Manufacturing method of rare earth bonded magnet

A resin composition with controlled melt viscosity and a compound powder method enhance the strength and density of rare earth bonded magnets by controlled heating and cooling, addressing the limitations of existing manufacturing methods.

JP7567284B2Active Publication Date: 2024-10-16RESONAC CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020140974
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-17
Filing Date
2020-08-24
Publication Date
2024-10-16
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing rare earth bonded magnets do not adequately enhance the strength of the molded bodies while maintaining excellent physical properties.

Method used

A resin composition with specific melt viscosity ranges and a compound powder containing rare earth magnetic powder and resin composition are used, with a method involving mixing, applying a magnetic field, and controlled heating and cooling to form a molded body.

Benefits of technology

The resin composition improves the mechanical strength and density of the molded body, allowing for higher packing density and enhanced properties of the rare earth bonded magnets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567284000003
    Figure 0007567284000003
  • Figure 0007567284000001
    Figure 0007567284000001
  • Figure 0007567284000002
    Figure 0007567284000002
Patent Text Reader

Abstract

To provide a resin composition allowing for further improving the strength of a molded body obtained from a compound powder containing a rare-earth magnetic powder and a resin composition.SOLUTION: A resin composition has a melt viscosity at 100°C of 1 Pa s or higher and 50 Pa s or lower, and a melt viscosity at 50°C after heating at 100°C for 30 minutes to be higher than that at 50°C before heating, and is solid at 25°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a compound powder, and a method for producing a rare earth bonded magnet. [Background technology]

[0002] Compound powders containing metal powders and resin compositions are used as raw materials for various industrial products, such as inductors, electromagnetic shields, and bonded magnets, depending on the physical properties of the metal powder (see Patent Document 1 below). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-154613 Summary of the Invention [Problem to be solved by the invention]

[0004] When manufacturing industrial products from compound powder, a molded body having a shape according to the application of the industrial product is made from the compound powder. For example, when manufacturing a rare earth bonded magnet, the compound powder is filled into a mold and heated while a magnetic field is applied to the compound powder (i.e., heat molding in a magnetic field) to obtain a molded body, which is then cooled to an appropriate temperature and removed from the mold to obtain a rare earth bonded magnet molded body. There is a demand for technology that can further improve the strength of the molded body while maintaining the excellent physical properties of a rare earth bonded magnet.

[0005] The present invention aims to provide a resin composition capable of improving the strength of a molded body obtained from a compound powder containing a rare earth magnetic powder and a resin composition. The present invention also aims to provide a compound powder containing such a resin composition, and a method for producing a rare earth bonded magnet using the resin composition. [Means for solving the problem]

[0006] A resin composition according to one aspect of the present invention has a melt viscosity at 100°C of 1 Pa·s or more and 50 Pa·s or less, a melt viscosity at 50°C after heating at 100°C for 30 minutes that is higher than the melt viscosity at 50°C before heating, and is a solid at 25°C.

[0007] In one embodiment, the resin composition may be mixed with a rare earth magnetic powder to obtain a rare earth bonded magnet, and in one embodiment, the resin composition may include an epoxy resin, a phenolic resin, and a compound having an epoxy group reactive group.

[0008] In one embodiment, the epoxy group reactive group may be an amino group.

[0009] In one embodiment, the content of the compound having an epoxy group-reactive group may be 1 to 20 parts by mass with respect to 100 parts by mass in total of the epoxy resin and the phenol resin.

[0010] In one embodiment, the content of the compound having an epoxy group-reactive group may be 1 to 30 parts by mass with respect to 100 parts by mass of the epoxy resin.

[0011] The compound powder according to one aspect of the present invention contains rare earth magnetic powder and the above-mentioned resin composition, and the mass ratio of the rare earth magnetic powder to the resin composition (rare earth magnetic powder / resin composition) is 94 / 6 to 99 / 1.

[0012] According to one aspect of the present invention, a method for producing a rare earth bonded magnet includes the steps of mixing a rare earth magnetic powder with the above-mentioned resin composition to prepare a compound powder, filling the compound powder into a mold and heating it at 80 to 120°C while applying a magnetic field to the compound powder to obtain a molded body, cooling the molded body after releasing the magnetic field, and removing the molded body, which has been cooled to 40 to 60°C, from the mold. Effect of the Invention

[0013] According to the present invention, it is possible to provide a resin composition capable of further improving the strength of a molded body obtained from a compound powder containing a rare earth magnetic powder and a resin composition. Also, according to the present invention, it is possible to provide a compound powder containing such a resin composition, and a method for producing a rare earth bonded magnet using the resin composition. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a diagram showing the melt viscosity measurement results of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Preferred embodiments of the present invention will be described below, however, the present invention is not limited to the following embodiments.

