Metal-resin composite electromagnetic shielding material

The metal-resin composite electromagnetic shielding material addresses moldability and shielding effectiveness issues by using laminated layers with optimized conductivity and thickness, ensuring high moldability and effective shielding in complex shapes.

JP7567095B2Active Publication Date: 2024-10-15JX NIPPON MINING & METALS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024521080
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-26
Filing Date
2023-09-15
Publication Date
2024-10-15
Estimated Expiration
2043-09-15

AI Technical Summary

Technical Problem

Existing electromagnetic shielding materials face issues with low moldability, cracking during molding, and reduced shielding effectiveness due to gaps and thickness requirements, especially in complex shapes and large volumes.

Method used

A metal-resin composite electromagnetic shielding material with specific conductivity and thickness parameters, laminated in a way that satisfies VFL > 0.24, allowing for high moldability and continuous formation even with irregularities up to 5 mm or more, using multiple metal and resin layers with optimized thickness and conductivity.

Benefits of technology

The material achieves high moldability and maintains effective electromagnetic shielding, reducing weight and manufacturing costs while ensuring continuous formation and improved shielding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567095000016
    Figure 0007567095000016
  • Figure 0007567095000017
    Figure 0007567095000017
  • Figure 0007567095000018
    Figure 0007567095000018
Patent Text Reader

Abstract

The present invention provides a metal resin composite electromagnetic shielding material which has high formability. This metal resin composite electromagnetic shielding material is obtained by stacking N metal layers (N is an integer of 1 or more) and M resin layers (M is an integer of 1 or more), and is characterized in that the Value of Forming Limit (VFL) thereof satisfies VFL > 0.24.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal-resin composite electromagnetic shielding material, and in particular to a metal-resin composite electromagnetic shielding material that can be used as a covering material or exterior material for electric and electronic devices. [Background technology]

[0002] In recent years, interest in global environmental issues has been growing worldwide, and environmentally friendly automobiles equipped with secondary batteries, such as electric vehicles and hybrid vehicles, are becoming more and more widespread. Many of these automobiles use a system in which the direct current generated by the secondary battery is converted to alternating current via an inverter, and the necessary power is then supplied to an AC motor to obtain driving force. Electromagnetic waves are generated due to the switching operation of the inverter, etc. Since electromagnetic waves cause reception interference for on-board audio equipment, wireless equipment, etc., measures have been taken to shield electromagnetic waves by housing the inverter or the battery and motor together with the inverter in a metal case.

[0003] However, metal electromagnetic shielding materials have low moldability and are heavy because they are metal. Therefore, a resin composition for insert molding containing a resin and an electromagnetic shielding filler (Patent Document 1: JP 2021-55113 A), a method for insert molding a mesh-like electromagnetic shielding body having a flat case development shape formed of a mesh-like metal body and constituting a central part of the case body and a folded side part around it in a mold (Patent Document 2: JP 4811245 A), and an electromagnetic shielding fabric characterized by being woven with a mixed yarn formed by Z-twisting and / or S-twisting a metal wire into one or more ordinary spinnable fibers (Patent Document 3: JP 2011-179162 A) have been devised. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-55113 [Patent Document 2] Patent No. 4811245 [Patent Document 3] JP 2011-179162 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when using resin mixed with conductive filler, the shielding performance per thickness is poor, and a larger thickness is required to obtain a high shielding effect for magnetic field shielding. Also, in the case of insert molding using mesh shielding bodies or electromagnetic wave shielding fabrics, there are problems with the shielding effect being reduced at the four corners due to gaps in the molded body, and the effect of shielding magnetic fields is also reduced. Therefore, a method to improve moldability using an approach different from conventional technology is needed.

[0006] Metal foils (metal layers) such as copper foils used in electromagnetic shielding materials generally have a thickness of several μm to several tens of μm, so they are prone to cracking when laminated with a resin film and molded. Therefore, it is important to suppress cracking and improve moldability.

