Electrode catalyst layer, membrane electrode assembly and polymer electrolyte fuel cell

The inclusion of fibrous materials with controlled P/Pt ratios and carbon fibers in the electrode catalyst layer addresses crack issues, maintaining membrane integrity and improving power generation performance in polymer electrolyte fuel cells.

JP7567310B2Active Publication Date: 2024-10-16TOPPAN HOLDINGS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020156525
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-17
Publication Date
2024-10-16
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Cracks in the electrode catalyst layer of polymer electrolyte fuel cells due to drying can expose the polymer electrolyte membrane, leading to reduced durability and power generation performance.

Method used

Incorporating a fibrous material with specific P/Pt ratios and average fiber diameters and lengths in the electrode catalyst layer, along with carbon fibers, to enhance flexibility, proton conductivity, and crack resistance.

Benefits of technology

Suppresses crack formation, maintains electrolyte membrane integrity, and enhances power generation performance by promoting proton conductivity and gas diffusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567310000002
    Figure 0007567310000002
  • Figure 0007567310000003
    Figure 0007567310000003
  • Figure 0007567310000004
    Figure 0007567310000004
Patent Text Reader

Abstract

To provide an electrode catalyst layer, a membrane electrode assembly, and a polymer electrolyte fuel cell capable of suppressing a decrease in the durability of the membrane electrode assembly and a reduction in power generation performance of the polymer electrolyte fuel cell by suppressing crack generation in the electrode catalyst layer.SOLUTION: Electrode catalyst layers 1, 2 include at least a catalyst material 6, carbon particles 5 loaded with the catalyst material 6, polyelectrolyte aggregates 7, and polyelectrolyte fibers 8. The amount of phosphorus (P) and the amount of platinum (Pt) in the electrode catalyst layers 1, 2, as obtained by elemental analysis by energy dispersive X-ray analysis (EDX), satisfy the following equation (1). 0<P / Pt≤3.0 ... Formula (1)SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode catalyst layer provided in a fuel cell, a membrane electrode assembly provided with an electrode catalyst layer, and a polymer electrolyte fuel cell. [Background technology]

[0002] In recent years, fuel cells have been attracting attention as an effective solution to environmental and energy problems. Fuel cells oxidize fuel such as hydrogen using an oxidizing agent such as oxygen, and convert the resulting chemical energy into electrical energy. Fuel cells are classified according to the type of electrolyte into alkaline, phosphoric acid, polymer, molten carbonate, solid oxide, etc. Polymer electrolyte fuel cells (PEFCs) operate at low temperatures, have high output density, and can be made compact and lightweight, so they are expected to be used as portable power sources, domestic power sources, and vehicle power sources.

[0003] A polymer electrolyte fuel cell (PEFC) has a structure in which an electrolyte membrane, a polymer electrolyte membrane, is sandwiched between a fuel electrode (anode) and an air electrode (cathode). By supplying a fuel gas containing hydrogen to the fuel electrode side and an oxidant gas containing oxygen to the air electrode side, electricity is generated through the following electrochemical reaction. Anode: H2 → 2H + + 2e - (Reaction 1) Cathode: 1 / 2O2+ 2H + + 2e - → H2O (reaction 2)

[0004] The anode and cathode are each a laminated structure including an electrode catalyst layer and a gas diffusion layer. Fuel gas supplied to the anode-side electrode catalyst layer generates protons and electrons in the presence of the electrode catalyst (Reaction 1). The protons pass through the polymer electrolyte and polymer electrolyte membrane in the anode-side electrode catalyst layer and move to the cathode. The electrons pass through an external circuit and move to the cathode. In the cathode-side electrode catalyst layer, the protons, electrons, and oxidant gas supplied from the outside react to produce water (Reaction 2). In this way, electricity is generated by electrons passing through an external circuit (Patent Document 1).

[0005] The electrode catalyst layer is generally composed of platinum-supported carbon and a polymer electrolyte. The carbon contributes to electron conduction during power generation, and the polymer electrolyte contributes to proton conduction. The balance of the types and contents of these greatly contributes to power generation performance. On the other hand, when generating electricity, the diffusibility of hydrogen and oxygen into the fuel cell (gas diffusibility) and the drainage performance of the water generated during power generation are also important. Fuel cells with high gas diffusibility and drainage performance can derive high power generation performance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-115299 A Summary of the Invention [Problem to be solved by the invention]

[0007] Incidentally, cracks may occur in the electrode catalyst layer due to shrinkage caused by drying during the formation of the electrode catalyst layer. The present inventors have found that when a crack is present in an electrode catalyst layer, the polymer electrolyte membrane is exposed from the crack in the membrane electrode assembly, and such exposure of the polymer electrolyte membrane is a factor in reducing the durability of the membrane electrode assembly and reducing the power generation performance of the solid polymer fuel cell. An object of the present invention is to provide an electrode catalyst layer, a membrane electrode assembly, and a polymer electrolyte fuel cell that can suppress a decrease in the durability of the membrane electrode assembly and a decrease in the power generation performance of the polymer electrolyte fuel cell by suppressing the generation of cracks in the electrode catalyst layer.

