Conductive composition for molded film, molded film and method for producing same, molded body and method for producing same

A conductive composition for molded films with specific resin and solvent properties addresses conductivity loss on uneven surfaces by enhancing adhesion and flexibility, ensuring stable conductive circuits on curved surfaces.

JP7567285B2Active Publication Date: 2024-10-16TOYO INK MFG CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020142037
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-25
Publication Date
2024-10-16
Estimated Expiration
2040-08-25

AI Technical Summary

Technical Problem

Existing methods for forming conductive circuits on uneven or curved surfaces face issues with conductivity loss due to tensile force and high-temperature stress, leading to breakage of the conductive layer.

Method used

A conductive composition for molded films containing specific resins, conductive fine particles, and solvents with defined boiling points and structural properties is used to form a conductive layer that suppresses conductivity loss, featuring a resin with a cyclic structure and ester bond, and solvents with aromatic and alicyclic structures to enhance adhesion and flexibility.

Benefits of technology

The solution results in a molded film with excellent conductivity that maintains integrity on uneven or curved surfaces, even under high-temperature stress, enabling the production of conductive circuits with reduced defects and improved adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567285000005
    Figure 0007567285000005
  • Figure 0007567285000006
    Figure 0007567285000006
  • Figure 0007567285000007
    Figure 0007567285000007
Patent Text Reader

Abstract

To provide a conductive composition for a molded film that can produce the molded film that is less prone to degradation in conductivity due to tensile force.SOLUTION: A conductive composition for a molded film contains a resin (A), conductive fine particles (B), and a solvent (C). The solvent (C) includes a solvent (C1) satisfying the following conditions (1) and (2) and a solvent (C2) satisfying the following conditions (1) and (3). Condition (1): the boiling point is 180°C or higher and 270°C or lower. Condition (2): it has an aromatic structure in the molecular structure. Condition (3): it has an alicyclic structure and an ester bond in the molecular structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive composition for a molded film, a molded film and a method for producing the same, a molded article and a method for producing the same. [Background technology]

[0002] Patent Document 1 discloses a specific conductive circuit integrated molded product having a resin molded body, a base film embedded flush with one surface of the resin molded body, and a conductive circuit disposed between the resin molded body and the base film. Patent Document 1 describes a method for manufacturing the conductive circuit integrated molded product, in which a base film on which a specific conductive circuit is formed is placed on the cavity surface of an injection molding die, and then molten resin is injected to injection mold a resin molded body. In Patent Document 1, the conductive circuit is formed by etching a specific transparent thin metal film.

[0003] A printing method using conductive ink has been considered as a method for forming a conductive circuit to replace the etching method. The method of printing conductive ink does not require any complicated steps compared to the etching method, and can easily form a conductive circuit, improving productivity and reducing costs. For example, Patent Document 2 discloses a specific conductive ink containing specific conductive fine particles and a specific epoxy resin as a low-temperature processing type conductive ink capable of forming a high-definition conductive pattern by screen printing. It is said that the screen printing makes it possible to form a thick conductive pattern, and thus realizes low resistance of the conductive pattern.

[0004] Furthermore, Patent Document 3 discloses a method for manufacturing a decorative sheet capable of expressing a three-dimensional effect, in which a laminate having a printed layer printed in a pattern on a transparent resin layer and a laminate sheet having a decorative layer on a base film are thermocompression-bonded to each other, thereby giving the decorative layer an uneven shape that follows the pattern of the printed layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-11691 A [Patent Document 2] JP 2011-252140 A [Patent Document 3] JP 2007-296848 A Summary of the Invention [Problem to be solved by the invention]

[0006] According to the method of Patent Document 1, a conductor can be easily provided on the surface of a molded body. On the other hand, there is an increasing demand for forming a conductive circuit on the surface of a substrate having various shapes, such as a substrate having an uneven surface or a curved surface. When a conductive circuit is formed by laminating a film having a conductive layer on the surface of such a substrate, the film needs to be deformed to match the surface shape of the substrate. When the film is deformed, a large tensile force may be generated partially in the conductive layer. The tensile force causes breakage of the conductive layer, and a decrease in conductivity becomes a problem. Furthermore, when forming a conductive circuit on a substrate having such an uneven surface or a curved surface, it is necessary to integrate the film and the substrate after or at the same time as deforming the film having the conductive layer, and in this integration process, stress is applied to the conductive circuit due to friction with the plastic substrate at high temperature. The stress at high temperature also causes breakage of the conductive layer, and a decrease in conductivity becomes a problem.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a conductive composition for a molded film capable of producing a molded film in which the decrease in conductivity due to tensile force and high-temperature stress is suppressed, a molded film in which the decrease in conductivity due to tensile force and high-temperature stress is suppressed, and a molded body with excellent conductivity and a method for producing the same. [Means for solving the problem]

[0008] The conductive composition for molded films according to the present embodiment is A conductive composition for producing a molded film for forming a conductive layer on a substrate surface having an uneven surface or a three-dimensional curved surface, comprising: Contains a resin (A), conductive fine particles (B), and a solvent (C), The solvent (C) includes a solvent (C1) which satisfies the following conditions (1) and (2), and a solvent (C2) which satisfies the following conditions (1) and (3). Condition (1) The boiling point is 180°C or higher and 270°C or lower. Condition (2) The molecular structure has an aromatic structure Condition (3) The molecular structure has an alicyclic structure and an ester bond.

[0009] In one embodiment of the conductive composition for molded films, the resin (A) has one or more glass transition points in the range of 0°C or higher and lower than 130°C, and does not have any glass transition point lower than 0°C.

[0010] In one embodiment of the conductive composition for molded films of this embodiment, the conductive fine particles (B) include one or more types of conductive fine particles selected from silver powder, copper powder, silver-coated powder, copper alloy powder, conductive oxide powder, and carbon fine particles.

[0011] In one embodiment of the conductive composition for a molded film of the present invention, the resin (A) has a cyclic structure in the main chain.

[0012] In one embodiment of the conductive composition for a molded film of the present invention, the resin (A) has an aromatic ring structure and an ester bond in the main chain.

[0013] In one embodiment of the conductive composition for a molded film of this embodiment, the total content of the solvent (C1) and the solvent (C2) is 40 parts by mass or more in 100 parts by mass of the solvent (C).

[0014] The molded film according to the present embodiment is a molded film having a conductive layer on a base film, The conductive layer is a cured product of the conductive composition for molded films of the present embodiment.

[0015] One embodiment of the molded film of the present invention is a molded film having a decorative layer and a conductive layer on a base film, The conductive layer is a cured product of the conductive composition for molded films of the present embodiment.

[0016] In one embodiment of the formed film of this embodiment, the base film is a film selected from polycarbonate, polymethyl methacrylate, polypropylene, and polyethylene terephthalate, or a laminate film thereof.

[0017] The molded article according to the present embodiment is a molded article in which a conductive layer is laminated on a substrate, The conductive layer is a cured product of the conductive composition for molded films of the present embodiment.

[0018] The first method for producing a molded body according to the present embodiment includes the steps of: printing the conductive composition for a molded film according to the present embodiment on a base film and drying the composition to produce a molded film; placing the formed film on a substrate; and b) integrating the molded film and the substrate by an overlay molding process.

[0019] The second method for producing a molded body according to the present embodiment includes the steps of: printing the conductive composition for a molded film according to the present embodiment on a base film and drying the composition to produce a molded film; forming the formed film into a predetermined shape; placing the formed film in an injection mold; and forming a substrate by injection molding and integrating the formed film with the substrate.

[0020] A third method for producing a molded body according to the present embodiment includes the steps of: printing the conductive composition for a molded film according to the present embodiment on a base film and drying the composition to produce a molded film; placing the formed film in an injection mold; The method includes a step of molding a substrate by injection molding and transferring the conductive layer in the molded film to the substrate side. Effect of the Invention

[0021] According to the present invention, it is possible to provide a conductive composition for a molded film capable of producing a molded film in which the decrease in conductivity due to tensile force and high-temperature stress is suppressed, a molded film in which the decrease in conductivity due to tensile force and high-temperature stress is suppressed, and a molded body with excellent conductivity and a method for producing the same. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a molded film according to the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the molded film of the present embodiment. [Diagram 3] FIG. 2 is a schematic process diagram showing an example of a first manufacturing method of a molded body. [Figure 4] FIG. 4 is a schematic process diagram showing another example of the second manufacturing method of a molded body. [Diagram 5] 5A to 5C are schematic process diagrams showing another example of the third manufacturing method of a molded body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The conductive composition for a molded film, the molded film, the molded article, and the method for producing the same according to the present embodiment will be described in detail below. In the present embodiment, the term "cured product" refers not only to products that have been cured by chemical reaction, but also to products that have been cured without chemical reaction, such as products that have been hardened by evaporation of a solvent.

[0024] [Conductive composition for molded films] Contains a resin (A), conductive fine particles (B), and a solvent (C), The solvent (C) includes a solvent (C1) which satisfies the following conditions (1) and (2), and a solvent (C2) which satisfies the following conditions (1) and (3). Condition (1) The boiling point is 180°C or higher and 270°C or lower. Condition (2) The molecular structure has an aromatic structure Requirement (3) The molecular structure has an alicyclic structure and an ester bond.

