Polyethylene powder and moldings

A polyethylene powder with controlled molecular weight, yellowness, whiteness, and density relationships addresses the challenge of stain detection in molded products, enhancing transparency and maintaining impact and abrasion resistance.

JP7566654B2Active Publication Date: 2024-10-15ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021017946
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-24
Filing Date
2021-02-08
Publication Date
2024-10-15
Estimated Expiration
2041-02-08

AI Technical Summary

Technical Problem

Existing polyethylene molded products lack ease of stain detection despite having excellent impact resistance and abrasion resistance, and there is a need for improved transparency.

Method used

A polyethylene powder with specific molecular weight, yellowness, whiteness, and density relationships, along with controlled metal content and melting temperatures, is formulated to enhance transparency and ease of stain detection.

Benefits of technology

The formulated polyethylene powder achieves both impact resistance and abrasion resistance while ensuring excellent transparency and ease of stain detection in molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566654000001
    Figure 0007566654000001
  • Figure 0007566654000002
    Figure 0007566654000002
Patent Text Reader

Abstract

To provide polyethylene powder that can achieve both of impact resistance and wear resistance in various moldings made from polyethylene powder, and has excellent transparency and allows stains to be detected easily.SOLUTION: Polyethylene powder has an ethylene unit and / or an ethylene unit and a C3-8 α-olefin unit as constitutional units. The polyethylene powder has a viscosity average molecular weight of 1,000,000 or more and 10,000,000 or less. When the polyethylene powder is molded into a sheet under compression molding conditions described in JIS K6936-2, the sheet molding has yellowness YI, whiteness WI, and density ρ each satisfying the following formula (1): 0.50≤(-YI)×WI / ρ<2.0.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyethylene powder and a molded article. [Background technology]

[0002] It has been known that polyethylene powder, particularly ultra-high molecular weight polyethylene powder, has a higher molecular weight than general-purpose polyethylene and is therefore excellent in stretchability, strength, chemical stability, and long-term reliability. For these reasons, polyethylene powder, particularly ultra-high molecular weight polyethylene powder, is used as a raw material for microporous membranes for separators of secondary batteries such as lead-acid batteries and lithium-ion batteries, and for molded articles such as fibers.

[0003] Furthermore, polyethylene powder, particularly ultra-high molecular weight polyethylene powder, is superior to general-purpose polyethylene in various properties such as impact resistance, abrasion resistance, sliding properties, low-temperature properties, chemical resistance, etc. Therefore, polyethylene powder, particularly ultra-high molecular weight polyethylene powder, is used as a lining material for hoppers, chutes, etc., bearings, gears, roller guide rails, and also as a raw material for molded articles such as bone substitutes, osteoconductive materials, and bone inducers.

[0004] On the other hand, because ultra-high molecular weight polyethylene powder has a high molecular weight, it is difficult to extrude the resin alone, so it is often molded using compression molding (press molding) or a special extruder such as a ram extruder. It is important that the various molded articles mentioned above have both impact resistance and abrasion resistance. From this perspective, Patent Documents 1 to 3 disclose techniques for achieving both impact resistance and abrasion resistance in a molded article using polyethylene powder. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-23171 A [Patent Document 2] Patent No. 4173444 [Patent Document 3] JP 2015-157905 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, in various molded articles made from the above-mentioned polyethylene powder as a raw material, in addition to having excellent impact resistance and abrasion resistance, there has been an increasing demand for the molded articles to have improved transparency so that dirt on the molded articles can be easily detected (hereinafter, this may be referred to as the ease of detecting dirt on the molded articles). However, the molded bodies described in the above Patent Documents 1 to 3 have not been verified in terms of ease of detecting dirt on the molded bodies, and there is a problem in that there is room for improvement in terms of ease of detecting dirt on such molded bodies.

[0007] In view of the above problems in the prior art, the present invention has an object to provide a polyethylene powder which can provide various molded articles made from the polyethylene powder as a raw material, which have both the impact resistance and abrasion resistance, and which has excellent transparency and allows easy detection of dirt thereon. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and as a result, have found that the above object can be solved by a polyethylene powder having a viscosity average molecular weight within a specified range, and in which the yellowness index YI, whiteness index WI and density ρ of a sheet molded product obtained by compression molding under the conditions specified in JIS K6936-2 satisfy specified relationships, thereby completing the present invention. That is, the present invention is as follows.

[0009] [1] Ethylene units, and / or ethylene units and α-olefin units having 3 to 8 carbon atoms and The viscosity average molecular weight is 1 million or more and 10 million or less, Yellowness (YI), whiteness (whiteness) of the sheet molded product under the compression molding conditions specified in JIS K6936-2 Chromaticity WI, density ρ (kg / m 3 ) satisfies the following formula (1): Polyethylene powder. 0.50≦(-YI)×WI / ρ<2.0...Formula (1) [2] The α-olefin is 1-propene or 1-butene, The polyethylene powder according to [1] above, having a constituent content of 1.0 mol% or less. [3] The bulk density of the composition according to [1] or [2] above is 0.30 g / mL or more and less than 0.60 g / mL. The polyethylene powder described. [4] Magnesium and titanium measured by inductively coupled plasma mass spectrometry (ICP / MS) The total content of aluminum element is 1 ppm or more and 50 ppm or less. The polyethylene powder according to any one of [3] to [4]. [5] Melting integral curves by differential scanning calorimetry (DSC) The temperature at 30% melting in the wire is 120℃ or more and 140℃ or less, and the temperature at 50% melting is is 125℃ or more and 145℃ or less, and the temperature at 70% melting is 130℃ or more and 150℃ or less. The polyethylene powder according to any one of [1] to [4] above. [6] Melting integral curves by differential scanning calorimetry (DSC) The temperature at 50% melting in the wire is 130° C. or higher and 140° C. or lower. Polyethylene powder. [7] A molded body of the polyethylene powder according to any one of [1] to [6] above. [8] The molded body according to [7] above, which is a compression molded body. [9] The molded article according to [7] above, which is an extrusion molded article.