Means for Solving the Problems

[0008] In order to solve the above problems, an electrode catalyst layer according to one aspect of the present invention is an electrode catalyst layer containing at least a catalyst, carbon particles carrying the catalyst, a polymer electrolyte, and a fibrous substance, wherein the amount of phosphorus (P) and the amount of platinum (Pt) obtained by elemental analysis by energy dispersive X-ray analysis (EDX) in the electrode catalyst layer satisfy the following formula (1). 0 < P / Pt ≦ 3.0 ··· Formula (1)

[0009] Further, in the electrode catalyst layer according to one aspect of the present invention, the average fiber diameter of the fibrous substance may be in the range of 100 nm or more and 500 nm or less. Further, in the electrode catalyst layer according to one aspect of the present invention, the average fiber length of the fibrous substance may be in the range of 1 μm or more and 150 μm or less. Further, the electrode catalyst layer according to one aspect of the present invention may further contain carbon fibers. Further, in the electrode catalyst layer according to one aspect of the present invention, the fibrous substance may be composed of a polymer electrolyte.

[0010] Further, a membrane electrode assembly according to one aspect of the present invention includes a polymer electrolyte membrane and a pair of electrode catalyst layers sandwiching the polymer electrolyte membrane, and at least one of the pair of electrode catalyst layers is the above-described electrode catalyst layer. Further, a polymer electrolyte fuel cell according to one aspect of the present invention includes the above-described membrane electrode assembly and a pair of separators sandwiching the membrane electrode assembly.

Effects of the Invention

[0011] According to one aspect of the present invention, the occurrence of cracks in the electrode catalyst layer can be suppressed. Since the number of cracks is reduced, the deformation of the electrolyte membrane due to humidity changes during power generation can be suppressed, making the membrane less likely to break. As a result, it is possible to prevent a decrease in the durability of the membrane electrode assembly and a decrease in the power generation performance of the solid polymer electrolyte fuel cell. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view showing an example of the configuration of a membrane electrode assembly according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view showing a first configuration example of an electrode catalyst layer according to an embodiment of the present invention. [Diagram 3] FIG. 4 is a cross-sectional view showing a second configuration example of an electrode catalyst layer according to an embodiment of the present invention. [Figure 4] 1 is an exploded perspective view showing an example of the configuration of a polymer electrolyte fuel cell equipped with a membrane electrode assembly according to an embodiment of the present invention; [Diagram 5] FIG. 2 is a diagram showing the results of elemental analysis by energy dispersive X-ray analysis (EDX) in examples and comparative examples of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. Note that the present invention is not limited to the embodiments described below, and modifications such as design changes can be made based on the knowledge of those skilled in the art, and such modified embodiments are also included in the scope of the present invention.

[0014] (Overall composition) Fig. 1 is a cross-sectional view showing a schematic configuration example of a membrane electrode assembly according to an embodiment of the present invention. As shown in Fig. 1, the membrane electrode assembly 10 includes a polymer electrolyte membrane 3 and two electrode catalyst layers, an air electrode-side electrode catalyst layer 1 and a fuel electrode-side electrode catalyst layer 2. The fuel electrode-side electrode catalyst layer 2 is an electrode catalyst layer used in the fuel electrode, which is the anode of the solid polymer electrolyte fuel cell, and the air electrode-side electrode catalyst layer 1 is an electrode catalyst layer used in the air electrode, which is the cathode of the solid polymer electrolyte fuel cell.

[0015] The polymer electrolyte membrane 3 is located between the air electrode side electrode catalyst layer 1 and the fuel electrode side electrode catalyst layer 2. In other words, the polymer electrolyte membrane 3 is sandwiched between a pair of electrode catalyst layers (the air electrode side electrode catalyst layer 1 and the fuel electrode side electrode catalyst layer 2). The air electrode side electrode catalyst layer 1 is in contact with one of the two surfaces (front side) of the polymer electrolyte membrane 3, and the fuel electrode side electrode catalyst layer 2 is in contact with the other of the two surfaces (rear side) of the polymer electrolyte membrane 3.

[0016] When viewed from the direction opposite to one surface of the polymer electrolyte membrane 3, the outer shape of the air electrode-side electrode catalyst layer 1 and the outer shape of the fuel electrode-side electrode catalyst layer 2 are substantially the same, and the outer shape of the polymer electrolyte membrane 3 is larger than the outer shapes of these electrode catalyst layers 1, 2. In other words, when the membrane electrode assembly 10 is viewed in its thickness direction, the air electrode-side electrode catalyst layer 1 and the fuel electrode-side electrode catalyst layer 2 overlap each other via the polymer electrolyte membrane 3, and the outer edge of the polymer electrolyte membrane 3 is exposed without overlapping with the air electrode-side electrode catalyst layer 1 or the fuel electrode-side electrode catalyst layer 2. The outer shape of the polymer electrolyte membrane 3 and the outer shapes of the electrode catalyst layers 1, 2 are not particularly limited and may be, for example, rectangular.