[0025] The present inventors have studied a screen-printable conductive composition in order to produce a molded film that is applicable to an uneven substrate surface and has process suitability for the integration process with a plastic substrate. In order to apply the composition to the production of a molded film, various adjustments were made to the resin structure, the conductive fine particles, and the solvent. As a result, the frequency of cracks occurring when the obtained molded film is tensile-deformed at a high temperature at which it can be molded varies depending on the type of solvent contained in the conductive composition, particularly the use of a mixed solvent consisting of a plurality of solvents each selected from two specific groups, and further, the frequency of occurrence of printing defects such as chipping and smearing when printed at high speed and the magnitude of change in resistance value during tensile deformation at the high temperature, especially when the degree of deformation is large, vary depending on the glass transition point and main chain structure of the resin combined with the mixed solvent. Based on these findings, the present inventors conducted a study and found that when a conductive composition that does not contain either one or both of a high-boiling point solvent having an aromatic structure and a high-boiling point solvent having both an alicyclic structure and an ester bond is printed and dried on a resin film, significant deterioration in the conductivity of the conductive layer pattern and cracking of the conductive layer occur when the molded film is deformed by pulling at a high temperature corresponding to its softening point, and further, when the printing speed is increased when printing the conductive composition, the frequency of occurrence of printing defects such as chipping and scratching increases significantly. The same was true when a conductive layer was provided on a decorative layer.

[0026] Even if the molded film has a conductive layer that cracks or a large change in resistance value occurs when deformed by pulling at such high temperatures, there is no problem when it is used alone as a flat film circuit board or when it is used in a bent state on a two-dimensional curved surface. However, when it is used as a molded film that is integrated with the shape of a non-flat substrate surface, such as an uneven shape or a three-dimensional curved shape, the molded film will be deformed. Therefore, it is predicted that the conductive layer cannot follow the deformation of the resin film and peels off or breaks from the base film, resulting in a decrease in the conductivity of the conductive layer. In addition, the uneven surface and three-dimensional curved surface in the present invention refer not only to a surface having a gently curved cross section, but also to a three-dimensional surface having an acute angle or a rectangular shape in general. In other words, it refers to a three-dimensional shape that cannot be established only by deforming a plane without expanding or contracting, such as a hemispherical, conical, cylindrical, or rectangular prism. In addition, when a certain three-dimensional shape has elements of both the above-mentioned plane or two-dimensional curved surface and a three-dimensional curved surface in a continuous three-dimensional surface, for example, a three-dimensional shape in which one or more partial hemispherical shapes are combined with a plane shape, it is a three-dimensional shape that cannot be established by deforming a plane as a whole without expanding or contracting, and is also considered to be a three-dimensional curved surface. In other words, the uneven surface and three-dimensional curved surface in the present invention cannot be realized by bending a flexible substrate or the like, and are shapes that can be realized, for example, by forming a moldable film by three-dimensional molding under heating.

[0027] Based on these findings, the inventors conducted extensive research and discovered that when a mixed solvent containing both a high-boiling point solvent having an aromatic structure and a high-boiling point solvent having both an alicyclic structure and an ester bond is contained, the change in resistance value that occurs when a molded film is pulled with a particularly large degree of deformation is small, and that when the conductive composition is printed at an increased printing speed and printing is performed in a state of increased productivity, the occurrence of printing defects such as chipping and scratching is highly suppressed, leading to the completion of the present invention. That is, the conductive composition for molded films of the present invention uses a resin, conductive fine particles, and a mixed solvent containing both a high-boiling point solvent having an aromatic structure and a high-boiling point solvent having both an alicyclic structure and an ester bond, and can easily produce a molded film having a thick conductive layer with excellent conductivity by screen printing or the like. In addition, a molded film produced using the conductive composition for molded films is prevented from decreasing in conductivity even when used on a non-flat substrate surface. Furthermore, by using the molded film, a molded product can be obtained in which a conductive circuit is formed on any surface, such as an uneven surface or a curved surface, on a substrate made of a three-dimensional plastic having practical strength.

[0028] The conductive composition for molded films of the present embodiment contains at least a resin (A), conductive fine particles (B), and a solvent (C), and may further contain other components as necessary. Each component of such a conductive composition for molded films will be described below.

[0029] <Resin (A)> The conductive composition of the present embodiment contains a binder resin (A) to provide film-forming properties and adhesion to the base film or decorative layer. In addition, in the present embodiment, the resin (A) can provide flexibility to the conductive layer. Therefore, the resin (A) can be contained to suppress breakage of the conductive layer due to stretching.

[0030] The resin (A) can be appropriately selected from resins used in conductive compositions. Examples of the resin (A) include acrylic resins, vinyl ether resins, polyether resins, polyester resins, polyurethane resins, epoxy resins, phenoxy resins, polycarbonate resins, polyvinyl chloride resins, polyolefin resins, styrene block copolymer resins, polyamide resins, and polyimide resins. These may be used alone or in combination of two or more.

[0031] The main chain structure of the resin (A) preferably contains a cyclic structure, and it is particularly preferable that the main chain structure has both an aromatic ring structure and an ester bond, because the high affinity with the solvent (C), described below, particularly (C1) and solvent (C2), leads to the spreading and entanglement of larger molecular chains of the resin (A) in the conductive composition, thereby improving the maintenance of conductivity during molding and tension and the ability to suppress defects during printing. In the present invention, the cyclic structure refers to an alicyclic structure, an aromatic ring structure, or a heterocyclic structure in which one ring is a 4- to 14-membered ring. Examples of the alicyclic structure include monocyclic structures such as a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cyclohexene ring, a cycloheptane ring, a cyclooctane ring, a cyclodecane ring, and a cyclotetradecane ring, and condensed ring structures such as a bornane ring, an isobornane ring, an adamantane ring, a decalin ring, and a steroid skeleton. Examples of the aromatic ring structure include monocyclic structures such as a benzene ring, a furan ring, a 1,4-dioxine ring, a pyrrole ring, a pyridine ring, a pyrazine ring, a triazine ring, an imidazole ring, a pyrazole ring, an oxazole ring, a thiazole ring, a thiophene ring, a triazole ring, and a tetrazole ring, and condensed ring structures such as a naphthalene ring, a tetralin ring, an azulene ring, an anthracene ring, a perylene ring, an indane ring, an indole ring, a benzofuran ring, a benzimidazole ring, and a benzoxazole ring. As in the above examples, in the present invention, a structure in which an aromatic ring structure is condensed or directly bonded to an alicyclic structure, and a heterocyclic structure exhibiting aromaticity are all considered to be aromatic ring structures. In the present invention, the heterocyclic structure refers to a heteroatom-containing (non-carbon atom) ring structure other than the above-mentioned aromatic ring structures, and examples thereof include a tetrahydrofuran ring, a pyran ring, a tetrahydropyran ring, a pyrrolidine ring, a piperidine ring, a piperazine ring, and an isocyanurate ring. The linking site of the cyclic structure in the main chain structure of the resin (A) is not particularly limited, and it is sufficient that the cyclic structure is linked to the main chain via a total of two or more covalent bonds from any one or two atoms constituting the cyclic structure.

[0032] In this embodiment, it is also preferable that the resin (A) has two or more substituents selected from a hydroxyl group, an amino group, a carboxyl group, and an acid anhydride group in one molecule. In this case, the resin (A) can be three-dimensionally crosslinked by combining with a crosslinking agent (D) described later, and can be suitably used in applications where hardness is required for the conductive layer.

[0033] When the resin (A) has a functional group selected from a hydroxyl group, an amino group, a carboxyl group, and an acid anhydride group, the functional group value is preferably 1 mgKOH / g or more and 400 mgKOH / g or less, and more preferably 2 mgKOH / g or more and 350 mgKOH / g or less. The details of the calculation method of the functional group value will be described in the examples below. When the resin (A) has multiple types of functional groups, the functional value is the sum of the functional groups. For example, when the resin (A) has a hydroxyl group and a carboxyl group, the functional value is the sum of the hydroxyl value and the acid value of the resin (A).

[0034] From the viewpoint of both maintaining electrical conductivity during stretching in molding and resistance to frictional stress with the base plastic at high temperatures in the integration step with the plastic base material, the glass transition temperature (Tg) of the resin (A) is preferably 0° C. or higher and 130° C. or lower, and more preferably 5° C. or higher and 120° C. or lower. From the same viewpoint, when the resin (A) has multiple glass transition points, it is preferable that none of the glass transition points is below 0° C.

[0035] In this embodiment, the resin (A) may be synthesized by the methods described in the Examples below or other known methods, or a commercially available product having the desired physical properties may be used. In this embodiment, the resin (A) may be used alone or in combination of two or more kinds.

[0036] The content of the resin (A) in the conductive composition of this embodiment is not particularly limited and may be appropriately adjusted according to the application, etc., but is preferably 5% by mass or more and 50% by mass or less, and more preferably 8% by mass or more and 40% by mass or less, based on the total solid content contained in the conductive composition. If the content of the resin (A) is equal to or more than the above lower limit, the film-forming property and the adhesion to the base film, etc. are improved, and flexibility can be imparted to the conductive layer. If the content of the resin (A) is equal to or less than the above upper limit, the content of the conductive fine particles (B) can be relatively increased, and a conductive layer with excellent conductivity can be formed.

[0037] <Conductive fine particles (B)> The conductive fine particles (B) exhibit conductivity when multiple conductive fine particles come into contact with each other within the conductive layer, and in this embodiment, an appropriate selection is made from those that can obtain conductivity without being heated at high temperatures. The conductive fine particles used in this embodiment include metal fine particles, carbon fine particles, conductive oxide fine particles, and the like. Examples of metal fine particles include powders of metal elements such as gold, silver, copper, nickel, chromium, palladium, rhodium, ruthenium, indium, aluminum, tungsten, malbutene, and platinum, as well as alloy powders such as copper-nickel alloys, silver-palladium alloys, copper-tin alloys, silver-copper alloys, and copper-manganese alloys, and metal-coated powders in which the surfaces of the above-mentioned metal element powders or alloy powders are coated with silver or the like. Examples of carbon fine particles include carbon black, graphite, and carbon nanotubes. Examples of conductive oxide fine particles include silver oxide, indium oxide, tin oxide, zinc oxide, and ruthenium oxide.