[10] The molded article according to [7] above, which is a stretched molded article.

[11] The molded article according to [7] above, which is a microporous membrane.

[12] The molded body according to [7] above, which is a fiber. Effect of the Invention

[0010] According to the present invention, it is possible to provide a polyethylene powder which can provide various molded articles made from the polyethylene powder as a raw material, which have both impact resistance and abrasion resistance, and which has excellent transparency and excellent ease of detection of dirt. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. It should be noted that the following embodiment is an example for explaining the present invention, and the present invention is not limited to the following content, and can be implemented in various modified forms within the scope that does not deviate from the gist of the present invention.

[0012] [Polyethylene powder] The polyethylene powder of the present embodiment has constituent units of ethylene units and / or ethylene units and α-olefin units having 3 to 8 carbon atoms, has a viscosity average molecular weight of 1 million to 10 million, and has a sheet molded product molded under the compression molding conditions specified in JIS K6936-2, and the relationship between the yellowness index YI, whiteness index WI, and density ρ satisfies the following mathematical formula (1): 0.50≦(-YI)×WI / ρ<2.0...Formula (1) The polyethylene powder of the present embodiment can provide various molded articles having both impact resistance and abrasion resistance, excellent transparency, and ease of detection of dirt.

[0013] (Constituent unit) The polyethylene powder of the present embodiment has as its constituent units ethylene units and / or ethylene units and α-olefin units having 3 or more and 8 or less carbon atoms. The α-olefin having 3 to 8 carbon atoms is copolymerizable with ethylene. The α-olefin having 3 to 8 carbon atoms is not particularly limited, but examples thereof include linear, branched, or cyclic α-olefins, such as those represented by the formula: CH 2 =CHR 1 (where R 1 is an aryl group having 1 to 6 carbon atoms; and at least one α-olefin selected from the group consisting of linear, branched or cyclic dienes having 4 to 7 carbon atoms. Among these, from the viewpoints of abrasion resistance, heat resistance, impact resistance and strength of the molded body, 1-propene and / or 1-butene are preferred as the α-olefin, and the constituent amount of these in the total monomers is preferably 1.0 mol % or less, more preferably 0.9 mol % or less, and even more preferably 0.8 mol % or less. From the viewpoints of excellent transparency and ease of detection of dirt, the content of these monomers in the total monomers is preferably 0.01 mol % or more, more preferably 0.04 mol % or more, and even more preferably 0.1 mol % or more.

[0014] In this specification, the naming of each monomer unit constituting a polymer follows the naming of the monomer from which the monomer unit is derived. For example, an "ethylene unit" refers to a structural unit of a polymer resulting from polymerization of a monomer, ethylene, and has a molecular structure in which two carbon atoms of ethylene form the polymer main chain. In addition, an "α-olefin unit" refers to a structural unit of a polymer resulting from polymerization of a monomer, α-olefin, and has a molecular structure in which two carbon atoms of an olefin derived from an α-olefin form the polymer main chain.

[0015] (viscosity average molecular weight) The polyethylene powder of this embodiment has a viscosity average molecular weight of 1 million or more and 10 million or less, preferably 1.2 million or more and 9.5 million or less, and more preferably 1.5 million or more and 9 million or less. When the viscosity average molecular weight is within the above range, a molded product made from the polyethylene powder of this embodiment as a raw material can achieve both abrasion resistance, heat resistance, impact resistance, strength, and molding processability.

[0016] The viscosity average molecular weight (Mv) of the polyethylene powder of this embodiment can be calculated from the intrinsic viscosity [η] (dL / g) obtained by extrapolating the reduced viscosity, which is determined under a temperature condition of 135° C. using multiple solutions in which polyethylene powder is dissolved in a decahydronaphthalene solution at different concentrations, to a concentration of 0, using the following formula (2). Specifically, it can be calculated by the method described in the Examples. Mv = (5.34 × 10 4 )×[η] 1.49 Formula (2)

[0017] The viscosity average molecular weight of the polyethylene powder of the present embodiment can be controlled within the above numerical range by adopting a method of making hydrogen present in the polymerization system or a method of adjusting the polymerization temperature in the polymerization step of the polyethylene powder.

[0018] The polyethylene powder of the present embodiment, in a sheet molded product obtained under the compression molding conditions specified in JIS K6936-2, has a yellowness index YI, a whiteness index WI, and a density ρ that satisfy the following mathematical formula (1). 0.50≦(-YI)×WI / ρ<2.0...Formula (1) (-YI) x WI / ρ is preferably 0.80 or more and less than 1.9, and more preferably 1.0 or more and less than 1.8. Since the polyethylene powder of the present embodiment satisfies the relationship of the above mathematical formula (1), in various molded articles made from the polyethylene powder of the present embodiment as a raw material, both impact resistance and abrasion resistance are achieved, while the effect of improving transparency is obtained, and the ease of detecting dirt is excellent. In order to control the polyethylene powder of the present embodiment so as to satisfy the above range, it is effective to adopt, for example, a method of adding a small amount of an aliphatic saturated alcohol of not less than 100 ppb and not more than 1 ppm after completion of polymerization, a method of adjusting the concentration of a solid catalyst component relative to an inert hydrocarbon medium to not less than 5 mg / L and not more than 15 mg / L, or a method of adjusting the oxygen concentration in a dryer during drying to not more than 100 ppm, which will be described later. The aliphatic saturated alcohol is not particularly limited, but for example, methanol and ethanol are more preferable. The yellowness index YI, whiteness index WI, and density ρ can be measured by the method described in the examples.