[0016] <Compound powder> The compound powder according to the present embodiment comprises a plurality (a large number) of rare earth magnetic particles and a resin composition that covers each of the rare earth magnetic particles. That is, each particle that constitutes the compound powder has a rare earth magnetic particle and a resin composition that covers the rare earth magnetic particle. For example, a layer containing a resin composition (such as a layer made of a resin composition) may cover the surface of the rare earth magnetic particle. Each particle that comprises a rare earth magnetic particle and a resin composition that covers the rare earth magnetic particle may be referred to as a "resin-coated particle".

[0017] The rare earth magnetic particles may contain at least a rare earth metal. The resin composition contains at least a resin. The resin composition may be a component that may include a resin, a curing agent, a curing accelerator, an additive, etc., and may be, for example, the remaining components (non-volatile components) excluding the organic solvent and the rare earth magnetic particles. The additives are the remaining components of the resin composition excluding the resin, the curing agent, and the curing accelerator. The additives are, for example, reactive diluents, coupling agents, flame retardants, etc. The compound powder may contain wax as an additive. The resin composition may be uncured. The resin composition may be semi-cured.

[0018] The melt viscosity of the resin composition at 100°C is 1 Pa·s or more and 50 Pa·s or less. The melt viscosity of the resin composition at 100°C may be 1.5 Pa·s or more and 30 Pa·s or less, or may be 2.0 Pa·s or more and 10 Pa·s or less. Note that 100°C is a guideline for the temperature when the compound powder is heat-molded in a magnetic field, and is a temperature at which the resin composition can have an appropriate fluidity.

[0019] By having the melt viscosity of the resin composition at 100°C be 1 Pa·sec or more, the mechanical strength of the molded body formed from the compound powder can be increased. On the other hand, by having the melt viscosity of the resin composition at 100°C be 50 Pa·sec or less, the friction (interface friction) between the rare earth magnetic particles contained in the compound powder and the resin composition is reduced. Therefore, in the process of forming a molded body from the compound powder, the rare earth magnetic particles are easily moved in the resin composition, and the rare earth magnetic particles are easily packed densely (through the resin composition). As a result, the ratio of the rare earth magnetic particles in the molded body can be increased, and the density of the molded body can be increased. The melt viscosity of the resin composition can be freely adjusted by the composition of the resin contained in the resin composition, the combination and compounding ratio of multiple types of resins, the combination and compounding ratio of each of the resin and reactive diluent, and the composition and compounding ratio of each of the curing agent, curing accelerator, and additive in the resin composition. However, the action and effect of the present invention are not limited to the above items.

[0020] The melt viscosity of the resin composition at 50°C after heating at 100°C for 30 minutes is higher than the melt viscosity at 50°C before heating. That is, the melt viscosity of the resin composition at 50°C when cooled after heating at 100°C is higher than the melt viscosity at 50°C when heated before heating at 100°C. 50°C is a guideline for the temperature when a molded body obtained by heat molding in a magnetic field is removed from the mold, and is a temperature at which the molded body can retain a small amount of flexibility compared to when cooled to room temperature. The melt viscosity of the resin composition after the thermal history does not return to the value before the thermal history, so that the mechanical strength of the molded body can be increased. The magnitude relationship between the melt viscosity at 50°C after heating at 100°C for 30 minutes and the melt viscosity at 50°C before heating can be adjusted, for example, by the melt viscosity of the epoxy resin, the melt viscosity of the phenol resin, the structure of the compound having an epoxy group reactive group, the compounding ratio of the epoxy resin and the compound having an epoxy group reactive group, etc.

[0021] The melt viscosity of the resin composition at 50°C before heating at 100°C can be 80 Pa·s or more and 800 Pa·s or less from the viewpoint of handling, and may be 90 Pa·s or more and 700 Pa·s or less. In addition, the melt viscosity of the resin composition at 50°C after heating at 100°C for 30 minutes may be 300 Pa·s or more and may be 800 Pa·s or more. This makes it easy to increase the mechanical strength of the molded body. The melt viscosity of the resin composition at 50°C after heating at 100°C for 30 minutes may be 1500 Pa·s or less and may be 800 Pa·s or less. This makes it easy to densify the molded body when the molded body obtained by compression molding is further subjected to cold isotropic pressing to obtain a molded body.

[0022] The resin composition is a solid at 25° C. Being a solid at 25° C., it can be made into a compound powder having excellent flowability and handleability.