[0038] In this embodiment, it is preferable to contain one or more conductive fine particles selected from silver powder, copper powder, silver-coated powder, copper alloy powder, conductive oxide powder, and carbon fine particles. By using these conductive fine particles (B), a conductive layer with excellent conductivity can be formed without sintering, and a conductive layer with excellent extensibility and conductivity retention performance when molded into a three-dimensional shape as a molded film described later can be formed.

[0039] The shape of the conductive fine particles (B) is not particularly limited, and spherical, flake-like, chain-aggregated, and other shapes can be used as appropriate. From the viewpoints of maintaining printability and maintaining conductivity during molding and stretching, flake-like or chain-aggregated shapes are particularly preferred. In the present invention, "spherical" refers to particles in general that are spherical, oval, crushed spherical, pebble-like, or polyhedral and have a low aspect ratio, specifically, particles with an aspect ratio of about 1 or more and 2 or less. In addition, in the present invention, "flake-like" refers to two-dimensional flat shapes generally called scale-like, plate-like, flat, sheet-like, etc., and among these, those with an aspect ratio of 3 or more and 500 or less are particularly preferred. In addition, in the present invention, "chain-aggregated" refers to amorphous shapes generally in which a plurality of the above-mentioned spherical conductive fine particles are directly fused or bonded together.

[0040] The D50 particle size of the conductive fine particles (B) is not particularly limited, but from the viewpoint of maintaining dispersibility and printability in the conductive composition, maintaining conductivity during molding, and resistance to injection molding process with molten resin or high temperature friction resistance of molded resin, it is preferably 0.2 μm or more and less than 30 μm, and particularly preferably 0.7 μm or more and less than 15 μm. In this embodiment, the average particle size of the conductive fine particles (B) is calculated as follows. In accordance with the laser diffraction and scattering method described in JIS M8511 (2014), a laser diffraction and scattering type particle size distribution measuring device (Microtrack 9220FRA manufactured by Nikkiso Co., Ltd.) is used to add an appropriate amount of conductive fine particles (B) to an aqueous solution containing 0.5 vol% of a commercially available surfactant polyoxyethylene octylphenyl ether (Triton X-100 manufactured by Roche Diagnostics Co., Ltd.) as a dispersant, and then irradiated with 40 W ultrasonic waves for 180 seconds while stirring, and then measurement was performed. The calculated median diameter (D50) value was taken as the average particle size of the conductive fine particles (B).

[0041] In the present embodiment, the conductive fine particles (B) may be used alone or in combination of two or more kinds. The content of the conductive fine particles (B) in the conductive composition of this embodiment is not particularly limited and may be appropriately adjusted according to the application, etc., but is preferably 50% by mass or more and 90% by mass or less, and more preferably 55% by mass or more and 85% by mass or less, based on the total solid content contained in the conductive composition. If the content of the conductive fine particles (B) is equal to or more than the above lower limit, a conductive layer with excellent conductivity can be formed. Also, if the content of the conductive fine particles (B) is equal to or less than the above upper limit, the content of the resin (A) can be increased, improving film-forming properties and adhesion to a base film, etc., and imparting flexibility to the conductive layer.

[0042] <Solvent (C)> In this embodiment, a solvent (C) is contained in order to dissolve the resin (A) and impart fluidity to impart printability, and to adjust the spread and entanglement of molecular chains in the composition of the resin (A). In addition, in this embodiment, the solvent (C) is contained, and the spread of the molecular chains is adjusted, and wettability is imparted to the base film during printing, thereby improving the patterning accuracy during printing.

[0043] The solvent (C) of the present invention includes both a high boiling point solvent (C1) having an aromatic structure and a high boiling point solvent (C2) having both an alicyclic structure and an ester bond. By including both the solvent (C1) and the solvent (C2), not only is the solubility of the resin (A) excellent and the infiltration suppression to the base film excellent, but also the appropriate wettability to the base film during printing is given, thereby improving the patterning accuracy, especially during high-speed printing, and the polymer chain of the resin (A) is widely developed in the solvent (C) and exhibits appropriate fluidity, and the polymer chains are well entangled with each other during the formation of the conductive layer, thereby obtaining the effect of suppressing local stress concentration on a microscale that leads to the disconnection of the connection (conductive path) between conductive particles in the conductive layer.

[0044] The solvent (C1) of the present invention can be used without any particular limitation as long as it has a boiling point of 180° C. or more and 270° C. or less and has an aromatic structure. In addition, even if the solvent (C1) is solid at room temperature alone, it can be used without any problem if it becomes liquid as a mixed solvent with the below-described solvent (C2) or other solvent. Examples of the aromatic ring structure include monocyclic structures such as a benzene ring, a furan ring, a 1,4-dioxine ring, a pyrrole ring, a pyridine ring, a pyrazine ring, a triazine ring, an imidazole ring, a pyrazole ring, an oxazole ring, a thiazole ring, a thiophene ring, a triazole ring, and a tetrazole ring; and condensed ring structures such as a naphthalene ring, a tetralin ring, an azulene ring, an indane ring, an indole ring, and a benzofuran ring. Specific examples of such a solvent (C1) include aromatic hydrocarbons such as planithen (1,2,3,4-tetramethylbenzene) (192°C), durene (1,2,4,5-tetramethylbenzene) (192°C), isodurene (1,2,3,5-tetramethylbenzene) (192°C), and tetralin (1,2,3,4-tetrahydronaphthalene) (209°C), aromatic ketones such as acetophenone (202°C), propiophenone (218°C), and phenylacetone (215°C), methyl benzoate (199°C), Examples of the solvent include aromatic esters such as ethyl benzoate (213°C), propyl benzoate (230°C), ethyl phenylacetate (226°C), and benzyl acetate (212°C), and aromatic alcohols such as benzyl alcohol (205°C), α-methylbenzyl alcohol (204°C), anise alcohol (259°C), 2-phenoxyethanol (247°C), 2-phenoxypropanol (244°C), and 2-(benzyloxy)ethanol (265°C), but are not limited thereto (the boiling points of each solvent are indicated in parentheses). The solvent (C1) can be used alone or in combination of two or more.

[0045] The solvent (C2) of the present invention can be used without any particular limitation as long as it has a boiling point of 180° C. or more and 270° C. or less and simultaneously has an alicyclic structure and an ester bond. In addition, even if the solvent (C2) is solid at room temperature alone, it can be used without any problem if it becomes liquid as a mixed solvent with the solvent (C1) or other solvents described later. Examples of the alicyclic structure include monocyclic structures such as a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cyclohexene ring, a cycloheptane ring, a cyclooctane ring, and a cyclodecane ring, and condensed ring structures such as a bornane ring, an isobornane ring, and a decalin ring. Specific examples of such a solvent (C2) include, but are not limited to, dihydroterpinyl acetate (220°C), terpinyl acetate (220°C), isobornyl acetate (227°C), 1-menthyl acetate (215°C), 1-carbyl acetate (229°C), cyclohexane-1-methyl carboxylate (183°C), etc. (The boiling point of each solvent is shown in parentheses.) Solvent (C2) can be used alone or in combination of two or more kinds. In addition, a solvent that satisfies the conditions of both the solvent (C1) and the solvent (C2) is considered to belong to the solvent (C1).

[0046] The solvent (C) of the present invention may contain a solvent (C3) other than the solvent (C1) and the solvent (C2). The solvent (C3) preferably has a boiling point of 180° C. or more and 270° C. or less, and examples thereof include glycol esters such as 2-ethoxy(2-ethoxy)ethyl acetate and 2-ethoxy(2-ethoxy)butyl acetate, glycol ethers such as 2-ethoxy(2-ethoxy)ethanol, 2-butoxy(2-ethoxy)ethanol, and diethylene glycol diethyl ether, but are not particularly limited thereto.

[0047] The total content of the solvent (C1) and the solvent (C2) in 100 parts by mass of the solvent (C) of the present invention is preferably 40 parts by mass or more and 100 parts by mass or less, from the viewpoint of effectively exhibiting the high-speed printability and the conductive path disconnection suppression property. In addition, the ratio of the solvent (C1) to the solvent (C2) is particularly preferably 15:85 to 85:15 (mass ratio).

[0048] <Optional ingredients> The conductive composition of the present invention may further contain other components as necessary, such as the crosslinking agent (D) described later, dispersants, friction resistance improvers, infrared absorbing agents, ultraviolet absorbing agents, fragrances, antioxidants, organic pigments, inorganic pigments, defoamers, silane coupling agents, plasticizers, flame retardants, moisturizing agents, etc.

[0049] <Crosslinking agent (D)>

[0050] In this embodiment, a crosslinking agent (D) may be additionally used to crosslink the resin (A). The crosslinking agent (D) may be appropriately selected from those having two or more reactive functional groups in one molecule that can form a crosslink with the reactive functional group of the resin (A). Examples of such reactive functional groups include an epoxy group, an isocyanate group, a blocked isocyanate group, an alkyloxyamino group, an aziridinyl group, an oxetanyl group, a carbodiimide group, and a β-hydroxyalkylamide group. The crosslinking agent (D) is preferably used in an amount of 0.05 to 30 parts by mass, and more preferably 0.3 to 25 parts by mass, per 100 parts by mass of the resin (A).