[0007] Metal-resin composite materials have high moldability and can be molded into complex shapes, but when a large amount is molded, the metal layer inside may crack during molding. Large cracks in the metal layer can lead to a decrease in shielding properties, so this needs to be prevented.

[0008] The present invention has been made in consideration of the above circumstances, and an object of one embodiment is to provide a metal-resin composite electromagnetic shielding material that has high moldability, i.e., is capable of conforming to irregularities of 5 mm or more. [Means for solving the problem]

[0009] As a result of intensive research, the inventors have found that a metal-resin composite electromagnetic shielding material in which the VFL (Value of Forming Limit) calculated from specific parameters satisfies certain conditions has high formability, and therefore can be molded into a continuous body, and is particularly capable of following irregularities of 5 mm or more. The present invention was completed based on the above findings, and is exemplified below.

[0010] [1] A metal-resin composite electromagnetic shielding material comprising N (where N is an integer of 1 or more) metal layers and M (where M is an integer of 1 or more) resin layers laminated together, A metal-resin composite electromagnetic wave shielding material characterized in that its VFL (Value of Forming Limit), calculated by the following formula, satisfies VFL>0.24.

number

[0011] According to one embodiment of the present invention, it is possible to provide a metal-resin composite electromagnetic shielding material having high moldability. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram for explaining a method for evaluating forming limits in accordance with ISO-12004-2-2008. [Diagram 2] 13 is a diagram showing the deformation angle and the distance between markings after deformation. FIG. [Diagram 3] FIG. 13 is a diagram showing a method for calculating the maximum strain ε1 and the minimum strain ε2 required to calculate the VFL. [Figure 4] 1 is a diagram showing an example of a crack penetrating a metal layer; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Next, the embodiments of the present invention will be described in detail. It should be understood that the present invention is not limited to the following embodiments, and that appropriate design changes, improvements, etc. may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0014] (1. Metal layer) There is no particular limitation on the material of the metal layer constituting the metal-resin composite electromagnetic shielding material according to one embodiment of the present invention. However, when the electrical conductivity of the metal layer of the metal-resin composite electromagnetic shielding material is σ (S / m) and the total thickness of the metal layer is d (m), the apparent conductance C is preferably C=σ×d>1.0×10 -11 It is preferable that (S) is satisfied. When multiple metal layers are provided, the conductivity of each layer is set to σ N (S / m), and the thickness of each layer is d N (m), the total apparent conductance C of the metal layer is C=Σσ N ×d N >1.0×10 -11It is preferable that (S) is satisfied. By satisfying this condition, a high shielding effect is ensured as a metal-resin composite electromagnetic wave shielding material.

[0015] In this specification, the electrical conductivity is measured based on the four-probe method defined in JIS K7194.

[0016] The metal layer surface may be formed with various surface treatment layers for the purpose of adhesion promotion, environmental resistance, heat resistance, rust prevention, etc. For example, in order to improve the environmental resistance and heat resistance required when the metal surface is the outermost layer, Au plating, Ag plating, Sn plating, Ni plating, Zn plating, Sn alloy plating (Sn-Ag, Sn-Ni, Sn-Cu, etc.), chromate treatment, etc. may be applied. These treatments may be combined. From the viewpoint of cost, Sn plating or Sn alloy plating is preferable. In addition, in order to improve the adhesion between the metal layer and the resin layer, or between the metal layers themselves, chromate treatment, roughening treatment, Ni plating, etc. may be applied. These treatments may be combined. Roughening treatment is preferable because it is easier to obtain adhesion. In addition, metal plating with high relative magnetic permeability may be provided in order to improve the shielding effect against a direct current magnetic field. Examples of metal plating with high relative magnetic permeability include Fe-Ni alloy plating and Ni plating.