[0023] The remaining particles, excluding the resin composition, from the compound powder may be referred to as "rare earth magnetic powder". The rare earth magnetic powder comprises a plurality of rare earth magnetic particles. The rare earth magnetic powder may consist of only rare earth magnetic particles. The resin composition may cover at least a part or the whole of each particle constituting the rare earth magnetic powder. The resin composition may adhere to the surface of each particle constituting the rare earth magnetic powder. The resin composition may adhere to the whole surface of each particle constituting the rare earth magnetic powder, or may adhere to only a part of the surface of the particle. The compound powder may comprise an uncured resin composition and a rare earth magnetic powder. The compound powder may comprise a semi-cured product of the resin composition (for example, a B-stage resin composition) and a rare earth magnetic powder. The compound powder may be formed from a rare earth magnetic powder and a resin composition.

[0024] The content of the rare earth magnetic powder in the compound powder may be 94 mass % or more and 99 mass % or less, or may be 95 mass % or more and 97 mass % or less, based on the total mass of the compound powder.

[0025] The content of the resin composition in the compound powder may be 1% by mass or more and 6% by mass or less, or 3% by mass or more and 5% by mass or less, based on the total mass of the compound powder. The mass ratio of the rare earth magnetic powder and the resin composition in the compound powder (rare earth magnetic powder / resin composition) may be 94 / 6 to 99 / 1, or 95 / 5 to 97 / 3.

[0026] The average particle size of each resin-coated particle constituting the compound powder may be, for example, 1 μm or more and 300 μm or less. The thickness of the resin composition (layer) covering the rare earth magnetic particles may be, for example, 0.1 μm or more and 10 μm or less. The average particle size of the rare earth magnetic particles may be, for example, 1 μm or more and 300 μm or less. The average particle size may be measured, for example, by a particle size distribution meter. The shape of the rare earth magnetic particles may be, for example, spherical, flat, prismatic or acicular, and is not particularly limited. When the shape of the rare earth magnetic particles is spherical, the density of the molded body tends to be high. The compound powder may contain multiple types of rare earth magnetic particles having different average particle sizes.

[0027] Depending on the composition or combination of the rare earth magnetic particles contained in the compound powder, the various properties such as electromagnetic properties of the molded body formed from the compound powder can be freely controlled, and the molded body can be used as various industrial products or their raw materials. The industrial products manufactured using the compound powder may be, for example, automobiles, medical devices, electronic devices, electrical devices, information and communication devices, home appliances, audio devices, and general industrial devices. For example, when the compound powder contains a permanent magnet such as SmFeN alloy or NdFeB alloy as the rare earth magnetic particles, the compound powder may be used as the raw material of a bonded magnet.

[0028] (Details of Resin Composition) The resin composition functions as a binder for the rare earth magnetic powder, and imparts mechanical strength to a molded body formed from the compound powder. For example, when the compound powder is molded under high pressure using a mold, the resin composition contained in the compound powder fills between the particles constituting the rare earth magnetic powder, binding the particles together. By curing the resin composition in the molded body, the cured resin composition binds the particles constituting the rare earth magnetic powder together more firmly, improving the mechanical strength of the molded body.

[0029] The resin composition may contain a thermosetting resin. The thermosetting resin may be, for example, at least one selected from the group consisting of an epoxy resin, a phenolic resin, and a polyamideimide resin. When the resin composition contains both an epoxy resin and a phenolic resin, the phenolic resin may function as a curing agent for the epoxy resin. The resin composition may contain a thermoplastic resin. The thermoplastic resin may be, for example, at least one selected from the group consisting of an acrylic resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, and polyethylene terephthalate. The resin composition may contain both a thermosetting resin and a thermoplastic resin. The resin composition may contain a silicone resin.

[0030] Since epoxy resins have excellent fluidity among thermosetting resins, the resin composition preferably contains an epoxy resin. The epoxy resin may be, for example, a resin having two or more epoxy groups in one molecule.

[0031] The epoxy resin may be a resin composition that is solid at room temperature (25°C) and has a melt viscosity of 1 Pa·s or more and 50 Pa·s or less at 100°C. In general, a solid epoxy resin having an ICI viscosity of 0.5 Pa·s or less is preferable. Examples of such epoxy resins include NC-3000L, NC-3000, NC-3000H, NC-7300L, EPPN-502H, RE-3035-L (all manufactured by Nippon Kayaku Co., Ltd.), jER-YX-4000, jER-YX-4000H, jER-YL-6121 (all manufactured by Mitsubishi Chemical Corporation), Epicron HP-7200L, and Epicron HP-4770 (all manufactured by DIC Corporation).