[0019] (Bulk density) The polyethylene powder of this embodiment has a bulk density of preferably 0.30 g / mL or more and 0.60 g / mL or less, more preferably 0.33 g / mL or more and 0.57 g / mL or less, and even more preferably 0.35 g / mL or more and 0.55 g / mL or less. When the bulk density of the polyethylene powder of the present embodiment is within the above range, the handleability of the polyethylene powder is improved. Generally, the bulk density varies depending on the catalyst used in the polymerization step, and therefore, it is possible to control the bulk density within the above-mentioned numerical range by appropriately selecting the catalyst. Moreover, by adjusting the polymerization temperature and the slurry concentration in the polymerization vessel, the bulk density can be controlled, and further, the productivity of polyethylene powder per unit catalyst can be controlled. For example, the bulk density of the polyethylene powder can be controlled by adjusting the polymerization temperature when polymerizing the polyethylene powder, and the bulk density can be reduced by increasing the polymerization temperature. The bulk density of the polyethylene powder can also be controlled by adjusting the slurry concentration in the polymerization vessel, and the bulk density can be increased by increasing the slurry concentration. In this way, by adjusting the polymerization temperature and the slurry concentration, the activity of the catalyst can be adjusted, and the productivity of polyethylene powder per unit catalyst can be controlled. The bulk density of the polyethylene powder can be measured by the method described in the examples.

[0020] (Total content of magnesium, titanium, and aluminum elements) The polyethylene powder of this embodiment preferably has a total content of magnesium, titanium, and aluminum elements of 1 ppm or more and 50 ppm or less, more preferably 2 ppm or more and 40 ppm or less, and even more preferably 3 ppm or more and 30 ppm or less. When the total content of magnesium, titanium, and aluminum elements in the polyethylene powder of this embodiment is within the above-mentioned range, the appearance of various molded articles made from the polyethylene powder as a raw material is improved, the loss rate of the molded articles due to the appearance is reduced, and the productivity can be improved. The total content of magnesium, titanium, and aluminum elements in the polyethylene powder of the present embodiment can be controlled, for example, by adjusting the productivity of the polyethylene powder per unit catalyst, and can be controlled within the above numerical range by increasing the productivity. The total content of magnesium, titanium, and aluminum elements in the polyethylene powder of this embodiment is measured by an inductively coupled plasma mass spectrometer (ICP / MS), and specifically, can be measured by the method described in the examples.

[0021] (Dependent scattering calorimetry (DSC) melting integral curve) In the polyethylene powder of this embodiment, the temperature at 30% melting in the melting integral curve by DSC (Differential Scanning Calorimetry) is preferably 120°C or more and 140°C or less, the temperature at 50% melting is 125°C or more and 145°C or less, and the temperature at 70% melting is preferably 130°C or more and 150°C or less. More preferably, the temperature at 30% melting is 122°C or more and 138°C or less, the temperature at 50% melting is 127°C or more and 143°C or less, and the temperature at 70% melting is 132°C or more and 148°C or less. Even more preferably, the temperature at 30% melting is 125°C or more and 135°C or less, the temperature at 50% melting is 130°C or more and 140°C or less, and the temperature at 70% melting is 135°C or more and 145°C or less. By being in the above range, various molded articles made from the polyethylene powder as a raw material can have both impact resistance and abrasion resistance, excellent transparency, and excellent ease of detection of dirt. As a method for ensuring that the melting temperature of the polyethylene powder falls within the above range, for example, a small amount of less than 1 ppm of an aliphatic saturated alcohol may be added after the completion of polymerization. The aliphatic saturated alcohol is not particularly limited, but examples of preferred ones include methanol and ethanol. The DSC can be measured by the method described in the Examples.

[0022] (Other Ingredients) The polyethylene powder of the present embodiment may be used in combination with various known additives, if necessary, such as a heat stabilizer, a lubricant, and a hydrogen chloride absorbent. Examples of heat stabilizers include, but are not limited to, heat stabilizers such as tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane and distearyl thiodipropionate; and weather stabilizers such as bis(2,2',6,6'-tetramethyl-4-piperidine)sebacate and 2-(2-hydroxy-t-butyl-5-methylphenyl)-5-chlorobenzotriazole. Furthermore, examples of lubricants and hydrogen chloride absorbents include, but are not limited to, fatty acid metal salts such as calcium stearate, magnesium stearate, zinc stearate, calcium palmitate, magnesium palmitate, and zinc palmitate.

[0023] [Molded body] The molded article of the present embodiment is obtained by molding the polyethylene powder of the present embodiment described above. The polyethylene powder may be molded as it is in various molding machines, or may be mixed with an organic peroxide and then molded in various molding machines.