[0017] (polymer electrolyte membrane) The polymer electrolyte membrane 3 is a membrane containing a polymer electrolyte. The polymer electrolyte used in the polymer electrolyte membrane 3 may be any polymer electrolyte having proton conductivity, and may be, for example, a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte. An example of the fluorine-based polymer electrolyte is Nafion (registered trademark: manufactured by DuPont). An example of the hydrocarbon-based polymer electrolyte is an engineering plastic or a compound in which a sulfonic acid group is introduced into a copolymer of an engineering plastic.

[0018] (electrode catalyst layer) Fig. 2 is a cross-sectional view showing a schematic diagram of a first configuration of the electrode catalyst layer of this embodiment. As shown in Fig. 2, each of the air electrode side electrode catalyst layer 1 and the fuel electrode side electrode catalyst layer 2 includes a catalyst substance-supporting carbon body 11 which is a carbon particle 5 supporting a catalyst substance (hereinafter also simply referred to as a "catalyst" or "catalyst particle") 6, a polymer electrolyte aggregate 7, and a polymer electrolyte fiber (fibrous material) 8 which is a fibrous polymer electrolyte.

[0019] The polymer electrolyte fiber 8 is, for example, an organic electrolyte fiber such as a fibrous material composed of an electrolyte. In the electrode catalyst layers 1 and 2, the polymer electrolyte aggregates 7 and the polymer electrolyte fibers 8 are positioned around the dispersed catalyst substance-supporting carbon bodies 11, and pores 9 are formed between these components. If the polymer electrolyte fiber 8 is an organic electrolyte fiber, it is possible to impart excellent flexibility to the electrode catalyst layers 1 and 2. If the polymer electrolyte fiber 8 is an organic electrolyte fiber composed of an electrolyte, it is possible to impart excellent flexibility to the electrode catalyst layers 1 and 2 while imparting excellent proton conductivity to the electrode catalyst layers 1 and 2.

[0020] The content of the polymer electrolyte fibers 8 is preferably within a range of 2% by mass to 50% by mass, more preferably within a range of 10% by mass to 30% by mass, and even more preferably within a range of 10% by mass to 20% by mass, relative to the content of the polymer electrolyte aggregates 7. When the content of the polymer electrolyte fibers 8 is within the above numerical range, pores 9 of a suitable size can be formed in a suitable amount.

[0021] As the catalyst material 6, platinum group elements such as platinum, palladium, ruthenium, iridium, rhodium, and osmium, as well as metals such as iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum, or alloys, oxides, and double oxides thereof can be used. Among these, platinum and platinum alloys are preferable. In addition, the particle size (average particle size D50) of these catalyst materials 6 is preferably in the range of 0.5 nm to 20 nm, more preferably in the range of 1 nm to 5 nm, since if it is too large, the activity of the catalyst decreases, and if it is too small, the stability of the catalyst decreases.

[0022] The carbon particles 5 may be any particles that are electrically conductive and not affected by the catalytic material 6. If the particle size (average particle size D50) of the carbon particles 5 is too small, it becomes difficult to form an electronic conduction path, and if it is too large, the electrode catalyst layers 1 and 2 become thick and the resistance increases, resulting in a decrease in output characteristics, so that the particle size is preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 10 nm to 100 nm. By supporting the catalyst material 6 on the carbon particles 5, which are particulate carbon materials, it is possible to increase the area of ​​the carbon material that can support the catalyst material 6, and to support the catalyst material 6 at a high density, thereby improving the catalytic activity.

[0023] The polymer electrolyte aggregate 7 is, for example, a mass of polymer electrolyte, which is an ionomer, aggregated by cohesive force. Here, the "cohesive force" means the Coulomb force or van der Waals force acting between ionomers. If the particle size (average particle size D50) of the polymer electrolyte aggregate 7 is too small, it is difficult to form an electronic conduction path, and if it is too large, the electrode catalyst layers 1 and 2 become thick and the resistance increases, resulting in a decrease in output characteristics. Therefore, the particle size (average particle size D50) is preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 10 nm to 100 nm. In this embodiment, the polymer electrolyte aggregate 7 is not limited to the form of an aggregate, and may be, for example, a non-aggregate of the polymer electrolyte. In addition, the particle size (average particle size D50) of the polymer electrolyte aggregate 7 is preferably larger than the particle size (average particle size D50) of the carbon particles 5. The particle size (average particle size D50) of the polymer electrolyte aggregates 7 is preferably in the range of 1.05 to 3 times, and more preferably in the range of 1.5 to 2 times, the particle size (average particle size D50) of the carbon particles 5. When the particle size (average particle size D50) of the polymer electrolyte aggregates 7 is within the above numerical range, pores 9 of a suitable size can be formed in a suitable amount. The polymer electrolyte fibers 8 are, for example, polymer electrolytes having an elongated shape due to cross-linking between polymer electrolytes.