[0032] It is also possible to use a semi-solid epoxy resin on the premise that it is added to a solid curing agent or a solid epoxy resin. By adding a semi-solid epoxy resin to a solid curing agent or a solid epoxy resin, it is possible to lower the melt viscosity of the resin composition while keeping the resin composition solid at room temperature. Examples of such semi-solid epoxy resins include RE-303S-L, RE-303S (all manufactured by Nippon Kayaku Co., Ltd.), Epicoat 825, Epicoat 827, Epicoat 828, Epicoat 828EL, Epicoat 828US, Epicoat 828XA, Epicoat 1001 (all manufactured by Mitsubishi Chemical Corporation), Epicron 860, Epicron 1050, Epicron 1055, Epicron HP-4032, Epicron HP-4032D (all manufactured by DIC Corporation).

[0033] In the compound having an epoxy group-reactive group, examples of the group having epoxy group reactivity include an amino group, a phenolic hydroxyl group, a carboxyl group, a thiol group, etc. An amino group is preferred in that it is less likely to react in the step of obtaining a compound powder and can increase the viscosity of the resin composition to a predetermined viscosity in a short time when heated.

[0034] As the compound having an amino group, a compound having a primary amino group or a secondary amino group is preferable. In addition, a silane compound is preferable from the viewpoint of dispersion stabilization of rare earth magnetic powder such as SmFeN and strength retention after heat treatment, and a compound generally called a coupling material is preferable. As the silane compound having an amino group, KBM-602: N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, KBM-603: N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, KBM-903: 3-aminopropyltrimethoxysilane, KBE-903: 3-aminopropyltriethoxysilane, KBE-9103P: 3-triethoxysilyl-N-(1,3-dimethylbuteridene)propylamine, KBM-573: N-phenyl-3-aminopropyltrimethoxysilane, KBM-6803: N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (all manufactured by Shin-Etsu Chemical Co., Ltd.). These can be used alone or in combination of two or more.

[0035] The content of the compound having an epoxy group reactive group may be 1 to 20 parts by mass, or 7 to 19 parts by mass, per 100 parts by mass of the epoxy resin and the phenolic resin (epoxy resin curing agent) in total. When the content is 1 part by mass or more, it is easy to make the melt viscosity reach a predetermined melt viscosity within the heat molding time, and when the content is 20 parts by mass or less, it is easy to increase the strength of the molded body.

[0036] The content of the compound having an epoxy group-reactive group may be 1 to 30 parts by mass, or 10 to 30 parts by mass, relative to 100 parts by mass of the epoxy resin. When the content is 1 part by mass or more, it is easy to make the melt viscosity reach a predetermined melt viscosity within the heat molding time, and when the content is 30 parts by mass or less, it is easy to increase the strength of the molded body.

[0037] The resin composition may contain a reactive diluent. The resin composition may contain an epoxy resin and a reactive diluent. The epoxy resin is diluted with the reactive diluent, so that the melt viscosity of the resin composition is easily adjusted within the above range. The reactive diluent may be, for example, at least one of a monoepoxy compound and a diepoxy compound. The reactive diluent may be a monofunctional epoxy resin. The reactive diluent may be, for example, at least one selected from the group consisting of an alkyl monoglycidyl ether, an alkylphenol monoglycidyl ether, and an alkyl diglycidyl ether. As a commercially available product of the alkyl monoglycidyl ether, for example, YED188 or YED111N manufactured by Mitsubishi Chemical Corporation may be used. As a commercially available product of the alkylphenol monoglycidyl ether, for example, EPICLON520 manufactured by DIC Corporation or YED122 manufactured by Mitsubishi Chemical Corporation may be used. As a commercially available product of the alkyl diglycidyl ether, for example, YED216M or YED216D manufactured by Mitsubishi Chemical Corporation may be used.

[0038] Curing agents are classified into those that cure epoxy resins at temperatures ranging from low to room temperature, and heat-curing curing agents that cure epoxy resins by heating. Examples of curing agents that cure epoxy resins at temperatures ranging from low to room temperature include aliphatic polyamines, polyaminoamides, and polymercaptans. Examples of heat-curing curing agents include aromatic polyamines, acid anhydrides, phenol novolac resins, and dicyandiamide (DICY).

[0039] When a curing agent that cures an epoxy resin in the range of low temperature to room temperature is used, the glass transition point of the cured product of the epoxy resin is low, and the cured product of the epoxy resin tends to be soft. As a result, the molded body formed from the compound powder also tends to be soft. Therefore, from the viewpoint of improving the heat resistance of the molded body, the curing agent is preferably a heat-curing type curing agent. The heat-curing type curing agent may more preferably be a phenolic resin, and further preferably a phenolic novolac resin. In particular, by using a phenolic novolac resin as the curing agent, it is easy to obtain a cured product of the epoxy resin with a high glass transition point. As a result, the heat resistance and mechanical strength of the molded body are easily improved.