[0017] When using copper foil, it is preferable to use a high purity copper foil because it improves shielding performance, and the purity is preferably 99.5% by mass or more, more preferably 99.8% by mass or more. As the copper foil, rolled copper foil, electrolytic copper foil, metallized copper foil, etc. can be used, but rolled copper foil, which has excellent flexibility and formability (formability includes drawing formability, the same applies below), is preferable. When alloy elements are added to the copper foil to make a copper alloy foil, the total content of these elements and unavoidable impurities is preferably less than 0.5% by mass. In addition, it is preferable to contain at least one selected from the group consisting of Sn, Mn, Cr, Zn, Zr, Mg, Ni, Si, and Ag in a total of 50 to 2000 ppm by mass, and / or P in a total of 10 to 50 ppm by mass in the copper foil, because this improves elongation compared to pure copper foil of the same thickness.

[0018] The thickness of the metal layer constituting the metal-resin composite electromagnetic shielding material according to one embodiment of the present invention is preferably 4 μm or more per layer. If the thickness is 4 μm or more, it is possible to avoid the metal layer from becoming difficult to handle, and to prevent the ductility of the metal layer from significantly decreasing and the moldability of the laminate from becoming insufficient. In addition, if the thickness of each layer is less than 4 μm, it becomes necessary to laminate a large number of metal layers in order to obtain an excellent electromagnetic shielding effect, which causes a problem of increased manufacturing costs. From this viewpoint, the thickness of each metal layer is more preferably 10 μm or more per layer, even more preferably 12 μm or more, and even more preferably 15 μm or more. On the other hand, if the thickness of each layer exceeds 100 μm, the moldability may be deteriorated, so the thickness of each layer is preferably 100 μm or less per layer, more preferably 50 μm or less, even more preferably 45 μm or less, and even more preferably 40 μm or less. The thickness of the metal layer can be measured, for example, by averaging the measured values ​​at four points on the sheet sample surface using a constant pressure thickness tester (THICKNESS METER B-1, manufactured by Toyo Seiki Seisakusho) in accordance with Method A in JIS K 6250:2019. The measurement can be performed with an indenter diameter of 5 mm and a pressure of 1.22 N applied to the indenter. If the thickness of the metal layer in the laminate is to be measured, the thickness cross section can be observed and measured using a SEM or the like.

[0019] Although the metal layer constituting the metal-resin composite electromagnetic shielding material may be one, from the viewpoint of improving moldability and shielding performance, it is preferable that the metal layer constituting the metal-resin composite electromagnetic shielding material is laminated in a plurality of sheets via a resin layer, and from the viewpoint of ensuring excellent electromagnetic shielding properties while reducing the total thickness of the metal-resin composite electromagnetic shielding material, it is more preferable that the metal layer is laminated in two or more sheets via a resin layer. By laminating two or more metal layers via a resin layer, the shielding effect is significantly improved compared to the case where the metal layer is a single layer or the case where two metal layers are laminated without a resin layer, even if the total thickness of the metal layers is the same. Even if the metal layers are directly laminated, the shielding effect is improved by increasing the total thickness of the metal layers, but in order to obtain a significant improvement effect, it is preferable to laminate the metal layers via a resin layer. That is, by laminating multiple metal layers constituting the laminate via a resin layer, the total thickness of the metal layers required to obtain the same electromagnetic shielding effect can be reduced, so that it is possible to achieve both weight reduction and electromagnetic shielding effect of the laminate. In this case, it is not necessary to directly overlap the metal layers, and it is also possible to configure the laminate so that some or all of the resin layers are overlapped. Of course, a configuration in which metal layers and resin layers are alternately laminated one by one is also possible.

[0020] This is believed to be because the presence of resin layers between the metal layers increases the number of times electromagnetic waves are reflected, resulting in attenuation of the electromagnetic waves. However, although the electromagnetic wave shielding properties improve with a larger number of metal layers, increasing the number of layers increases the number of lamination steps, leading to increased manufacturing costs, and the shielding improvement effect also tends to saturate, so the number of metal layers constituting the metal-resin composite electromagnetic wave shielding material is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less.

[0021] In one embodiment of the present invention, when multiple metal layers are formed, all the metal layers may be made of the same material, or different materials may be used for each layer. In addition, all the metal layers may have the same thickness, or the thickness may differ for each layer.