[0024] The polymer electrolyte constituting the aggregate 7 and the polymer electrolyte fiber 8 may each be a polymer electrolyte having proton conductivity, and for example, a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte may be used. As the fluorine-based polymer electrolyte, for example, Nafion (registered trademark: manufactured by DuPont), Flemion (registered trademark) manufactured by Asahi Glass Co., Ltd., Aciplex (registered trademark) manufactured by Asahi Kasei Corporation, or Aquivion (registered trademark) manufactured by Solvay may be used. As the hydrocarbon-based polymer electrolyte, for example, an electrolyte such as sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, sulfonated polyphenylene, sulfonated polyimide, or acid-doped polybenzoazoles may be used.

[0025] The polymer electrolyte constituting the aggregates 7 and the polymer electrolyte fibers 8 may be the same as or different from each other. Furthermore, the polymer electrolyte constituting the aggregates 7, the polymer electrolyte constituting the polymer electrolyte fibers 8, and the polymer electrolyte constituting the polymer electrolyte membrane 3 may be the same as or different from each other. In order to improve the adhesion between the electrode catalyst layers 1, 2 and the polymer electrolyte membrane 3, the polymer electrolyte contained in the electrode catalyst layers 1, 2 and the polymer electrolyte membrane 3 are preferably made of the same material.

[0026] By including the polymer electrolyte fibers 8 in the electrode catalyst layers 1, 2, the polymer electrolyte fibers 8 are entangled with each other and function as a support in the electrode catalyst layers 1, 2, thereby suppressing breakage (cracks) and the like in the electrode catalyst layers 1, 2, which is one factor that causes a decrease in durability of the membrane electrode assembly 10. Therefore, compared to the conventional case in which the electrode catalyst layers 1, 2 are composed only of the catalyst substance-supporting carbon body 11 and the polymer electrolyte aggregates 7, it is possible to suppress the occurrence of cracks in the electrode catalyst layers 1, 2.

[0027] The present inventors have focused on the amounts of P (phosphorus) and Pt (platinum) contained in the electrode catalyst layers 1 and 2 and discovered that by adjusting the ratio of the amounts, it is possible to determine an appropriate amount of polymer electrolyte fiber 8 to be added to the electrode catalyst layers 1 and 2. This point will be explained below.

[0028] The polymer electrolyte fibers 8 in the electrode catalyst layers 1, 2 are preferably added so that the amounts of P (phosphorus) and Pt (platinum) obtained by elemental analysis by energy dispersive X-ray analysis (EDX) on a cross section of the electrode catalyst layers 1, 2 in the thickness direction of the electrode catalyst layers 1, 2 satisfy the following formula (1). Here, the P (phosphorus) to be measured is an element thought to contribute to proton conductivity, and is the P (phosphorus) contained in the polymer electrolyte fibers 8. In other words, the polymer electrolyte fibers 8 may be a phosphorus (P)-containing organic electrolyte fibrous material. The ratio of the amount of P (phosphorus) to the amount of Pt (platinum) (P / Pt) can be determined from the peak intensity ratio of the EDX spectrum, which is the analysis result of the above-mentioned energy dispersive X-ray analysis (EDX).

[0029] 0.1≦P / Pt≦3.0...Equation (1) If the amount of polymer electrolyte fibers 8 added to the electrode catalyst layers 1 and 2 is within the range that satisfies the above formula (1), proton conduction in the electrode catalyst layers 1 and 2 is promoted, making it possible to improve the output of the fuel cell. In this embodiment, the measurement position of the elemental analysis by energy dispersive X-ray analysis (EDX) is not limited to the cross section of the electrode catalyst layers 1 and 2, and may be the surface of the electrode catalyst layers 1 and 2. If the measurement position of the elemental analysis by energy dispersive X-ray analysis (EDX) is the cross section of the electrode catalyst layers 1 and 2, the electrode catalyst layers 1 and 2 are broken in their thickness direction immediately before the elemental analysis to expose (form) the cross section that is the measurement surface, thereby reducing the possibility of impurities being mixed into the cross section of the electrode catalyst layers 1 and 2 (contamination of the measurement point) and improving the measurement accuracy. In addition, if the measurement position of the elemental analysis by energy dispersive X-ray analysis (EDX) is the surface of the electrode catalyst layers 1 and 2, the elemental analysis measurement becomes extremely easy. Therefore, even if the surface of the electrode catalyst layers 1 and 2 is contaminated with impurities, the number of measurements of the elemental analysis can be easily increased, and the S / N ratio (ratio of signal intensity / noise intensity) can be easily increased.