[0040] The phenolic resin may be at least one selected from the group consisting of, for example, aralkyl type phenolic resin, dicyclopentadiene type phenolic resin, salicylaldehyde type phenolic resin, novolac type phenolic resin, copolymer type phenolic resin of benzaldehyde type phenol and aralkyl type phenol, paraxylylene and / or metaxylylene modified phenolic resin, melamine modified phenolic resin, terpene modified phenolic resin, dicyclopentadiene type naphthol resin, cyclopentadiene modified phenolic resin, polycyclic aromatic ring modified phenolic resin, biphenyl type phenolic resin, and triphenylmethane type phenolic resin. The phenolic resin may be a copolymer composed of two or more of the above. As a commercially available phenolic resin, for example, Tamanol 758 manufactured by Arakawa Chemical Industries Co., Ltd., or HP-850N manufactured by Hitachi Chemical Co., Ltd. may be used.

[0041] The phenol novolac resin may be, for example, a resin obtained by condensing or co-condensing phenols and / or naphthols with aldehydes under an acid catalyst. The phenols constituting the phenol novolac resin may be, for example, at least one selected from the group consisting of phenol, cresol, xylenol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol. The naphthols constituting the phenol novolac resin may be, for example, at least one selected from the group consisting of α-naphthol, β-naphthol, and dihydroxynaphthalene. The aldehydes constituting the phenol novolac resin may be, for example, at least one selected from the group consisting of formaldehyde, acetaldehyde, propionaldehyde, benzaldehyde, and salicylaldehyde.

[0042] The curing agent may be, for example, a compound having two phenolic hydroxyl groups in one molecule. The compound having two phenolic hydroxyl groups in one molecule may be, for example, at least one selected from the group consisting of resorcin, catechol, bisphenol A, bisphenol F, and substituted or unsubstituted biphenol.

[0043] The resin composition may contain one type of phenolic resin among the above. The resin composition may contain multiple types of phenolic resin among the above. The resin composition may contain one type of curing agent among the above. The resin composition may contain multiple types of curing agents among the above.

[0044] The ratio of the active group (phenolic OH group) in the curing agent that reacts with the epoxy group in the epoxy resin may be preferably 0.5 to 1.5 equivalents, more preferably 0.9 to 1.4 equivalents, and even more preferably 1.0 to 1.2 equivalents relative to 1 equivalent of the epoxy group in the epoxy resin. When the ratio of the active group in the curing agent is less than 0.5 equivalents, the amount of OH per unit weight of the cured epoxy resin decreases, and the curing speed of the resin composition (epoxy resin) decreases. When the ratio of the active group in the curing agent is less than 0.5 equivalents, the glass transition temperature of the obtained cured product decreases, or sufficient elastic modulus of the cured product cannot be obtained. On the other hand, when the ratio of the active group in the curing agent exceeds 1.5 equivalents, the mechanical strength of the molded product formed from the compound powder after curing tends to decrease. However, even when the ratio of the active group in the curing agent is outside the above range, the effect of the present invention can be obtained.

[0045] The resin composition may contain a curing catalyst. By using the curing catalyst, the mechanical strength of the molded body can be increased. As the curing catalyst, for example, tetrabutylphosphonium tetraphenylborate, which is a tetra-substituted phosphonium tetra-substituted borate, can be mentioned.

[0046] The curing accelerator is not limited as long as it is a composition that reacts with an epoxy resin to promote curing of the epoxy resin. The curing accelerator may be, for example, an imidazole such as an alkyl group-substituted imidazole or benzimidazole. The resin composition may contain one type of curing accelerator. The resin composition may contain multiple types of curing accelerators. By containing a curing accelerator as a component of the resin composition, the moldability and releasability of the compound are easily improved. In addition, by containing a curing accelerator as a component of the resin composition, the mechanical strength of a molded body (e.g., electronic parts) manufactured using the compound is improved, and the storage stability of the compound under high temperature and high humidity environments is improved.

[0047] The amount of the curing accelerator is not particularly limited as long as it is an amount that can obtain a curing acceleration effect. However, from the viewpoint of improving the curability and fluidity of the resin composition when absorbing moisture, the amount of the curing accelerator may be preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 1 part by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the epoxy resin. The content of the curing accelerator is preferably 0.001 parts by mass or more and 5 parts by mass or less, relative to the total mass of the epoxy resin and the curing agent (e.g., phenolic resin). When the amount of the curing accelerator is 0.1 parts by mass or more, a sufficient curing acceleration effect is easily obtained. When the amount of the curing accelerator is 30 parts by mass or less, the storage stability of the compound powder is not likely to decrease. However, even if the amount and content of the curing accelerator are outside the above range, the effect of the present invention can be obtained.