[0051] Furthermore, in this embodiment, it is particularly preferable to combine the resin (A) having two or more first reactive functional groups selected from hydroxyl groups or amino groups in one molecule and the crosslinking agent (D) with a blocked isocyanate. The blocked isocyanate is not particularly limited, and may be an isocyanate compound in which the isocyanate group of a bifunctional isocyanate such as hexamethylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, isophorone diisocyanate, or a bifunctional or higher isocyanate such as an allophanate, biuret, adduct, prepolymer, or isocyanurate is protected (blocked) with ε-caprolactam, MEK oxime, etc. Specific examples include those in which the isocyanate group of the above isocyanate compound is blocked with ε-caprolactam, MEK oxime, cyclohexanone oxime, pyrazole, 3,5-dimethylpyrazole, diisopropylamine, diethyl malonate, ethyl acetoacetate, phenol, etc. By using such a combination, a conductive layer can be obtained which is particularly strong and has excellent adhesion to substrates at high temperatures due to the crosslinking point structure generated by crosslinking, and in which the decrease in conductivity due to tensile force is particularly suppressed.

[0052] <Method of manufacturing conductive composition> The method for producing the conductive composition of this embodiment may be any method for dissolving or dispersing the resin (A), the conductive fine particles (B), the wire-shaped fine particles (C), and other components used as necessary, and the conductive composition can be produced by mixing them by a known mixing means.

[0053] [Formed film] The molded film of this embodiment is a molded film having a conductive layer on a base film, The conductive layer is a cured product of the conductive composition for molded films. According to the molded film of this embodiment, a molded article can be obtained in which a conductive circuit is formed on any substrate surface, such as an uneven surface or a curved surface. According to the molded film of this embodiment, a molded article can be obtained in which a conductive circuit is formed on any substrate surface, such as an uneven surface or a curved surface. The layer structure of the molded film of this embodiment will be described with reference to Figures 1 and 2. Figures 1 and 2 are schematic cross-sectional views showing an example of the molded film of this embodiment. The molded film 10 shown in the example of Fig. 1 has a conductive layer 2 on a base film 1. The conductive layer 2 may be formed on the entire surface of the base film 1, or may be formed in a desired pattern as in the example of Fig. 1. The molded film 10 shown in the example of Fig. 2 has a decorative layer 3 on a base film 1, and a conductive layer 2 on the decorative layer 3. As shown in the example of Fig. 2, the molded film 10 may also have, on the conductive layer 2, an electronic component 4 and a pin 5 for connecting to an output circuit. Although not shown, a resin layer for protecting the conductive layer or the electronic component 4 may be provided on the conductive layer 2 or the electronic component 4, and the resin layer may serve as an adhesive layer or bonding layer for improving adhesion to the substrate described below. In addition, although not shown in the figure, when the molded film 10 of this embodiment has a decorative layer 3, in addition to the example of Figure 2, it may have a layer structure having a decorative layer 3 on one side of the base film 1 and a conductive layer 2 on the other side. The molded film of the present embodiment comprises at least a base film and a conductive layer, and may have other layers as required. Each layer of such a molded film will be described below.

[0054] <Base film> In this embodiment, the base film can be appropriately selected from those having flexibility and extensibility to such an extent that it can follow the shape of the substrate surface under the molding temperature conditions when the substrate is formed, and it is preferable to select the base film according to the use of the molded body and the manufacturing method of the molded body. For example, when the overlay molding method or the film insert method described below is adopted as a method for producing a molded body, the base film remains in the molded body, so the base film can be selected taking into consideration its function as a protective layer for the conductive layer. On the other hand, when an in-mold transfer method, which will be described later, is employed as a method for producing a molded article, it is preferable to select a base film having releasability.

[0055] The base film can be appropriately selected from the above viewpoints, and may be, for example, a film such as polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polystyrene, polyimide, polyamide, polyethersulfone, polyethylene naphthalate, polybutylene terephthalate, polyvinyl chloride, polyethylene, polypropylene, cycloolefin polymer, ABS (acrylonitrile-butadiene-styrene copolymer resin), AES (acrylonitrile-ethylene-styrene copolymer resin), Kaidac (acrylic modified vinyl chloride resin), modified polyphenylene ether, and a polymer alloy consisting of two or more of these resins, or a laminated film thereof. Among them, a film selected from polycarbonate, polymethyl methacrylate, polypropylene, and polyethylene terephthalate, or a laminated film thereof is preferable. As the laminated film, a laminated film of polycarbonate and polymethyl methacrylate is preferable. The method for producing the laminated film of polycarbonate and polymethyl methacrylate is not particularly limited. A polycarbonate film and a polymethyl methacrylate film may be laminated together, or polycarbonate and polymethyl methacrylate may be co-extruded to form a laminated film. It is also preferable that the surface of these base films is subjected to a modification treatment such as a corona treatment.

[0056] In addition, if necessary, an anchor coat layer may be provided on the base film and the conductive composition may be printed on the anchor coat layer for the purpose of improving the printability of the conductive composition. The anchor coat layer is not particularly limited as long as it has good adhesion to the base film and further to the conductive composition and follows the film during molding, and organic fillers such as resin beads and inorganic fillers such as metal oxides may also be added as necessary. The method of providing the anchor coat layer is not particularly limited, and it can be obtained by coating, drying, and curing using a conventionally known coating method. Furthermore, if necessary, in order to prevent the surface of the molded body from being scratched, a hard coat layer may be provided on the base film, and a conductive composition and, if necessary, a decorative layer may be printed on the opposite side. The hard coat layer is not particularly limited as long as it has good adhesion to the base film and surface hardness and follows the film during molding, and organic fillers such as resin beads and inorganic fillers such as metal oxides may also be added as necessary. The method for providing the hard coat layer is not particularly limited, and it can be obtained by applying, drying, and curing using a conventionally known coating method.

[0057] When the molded film of this embodiment has a decorative layer, it is preferable to select a base film having transparency.

[0058] The thickness of the base film is not particularly limited, but can be, for example, from 10 μm to 500 μm, and preferably from 20 μm to 450 μm.

[0059] <Conductive layer> In the molded film of this embodiment, the conductive layer is a cured product of the conductive composition. The conductive layer may be a patterned conductive layer or a solid conductive layer. The method for forming the conductive layer is not particularly limited, but in this embodiment, it is preferable to form it by screen printing, pad printing, stencil printing, screen offset printing, dispenser printing, gravure offset printing, reverse offset printing, or microcontact printing, and it is more preferable to form it by screen printing. In the screen printing method, it is preferable to use a fine mesh screen, particularly a fine mesh screen of about 300 to 650 mesh, in order to meet the demands of high-definition conductive circuit patterns. In this case, the open area of ​​the screen is preferably about 20 to 50%. The screen wire diameter is preferably about 10 to 70 μm. Types of screens include polyester screens, combination screens, metal screens, nylon screens, etc. When printing with a highly viscous paste, a high-tension stainless steel screen can be used. The squeegee for screen printing may be round, rectangular, or square, and an abrasive squeegee may be used to reduce the attack angle (the angle between the plate and the squeegee during printing). Other printing conditions may be appropriately designed from conventionally known conditions.

[0060] The conductive composition is printed by screen printing, and then heated to dry and cause a crosslinking reaction and harden. For sufficient volatilization of the solvent and crosslinking reaction, the heating temperature is preferably 80 to 230° C. and the heating time is preferably 10 to 120 minutes, thereby making it possible to obtain a patterned conductive layer. The pattern of the conductive layer is not particularly limited, and may be, for example, a straight line, a curve, a mesh, a solid pattern or a solid pattern having a partial square, circle, diamond shape, or any combination thereof, or the entire conductive layer may be a solid pattern on one side, and is not limited as long as the conductive layer functions as a conductive circuit or as a part of a conductive circuit. The patterned conductive layer may be provided with an insulating layer, if necessary, so as to cover the conductive pattern. The insulating layer is not particularly limited, and any known insulating layer may be used.

[0061] The thickness of the conductive layer may be appropriately adjusted depending on the required conductivity, etc., and is not particularly limited. For example, it can be 0.5 μm or more and 20 μm or less, and preferably 1 μm or more and 15 μm or less.

[0062] <Decorative layer> The molded film of the present embodiment may have a decorative layer from the viewpoint of the design of the resulting molded article. The decorative layer may be a layer having a single color, or may have any pattern. For example, the decorative layer can be formed by preparing a decorative ink containing a coloring material, a resin, and a solvent, and then applying the decorative ink to the base film by a known printing method. The coloring material can be appropriately selected from known pigments and dyes, and the resin is preferably appropriately selected from the same resins as the resin (A) in the conductive composition of the present embodiment. The thickness of the decorative layer is not particularly limited, but may be, for example, from 0.5 μm to 10 μm, and preferably from 1 μm to 5 μm.

[0063] [Molded body] The molded article of this embodiment is a molded article having at least a conductive layer laminated on a substrate, and the conductive layer is a cured product of the conductive composition for molded films according to any one of claims 1 to 5. The molded article of this embodiment is formed from a molded film using the conductive composition for molded films of this embodiment, and therefore is a molded article having a conductive circuit formed on any surface, such as an uneven surface or a curved surface. Hereinafter, three embodiments of the method for producing the molded body of the present embodiment will be described. Note that the molded body of the present embodiment may be produced by using the conductive composition of the present embodiment, and the method is not limited to these embodiments.