[0030] If the average fiber diameter of the polymer electrolyte fibers 8 is 2 μm or less, a suitable fineness for use as a fiber material contained in the electrode catalyst layers 1 and 2 is ensured. In order to improve the output of a polymer electrolyte fuel cell, it is desirable that the gas supplied to the electrode catalyst layers 1, 2 is appropriately diffused into the electrode catalyst layers 1, 2 through the pores 9 formed in the electrode catalyst layers 1, 2, and that, particularly at the air electrode, water produced by an electrode reaction is appropriately discharged through the pores 9. In addition, the presence of the pores 9 facilitates the formation of an interface at which the gas, the catalyst material-supporting carbon body 11, and the polymer electrolyte come into contact, promoting the electrode reaction, which also makes it possible to improve the output of the polymer electrolyte fuel cell.

[0031] From the above viewpoints, it is preferable that the electrode catalyst layers 1, 2 have an appropriate size and an appropriate amount of pores 9. If the average fiber diameter of the polymer electrolyte fibers 8 is 1 μm or less, sufficient gaps are formed in the structure in which the polymer electrolyte fibers 22 are entangled in the electrode catalyst layers 1, 2, ensuring sufficient pores 9, making it possible to improve the output of the fuel cell. Furthermore, if the average fiber diameter of the polymer electrolyte fibers 8 is within the range of 100 nm or more and 500 nm or less, the output of the solid polymer electrolyte fuel cell is particularly increased.

[0032] The average fiber length of the polymer electrolyte fibers 8 is greater than the average fiber diameter and is preferably in the range of 1 μm to 150 μm, more preferably in the range of 80 μm to 100 μm. If the average fiber length of the polymer electrolyte fibers 8 is within the above range, aggregation of the polymer electrolyte fibers 8 is suppressed in the electrode catalyst layers 1 and 2, and pores 9 are easily formed. Furthermore, if the average fiber length of the polymer electrolyte fibers 8 is within the above range, a structure in which the polymer electrolyte fibers 8 are entangled is suitably formed in the electrode catalyst layers 1 and 2, thereby increasing the strength of the electrode catalyst layers 1 and 2 and improving the effect of suppressing the occurrence of cracks.

[0033] 3 is a cross-sectional view showing a schematic diagram of a second configuration of the electrode catalyst layer of this embodiment. As shown in FIG. 3, each of the air electrode side electrode catalyst layer 1 and the fuel electrode side electrode catalyst layer 2 may contain carbon fibers 12 in addition to the catalyst substance-supporting carbon body 11, the polymer electrolyte aggregates 7, and the polymer electrolyte fibers 8. The carbon fiber 12 is a fibrous structure containing carbon as a constituent element. Examples of the carbon material used for the carbon fiber 12 include fibrous carbon materials such as carbon fibers, carbon nanofibers, and carbon nanotubes. Among the above-mentioned materials, it is particularly preferable to use carbon nanofibers or carbon nanotubes.

[0034] The average fiber diameter of the carbon fibers 12 is preferably 200 nm or less, and more preferably 150 nm or less. If the average fiber diameter of the carbon fibers 12 is 200 nm or less, the carbon fibers 12 are ensured to have an appropriate fineness as a fiber material to be contained in the electrode catalyst layers 1 and 2. If the average fiber diameter of the carbon fibers 12 is 10 nm or more, the carbon fibers 12 are ensured to have an appropriate thickness, which increases the strength of the electrode catalyst layers 1 and 2 and enhances the effect of suppressing the occurrence of cracks. The average fiber length of the carbon fibers 12 is preferably in the range of 1 μm to 200 μm, and more preferably in the range of 5 μm to 100 μm. If the average fiber length of the carbon fibers 12 is within the above range, a structure in which the polymer electrolyte fibers 8 and the carbon fibers 12 are entangled is suitably formed in the electrode catalyst layers 1 and 2, thereby increasing the strength of the electrode catalyst layers 1 and 2 and improving the effect of suppressing the occurrence of cracks.

[0035] In the second configuration, the fiber materials, that is, the polymer electrolyte fibers 8 and the carbon fibers 12, are entangled and function as a support in the electrode catalyst layers 1 and 2, so that the occurrence of cracks in the electrode catalyst layers 1 and 2 is suppressed, as in the first configuration. The content of carbon fiber 12 is preferably in the range of 2 mass % to 50 mass % relative to the content of polymer electrolyte aggregate 7, more preferably in the range of 10 mass % to 40 mass %, and even more preferably in the range of 20 mass % to 40 mass %. When the content of polymer electrolyte fiber 8 is within the above numerical range, pores 9 of suitable size and in suitable amount can be formed in electrode catalyst layers 1 and 2.