[0048] From the viewpoint of environmental safety, recyclability, moldability, and low cost of the compound powder, the resin composition may contain a flame retardant. The flame retardant may be, for example, at least one selected from the group consisting of bromine-based flame retardants, phosphorus-based flame retardants, hydrated metal compound-based flame retardants, silicone-based flame retardants, nitrogen-containing compounds, hindered amine compounds, organometallic compounds, and aromatic engineering plastics. The compound powder may contain one of the above flame retardants, or may contain multiple of the above flame retardants.

[0049] Examples of rare earth magnetic powder include samarium-cobalt magnetic powder (SmCo), neodymium-iron-boron magnetic powder (NdFeB), and samarium-iron-nitride magnetic powder (SmFeN). The rare earth magnetic powder is produced, for example, by a rapid solidification method. In the rapid solidification method, a molten magnet alloy is discharged onto the surface of a rotating water-cooled roll to rapidly cool and solidify the molten magnet alloy to produce a quenched alloy. The quenched alloy is then pulverized to produce a rare earth magnetic powder. Rare earth magnetic powder produced by a hydrogenation disproportionation desorption recombination (HDDR) method may also be used.

[0050] The shape of each particle of the rare earth magnetic powder may be spherical. The shape of each particle of the rare earth magnetic powder may be flat (for example, the aspect ratio of the shape of the powder particle = minor axis / major axis is 0.3 or less). Examples of such powders include the powder for Ti-containing nanocomposite magnets described in WO 2006 / 064794 and WO 2006 / 101117 and the powder described in U.S. Pat. No. 4,802,931. When a rare earth magnetic powder having a flat shape is used in a compound for rare earth bonded magnets, the rare earth magnetic powder is laminated relatively orderly during compression molding. This makes it difficult for gaps and resin pools to form between the rare earth magnetic powders, making it easier to pack the rare earth magnetic powders at a high density. Therefore, it is preferable that the rare earth magnetic powder has a flat shape. Non-pulverized powder (spherical powder) obtained by the build-up method of Nichia Corporation can also be used.

[0051] The average particle size of the rare earth magnetic powder is preferably 1 to 200 μm, and more preferably 2 to 100 μm. The average particle size of the rare earth magnetic powder can be measured by a laser diffraction particle size distribution measuring device.

[0052] <Compound powder manufacturing method> The method for producing the compound powder is not particularly limited, but may be, for example, as follows. First, a resin solution is prepared by uniformly stirring and mixing a resin, a rare earth magnetic powder, and an organic solvent. In other words, a resin solution is prepared by mixing the above-mentioned resin composition, a rare earth magnetic powder, and an organic solvent. The resin solution may contain a curing agent. The resin solution may contain a curing accelerator or a curing catalyst. The resin solution may contain additives such as a reactive diluent, a coupling agent, a flow aid, a flame retardant, and a lubricant. The organic solvent is not particularly limited as long as it is a liquid that dissolves the resin composition. The organic solvent may be, for example, at least one selected from the group consisting of acetone, N-methylpyrrolidinone (N-methyl-2-pyrrolidone), γ-butyrolactone, dimethylformamide, dimethylsulfoxide, methyl ethyl ketone, methyl isobutyl ketone, toluene, and xylene.

[0053] Subsequently, the organic solvent is sufficiently removed from the resin solution to obtain a compound powder. With the removal of the organic solvent, the resin composition adheres to the surface of each particle constituting the rare earth magnetic powder. The resin composition may adhere to the entire surface of each particle constituting the rare earth magnetic powder, or may adhere to only a part of the surface of the particle. The method of removing the organic solvent from the resin solution is not particularly limited. For example, the organic solvent can be removed from the resin solution by drying the resin solution. The method of drying the resin solution may be, for example, vacuum drying. When producing a molded body, a lubricant may be added to the compound powder obtained above in order to reduce damage to the mold. The lubricant is not particularly limited. The lubricant may be, for example, at least one selected from the group consisting of metal soap and wax-based lubricants. The compound powder is obtained by the above method. It is not necessary to add the lubricant to the compound powder. That is, in order to reduce damage to the die, a dispersion liquid may be prepared by dispersing the lubricant in a suitable dispersion medium, and this dispersion liquid may be applied to the wall surface inside the die (the wall surface that comes into contact with the punch), and the applied dispersion liquid may be dried.

[0054] <Manufacturing method of rare earth bonded magnets> The compound powder is filled into a metal mold, a molded body is formed using the metal mold, a magnetic field is applied to orient the magnet powder, and the molded body is then removed from the metal mold to obtain a molded body. The obtained molded body is then hardened via a heating process to obtain a rare earth bonded magnet. In the process of forming the molded body, it is more preferable to mold the compound powder while heating it.