[0022] Therefore, in the metal-resin composite electromagnetic shielding material according to one embodiment of the present invention, the total thickness of all the metal layers can be 15 to 150 μm, or can be 100 μm or less, 80 μm or less, or 60 μm or less.

[0023] (2. Resin Layer) In the metal-resin composite electromagnetic shielding material according to one embodiment of the present invention, a resin layer is sandwiched between metal layers, and thus a significant improvement in the electromagnetic shielding effect is obtained by stacking a plurality of metal layers. Although the shielding effect is improved by increasing the total thickness of the metal layers even when the metal layers are directly stacked, in order to obtain a significant improvement effect, it is preferable to stack the metal layers via a resin layer. This is thought to be because the presence of a resin layer between the metal layers increases the number of reflections of the electromagnetic waves, thereby attenuating the electromagnetic waves.

[0024] A resin layer having a large impedance difference with the metal layer is preferable in terms of obtaining an excellent electromagnetic wave shielding effect. To generate a large impedance difference, the resin layer needs to have a small relative dielectric constant, which is preferably 10.0 (value at 20°C; the same applies below) or less, more preferably 5.0 or less, and even more preferably 3.5 or less. In principle, the relative dielectric constant cannot be smaller than 1.0. For commonly available materials, the minimum is about 2.0, and even if it is lowered further to approach 1.0, the increase in shielding effect is limited, while the material itself becomes special and expensive. Considering the balance between cost and function, the relative dielectric constant is preferably 2.0 or more, and more preferably 2.2 or more.

[0025] Specifically, from the viewpoint of moldability, synthetic resins are particularly preferred as materials constituting the resin layer. Fiber reinforcement materials such as carbon fiber, glass fiber, and aramid fiber can also be mixed into the resin layer. In addition, from the viewpoint of improving shielding properties, magnetic materials may be mixed into the resin layer within a range that does not affect the present invention. As synthetic resins, from the viewpoint of availability and moldability, polyesters such as PET (polyethylene terephthalate), PEN (polyethylene naphthalate), and PBT (polybutylene terephthalate), olefin resins such as polyethylene and polypropylene, polyamide, polyimide, liquid crystal polymer, polyacetal, fluorine resin, polyurethane, acrylic resin, epoxy resin, silicone resin, phenol resin, melamine resin, ABS resin, polyvinyl alcohol, urea resin, polyvinyl chloride, polycarbonate, polystyrene, styrene butadiene rubber, etc. are listed, and among these, PET, PEN, polyamide, and polyimide are preferred for reasons of moldability and cost. The synthetic resin may be an elastomer such as urethane rubber, chloroprene rubber, silicone rubber, fluororubber, styrene-based, olefin-based, PVC-based, urethane-based, or amide-based. All of the resin layers used in the metal-resin composite electromagnetic shielding material according to one embodiment of the present invention may be made of the same resin material, or different resin materials may be used for each layer. From the viewpoint of moldability, it is preferable that some or all of the resin layers are insulating layers.

[0026] The resin material can be laminated in the form of a film or fiber. The resin layer can be formed by applying an uncured resin composition to the metal layer and then curing it, but it is preferable to use a resin film that can be attached to the metal layer for ease of production. In particular, a PET film can be preferably used. In particular, the strength of the shielding material can be increased by using a biaxially stretched film as the PET film.

[0027] The thickness of the resin layer is not particularly limited, but since the (elongation) breaking strain of the shielding material tends to decrease when the thickness per layer is thinner than 4 μm, the thickness per layer of the resin layer is preferably 4 μm or more, more preferably 7 μm or more, even more preferably 9 μm or more, even more preferably 10 μm or more, even more preferably 20 μm or more, even more preferably 40 μm or more, even more preferably 80 μm or more, and even more preferably 100 μm or more. On the other hand, even if the thickness per layer exceeds 600 μm, the (elongation) breaking strain of the shielding material tends to decrease. Therefore, the thickness per layer of the resin layer is preferably 600 μm or less, more preferably 500 μm or less, even more preferably 400 μm or less, even more preferably 250 μm or less, and even more preferably 200 μm or less. In one embodiment of the present invention, all the resin layers may have the same thickness, or the thickness may differ from layer to layer. Here, one resin layer means a portion in which the resin is continuous without any metal layer interposed. For example, even when a plurality of resin films are continuously laminated in the manufacturing process of an electromagnetic wave shielding material, since there is no metal layer interposed between these films and it appears to be one continuous body, it is regarded as one resin layer. The thickness of the resin layer can be measured by the same method as the above-mentioned method for measuring the thickness of the metal layer.