[0036] Furthermore, the average fiber diameter of the carbon fibers 12 is preferably smaller than the average fiber diameter of the polymer electrolyte fibers 8, more preferably within the range of 10% to 70% of the average fiber diameter of the polymer electrolyte fibers 8, even more preferably within the range of 20% to 50%, and most preferably within the range of 30% to 40%. Furthermore, the average fiber length of the carbon fibers 12 is preferably shorter than the average fiber length of the polymer electrolyte fibers 8, more preferably within the range of 10% to 70% of the average fiber length of the polymer electrolyte fibers 8, even more preferably within the range of 20% to 50%, and most preferably within the range of 30% to 40%. When the average fiber diameter and average fiber length of the carbon fibers 12 are within the above numerical ranges, a suitable amount of pores 9 of a suitable size can be formed in the electrode catalyst layers 1 and 2 .

[0037] Here, even if the electrode catalyst layers 1 and 2 contain only carbon fibers 12 as the fiber material and do not contain polymer electrolyte fibers 8, it is possible to suppress the occurrence of cracks by forming a structure in which the carbon fibers 12 are entangled. However, since the carbon fibers 12 contribute only to electron conduction and do not contribute to proton conduction, in a form in which the fiber material contained in the electrode catalyst layers 1 and 2 is composed only of the carbon fibers 12, the proportion of the polymer electrolyte contained in the electrode catalyst layers 1 and 2 decreases, and the proton conductivity in the electrode catalyst layers 1 and 2 tends to decrease. In that case, it is possible to compensate for the proton conductivity by increasing the amount of the polymer electrolyte aggregates 7, but the number of pores 9 decreases, so that the gas diffusibility, drainage, etc. tend to decrease.

[0038] In contrast, in the present embodiment, the fiber material contained in the electrode catalyst layers 1 and 2 contains polymer electrolyte fibers 8, and therefore, compared to an embodiment in which the fiber material is only carbon fibers 12, it is possible to promote proton conduction in the electrode catalyst layers 1 and 2 while ensuring pores 9. To extract electrons generated by the electrode reaction, the electrode catalyst layers 1 and 2 also need to have electron conductivity. If the electrode catalyst layers 1 and 2 contain polymer electrolyte fibers 8 and carbon fibers 12 as fiber materials, the proton conductivity, electron conductivity, and the state of formation of pores 9 in the electrode catalyst layers 1 and 2 are each favorable, and it is possible to improve the output of the solid polymer electrolyte fuel cell.

[0039] The average fiber diameter and the average fiber length of the polymer electrolyte fibers 8 and the carbon fibers 12 can be measured, for example, by observing the cross section of the electrode catalyst layer using a scanning electron microscope. For example, the average fiber diameter is the average value of the maximum diameter of each fiber contained in three or more measurement areas of 30 μm×30 μm in the cross section. Also, for example, the average fiber length is the average value of the maximum length of each fiber contained in three or more measurement areas of 30 μm×30 μm in the cross section.

[0040] 4 is an exploded perspective view showing an example of the configuration of a unit cell 20 of a polymer electrolyte fuel cell equipped with a membrane electrode assembly 10. An air electrode side gas diffusion layer 17C and a fuel electrode side gas diffusion layer 17A are disposed facing the air electrode side electrode catalyst layer 1 and the fuel electrode side electrode catalyst layer 2 of the membrane electrode assembly 10, respectively. Furthermore, a laminate composed of the membrane electrode assembly 10, the air electrode side gas diffusion layer 17C, and the fuel electrode side gas diffusion layer 17A is sandwiched between an air electrode side separator 18C and a fuel electrode side separator 18A to form a unit cell 20. A pair of separators 18A, 18C is formed from a material that is both electrically conductive and gas impermeable, and is provided with an air electrode side gas flow path 19C for circulating a reactant gas, which is arranged facing the air electrode side gas diffusion layer 17C, and a fuel electrode side gas flow path 19A for circulating a reactant gas, which is arranged facing the fuel electrode side gas diffusion layer 17A.

[0041] In this single cell 20, an oxidant such as air or oxygen is supplied through the air electrode side gas flow passage 19C of the air electrode side separator 18C and through the air electrode side gas diffusion layer 17C to the membrane electrode assembly 10, and a fuel gas containing hydrogen or an organic fuel is supplied through the fuel electrode side gas flow passage 19A of the fuel electrode side separator 18A and through the fuel electrode side gas diffusion layer 17A to the membrane electrode assembly 10, thereby causing the electrochemical reactions (reaction 1) and (reaction 2) described above in the membrane electrode assembly 10 and generating electricity. The unit cell 20 of the polymer electrolyte fuel cell may be used in the state of the unit cell shown in FIG. 4, or a plurality of unit cells 20 may be stacked and connected in series to be used as one fuel cell.

[0042] The membrane electrode assembly 10 may be configured to include the above-mentioned gas diffusion layers 17A, 17C in addition to the polymer electrolyte membrane 3 and the electrode catalyst layers 1, 2. The solid polymer fuel cell 20 may include the membrane electrode assembly 10 having a gasket 4 on at least one surface of the polymer electrolyte membrane 3, the gasket 4 having a function of preventing gases and the like supplied to the electrode catalyst layers 1, 2 from leaking from the fuel cell (see FIG. 1). The gasket 4 may be disposed so as to surround the outer periphery of the laminate consisting of the polymer electrolyte membrane 3 and the electrode catalyst layers 1, 2.