[0064] <First manufacturing method> A first method for producing a molded body according to the present embodiment includes the steps of: printing the conductive composition for a molded film according to the present embodiment on a base film and drying the composition to produce a molded film; placing the formed film on a substrate; and b) integrating the molded film and the substrate by an overlay molding process. The following description will be given with reference to FIG. 3, but as the method for producing the molded film is as described above, the description will be omitted here.

[0065] Fig. 3 is a schematic process diagram showing an example of a first manufacturing method of a molded body. Fig. 3(A) to (C) each illustrate a molded film 10 and a substrate 20 arranged in a chamber box of a TOM (Three dimension Overlay Method) molding machine, while Fig. 3(B) and (C) omit the chamber box. In the first manufacturing method, first, the substrate 20 is placed on the table of the lower chamber box 22. Next, the molded film 10 of the present embodiment is passed between the upper chamber box 21 and the lower chamber box 22 and placed on the substrate 20. At this time, the molded film 10 may be placed so that the conductive layer faces either the substrate 20 side or the opposite side to the substrate 20, and this is selected depending on the final use of the molded body. Next, the upper and lower chamber boxes are placed in a vacuum state, and the molded film is heated. Next, the table is raised to raise the substrate 20 15. Next, only the inside of the upper chamber box 21 is opened to the atmosphere (FIG. 3(B)). At this time, the molded film is pressed against the substrate side 16, and the molded film 10 and the substrate 20 are bonded together and integrated (FIG. 3(C)). In this manner, a molded body 30 can be obtained.

[0066] In the first manufacturing method, the base material 20 can be prepared in advance by any method. In the first manufacturing method, the material of the base material 20 is not particularly limited, and the base material 20 may be made of resin or metal.

[0067] In this first manufacturing method, the frictional stress with the substrate plastic at high temperatures in the above-mentioned integration step with the substrate is caused by the frictional stress between the conductive circuit of the molded film and the substrate at high temperatures when the molded film in Fig. 3(C) is pressed 16 toward the substrate and the molded film 10 and substrate 20 are bonded together to be integrated. That is, in this first manufacturing method, the conductive layer is simultaneously subjected to a load due to tensile stress during molding and frictional stress with the substrate plastic at high temperatures.

[0068] <Second manufacturing method> A second method for producing a molded body according to the present embodiment includes the steps of: printing the conductive composition for molded film according to the present embodiment on a base film and drying the composition to produce a molded film; forming the formed film into a predetermined shape; placing the formed film in an injection mold; and forming a substrate by injection molding and integrating the formed film with the substrate. Hereinafter, the method will be described with reference to Fig. 4. The second manufacturing method is sometimes called a film insert method.

[0069] FIG. 4 is a schematic process diagram showing an example of the second manufacturing method of the molded body. In the second manufacturing method, the molded film 10 is molded into a predetermined shape in advance by a mold 11 (FIG. 4(A)). After or while being softened by heating, the molded film 10 is suctioned into the mold by vacuum or pressed against the mold by compressed air, or both, and molded by the mold 11 (FIG. 4(B)). At this time, the molded film 10 may be molded so that the conductive layer faces either the substrate 20 side described later or the opposite side to the substrate 20, and this is selected depending on the final use of the molded body. Next, the molded molded film 10 is placed in a mold 12 for injection molding (FIGS. 4(C) to 4(D)). Next, resin is injected 14 from an opening 13 to form the substrate 20, and the molded film 10 and the substrate 20 are integrated to obtain a molded body 30 (FIG. 4(E)).

[0070] In the second manufacturing method, it is not necessary to prepare the substrate 20 in advance, and the molding of the substrate and the integration with the molded film can be performed simultaneously. The material of the substrate 20 can be appropriately selected from known resins used for injection molding.

[0071] In this second manufacturing method, the frictional stress with the base plastic at high temperatures in the above-mentioned integration step with the substrate is caused by the frictional stress that the conductive layer on the molded film receives when high-temperature molten resin is injected into a mold when resin is injected 14 from opening 13 in Fig. 4(E) to form substrate 20 and the molded film 10 and substrate 20 are integrated. That is, in this second manufacturing method, the conductive layer is subjected to a load due to tensile stress during molding, and then is subjected to frictional stress with the base plastic at high temperatures in a separate step.

[0072] <Third manufacturing method> The third method for producing a molded body according to the present embodiment includes the steps of: printing the conductive composition for molded film according to the present embodiment on a base film by screen printing; and drying the composition to produce a molded film. placing the formed film in an injection mold; The method includes a step of molding a substrate by injection molding and transferring the conductive layer in the molded film to the substrate side. Hereinafter, the method will be described with reference to Fig. 5. The third manufacturing method is sometimes called an in-mold transfer method.

[0073] FIG. 5 is a schematic process diagram showing an example of the third manufacturing method of the molded body. In the third manufacturing method, the molded film 10 is selected and used as a base film having releasability. The molded film 10 is placed in a mold 12 for injection molding so that the conductive layer faces the substrate 20 side described later (FIG. 5(A)). Next, resin is injected 14 from an opening 13 to form the substrate 20, and the molded film 10 and the substrate 20 are adhered to each other, and at least the conductive layer is transferred to the substrate 20 side (FIG. 5(B)), and the molded body 30 is obtained (FIG. 5(C)). In addition, when the molded film 10 has a decorative layer, the decorative layer and the conductive layer are transferred.

[0074] In the third manufacturing method, since it is not necessary to cut the base film, a long base film can be arranged as shown in the example of Fig. 5. The material of the substrate 20 can be appropriately selected from known resins used for injection molding.

[0075] In this third manufacturing method, the frictional stress with the base plastic at high temperatures in the above-mentioned integration step with the base material is caused by the frictional stress that the conductive layer on the molded film receives when high-temperature molten resin is injected into the mold when resin is injected 14 from the opening 13 in Fig. 5(C) to form the base material 20 and the molded film 10 and the base material 20 are adhered to each other. That is, in this third manufacturing method, the conductive layer is simultaneously subjected to a load due to tensile stress during molding and frictional stress with the base plastic at high temperatures.

[0076] The molded articles obtained in this way make it possible to mount circuits, touch sensors and various electronic components on the plastic housings of home appliances, automobile parts, robots, drones, etc. They are also extremely useful for making electronic devices lighter, thinner, shorter and smaller, improving design freedom and increasing functionality. EXAMPLES

[0077] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the present invention in any way. In the examples, "parts" means "parts by mass" and "%" means "% by mass". The weight average molecular weight in the examples is a polystyrene-equivalent molecular weight measured using a GPC (gel permeation chromatography) "HLC-8320" manufactured by Tosoh Corporation.

[0078] In the examples, the "functional group value" is calculated based on the molecular weight per functional group of each raw material (this is referred to as the functional group equivalent) and is expressed as the amount of functional groups per 1 g of raw material converted into an equimolar amount of potassium hydroxide (mg) using the following formula. (Functional group value) [mgKOH / g] = (56.1 x 1000) / (functional group equivalent) The above-mentioned functional group value is a general term for an amount expressed, for example, as an acid value when the functional group is a carboxyl group, a hydroxyl value when the functional group is a hydroxyl group, or an amine value when the functional group is an amino group. When comparing the functional group ratios of substances having different functional groups, those having the same value of the above-mentioned functional group value can be considered to have the same molar amount of functional groups.

[0079] When titration of potassium hydroxide is used to quantify the functional groups such as carboxyl groups and hydroxyl groups, the above-mentioned functional group values ​​(acid value and hydroxyl value) can be directly determined from the appropriate amount of potassium hydroxide used for neutralization using a known and commonly used measurement method specified in, for example, JIS K 0070, and can be treated in the same way as the values ​​calculated by the above-mentioned calculation formula. In addition, even when the titration with potassium hydroxide is not used to determine the functional group value, such as isocyanate groups, the functional group value can be calculated in terms of potassium hydroxide for convenience by using the functional group equivalent weight derived from each measured value representing the amount of functional group and the above calculation formula. A specific calculation example is shown below.

[0080] Calculation example: Calculate the amount of isocyanate in trifunctional isocyanate compound "X" that has an isocyanate group and is 23% as measured by the method specified in JIS K 6806 (method of reacting isocyanate groups with n-dibutylamine and titrating the remaining n-dibutylamine with an aqueous hydrochloric acid solution). The functional group equivalent of trifunctional isocyanate compound "X" is calculated as follows from the above isocyanate amount (%) and the molecular weight of the isocyanate group (NCO = 44g / mol). (Functional group equivalent of "X") = 1 / (0.23 / 44) = 191.3 From the functional group equivalent of this trifunctional isocyanate compound "X" and the above-mentioned formula for functional group value, the functional group value of the trifunctional isocyanate compound "X" can be calculated as follows. (Functional value of trifunctional isocyanate compound "X") [mgKOH / g] =(56.1×1000) / 191.3=293.3

[0081] <Resin (A1)~(A4)> The following resins were used as resins (A1) to (A4). Resin (A1): Arkema acrylic thermoplastic elastomer, Nanostrength M22 (block copolymer of acrylic monomers (PMMA-b-PBA-b-PMMA; b = block), weight average molecular weight: 40,000, glass transition point: -40°C, 105°C (has two glass transition points), has no cyclic structure or ester bond in the main chain. Resin (A2): Acrylic resin manufactured by Mitsubishi Chemical Corporation, Dianal BR-106, weight average molecular weight 60,000, glass transition point 50°C, no cyclic structure or ester bond in the main chain. Resin (A3): Phenoxy resin manufactured by InChem, PKHC, weight average molecular weight 43,000, glass transition point 67°C, has hydroxyl groups (functionality 198 mg KOH / g), has a cyclic structure (aromatic ring structure) in the main chain and does not have an ester bond. Resin (A4): Cellulose ester resin manufactured by Eastman Chemical Company, CAB551-0.2, weight average molecular weight 70,000, glass transition point 100°C, has hydroxyl groups (functional value 54 mgKOH / g), has a cyclic structure in the main chain and does not have an ester bond. Resin (A5): Ethyl cellulose resin manufactured by Nisshin Chemical Industry Co., Ltd., Ethocel STD45, weight average molecular weight 135,000, glass transition point 129°C, has a cyclic structure in the main chain and does not have an ester bond.