[0055] Specifically, the manufacturing method for rare earth bonded magnets includes the steps of mixing rare earth magnetic powder with the above-mentioned resin composition to prepare a compound powder, filling the compound powder into a mold and heating it at 80 to 120°C while applying a magnetic field to the compound powder to obtain a molded body, cooling the molded body after releasing the magnetic field, and removing the molded body, which has been cooled to 40 to 60°C, from the mold.

[0056] The compound powder may be molded by either dry molding or wet molding. For example, in the case of dry molding using a hydraulic press, the compound powder may be compression molded while being held at a molding pressure of 10 to 500 MPa for 1 to 60 minutes to produce a compression molded body. The obtained molded body may be further subjected to cold isotropic pressing.

[0057] The application of a magnetic field to the compound powder can be carried out by using a non-magnetic mold that allows a magnetic field to pass through, and an orientation device that can generate a magnetic field according to the direction and magnitude of an applied current.

[0058] The heating means for the compound powder can be selected according to the type of mold, and examples thereof include electric, infrared, and high-frequency methods. The heating temperature can be appropriately selected according to the resin composition, and may be 80 to 120°C, 90 to 110°C, or 100°C. By heating the compound powder at an appropriate temperature, it is possible to generate an appropriate fluidity in the resin composition. As a result, in the process of forming a molded body from the compound powder, the rare earth magnetic particles are easily moved in the resin composition, and the rare earth magnetic particles are easily densely packed (through the resin composition). The holding time at the maximum heating temperature can be appropriately selected according to the resin composition, and may be 20 minutes or more, 30 minutes or more, 50 minutes or more, or 60 minutes or more. The upper limit of the holding time is not particularly limited, but it can be 80 minutes from the viewpoint of obtaining a high-density molded body by further performing cold isotropic pressing on the molded body obtained by compression molding.

[0059] The method of cooling the compound powder is not particularly limited, and includes natural cooling, water cooling, and the like. The temperature at which the molded body is removed from the mold can be appropriately selected according to the resin composition, and may be 40 to 60°C, 45 to 55°C, or 50°C. A molded body at this temperature can have a little more flexibility than one cooled to room temperature. This allows the molded body to be removed from the mold while suppressing damage to the molded body. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.

[0061] (Details of various ingredients) YX-4000H (Mitsubishi Chemical Corporation): Epoxy resin, epoxy equivalent 192 NC-3000L (manufactured by Nippon Kayaku Co., Ltd.): epoxy resin, epoxy equivalent 272 NC-3000H (manufactured by Nippon Kayaku Co., Ltd.): Epoxy resin, epoxy equivalent 290 NC-7300L (manufactured by Nippon Kayaku Co., Ltd.): epoxy resin, epoxy equivalent 210 jER-YL-6121 (Mitsubishi Chemical Corporation): Epoxy resin, epoxy equivalent 175 Epiclon HP-7200L (DIC Corporation): Epoxy resin, epoxy equivalent 247 Epiclon HP-4770 (DIC Corporation): Epoxy resin, epoxy equivalent 205 HP860 (DIC Corporation): Liquid epoxy resin, epoxy equivalent 245 HP-850N (Hitachi Chemical Co., Ltd.): Phenol resin, hydroxyl equivalent 108 KBM-573 (Shin-Etsu Chemical Co., Ltd.): N-phenyl-3-aminopropyltrimethoxysilane PX4PB (manufactured by Hokko Chemical Co., Ltd.): Tetra-substituted phosphonium and tetra-substituted borate, tetrabutylphosphonium tetraphenylborate SmFeN powder (manufactured by Nichia Corporation): average particle size 3.0 μm, spherical

[0062] Example 1 (Preparation of compound powder) In a 300 ml eggplant-shaped flask, 5.12 g of YX-4000H as an epoxy resin, 2.88 g of HP-850N as a phenolic resin, 0.6 g of KBM-573 as an epoxy group reactive compound, and 0.248 g of PX-4PB as a curing catalyst were weighed and dissolved in 50 ml of acetone. After the materials were completely dissolved, 192 g of SmFeN powder was added and stirred for 10 minutes, and then the acetone was distilled off at 25 ° C. with an evaporator. When almost no liquid was visible, the lumps were broken up, and then the pressure was reduced again with an evaporator for 30 minutes. The contents were spread on a tray, placed in a vacuum dryer, and vacuum-dried at room temperature for one day. The dried material (lumps) was placed in a plastic bag and crushed with a hammer to make a compound powder.