[0043] (Method of manufacturing electrode catalyst layer) The electrode catalyst layers 1 and 2 of this embodiment can be manufactured by preparing a slurry for the electrode catalyst layers, applying it to a substrate or the like, and drying it. The electrode catalyst layer slurry is produced by adding a powdered polymer electrolyte or a polymer electrolyte solution in which a powdered polymer electrolyte is dissolved or dispersed, a catalyst substance-supporting carbon body 11, and polymer electrolyte fibers 8 to a solvent and mixing them. The polymer electrolyte fibers 8 are formed, for example, by using an electrospinning method. When forming the electrode catalyst layers 1 and 2 of the second configuration, carbon fibers 12 are further added to the electrode catalyst layer slurry.

[0044] The solvent for the electrode catalyst layer slurry is not particularly limited, but it is preferable that the solvent can disperse or dissolve the polymer electrolyte. Commonly used solvents include water, alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, and tert-butyl alcohol, ketones such as acetone, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isobutyl ketone, methyl amyl ketone, pentanone, heptanone, cyclohexanone, methylcyclohexanone, acetonylacetone, diethyl ketone, dipropyl ketone, and diisobutyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, and diethylene glycol dimethyl ether. Other examples of the solvent that may be used include ethers such as ether, anisole, methoxytoluene, diethyl ether, dipropyl ether, and dibutyl ether, amines such as isopropylamine, butylamine, isobutylamine, cyclohexylamine, diethylamine, and aniline, esters such as propyl formate, isobutyl formate, amyl formate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, pentyl acetate, isopentyl acetate, methyl propionate, ethyl propionate, and butyl propionate, and other esters such as acetic acid, propionic acid, dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. Examples of glycol and glycol ether solvents include ethylene glycol, diethylene glycol, propylene glycol, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diacetone alcohol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol.

[0045] The substrate used when forming the electrode catalyst layers 1 and 2 may be, for example, a transfer substrate which is peeled off after the electrode catalyst layers 1 and 2 are transferred to the polymer electrolyte membrane 3. The transfer substrate may be, for example, a resin film. Alternatively, the substrate used when forming the electrode catalyst layers 1 and 2 may be the polymer electrolyte membrane 3 or the gas diffusion layers 17A and 17C.

[0046] Examples of the method for applying the electrode catalyst layer slurry to the substrate include, but are not limited to, a doctor blade method, a die coating method, a dipping method, a screen printing method, a laminator roll coating method, and a spray method. Examples of the method for drying the slurry for the electrode catalyst layer applied to the substrate include hot air drying and IR drying. The drying temperature for the slurry for the electrode catalyst layer may be within a range of 40° C. to 200° C., and preferably within a range of 40° C. to 120° C. The drying time for the slurry for the electrode catalyst layer may be within a range of 0.5 minutes to 1 hour, and preferably within a range of 1 minute to 30 minutes.

[0047] When a transfer substrate or gas diffusion layers 17A, 17C are used as the substrates used in forming the electrode catalyst layers 1, 2, the electrode catalyst layers 1, 2 are bonded to the polymer electrolyte membrane 3 by thermocompression bonding. When a transfer substrate is used as the substrate, the transfer substrate is peeled off from the electrode catalyst layers 1, 2 after bonding the electrode catalyst layers 1, 2. When gas diffusion layers 17A, 17C are used as the substrates, peeling off the substrate is not necessary. In a manufacturing method using a polymer electrolyte membrane 3 as the substrate for forming the electrode catalyst layers 1 and 2, the electrode catalyst layers 1 and 2 are formed directly on the surfaces of the polymer electrolyte membrane 3. This increases the adhesion between the polymer electrolyte membrane 3 and the electrode catalyst layers 1 and 2, and also prevents the electrode catalyst layers 1 and 2 from collapsing (the pores 9 from collapsing) because no pressure is required to bond the electrode catalyst layers 1 and 2. Therefore, it is preferable to use the polymer electrolyte membrane 3 as the substrate for forming the electrode catalyst layers 1 and 2.

[0048] Here, since the polymer electrolyte membrane 3 generally has a characteristic that the degree of swelling and shrinking is large, when the polymer electrolyte membrane 3 is used as a substrate, the volume change of the substrate in the drying process of the coating film that becomes the electrode catalyst layers 1 and 2 is large compared to when a transfer substrate or a gas diffusion layer 17A or 17C is used as a substrate. Therefore, if the electrode catalyst layer does not contain a fiber material as in the conventional configuration, cracks are likely to occur in the electrode catalyst layer. In contrast, in the electrode catalyst layers 1 and 2 of this embodiment, even if the volume of the substrate, the polymer electrolyte membrane 3, changes significantly in the process of producing the electrode catalyst layers 1 and 2, the occurrence of cracks is suppressed by the inclusion of a fiber material, so that a manufacturing method using the polymer electrolyte membrane 3 as a substrate for forming the electrode catalyst layers 1 and 2 can be used. The polymer electrolyte fuel cell 20 is manufactured by assembling the gas diffusion layers 17A, 17C and the separators 18A, 18C to the membrane electrode assembly 10, and further providing a gas supply mechanism and the like.