[0024] (organic peroxide) The organic peroxide used in molding the polyethylene powder functions as an organic peroxide crosslinking agent. The organic peroxide is not particularly limited as long as it is an organic substance that contributes to crosslinking of the ethylene polymer and has an atomic group -OO- in the molecule, and examples thereof include organic peroxides such as dialkyl peroxides, diacyl peroxides, hydroperoxides, and ketone peroxides; organic peresters such as alkyl peresters; and peroxydicarbonates. The organic peroxide is not limited to the following, but specific examples thereof include dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl perbenzoate, tert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, tert-butylcumyl peroxide, α,α'-di(tert-butylperoxy)diisopropylbenzene, and the like. Among these, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane (trade name "Perhexa 25B" manufactured by Nippon Oil & Fats Co., Ltd.), 2,5-dimethyl-2,5-bis(t-butyloxy)hexyne-3 (trade name "Perhexyne 25B" manufactured by Nippon Oil & Fats Co., Ltd.), dicumyl peroxide, and 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane are preferred.

[0025] (Polyethylene powder molding method, various molded products) The method for molding the polyethylene powder of the present embodiment is not particularly limited, but examples thereof include compression molding (press molding), extrusion molding, and stretch molding. Compression molding is a method in which raw material powder is uniformly spread in a mold, heated and pressurized to form the powder, and then cooled and removed. This method produces a compression molded body. A plate-shaped product may be used as is, or a block may be made and then cut into a final product. In extrusion molding, a screw extruder or a ram extruder that extrudes by moving a piston back and forth is used. This method produces extrusion molded products. By changing the shape of the extruder outlet, molded products of various shapes such as sheets, flat plates, irregular shapes, and pipes can be obtained. Examples of the stretch molding include a method of performing film processing by stretching a sheet, and a method of performing fiber processing by stretching a strand, etc. By this method, a stretch molded product can be obtained.

[0026] [Method for producing polyethylene powder] The method for producing the polyethylene powder of the present embodiment is not particularly limited, and examples thereof include a method using a general Ziegler-Natta catalyst or a metallocene catalyst. In particular, a method using a Ziegler-Natta catalyst is preferred. As the Ziegler-Natta catalyst, those disclosed in

[0032] to

[0068] of the above-mentioned Patent Document 3 can be used. When the solid catalyst component and the organometallic compound component (hereinafter, both may be collectively referred to as "catalyst") are added to the polymerization system of an ethylene-based polymer, they may be added separately to the polymerization system, or they may be mixed in advance and then added to the polymerization system. When the solid catalyst component and the organometallic compound component are combined, the ratio of the two is not particularly limited, but the organometallic compound component is preferably 0.01 mmol to 1,000 mmol, more preferably 0.1 mmol to 500 mmol, and even more preferably 1 mmol to 100 mmol per 1 g of the solid catalyst component. By mixing the two, electrostatic adhesion to storage tanks, piping, etc. can also be prevented.

[0027] In the process for producing polyethylene powder, a method for polymerizing monomers includes a suspension polymerization method in which ethylene or a monomer containing ethylene and an α-olefin having 3 to 8 carbon atoms is polymerized. The suspension polymerization method is preferred from the viewpoint of efficient removal of heat of polymerization. In the suspension polymerization method, an inert hydrocarbon medium can be used as a medium, and further, the olefin itself can be used as a solvent. Examples of the inert hydrocarbon medium include, but are not limited to, aliphatic hydrocarbons such as propane, butane, isobutane, pentane, isopentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethyl chloride, chlorobenzene, and dichloromethane; and mixtures thereof. Furthermore, when producing the polyethylene powder of this embodiment, the catalyst concentration in the inert hydrocarbon medium is preferably 5 mg / L or more and 15 mg / L or less.

[0028] The polymerization temperature in the production process of the polyethylene powder of the present embodiment is usually preferably 20° C. or higher and 100° C. or lower, more preferably 30° C. or higher and 95° C. or lower, and even more preferably 40° C. or higher and 90° C. or lower. A polymerization temperature of 20° C. or higher allows for industrially efficient production. On the other hand, a polymerization temperature of 100° C. or lower allows for continuous and stable operation.

[0029] The polymerization pressure in the production process of the polyethylene powder of this embodiment is usually preferably normal pressure or more and 15 MPa or less, more preferably 0.1 MPa or more and 14 MPa or less, and even more preferably 0.2 MPa or more and 13 MPa or less. When the polymerization pressure is normal pressure or more, a polyethylene powder having a high total metal content and a high total chlorine content tends to be obtained, and when the polymerization pressure is 13 MPa or less, a polyethylene powder having a low total metal content and a low total chlorine content tends to be stably produced. That is, by setting the polymerization pressure within the above-mentioned range, the total metal amount and the total chlorine amount can be controlled within appropriate ranges.

[0030] Moreover, in the polyethylene powder of this embodiment, the polymerization process can be carried out in two or more stages having different reaction conditions. Furthermore, as described in, for example, German Patent Application Publication No. 3127133, the viscosity average molecular weight of the resulting polyethylene powder can be controlled by adopting a method of making hydrogen present in the polymerization system or a method of changing the polymerization temperature. By adding hydrogen as a chain transfer agent to the polymerization system, it is possible to control the viscosity average molecular weight within an appropriate range. When hydrogen is added to the polymerization system, the molar fraction of hydrogen is preferably 0.01 mol% or more and 30 mol% or less, more preferably 0.01 mol% or more and 25 mol% or less, and even more preferably 0.01 mol% or more and 20 mol% or less. In addition, in this embodiment, in addition to the above-mentioned components, other known components useful for producing polyethylene powder may be contained.

[0031] When polymerizing the polyethylene powder of this embodiment, it is preferable to use an antistatic agent such as STATSAFE3000 manufactured by Innospec in order to suppress electrostatic adhesion of the polymer to the polymerization reactor. The STATSAFE3000 can be diluted in an inert hydrocarbon medium and added to the polymerization reactor by a pump or the like. The amount added is preferably 0.1 ppm or more and 50 ppm or less, more preferably 20 ppm or more and 50 ppm or less, based on the amount of polyethylene powder produced per unit time.