[0063] (Preparation of resin composition for melt viscosity measurement) In a 300 ml eggplant-shaped flask, 5.12 g of YX-4000H as an epoxy resin, 2.88 g of HP-850N as a phenolic resin, 0.6 g of KBM-573 as an epoxy group reactive compound, and 0.248 g of PX-4PB as a curing catalyst were weighed and dissolved in 50 ml of acetone. After the materials were completely dissolved, the acetone was distilled off at 25°C using an evaporator. When almost no liquid was visible, the flask was placed in a vacuum dryer, and vacuum-dried at room temperature for one day to obtain a resin composition for melt viscosity measurement.

[0064] (Examples 2 to 11, Comparative Examples 1 to 2) The amounts of each raw material added were blended according to Tables 1 and 2 (units of each raw material: g), and compound powders and resin compositions for melt viscosity measurement were obtained in the same manner as in Example 1. All resin compositions were solid at 25°C. In the table, in the column "KBM-573 amount," "binder resin basis" refers to the amount per 100 parts by mass of the epoxy resin and phenolic resin combined, and "epoxy resin basis" refers to the amount per 100 parts by mass of the epoxy resin.

[0065] (Melt Viscosity Measurement) The melt viscosity was measured using a rheometer MCR301 manufactured by Anton Paar. The resin composition for melt viscosity measurement obtained in each example was heated from 30°C to 100°C at a heating rate of 10°C / min, held at 100°C for 30 minutes, and then cooled to 50°C at 10°C / min. The melt viscosity at 50°C during heating before heating ("initial viscosity of resin" in the table), the minimum melt viscosity when held at 100°C ("minimum melt viscosity" in the table), and the melt viscosity at 50°C during cooling ("viscosity after heat treatment" in the table) were measured values. FIG. 1 is a diagram showing the melt viscosity measurement results of Example 1.

[0066] (Preparation of molded specimens for crushing strength measurement) The compound powder obtained in each example was compression molded using a hydraulic press at a mold temperature of 100°C and a molding pressure of 100MPa for 30 minutes. The mold temperature was then cooled to 50°C, and the molded body was removed from the mold. In this way, a compression molded body having a cubic shape of 7mm x 7mm x 7mm was produced. The molded body obtained from the compound powder of the comparative example could not be removed from the mold due to insufficient strength.

[0067] (Measurement of crushing strength) The crushing strength was measured using a universal compression tester (AG-10TBR, manufactured by Shimadzu Corporation). The compression molded bodies obtained above were used as test pieces, and a compressive pressure was applied to each test piece from the height direction in a 25°C environment. The crushing strength (MPa) was calculated from the maximum value of the compressive pressure when the test piece was destroyed by the compressive pressure.

[0068] [Table 1]

[0069] [Table 2]

Claims

1. A process for preparing a compound powder by mixing a rare earth magnetic powder and a resin composition; a step of filling the compound powder into a mold and applying a magnetic field to the compound powder while heating the compound powder at 80 to 120° C. to obtain a molded body; cooling the molded body after the magnetic field is released; removing the molded body cooled to 40 to 60°C from the mold; Equipped with The resin composition has a melt viscosity at 100°C of 1 Pa·s or more and 50 Pa·s or less, a melt viscosity at 50°C after heating at 100°C for 30 minutes that is higher than the melt viscosity at 50°C before heating, and is a solid at 25°C. A manufacturing method for rare earth bonded magnets.

2. The manufacturing method described in claim 1, wherein the resin composition comprises an epoxy resin, a phenolic resin, and a compound having an epoxy group reactive group.

3. The method according to claim 2 , wherein the epoxy-reactive group is an amino group.

4. The method according to claim 2 or 3, wherein the content of the compound having an epoxy group-reactive group is 1 to 20 parts by mass per 100 parts by mass of the epoxy resin and the phenol resin in total.

5. The method according to any one of claims 2 to 4, wherein the content of the compound having an epoxy group-reactive group is 1 to 30 parts by mass per 100 parts by mass of the epoxy resin.

6. A manufacturing method described in any one of claims 1 to 5, wherein the mass ratio of the rare earth magnetic powder and the resin composition in the compound powder (rare earth magnetic powder / resin composition) is 94 / 6 to 99 / 1.

Citation Information

Patent Citations

  • Insulation layer formation treatment liquid of magnetic powder for dust core and its insulation layer formation method, dust core using it, and electric device using dust core

    JP1998154613A

  • Composition for resin-bonded magnet and resin-bonded magnet manufactured by using the same

    JP2003142307A

  • Magnetic anisotropic bonded magnet and its manufacturing method

    JP2003272943A

  • Filled epoxy resin composition and its manufacturing method

    JP2006156964A

  • Spherical magnet compound and rare-earth-ferrous bond magnet

    JP2014107429A