[0028] Generally, the resin layer has higher ductility than the metal layer. Therefore, by supporting both sides of each metal layer with a resin layer, the ductility of the shielding metal layer is significantly improved, and the moldability of the laminate is significantly improved. From the viewpoint of improving the moldability, it is preferable to stack the metal layers via a resin layer rather than stacking the metal layers directly on each other.

[0029] The surface of the resin layer may be subjected to various surface treatments for the purpose of promoting adhesion with the metal layer, etc. For example, the adhesion with the shielding metal layer can be improved by applying a primer coat or a corona treatment to the surface of the resin layer to be attached to the shielding metal layer.

[0030] (3. Electromagnetic Shielding Materials) In one embodiment of the present invention, there is provided a metal-resin composite electromagnetic shielding material comprising N (where N is an integer of 1 or more) metal layers and M (where M is an integer of 1 or more) resin layers laminated together, the metal-resin composite electromagnetic shielding material being characterized in that the Value of Forming Limit (VFL) calculated by the following formula satisfies VFL>0.24.

number

[0031] There are no particular limitations on N as long as it is an integer of 1 or more, and a higher electromagnetic wave shielding effect can be obtained by increasing N. However, as described above, N is typically 1, 2, 3, 4, or 5.

[0032] Although M is not particularly limited as long as it is an integer of 1 or more, in order to sandwich a resin layer between metal layers and improve the electromagnetic wave shielding effect, M is typically M=N+1, M=N-1, or M=N. From the viewpoint of earth connection, etc., it is preferable that at least one of the outermost layers is a metal layer.

[0033] The method for calculating the VFL will be described in detail below. The inventors have found that the larger the VFL calculated from the above formula, the higher the moldability.

[0034] The forming limit is evaluated using a die for FLD (forming limit diagram) (Fig. 1). The die is designed by reducing the size specified in ISO-12004-2-2008 by 25%. The punch dimensions are D = 22.5 mm, R part R f = 2mm, 4mm or 6mm. Die R d= 2mm. The clearance between the punch and the die is 2.25mm. A W-shaped notch is attached to the blank holder, and the initial pressure of the die is set to 4000N to prevent the test piece from being pulled in during molding. When setting the test piece, a drive plate is sandwiched between the test piece and the stripper plate to reduce the effects of material and friction. Nitto Denko Corporation's Nitoflon No. 900UL (thickness 0.05mm) can be used as the drive plate. The drive plate has an outer diameter of φ60mm and a φ2mm hole in the center. A circular test piece with a diameter of φ60mm is cut out, a grid-like marking is made near the center with a pitch of 1mm, and the punch extrusion depth is increased by 0.5mm at a time to form the test piece. Three test pieces are prepared for each depth, and four arbitrary squares in the grid near the center of each test piece are observed under a microscope. The punch extrusion depth at which cracks penetrating the metal layer are observed in 50% or more (i.e., six or more of a total of twelve observation points) is recorded. The size of each square at that punch extrusion depth (L 1 , L 2 , L 3 , L 4 ), deformation angle (θ 1 , θ 2 ) is measured using a microscope (Figure 2).

[0035] Next, for the above four masses of each test piece, the average length and average deformation angle of the mass after deformation were calculated according to the following formula: Calculate TIFF0007567095000003.tif915.

number

number

number

[0036] Next, referring to FIG. 3, a true strain ε corresponding to the maximum strain and the minimum strain in the mass is calculated based on the average length and the average deformation angle. 1and ε 2 Calculate.