[0032] As a method for drying the polyethylene powder of this embodiment after polymerization, a drying method that does not apply high heat is preferable from the viewpoint of preventing deformation of the powder and thermal fusion of powder particles. The type of dryer is preferably a rotary kiln type, a paddle type, a fluidized dryer, etc. The drying temperature is preferably 50° C. or higher and 150° C. or lower, more preferably 70° C. or higher and 100° C. or lower. It is also effective to introduce an inert gas such as nitrogen into the dryer to promote drying, and specifically, it is preferable to set the oxygen concentration in the dryer to less than 100 ppm.

[0033] [Uses of Molded Articles] The polyethylene powder of the present embodiment can be processed by various processing methods. Furthermore, the molded article of the polyethylene powder of this embodiment can be used for various purposes. The main applications of the material include microporous membranes, for example, separators for secondary batteries such as lithium ion secondary batteries and lead-acid batteries, fibers, non-adhesive properties, and low friction coefficient lining materials for hoppers, chutes, etc., and also materials requiring self-lubrication, a low friction coefficient, and abrasion resistance, such as bearings, gears, roller guide rails, bone substitute materials, osteoconductive materials, or bone inductive materials. EXAMPLES

[0034] Hereinafter, the present embodiment will be described in more detail using specific examples and comparative examples, but the present embodiment is not limited in any way by the following examples and comparative examples. The methods for measuring various characteristics and physical properties are shown below.

[0035] [Measurement method and conditions] (1) Viscosity average molecular weight (Mv) The viscosity average molecular weight of the polyethylene powder was determined by the method shown below in accordance with ISO1628-3 (2010). First, 20 mg of polyethylene powder was weighed into a melting tube, and the melting tube was purged with nitrogen. Then, 20 mL of decahydronaphthalene (containing 1 g / L of 2,6-di-t-butyl-4-methylphenol) was added and stirred at 150°C for 2 hours to dissolve the polyethylene powder and obtain a solution. The solution was placed in a thermostatic bath at 135°C and the drop time (ts) between the marked lines was measured using a Canon-Fenske viscometer (Shibata Scientific Instruments Co., Ltd.: product number -100). Similarly, the drop time (ts) between the marked lines was measured for samples in which the polyethylene powder was changed to 10 mg, 5 mg, and 2.5 mg. As a blank, the fall time (tb) of decahydronaphthalene alone without adding polyethylene powder was measured. The reduced viscosity (ηsp / C) of the polyethylene powder obtained according to the following formula (3) was plotted to derive a linear equation between the concentration (C) (unit: g / dL) and the reduced viscosity (ηsp / C) of the polyethylene powder, and the intrinsic viscosity ([η]) extrapolated to a concentration of 0 was calculated. ηsp / C=(ts / tb-1) / 0.1 (unit: dL / g) Formula (3) Next, the viscosity average molecular weight (Mv) was calculated using the above-mentioned value of the intrinsic viscosity [η] according to the following formula (4). Mv = (5.34 × 10 4 )×[η] 1.49 Formula (4)

[0036] (2) α-Olefin unit content The content (mol%) of polymerization units derived from α-olefin in the polyethylene powder was measured according to the method disclosed in Macromolecules, 10, 773 (1977) by GJ Ray et al. 13 The intensity was calculated from the area intensity of the methylene carbon signal observed in the C-NMR spectrum. Measuring device: JEOL ECS-400 Observation kernel: 13 C Observation frequency: 100.53MHz Pulse width: 45° (7.5μsec) Pulse program: single pulse dec PD: 5sec Measurement temperature: 130℃ Accumulation count: 30,000 times or more Reference: PE(-eee-) signal is 29.9ppm Solvent: orthodichlorobenzene-d4 Sample concentration: 5 to 10% by mass Melting temperature: 130~140℃

[0037] (3) Yellowness YI, whiteness WI A compression molded sheet was produced using the polyethylene powder according to the compression molding conditions for test pieces described in JIS K6936-2, and the yellowness index YI and whiteness index WI were measured using a CR-20 Color Reader (manufactured by Konica Minolta Japan, Inc.).

[0038] (4) Bulk density The bulk density of the polyethylene powder was measured in accordance with JIS K-6721:1997.

[0039] (5) Density (ρ) Density was measured according to ASTM D 1505. The test pieces were prepared by preparing a compression molded sheet according to the compression molding conditions for test pieces described in JIS K6936-2, and cutting out a piece from the sheet, annealing it at 120°C for 1 hour, and then cooling it at 25°C for 1 hour.

[0040] (6) The total content of magnesium, titanium, and aluminum elements The total amount of magnesium, titanium, and aluminum elements in the polyethylene powder was determined by pressure decomposing the polyethylene powder using a microwave decomposition apparatus (ETHOS TC, manufactured by Milestone General Co., Ltd.) and measuring the elemental concentrations of magnesium, titanium, and aluminum as metals in the polyethylene powder using an ICP-MS (inductively coupled plasma mass spectrometer, model X-series X7, manufactured by Thermo Fisher Scientific Co., Ltd.) using the internal standard method, and calculating the sum of the elemental concentrations.

[0041] (7) Temperature at which a given amount is melted based on the melting integral curve measured by DSC The melting integral curve of the polyethylene powder by DSC was measured using a DSC (manufactured by PerkinElmer, product name: DSC8000). 8 to 10 mg of polyethylene powder was inserted into an aluminum pan and placed in the DSC. After holding at 50°C for 1 minute, the temperature was raised to 190°C at a heating rate of 10°C / min. The melting curve was integrated to determine the temperatures at 30% melting, 50% melting, and 70% melting, with the temperature before the start of melting being 0% and the temperature at the end of melting being 100%.

