 210 m 2 / g, conductivity is 1.79S / m, tensile stress is 1.38MPa, and shielding effectiveness is 10.8dB.

[0070] Experimental example

[0071] The inventors tested the relevant properties according to GJB 6190-2008 "Measurement Method for Shielding Effectiveness of Electromagnetic Shielding Materials", and the results are shown in Table 1 below:

[0072] Table 1

[0073]

[0074] As shown in Table 1, by adding black phosphorus, the shielding effectiveness and conductivity of the electromagnetic shielding material in the embodiment are significantly improved. The increase in conductivity shows that the aerogel with the addition of black phosphorus has good conductive properties, and the electron shielding effectiveness exceeds 20 dB, which shows that the aerogel with the addition of black phosphorus has good absorption loss.

[0075] Figure 1-5 This is a SEM image of the aerogel structure prepared in Example 5. From the electron microscope scanning image, it can be seen that the aerogel finally obtained in Example 5 exhibits a rich porous structure, and most of the black phosphorus is evenly attached to the fibers; Figure 6 This is the thermal stability curve of the aramid nanofiber aerogel prepared in Example 1. From this figure, it can be seen that the obtained aramid nanofiber aerogel can remain stable even at 600°C and can withstand higher temperatures.

[0076] The black phosphorus-loaded aramid nanofiber aerogel prepared in the above embodiment has good flexibility, can be adapted to various devices or structures of complex shapes, can be adhered to irregular surfaces, and can be used in some occasions where high shape adaptability is required. In the field of electronic equipment, it can be adhered to the outer casing of the device to block the influence of external electromagnetic waves on the internal circuit of the device.

[0077] In summary, the electromagnetic shielding composite aerogel material is prepared by mixing aramid nanofiber hydrogel with black phosphorus, and through two solvent replacements and a vacuum freeze-drying process. The aerogel has the characteristics of high thermal stability and low thermal conductivity, corrosion resistance, high temperature resistance, etc., and has better sound wave absorption and electromagnetic shielding effects, and is suitable for sound wave absorption and electromagnetic protection in complex environments.

[0078] The embodiments described above are only descriptions of the preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary engineering and technical personnel in the field should fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a black phosphorus-loaded aramid nanofiber aerogel electromagnetic shielding material, characterized in that: The preparation steps are as follows: (1) preparing an aramid nanofiber dispersion in a mixed system of an organic solvent and an alkali, then uniformly mixing the aramid nanofiber dispersion with deionized water, and filtering to obtain an aramid nanofiber hydrogel; (2) taking an appropriate amount of black phosphorus powder and ultrasonically dispersing it in deionized water for 0.5-1 h to obtain a black phosphorus dispersion; (3) emulsifying and stirring the aramid nanofiber hydrogel and the black phosphorus dispersion for 40-60 minutes to uniformly mix them to obtain a black phosphorus / aramid nanofiber mixed hydrogel; (4) placing the black phosphorus / aramid nanofiber hybrid hydrogel in a tert-butyl alcohol aqueous solution and performing two solvent exchanges; (5) subjecting the solvent exchanged hydrogel to vacuum-assisted filtration to form a block hydrogel; (6) The block hydrogel is subjected to supercritical drying and vacuum freeze drying to obtain aramid nanofiber / black phosphorus aerogel.

2. The preparation method according to claim 1, characterized in that: The aramid nanofibers described in step (1) are para-aramid nanofibers, and the diameter of the para-aramid nanofibers is 10 to 100 nm, and the length is 100 nm to 1000 μm.

3. The preparation method according to claim 1, characterized in that: The dosage ratio of the aramid fiber, alkali and organic solvent in step (1) is preferably (1-20):(1-10):450, wherein the aramid fiber and alkali are measured in grams, and the organic solvent is measured in milliliters; the alkali used is solid potassium hydroxide, and the organic solvent is dimethyl sulfoxide.

4. The preparation method according to claim 2, characterized in that: The diameter of the para-aramid nanofiber is 40-60 nm, and the length is 100-200 μm.

5. The preparation method according to claim 1, characterized in that: In step (2), the black phosphorus solid content is 0.5-2wt%, and the ultrasonic time is 1h.

6. The preparation method according to claim 1, characterized in that: In step (3), the volume ratio of the black phosphorus dispersion to the aramid nanofiber hydrogel is 1:(2-4), and the stirring time is 40 minutes.

7. The preparation method according to claim 1, characterized in that: In the step (4), the first solvent replacement time is 12-24 hours; the second solvent replacement time is 8-24 hours.

8. The preparation method according to claim 1, characterized in that: During the first solvent replacement in step (4), the volume ratio of tert-butanol to deionized water is 1:(1-3), and the first replacement time is 12-24 hours; during the second solvent replacement, the volume ratio of tert-butanol to deionized water is 1:(1-2), and the second replacement time is 8-24 hours.

9. The preparation method according to claim 1, characterized in that: The vacuum-assisted filtration in step (5) uses a circulating water vacuum pump for filtration.

10. The preparation method according to claim 1, characterized in that: The supercritical drying temperature in step (6) is 50°C, the supercritical drying time is 12-24h, and the critical pressure is 20MPa; the vacuum drying temperature is preferably -55°C, the air pressure is 5Pa, and the time is 24 to 72h.

Citation Information

Cited By

  • Aramid nanofiber low-frequency wave-absorbing composite material and preparation method thereof

    CN119465686A

  • Aramid nanofiber low-frequency wave-absorbing composite material and preparation method thereof

    CN119465686B

  • Para-aramid diaphragm and preparation method thereof

    CN119764747A