[0037] ε 1 and ε 2 The calculation procedure is as follows: first,

number

number

number

number

number

number

[0038] Finally, the maximum depth d at which the crack penetrating the metal layer became less than 50% was defined as the forming limit, and the VFL (Value of Forming Limit) for each mass was calculated using the following formula. In order to reduce measurement variability, the VFLs calculated for each mass were averaged to determine the VFL for the test piece.

number

[0039] Note that a crack penetrating a metal layer means a crack penetrating the outermost metal layer when the metal layer is the outermost layer (Fig. 4(A)), and when the metal layer is not the outermost layer but is covered with a resin layer, it means that the resin layer is peeled off and a crack penetrating the inner metal layer closest to the resin layer is confirmed (Fig. 4(B)). When both the resin layer and the metal layer are cracked, even if no cracks have occurred in the metal layer in the four observed squares, it is considered that there are cracks penetrating the metal layer in all squares (Fig. 4(C)).

[0040] When the VFL calculated by the above procedure exceeds 0.24, it was found that the molding limit of the metal-resin composite electromagnetic shielding material is 5.0 mm or more, and the molding processability is high. Therefore, when the VFL exceeds 0.24, it is possible to mold it as a continuum, and it is possible to follow irregularities of, for example, 5 mm or more. From this viewpoint, the VFL is preferably 0.26 or more, more preferably 0.28 or more, even more preferably 0.30 or more, even more preferably 0.32 or more, even more preferably 0.34 or more, even more preferably 0.36 or more, even more preferably 0.38 or more, and even more preferably 0.40 or more. The upper limit of the VFL is not particularly limited, but it can be set to 0.50 or less, for example, from the viewpoint of productivity and cost.

[0041] The method for improving the VFL is not particularly limited, but examples include a method for adjusting the thickness of each metal layer or a method for adjusting the elongation of a resin layer.

[0042] The metal-resin composite electromagnetic shielding material according to each embodiment of the present invention can be used for various electromagnetic shielding applications, such as a covering or exterior material for electric / electronic devices (e.g., inverters, communication devices, resonators, electron tubes / discharge lamps, electric heating devices, electric motors, generators, electronic components, printed circuits, medical devices, etc.), a covering material for harnesses and communication cables connected to electric / electronic devices, an electromagnetic shielding sheet, an electromagnetic shielding panel, an electromagnetic shielding bag, an electromagnetic shielding box, an electromagnetic shielding room, etc. Also, it is possible to insert mold the metal-resin composite electromagnetic shielding material according to each embodiment of the present invention as an insert part. Furthermore, in order to improve the electromagnetic shielding effect, an electromagnetic shielding sheet such as a magnetic sheet can be attached to the inside and / or outside of the metal-resin composite electromagnetic shielding material according to the present invention, as long as it does not affect the present invention. EXAMPLES

[0043] Examples of the present invention will be described below together with comparative examples, which are provided for a better understanding of the present invention and its advantages, and are not intended to limit the invention.

[0044] As the metal layer, three types of rolled copper foil (Type A: crystal grain size 300 μm or more; Type B: crystal grain size 10 μm or more; Type C: crystal grain size less than 10 μm, when measured from the surface using EBSD (crystal orientation analysis)) and two types of aluminum foil (Type A: A8021 material; Type B: A8021 material annealed at 300 °C for 1 hour) were prepared, and three types of resin (PET: polyethylene terephthalate film, PE: polyethylene film, PC: polycarbonate film) were prepared as the resin layer. The thickness and conductivity of each type of copper foil and the thickness of each type of resin are as shown in Table 1. In Table 1, the "Filler" column indicates that no filler was added, and that the "O" indicates that the resin contained filler.

[0045] For each example, lamination was performed according to the laminate structure shown in Table 1. A urethane adhesive was used as the adhesive for lamination. The order of each layer shown in the laminate structure is the order of lamination. Note that "Resin" means the resin layer, and "Metal" means the metal layer. There is an adhesive layer between each resin layer and each metal layer, but this is omitted in Table 1.