[0082] <Synthesis Example 1: Synthesis of Resin (A6)> A reactor equipped with an agitator, a thermometer, a rectifying tube, a nitrogen gas inlet tube, and a pressure reducing device was charged with 14.5 parts of dimethyl isophthalate, 14.5 parts of dimethyl terephthalate, 12.0 parts of ethylene glycol, 18.0 parts of neopentyl glycol, and 0.03 parts of tetrabutyl titanate, and gradually heated to 180 ° C. while stirring under a nitrogen stream, and an ester exchange reaction was carried out at 180 ° C. for 3 hours, the acid value was measured, and when it became 15 or less, the pressure in the reactor was gradually reduced to 1 to 2 torr, and when it reached a predetermined viscosity, the reaction was stopped and the mixture was removed, transferred to a fluorine-treated pallet, and cooled to obtain a polyester resin (A6) having a weight average molecular weight of 45,000, a glass transition point of 58 ° C., a hydroxyl group (functional group value 5 mg KOH / g), and an aromatic ring structure and an ester bond in the main chain.

[0083] <Synthesis Example 2: Synthesis of Resin (A7)> In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, 127.0 parts of a polyester polyol obtained from isophthalic acid and 3-methyl-1,5 pentanediol (Kuraray Co., Ltd.'s "Kuraray Polyol P-2030"), 19.0 parts of isophorone diisocyanate, and 36.5 parts of toluene were charged and reacted under a nitrogen gas flow at 90°C for 3 hours, and then 5.5 parts of isophorone diamine was added and reacted for a further 2 hours at 90°C. The reaction was then stopped by cooling, and finally the mixture was removed and transferred to a fluorine-treated surface pallet and dried in a hot air drying oven at 120°C for 5 hours and then vacuum dried for 24 hours to obtain a solid urethane resin (A7) having a weight average molecular weight of 35,000, a glass transition point of 5°C, amino groups (functional group value 4 mgKOH / g), and an aromatic ring structure and an ester bond in the main chain.

[0084] The following conductive particles, solvent, and crosslinking agent were used. <Conductive fine particles (B1)~(B5)> Conductive fine particles (B1): Flake silver powder manufactured by Fukuda Metal Foil & Powder Co., Ltd., average particle size 5.2 μm ·Conductive fine particles (B2): Manufactured by Fukuda Metal Foil and Powder Co., Ltd., chain agglomerated silver powder, average particle size 1.7μm Conductive fine particles (B3): Mitsui Mining & Smelting Co., Ltd., silver-coated copper powder, silver coating amount 10%, average particle size 2.0 μm Conductive fine particles (B4): Ishihara Sangyo Kaisha, needle-shaped conductive Sb-doped tin oxide powder, average particle size 2.9 μm Conductive fine particles (B5): Expanded graphite, manufactured by Ito Graphite Co., Ltd., average particle size 15 μm

[0085] <Solvents (C1-1) to (C1-10)> Solvent (C1-1): 1,2,3,4-tetrahydronaphthalene, boiling point 209℃ Solvent (C1-2): TonenGeneral Sekiyu T-SOL150, a mixture of high boiling point aromatic hydrocarbons, boiling point 184°C Solvent (C1-3): Propiophenone, boiling point 218℃ Solvent (C1-4): Methyl benzoate, boiling point 199℃ Solvent (C1-5): Ethyl benzoate, boiling point 213℃ Solvent (C1-6): Propyl benzoate, boiling point 230℃ Solvent (C1-7): Ethyl phenylacetate, boiling point 226℃ Solvent (C1-8): benzyl acetate, boiling point 212℃ Solvent (C1-9): Benzyl alcohol, boiling point 205℃ Solvent (C1-10): 2-phenoxypropanol, boiling point 244℃

[0086] <Solvents (C2-1) ~ (C2-5)> Solvent (C2-1): Dihydroterpinyl acetate, boiling point 220℃ Solvent (C2-2): Terpinyl acetate, boiling point 220℃ Solvent (C2-3): Isobornyl acetate, boiling point 227℃ Solvent (C2-4): 1-menthyl acetate, boiling point 215℃ Solvent (C2-5): Methyl cyclohexane-1-carboxylate, boiling point 183℃

[0087] <Other solvents (C3-1)~(C3-5)> Solvent (C3-1): 2-methoxypropanol, boiling point 120℃ Solvent (C3-2): Diethylene glycol monoethyl ether acetate, boiling point 217℃ Solvent (C3-3): Dipropylene glycol monomethyl ether, boiling point 194℃ Solvent (C3-4): Diethylene glycol monobutyl ether, boiling point 230℃ Solvent (C3-5): ExxonMobil Chemical, Exxol D-80, a mixture of high boiling alicyclic hydrocarbons and high boiling aliphatic hydrocarbons, boiling point 205°C

[0088] <Crosslinking agent (D1)> Crosslinker (D1): Blocked isocyanate solution manufactured by Baxeneden Chemicals, Trixene BI7982, containing three blocked isocyanate groups per molecule (functionality 195 mg KOH / g), non-volatile content 70% (solvent (C3-1): 2-methoxypropanol)

[0089] <Production Example 1: Creation of Decorative Ink (E1)> 200 parts of resin solution (only resin (A6)) consisting of 80 parts of resin (A2) and 120 parts of solvent (C3-2) was prepared, and 20 parts of phthalocyanine blue pigment (LIONOL BLUE FG7351 manufactured by Toyo Color Co., Ltd.) and 10 parts by mass of titanium oxide pigment (TIPAQUE CR-93 manufactured by Ishihara Sangyo Kaisha, Ltd.) were stirred and mixed therein, and the mixture was kneaded with a three-roll mill (manufactured by Kodaira Seisakusho Co., Ltd.). After that, 5 parts of isocyanate crosslinking agent (Desmodur N3300 manufactured by Sumika Covestro Urethane Co., Ltd., non-volatile content 100%) and 90 parts of solvent (E2) were added and stirred and mixed uniformly to obtain decorative ink (G1).

[0090] <Example 1: Preparation of conductive composition for molded film (F1)> 20.0 parts of resin (A1) was dissolved in a mixed solvent consisting of 15.0 parts of solvent (C1-1) and 15.0 parts of solvent (C2-1), stirred and mixed with 80.0 parts of conductive fine particles (B1), kneaded with a three-roll mill (manufactured by Kodaira Seisakusho), and then stirred and mixed uniformly with a planetary mixer to obtain a conductive composition (F1) for molded films.

[0091] <Examples 2 to 56: Preparation of conductive compositions (F2) to (F56) for molded films> Conductive compositions for molded films (F2) to (F56) were obtained in the same manner as in Example 1, except that the types and amounts of resin, solvent, conductive fine particles, and crosslinking agent (when a crosslinking agent was used, the crosslinking agent was added immediately before uniform stirring and mixing with a planetary mixer) were changed as shown in Table 1. The numerical values ​​for each material in Tables 1 to 4 are all in parts by mass.

[0092] <Comparative Examples 1 to 9: Preparation of Conductive Compositions (F57) to (F65) for Molded Films> Conductive compositions for molded films (F57) to (F65) were obtained in the same manner as in Example 1, except that the types and amounts of resin, solvent, conductive fine particles, and crosslinking agent in Example 1 were changed as shown in Table 4.

[0093] <Examples 57 to 112 and Comparative Examples 10 to 18> Conductive compositions for molded films (F1) to (F65) were each printed on a polycarbonate (PC) base film (Teijin, Panlite 2151, thickness 300 μm, 300 mm × 210 mm) using a screen printer (Minoscreen, Minomat SR5575 semi-automatic screen printer) at a printing speed of 100 mm. Then, by heating in a hot air drying oven at 120 ° C. for 30 minutes, a molded film was obtained with a conductive layer having a square solid pattern with a width of 15 mm, a length of 30 mm, and a thickness of 10 μm, a linear pattern with a line width of 3 mm, a length of 60 mm, and a thickness of 10 μm, and a stripe pattern with a line width of 150 μm, a line distance of 150 μm, and a length of 60 mm.

[0094] <Example 113> The decorative ink (G1) was applied to a polycarbonate base film (Teijin, Panlite 2151, thickness 300 μm, 300 mm x 210 mm) using a blade coater so that the dry film thickness was 2 μm, and the film was heated at 120°C for 30 minutes to form a decorative layer. Next, in Example 60, the above-mentioned film with decorative layer was used instead of the polycarbonate base film, and a conductive layer was formed on the decorative layer, and a molded film having a polycarbonate film, a decorative ink layer, and a conductor laminated in that order was obtained in the same manner as in Example 60.