[0042] (8) Evaluation of the ease of detecting dirt on molded products A mixture of 28 kg of polyethylene powder with 10 ppm of carbon black (manufactured by Yoneyama Pharmaceutical Co., Ltd.) was poured into a 1 m square, 3 cm high mold in a hot press molding machine in a natural falling state, and compression molded for 12 hours at a set temperature of 210°C and a gauge pressure of 10 MPa. A molded body was then obtained by a cooling process in which heating was stopped while maintaining the pressure. The molded product was cut into 20 cm square pieces, and the resulting 25 20 cm square pieces were visually evaluated to confirm with the naked eye whether or not there was any carbon black contamination. The criteria for judgment are as follows: ○: Eight or more molded pieces were found to be dirty. △: The number of molded bodies with confirmed stains was between 4 and 7. ×: Three or fewer molded pieces were found to be dirty.

[0043] (9) Impact resistance evaluation A compression molded sheet was prepared using the polyethylene powder according to the compression molding conditions for test pieces specified in JIS K6936-2. The average cooling rate was changed to 1°C / min. The obtained compression molded sheet was cut into a test piece according to JIS K7111-1 / 1fA, and a Charpy impact test was carried out according to the method described in JIS K7111-1. The test results were judged according to the following criteria. ○ Charpy impact strength is 80kJ / m 2 End △ Charpy impact strength is 60kJ / m 2 More than 80kJ / m 2 less than × Charpy impact strength is 60kJ / m2 less than

[0044] (10) Abrasion resistance evaluation A compression molded sheet was prepared in the same manner as in (9) above. The average cooling rate was changed to 1°C / min. The compression molded sheet was cut to a size of 60 mm x 35 mm x 4 mm thick to obtain a test piece, which was then attached to a rotating shaft and placed in a sand slurry of 2 kg of No. 4 silica sand and 2 L of water. A wear test was then carried out at a rotation speed of 1,750 rpm for a test time of 24 hours. From the mass measurement results before and after the test, the wear loss ratio was calculated using the following formula (5). The evaluation criteria are as follows: ○ Wear loss ratio is 5% or less △: Wear loss ratio exceeds 5% and is 8% or less ×: Wear loss ratio exceeds 8% Wear loss ratio (%) = (W1-W2) / W1×100 Formula (5) W1 = mass before wear test, W2 = mass after wear test

[0045] [Catalyst Synthesis Example 1: Preparation of Solid Catalyst Component [A]] (1) Synthesis of raw material (a-1) In an 8L stainless steel autoclave that had been thoroughly substituted with nitrogen, add 1mol / L of Mg 6 (C 4 H 9 ) 12 Al(C 2 H 5 ) 3 2,000mL of hexane solution (equivalent to 2000mmol of magnesium and aluminum) was charged, and 146mL of 5.47mol / L n-butanol hexane solution was added dropwise over 3 hours while stirring at 50℃. After completion of the addition, the line was washed with 300mL of hexane. Stirring was continued for another 2 hours at 50℃. After the reaction was completed, the mixture was cooled to room temperature and used as raw material (a-1). The magnesium concentration of the raw material (a-1) was 0.704 mol / L.

[0046] (2) Synthesis of raw material (a-2) In an 8L stainless steel autoclave that had been thoroughly substituted with nitrogen, add 1mol / L of Mg 6 (C 4 H 9 ) 12 Al(C 2 H 5 ) 3 While stirring at 80°C, 240 mL of a hexane solution of 8.33 mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.) was pumped in, and stirring was continued at 80°C for a further 2 hours. After the reaction was completed, the mixture was cooled to room temperature and used as raw material (a-2). The total concentration of magnesium and aluminum in the raw material (a-2) was 0.786 mol / L.

[0047] (3) Synthesis of Support (A-1) An 8 L stainless steel autoclave that had been thoroughly purged with nitrogen was charged with 1,000 mL of a 1 mol / L hexane solution of hydroxytrichlorosilane, and 1,340 mL (corresponding to 0.943 mol of magnesium) of the hexane solution of the raw material (a-1) was added dropwise over 3 hours at 65°C. The reaction was continued for another 1 hour with stirring at 65°C. After the reaction was completed, the supernatant was removed and the carrier was washed four times with 1,800 mL of hexane to obtain carrier (A-1). Analysis of carrier (A-1) revealed that the amount of magnesium contained per gram of solid was 7.5 mmol.

[0048] (4) Preparation of solid catalyst component [A] 1,970 mL of a hexane slurry containing 110 g of the (A-1) carrier was stirred at 10° C., and 103 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 mL of the raw material (a-2) were simultaneously added to the hexane slurry over a period of 3 hours. After the addition, the reaction was continued at 10° C. for 1 hour. After the reaction was completed, the supernatant was removed, and the unreacted raw material components were removed by washing four times with hexane to prepare a solid catalyst component [A].

[0049] [Production of polyethylene powder] Under the conditions shown in Tables 1 and 2 below, and under the conditions shown in the following Examples and Comparative Examples, hexane, ethylene, α-olefin, hydrogen, the solid catalyst component [A], a co-catalyst component, and STATSAFE3000 (manufactured by The Associated Octel Company) were continuously supplied to a 300 L vessel-type polymerization reactor equipped with a stirrer, to produce a polyethylene powder as described below.