[0046] (Evaluation of moldability) For each of the examples and comparative examples, the mold limit depth was evaluated using the mold for the FLD (forming limit diagram) described above, and the VFL was calculated from the amount of distortion at that time. As shown in Table 1, the mold limit depth was 5.0 mm or more in the examples, and the moldability was excellent. In this case, the VFL value was higher than 0.24. In Table 1, "moldability" indicated as "◎" means that the mold limit depth is 8.5 mm or more, "◯" means that the mold limit depth is 5.0 mm or more and less than 8.5 mm, "△" means that the mold limit depth is 4.0 mm or more and less than 5.0 mm, and "×" means that the mold limit depth is less than 4.0 mm.

[0047] (Shielding performance evaluation) Then, for each example and comparative example, the apparent conductance C=σ×d(S) was calculated from the conductivity σ(S / m) of the metal layer and the total thickness d(m). The conductivity of the metal layer was obtained by the above-mentioned four-probe method, and the thickness of the metal layer was measured by the above-mentioned method using a constant pressure thickness tester (THICKNESS METER B-1, manufactured by Toyo Seiki Seisakusho) for each metal layer before lamination with the resin. In addition, for each example and comparative example, the magnetic field shielding effect was evaluated at a frequency of 500 kHz under room temperature (25° C.) conditions using a magnetic field measuring tool of a KEC method shielding effect measuring device (manufactured by Techno Science Co., Ltd., JSE-KEC) and a network analyzer (manufactured by Keysight Technologies, E5080). The calculation results of the apparent conductance C and the measurement results of the shielding effect are shown in Table 1. It can be seen that the examples of the present invention were able to maintain the shielding effect while improving the moldability. In Table 1, a "shielding effect" marked with "◯" means that the shielding effect is 10 dB or more in the 500 kHz frequency band, as measured by the KEC method, and a "×" means that the shielding effect is less than 10 dB in the 500 kHz frequency band, as measured by the KEC method.

[0048] [Table 1]

[0049] As can be seen from Table 1, the metal-resin composite electromagnetic shielding material of the embodiment of the present invention had excellent moldability due to a VFL exceeding 0.24. In addition, the shielding effect was also maintained at a high level. In addition, although multiple resin films were continuously laminated as the resin layer as in Example 24, the portions without the metal layer were combined into one resin layer.

Claims

1. A metal-resin composite electromagnetic shielding material comprising N (where N is an integer of 1 or more) metal layers and M (where M is an integer of 1 or more) resin layers laminated together, A metal-resin composite electromagnetic shielding material, characterized in that the VFL (Value of Forming Limit) calculated from the following formula according to the procedure described in the specification satisfies VFL>0.

24. [0010] (In the formula, ε 1 and ε 2 are true strains corresponding to the maximum strain and the minimum strain calculated for a 1 mm pitch mass of the metal-resin composite electromagnetic shielding material by the method described in the specification.)

2. The apparent conductance C of the metal layer is C=σ×d>1.0×10, where σ is the electrical conductivity of the metal layer and d is the total thickness of the metal layer. -11 2. The metal-resin composite electromagnetic shielding material according to claim 1, which satisfies (S).

3. 3. The metal-resin composite electromagnetic shielding material according to claim 1, wherein each metal layer has a thickness of 4 to 100 μm.

4. 3. The metal-resin composite electromagnetic shielding material according to claim 1, wherein each of the resin layers has a thickness of 4 to 600 μm.

5. 3. The metal-resin composite electromagnetic shielding material according to claim 1, wherein the total thickness of each metal layer is 15 to 150 μm.

6. A covering or exterior material for electric / electronic equipment, comprising the metal-resin composite electromagnetic shielding material according to claim 1 or 2.

7. An electric / electronic device comprising the covering material or exterior material according to claim 6.

Citation Information

Patent Citations

  • JP1973011245B1

  • Electromagnetic wave shield woven fabric, electromagnetic wave shield sheet, electromagnetic wave shield material, and electromagnetic wave shield casing

    JP2011179162A

  • Sealing body of electronic component

    JP2021055113A

  • Electromagnetic wave shield material

    JP2022091579A