[0095] <Example 114> In Example 60, a two-layer co-extrusion film of polycarbonate resin / acrylic resin (Technoloy C001, manufactured by Sumitomo Chemical Co., Ltd., thickness 125 μm, 300 mm x 210 mm) was used instead of the polycarbonate base film, and a conductive composition for molded films was printed on the polycarbonate resin side, except that a molded film was obtained in the same manner as in Example 60.

[0096] <Example 115> A molded film was obtained in the same manner as in Example 60, except that an acrylic resin film (Technoloy S001G, manufactured by Sumitomo Chemical Co., Ltd., thickness 250 μm, 300 mm x 210 mm) was used instead of the polycarbonate base film, and the drying conditions in the hot air drying oven were 80°C and 30 minutes.

[0097] <Example 116> In Example 60, an easily moldable PET resin film (Emron PETG resin sheet, thickness 250 μm, 300 mm x 210 mm, manufactured by Morino Kako Co., Ltd.) was used instead of the polycarbonate base film, and the drying conditions in the hot air drying oven were 70°C and 30 minutes, except that a molded film was obtained in the same manner as in Example 60.

[0098] <Example 117> A molded film was obtained in the same manner as in Example 60, except that a polypropylene film (Idemitsu Unitech, Pure Thermo AG-306, thickness 200 μm, 300 mm x 210 mm) was used instead of the polycarbonate film, and the drying conditions in the hot air drying oven were 80°C and 30 minutes.

[0099] [(1) Volume resistivity measurement] The volume resistivity (Ω·cm) of the 15 mm×30 mm square solid conductive layers formed on the molded films of Examples 57 to 117 and Comparative Examples 10 to 18 was measured using a resistivity meter (Mitsubishi Chemical Analytech Co., Ltd., Loresta GP MCP-T610 resistivity meter, JIS-K7194 compliant, 4-terminal 4-probe constant current application method) (4-terminal probes spaced 0.5 cm apart). The results are shown in Tables 1 to 4.

[0100] [(2) Peel adhesion evaluation] The conductive layer formed on the molded film of Examples 57 to 117 and Comparative Examples 10 to 18 was cut into a square shape of 15 mm x 30 mm with a cutter knife using a 1 mm interval cross-cut guide manufactured by Gardner Co., Ltd., and cut into a grid pattern of 10 x 10 squares so as to penetrate the conductive layer. Cellophane tape manufactured by Nichiban Co., Ltd. was attached to the conductive layer, and the trapped air was removed to ensure good adhesion, and then the tape was peeled off vertically. The degree of peeling of the coating film was evaluated as follows according to the ASTM-D3519 standard. The results are shown in Tables 1 to 4. (Evaluation criteria for peel adhesion) A: Rating 5B to 4B, excellent adhesion B: The rating is 5B to 4B, but the coating film has undergone cohesive failure and part of the coating film on the surface side has come off. C: Rating 3B or lower, poor adhesion

[0101] [(3) Evaluation of high-speed printing] The stripe patterns formed on the molded films of Examples 57 to 117 and Comparative Examples 10 to 18, each having a line width of 150 μm, a line spacing of 150 μm, and a length of 60 mm, were observed using a digital microscope (Keyence VHX-6000) and evaluated as follows. The results are shown in Tables 1 to 4. (High-speed printability evaluation standard) A: No chipping or scratching of the pattern, excellent linearity B: The pattern is slightly constricted, but there are no or very minor chips or scratches. C: There is noticeable chipping or fading of the pattern, and the printability is poor.

[0102] [(4) Wiring resistance evaluation] The formed films of Examples 57 to 117 and Comparative Examples 10 to 18 were cut into a length of 70 mm and a width of 10 mm so that the conductive layer of the linear pattern of 3 mm x 60 mm formed in the film was in the center, and used as a measurement coupon. On the surface of the measurement coupon opposite the conductive layer, two lines perpendicular to the conductive layer from the longitudinal end were added with oil-based marker at 4 cm intervals as marks. The resistance values ​​of the positions at 4 cm intervals according to these marks were measured using a tester, and these were taken as wiring resistance (Ω). The results are shown in Tables 1 to 4.

[0103] [(5) Hot stretching evaluation 1] The measurement coupons of Examples 57 to 114 and Comparative Examples 10 to 18 were stretched in the longitudinal direction at a stretching speed of 10 mm / min to an elongation rate of 125% in a heating oven at 160°C. After removing from the oven and cooling, the presence or absence of disconnection was evaluated using an optical microscope. In addition, the wiring resistance (Ω) was measured at positions corresponding to 4 cm intervals based on the original mark in the same manner as in the measurement of the wiring resistance described above, and the wiring resistance after stretching / wiring resistance before stretching was defined as the resistance variation rate (times) during thermal stretching, and each was evaluated according to the following criteria. The results are shown in Tables 1 to 4. (Whether or not there is a break in the wire) A: No breaks were observed. B: 1 to 2 minor cracks were found C: Severe disconnection or peeling of the conductive coating was confirmed. (Resistance variation rate during hot stretching) A: 5 times or more but less than 10 times B: 10 times or more but less than 100 times C: 100 times or more

[0104] The elongation rate is a value calculated as follows. (Elongation rate) [%] = {(length after stretching - length before stretching) / (length before stretching)} x 100

[0105] [(6) Hot stretching evaluation 2] The heat stretching was evaluated according to the following criteria in the same manner as in the heat stretching evaluation 1, except that the elongation rate was changed to 150%. The results are shown in Tables 1 to 4. (Whether or not there is a break in the wire) A: No breaks were observed. B: 1 to 2 minor cracks were found C: Severe disconnection or peeling of the conductive coating was confirmed. (Resistance variation rate during hot stretching) A: 10 times or more but less than 100 times B: 100 times or more but less than 1000 times C:1000 times or more

[0106] [(7) Hot stretching evaluation 3] The measurement coupons of Examples 115 to 117 were stretched in the longitudinal direction in a heating oven at 120° C. at a pulling speed of 10 mm / min to an elongation rate of 125%. After removing from the oven and cooling, the presence or absence of disconnection was evaluated using an optical microscope. In addition, the wiring resistance (Ω) was measured at positions corresponding to 4 mm intervals based on the original mark in the same manner as in the measurement of the wiring resistance described above, and the wiring resistance after stretching / wiring resistance before stretching was defined as the resistance variation rate (times) during thermal stretching, and each was evaluated according to the following criteria. The results are shown in Table 4. (Whether or not there is a break in the wire) A: No breaks were observed. B: 1 to 2 minor cracks were found C: Severe disconnection or peeling of the conductive coating was confirmed. (Resistance variation rate during hot stretching) A: 5 times or more but less than 10 times B: 10 times or more but less than 100 times C: 100 times or more

[0107] [(8) Hot stretching rating 4] The heat stretching evaluation was performed in the same manner as in the heat stretching evaluation 3, except that the elongation rate was changed to 150%, and the evaluation was performed according to the following criteria. The results are shown in Table 4. (Whether or not there is a break in the wire) A: No breaks were observed. B: 1 to 2 minor cracks were found C: Severe disconnection or peeling of the conductive coating was confirmed. (Resistance variation rate during hot stretching) A: 10 times or more but less than 100 times B: 100 times or more but less than 1000 times C:1000 times or more

[0108] [(9) Process durability evaluation during manufacturing of molded products by overlay molding 1] A rectangular parallelepiped ABS resin molded product having a height of 10 mm and a length and width of 30 mm x width of 30 mm was placed so as to face the conductor side surface so as to overlap the position of the linear pattern of 3 mm x 60 mm of the molded film of Examples 57 to 114 and Comparative Examples 10 to 18, and overlay molding was performed at a set temperature of 160 ° C. using a TOM molding machine (manufactured by Fuse Vacuum Co., Ltd.) to obtain a molded product in which the molded film molded into a rectangular parallelepiped shape and the ABS resin molded product are integrated. The scraping and resistance variation rate of the linear pattern wiring of this molded product were confirmed. The resistance variation rate was evaluated by measuring the wiring resistance (Ω) at a position corresponding to a 6 cm interval based on the original mark, and the wiring resistance after stretching / wiring resistance before stretching was defined as the resistance variation rate (times) during hot stretching, and each was evaluated according to the following criteria. The results are shown in Tables 1 to 4. (Presence or absence of disconnection and resistance fluctuation rate) A: No wear on the wiring is observed, and the resistance fluctuation rate is between 10 times and 50 times. B: 1-2 chipped wire ends due to wear and tear, or resistance fluctuation rate is 50x or more but less than 500x C: One or more breaks in the wiring due to scraping were confirmed.

[0109] [(10) Process durability evaluation during manufacturing of molded products by overlay molding 2] A molded body was obtained in the same manner as in the process resistance evaluation 1 during the manufacture of a molded body by overlay molding, except that the 3 mm × 60 mm linear patterns of the molded films of Examples 115 to 117 were used and overlay molding was performed at 120 ° C. The scraping of the linear pattern wiring during overlay molding and the resistance variation rate were evaluated. The results are shown in Table 4.