[0050] (Example 1: PE-1) The polymerization temperature was maintained at 58° C. by jacket cooling. Hexane was fed at 55 L / hr. As the catalyst, a mixture of triisobutylaluminum and diisobutylaluminum hydride as promoter components and the solid catalyst component [A] were used. The solid catalyst component [A] was added to the polymerizer at a rate of 0.7 g / hour, and the mixture of triisobutylaluminum and diisobutylaluminum hydride was added to the polymerizer at a rate of 9 mmol / hour. The solid catalyst component [A] and the mixture of triisobutylaluminum and diisobutylaluminum hydride were added in equal amounts at a rate of 5 L / hour. Similarly, STATSAFE3000 was added to the polyethylene powder at a concentration of 15 ppm. In addition, 1-butene was continuously added as an α-olefin so that the concentration of 1-butene was 6.6 mol % based on the gas phase ethylene concentration. The polymerization pressure was maintained at 0.3 MPa by continuously feeding ethylene. Under these conditions, the contents of the polymerization reactor were thoroughly stirred to make the contents uniform. The production rate of polyethylene powder was 10 kg / hour. The catalytic activity was 30,000 g-PE / g-solid catalyst component [A]. The polyethylene polymerization slurry was continuously discharged into a flash drum at a pressure of 0.05 MPa so that the level of the polymerization reactor was kept constant, and unreacted ethylene was separated. It was then continuously passed through a solvent separation process and then sent to a drying process. The dryer was a drum type with a nitrogen gas flow and a jacket temperature of 80°C, and the oxygen concentration inside the dryer was adjusted to 80 ppm. There was no presence of polymer aggregates, and the slurry extraction pipe did not become clogged, allowing for stable continuous operation. Methanol was added to the obtained polyethylene powder as an aliphatic saturated alcohol, adjusting the concentration to 150 ppb, and the mixture was mixed uniformly in a Henschel mixer. The mixture was then passed through a sieve with 425 μm openings to remove any material that did not pass through the sieve. The polyethylene powder (PE-1) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0051] Example 2 After the drying step, calcium stearate (C60, manufactured by Dainichi Chemical Co., Ltd.) was mixed in the polyethylene powder to a concentration of 1,000 ppm when the mixture was uniformly mixed using a Henschel mixer. The other conditions were the same as those in Example 1. The polyethylene powder (PE-2) obtained as above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0052] Example 3 The α-olefin used was 1-propene. Other conditions were the same as in Example 1. The polyethylene powder (PE-3) obtained as above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0053] Example 4 Ethanol was used as the aliphatic saturated alcohol. Other conditions were the same as in Example 1. The polyethylene powder (PE-4) obtained as above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0054] Example 5 The polymerization temperature was kept at 77°C. 1-butene was continuously added as an α-olefin so that the concentration was 6.4 mol% based on the gas phase ethylene concentration. Hydrogen was continuously added so that the concentration was 0.9 mol% based on the gas phase ethylene concentration. The other conditions were the same as in Example 1. The polyethylene powder (PE-5) obtained as above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0055] Example 6 The polymerization temperature was kept at 45° C. 1-butene was continuously added as an α-olefin so that the concentration of 1-butene was 7.0 mol % relative to the gas phase ethylene concentration. The polymerization pressure was kept at 0.5 MPa. Other conditions were the same as those in Example 1. The polyethylene powder (PE-6) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0056] Example 7 The polymerization temperature was kept at 73° C. 1-butene was continuously added as an α-olefin so that the concentration was 0.3 mol % relative to the gas phase ethylene concentration. The polymerization pressure was kept at 0.15 MPa. Other conditions were the same as those in Example 1. The polyethylene powder (PE-7) obtained as above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0057] Example 8 The polymerization temperature was kept at 57° C. Other conditions were the same as in Example 7. The polyethylene powder (PE-8) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0058] Example 9 The polymerization temperature was kept at 58°C, 1-butene was continuously added as an α-olefin so that the concentration was 2.0 mol% relative to the gas phase ethylene concentration, and the oxygen concentration in the dryer was adjusted to 150 ppm by flowing nitrogen gas through the dryer. The other conditions were the same as in Example 1. The polyethylene powder (PE-9) obtained as described above was evaluated by the above method. The evaluation results are shown in Table 1.

[0059] Example 10 The oxygen concentration in the dryer was adjusted to 80 ppm by flowing nitrogen gas in the dryer, and the supply of hexane was adjusted to 40 L / hour. Other conditions were the same as in Example 9. The polyethylene powder (PE-10) obtained as described above was evaluated by the above method. The evaluation results are shown in Table 1.

[0060] Example 11 The oxygen concentration in the dryer was adjusted to 80 ppm by passing nitrogen through the dryer, and the obtained polyethylene powder was uniformly mixed in a Henschel mixer without adding methanol. The other conditions were the same as in Example 9. The polyethylene powder (PE-11) obtained as described above was evaluated by the above method. The evaluation results are shown in Table 1.