[0110] [(11) Process resistance evaluation during manufacturing of molded products by film insert molding 1] A block-shaped metal mold having a rectangular protrusion in the center measuring 30 mm x 30 mm x 10 mm with a step of 10 mm was placed facing the opposite side of the conductor so as to overlap the position of the 3 mm x 60 mm linear pattern of the molded films of Examples 57 to 114 and Comparative Examples 10 to 18, and overlay molding was performed at a set temperature of 160°C using a TOM molding machine (manufactured by Fuse Vacuum Co., Ltd.) to obtain a moldable film molded into a rectangular parallelepiped shape and with a patterned conductor on the inside. Next, the molded film molded into the rectangular parallelepiped shape was set in an injection molding machine (IS170 (i5), manufactured by Toshiba Machine Co., Ltd.) equipped with a valve gate type in-mold molding test mold, and a molded body integrated with the molded film with a patterned conductor was obtained by injection molding PC / ABS resin (LUPOYPC / ABSHI5002, manufactured by LG Chem Co., Ltd.) (injection conditions: screw diameter 40 mm, cylinder temperature 260 ° C., mold temperature (fixed side, movable side) 60 ° C., injection pressure 160 MPa (80%), holding pressure 100 MPa, injection speed 60 mm / sec (28%), injection time 4 seconds, cooling time 20 seconds). Washout due to injection of molten resin of the linear pattern of this molded body (deformation or disconnection of the wiring pattern due to the temperature and injection pressure of the molten thermoplastic resin) and resistance variation rate were confirmed. The resistance variation rate was evaluated by measuring the wiring resistance (Ω) at positions corresponding to 6 cm intervals based on the original mark, and the wiring resistance after stretching / wiring resistance before stretching was defined as the resistance variation rate (times) during thermal stretching. The results are shown in Tables 1 to 4. (Presence or absence of disconnection and resistance fluctuation rate) A: No washout of wiring is observed, and the resistance fluctuation rate is between 10 times and 50 times. B: Wiring distortion due to mild washout is confirmed, or resistance fluctuation rate is 50 times or more but less than 500 times. C: One or more breaks due to washout in the wiring are confirmed.

[0111] [(12) Process resistance evaluation during manufacturing of molded products by film insert molding 2] A molded body was obtained in the same manner as in the process resistance evaluation 1 during the manufacture of a molded body by overlay molding, except that the 3 mm x 60 mm linear patterns of the molded films of Examples 115 to 117 were used and overlay molding was performed at 120 ° C. The degree of washout and the resistance variation rate due to the injection of molten resin of the linear pattern during film insert molding were evaluated. The results are shown in Table 4.

[0112] [Table 1]

[0113] [Table 2]

[0114] [Table 3]

[0115] [Table 4]

[0116] [Summary of results] It was found that the conductive layers formed using the conductive compositions of Comparative Examples 10 to 18, which did not simultaneously contain the solvents (C1) and (C2) as solvent components, broke or had an increased resistance when stretched at high temperatures during the three-dimensional molding process of the molded film, especially when the stretching elongation was large. In addition, there was a tendency for the pattern to chip or fade when printed at a high printing speed.

[0117] On the other hand, from the results of Examples 57 to 117, the conductive composition of this embodiment did not break even when the stretching elongation was large when stretched at high temperatures during the three-dimensional molding process of the molded film, and the increase in resistance value was also well suppressed. This is presumably because the solvent component of the conductive composition of this embodiment contains a solvent (C1) having an aromatic structure and a solvent (C2) having an alicyclic structure and an ester bond, so that the polymer chains of the resin (A) component are widely developed in the solvent (C) and the polymer chains are well entangled with each other when the conductive layer is formed, thereby exhibiting excellent cohesive force and conductivity retention properties at high temperatures of the conductive layer that can withstand stretching at high temperatures and large elongations during molding, and also achieving printability at high printing speeds without impairing both. At the same time, the inclusion of solvent (C1) and solvent (C2) highly suppressed the infiltration of the solvent near the interface between the base film and the conductive layer, which is important as the scaffold for the conductive layer, and is believed to have been effective in suppressing breakage when stretched at high temperatures and large elongations during molding, and suppressing printing defects (presumably due to suppression of the increase in viscosity of the conductive composition due to solvent absorption at the moment of contact with the substrate during printing). The balance of properties of stretching at high temperatures and large elongations during molding and printability at high printing speeds was excellent in terms of suppressing resistance increases and breakage, especially when used in combination with a resin that has at least one glass transition point between 0°C and 130°C and none below 0°C. This is believed to be due to the fact that the polymer chains are less likely to slip out of the entanglement of the polymer chains of resin (A) when softened at the molding temperature, making it less likely that voids that cause breakage will be formed. Furthermore, when used in combination with a resin having a cyclic structure in the main chain, particularly a resin having both an aromatic ring structure and an ester bond as the cyclic structure, it was particularly excellent in that it was less likely to cause an increase in resistance value or defects during printing. Although the mechanism by which such properties are exhibited is unclear, it is speculated that the high polar affinity resulting from the structural similarity between resin (A) and solvents (C1) and (C2) allows the polymer chains of the resin (A) component to spread widely in solvent (C) and exhibit appropriate fluidity, and when the conductive layer is formed, the polymer chains are well entangled with each other, resulting in the expression of toughness capable of suppressing local stress concentration on a microscale that would lead to the disconnection of the connection (conductive path) between conductive particles in the conductive layer.

[0118] Furthermore, due to the above-mentioned characteristics, a molded film having a conductive layer of the conductive composition of the present invention has been able to obtain an excellent wiring-integrated molded body even when the substrate surface has an uneven three-dimensional shape, particularly a complex three-dimensional shape having steep steps.

[0119] Thus, the molded film and wiring-integrated molded body using the conductive composition of this embodiment can be directly applied to plastic housings and three-dimensional parts for home appliances, automobile parts, robots, drones, etc., to make it possible to directly fabricate lightweight and space-saving circuits, touch sensors, antennas, heating elements (heaters), electromagnetic shields, inductors (coils), resistors, and mount various electronic components without compromising design freedom. Also, it is extremely useful for making electronic devices lighter, thinner, shorter, and smaller, improving design freedom, and making them more multifunctional. [Explanation of symbols]

[0120] 1 Base film 2 Conductive layer 3 Decorative layer 4. Electronic Components 5-pin 10 Forming film 11 Mold 12 Injection mold 13 Opening 14 Injection 15 Increase 16 Pressurization 17 Resin 20 Base material 21 Upper chamber box 22 Lower chamber box 30 Molded body

Claims

1. A conductive composition for producing a molded film for forming a conductive layer on a substrate surface having an uneven surface or a three-dimensional curved surface, comprising: Contains a resin (A), conductive fine particles (B), and a solvent (C), The solvent (C) includes a solvent (C1) that satisfies the following conditions (1) and (2), and a solvent (C2) that satisfies the following conditions (1) and (3) (excluding the solvent (C1)): the mass ratio of the solvent (C1) to the solvent (C2) is 15:85 to 85:15; A conductive composition for molded films, wherein the total content of the solvent (C1) and the solvent (C2) is 30 parts by mass or more per 100 parts by mass of the solvent (C). Condition (1) The boiling point is 180° C. or higher and 270° C. or lower. Condition (2) Having an aromatic structure in the molecular structure Condition (3) Having an alicyclic structure and an ester bond in the molecular structure

2. 2. The conductive composition for formed films according to claim 1, wherein the resin (A) is a resin having at least one glass transition point in the range of 0°C or higher and lower than 130°C, and no glass transition point lower than 0°C.

3. 3. The conductive composition for molded films according to claim 1 or 2, wherein the conductive fine particles (B) comprise one or more conductive fine particles selected from silver powder, copper powder, silver-coated powder, copper alloy powder, conductive oxide powder, and carbon fine particles.

4. The conductive composition for molded films according to any one of claims 1 to 3, wherein the resin (A) has a cyclic structure in its main chain.

5. The conductive composition for molded films according to any one of claims 1 to 4, wherein the resin (A) has an aromatic ring structure and an ester bond in the main chain.

6. The conductive composition for molded films according to any one of claims 1 to 5, wherein the total content of the solvent (C1) and the solvent (C2) is 40 parts by mass or more per 100 parts by mass of the solvent (C).

7. A molded film having a conductive layer on a base film, A molded film, wherein the conductive layer is a cured product of the conductive composition for molded films according to any one of claims 1 to 6.

8. A molded film having a decorative layer and a conductive layer on a base film, A molded film, wherein the conductive layer is a cured product of the conductive composition for molded films according to any one of claims 1 to 6.

9. The molded film according to any one of claims 7 to 8, wherein the base film is a film selected from the group consisting of polycarbonate, polymethyl methacrylate, polypropylene, and polyethylene terephthalate, or a laminate film thereof.

10. A molded article having a conductive layer laminated on a substrate, A molded article, wherein the conductive layer is a cured product of the conductive composition for molded films according to any one of claims 1 to 6.

11. A step of producing a molded film by printing the conductive composition for molded films according to any one of claims 1 to 6 on a base film and drying it; placing the formed film on a substrate; and a step of integrating the molded film and the substrate by an overlay molding method.

12. A step of producing a molded film by printing the conductive composition for molded films according to any one of claims 1 to 6 on a base film and drying it; forming the formed film into a predetermined shape; placing the formed film in an injection mold; A method for producing a molded article, comprising the steps of: molding a substrate by injection molding; and integrating the molded film with the substrate.

13. A step of producing a molded film by printing the conductive composition for molded films according to any one of claims 1 to 6 on a base film and drying it; placing the formed film in an injection mold; A method for producing a molded article, comprising the steps of: molding a substrate by injection molding; and transferring a conductive layer in the molded film to the substrate.

Citation Information

Patent Citations

  • Conductive paste

    JP2007158073A

  • Decorative sheet and manufacturing process for the same

    JP2007296848A

  • Electroconductive ink, and laminate with electroconductive pattern and method for producing the same

    JP2011252140A

  • Conductive circuit integrated molded product and method of manufacturing the same

    JP2012011691A

  • Conductive composition for molding film, molding film, molded body, and manufacturing method therefor

    JP2019189680A