[0061] Comparative Example 1 The polymerization temperature was kept at 83°C. 1-butene was continuously added as an α-olefin so that the concentration was 6.2 mol% relative to the gas-phase ethylene concentration. Hydrogen was continuously added so that the concentration was 0.2 mol% relative to the gas-phase ethylene concentration. The supply of hexane was adjusted to 40 L / hour. Furthermore, the oxygen concentration in the dryer was adjusted to 150 ppm by causing a nitrogen stream in the dryer. Other conditions were the same as in Example 1. The polyethylene powder (PE-12) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0062] Comparative Example 2 The supply of hexane was adjusted to 55 L / hour, and the obtained polyethylene powder was mixed uniformly in a Henschel mixer without adding methanol. The other conditions were the same as those in Comparative Example 1. The polyethylene powder (PE-13) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0063] Comparative Example 3 The oxygen concentration in the dryer was adjusted to 80 ppm, and the obtained polyethylene powder was uniformly mixed in a Henschel mixer without adding methanol. The other conditions were the same as those in Comparative Example 1. The polyethylene powder (PE-14) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0064] Comparative Example 4 The obtained polyethylene powder was mixed uniformly in a Henschel mixer without adding methanol. The other conditions were the same as those in Comparative Example 1. The polyethylene powder (PE-15) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0065] Comparative Example 5 The polymerization temperature was kept at 75° C. No α-olefin was added. No aliphatic saturated alcohol was added. The other conditions were the same as those in Example 1. The polyethylene powder (PE-16) obtained as above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0066] Comparative Example 6 The polymerization temperature was maintained at 73°C. 1-butene was continuously added as an α-olefin so that the concentration was 0.3 mol% relative to the gas phase ethylene concentration. No aliphatic saturated alcohol was added. When the mixture was uniformly mixed using a Henschel mixer after drying, calcium stearate (C60, manufactured by Dainichi Chemical Co., Ltd.) was mixed to a concentration of 1,000 ppm relative to the polyethylene powder. Other conditions were the same as in Example 1. The polyethylene powder (PE-17) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0067] Comparative Example 7 The polymerization temperature was kept at 47° C. No α-olefin was added. The polymerization pressure was kept at 0.4 MPa. No aliphatic saturated alcohol was added. The other conditions were the same as those in Example 1. The polyethylene powder (PE-18) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0068] Comparative Example 8 The polymerization temperature was maintained at 80°C. 1-butene was continuously added as an α-olefin to give a concentration of 0.15 mol% relative to the gas-phase ethylene concentration. Hydrogen was continuously added to give a concentration of 0.2 mol% relative to the gas-phase ethylene concentration. The polymerization pressure was maintained at 0.15 MPa. No aliphatic saturated alcohol was added. When uniformly mixing using a Henschel mixer after drying, calcium stearate (Dainichi Chemical Co., Ltd., C60) was mixed to a concentration of 500 ppm relative to the polyethylene powder. Other conditions were the same as in Example 1. The polyethylene powder (PE-19) obtained as described above was evaluated by the above-mentioned method. The evaluation results are shown in Table 2.

[0069] [Table 1]

[0070] [Table 2]

[0071] It was found that the polyethylene powders of Examples 1 to 11 gave molded articles that were excellent in impact resistance and abrasion resistance, as well as in transparency and ease of detecting dirt. [Industrial Applicability]

[0072] INDUSTRIAL APPLICABILITY The polyethylene powder of the present invention has industrial applicability as a lining material for hoppers, chutes, etc., which is non-adhesive and has a low coefficient of friction; as a material for bearings, gears, roller guide rails, bone substitutes, osteoconductive materials or bone inductive materials, separators for secondary batteries such as lithium ion secondary batteries and lead-acid batteries, and fibers, which are required to have self-lubrication, a low coefficient of friction and abrasion resistance.

Claims

1. Ethylene units, and / or ethylene units and α-olefin units having 3 to 8 carbon atoms and The viscosity average molecular weight is 1 million or more and 10 million or less, Yellowness index (YI) and whiteness index (whiteness) of the sheet molded product obtained by compression molding under the conditions specified in JIS K6936-2 The chromaticity WI and density ρ (kg / m 3 ) satisfy the following formula (1): Polyethylene powder. 0.50≦(-YI)×WI / ρ<2.0...Formula (1)

2. The α-olefin is 1-propene or 1-butene, The polyethylene powder according to claim 1, having a constituent content of 1.0 mol% or less.

3. The method according to claim 1 or 2, wherein the bulk density is 0.30 g / mL or more and less than 0.60 g / mL. Polyethylene powder.

4. Magnesium and titanium measured by inductively coupled plasma mass spectrometry (ICP / MS) 2. The total content of aluminum elements is 1 ppm or more and 50 ppm or less according to claim 1 .

4. The polyethylene powder according to any one of claims 3 to 4.

5. Melting integral curve by differential scanning calorimetry (DSC) The temperature at 30% melting in the wire is 120° C. or more and 140° C. or less, The temperature at 50% melting is 125° C. or more and 145° C. or less, The temperature at 70% melting is 130°C or higher and 150°C or lower. The polyethylene powder according to any one of claims 1 to 4.

6. Melting integral curve by differential scanning calorimetry (DSC) The temperature at 50% melting in the wire is 130° C. or more and 140° C. or less. The polyethylene powder according to claim 5.

7. A molded article of the polyethylene powder according to any one of claims 1 to 6.

8. The molded article according to claim 7, which is a compression molded article.

9. The molded article according to claim 7, which is an extrusion molded article.

10. The molded article according to claim 7, which is a stretched molded article.

11. The molded article according to claim 7, which is a microporous membrane.

12. The molded article according to claim 7, which is a fiber.

Citation Information

Patent Citations

  • Ultra-high-molecular-weight polyethylene particulate excellent in heat resistance and method for producing the same

    JP2007023171A

  • Ultra-high molecular weight ethylene-based copolymer powder, and molding

    JP2015157905A

  • Polyethylene powder and fiber

    JP2017088773A

  • Polyethylene powder, sintered porous sheet, adsorption buffer material and battery separator

    JP2019038931A

  • Ethylene polymer particle and molded body

    JP2020180234A