[0049] [Example] Next, an embodiment based on the present invention will be described. [Example 1] 20 g of platinum-supported carbon (TEC10E50E, Tanaka Kikinzoku) was placed in a container, water was added and mixed, and then polymer electrolyte fibers (acid-doped polybenzoazoles), 1-propanol, and polymer electrolyte (Nafion (registered trademark) dispersion, Wako Pure Chemical Industries) were added and stirred to obtain a slurry for an electrode catalyst layer. The average fiber diameter of the polymer electrolyte fibers was 400 nm, and the average fiber length was 30 μm. In this example, the average fiber diameter is rounded off to the nearest one place, and the average fiber length is rounded off to the nearest one decimal place. The mass of the polymer electrolyte was 100% by mass relative to the mass of the carbon particles, the mass of the polymer electrolyte fibers was 10% by mass relative to the mass of the carbon particles, the proportion of water in the dispersion medium was 50% by mass, and the solid content concentration was 10% by mass to prepare a slurry for an electrode catalyst layer.

[0050] The obtained electrode catalyst layer slurry was applied to a polymer electrolyte membrane (Nafion212, manufactured by DuPont) by die coating and dried in an oven at 80° C. to obtain a membrane electrode assembly of Example 1 including a pair of electrode catalyst layers and a polymer electrolyte membrane. Furthermore, this membrane electrode assembly was sandwiched between two gas diffusion layers (SIGRACET 29BC: manufactured by SGL), and a solid polymer electrolyte fuel cell of Example 1 was constructed using a JARI standard cell.

[0051] [Example 2] An electrode catalyst layer and a membrane electrode assembly for a polymer electrolyte fuel cell of Example 2 were obtained in the same manner as in Example 1, except that the mass of the polymer electrolyte fibers was 30 mass % relative to the mass of the carbon particles.

[0052] [Example 3] An electrode catalyst layer and a membrane electrode assembly for a polymer electrolyte fuel cell of Example 3 were obtained in the same manner as in Example 1, except that a slurry for an electrode catalyst layer used in Example 3 was obtained by further adding and stirring carbon fibers (fiber diameter: approximately 150 nm, fiber length: approximately 10 μm) to the slurry for an electrode catalyst layer prepared in Example 1 so that the mass of the carbon fibers was 10 mass % relative to the mass of the carbon particles.

[0053] [Comparative Example 1] An electrode catalyst layer and a membrane electrode assembly for a polymer electrolyte fuel cell of Comparative Example 1 were obtained in the same manner as in Example 1, except that the mass of the polymer electrolyte fibers was 50 mass % relative to the mass of the carbon particles.

[0054] [Comparative Example 2] An electrode catalyst layer and a membrane electrode assembly for a polymer electrolyte fuel cell of Comparative Example 2 were obtained in the same manner as in Example 1, except that the polymer electrolyte fibers were not added.

[0055] [Comparative Example 3] An electrode catalyst layer and a membrane electrode assembly for a polymer electrolyte fuel cell of Comparative Example 3 were obtained in the same manner as in Example 3, except that the polymer electrolyte fibers were not added.

[0056] [Power generation performance evaluation] For the measurement of power generation performance, in accordance with the "Cell Evaluation and Analysis Protocol" published by the New Energy and Industrial Technology Development Organization (NEDO), a JARI standard cell was used as the evaluation unit cell, in which gas diffusion layers, gaskets, and separators were placed on both sides of the membrane electrode assembly and clamped to a specified surface pressure. Then, IV measurement (standard conditions) described in the "Cell Evaluation and Analysis Protocol" was performed. The measurement results of the power generation performance of the evaluation single cells using the electrode catalyst layers of Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 1. Regarding the power generation performance, when the current was 30 A or more at a voltage of 0.6 V, it was rated as "○", and when it was less than 30 A, it was rated as "×". If the evaluation result was "○", there was no problem in using the power generation performance.

[0057] [Elemental analysis evaluation of electrode catalyst layer] After carrying out the above-mentioned power generation performance evaluation, elemental analysis by energy dispersive X-ray analysis (EDX) was carried out on each of the electrode catalyst layers of Examples 1 to 3 and Comparative Examples 1 to 3. The evaluation results are shown in Fig. 5. Fig. 5 is a graph in which the ratio (P / Pt) of the amount of P (phosphorus) to the amount of Pt (platinum) obtained by elemental analysis by energy dispersive X-ray analysis (EDX) on the cross section of each of the electrode catalyst layers of Examples 1 to 3 and Comparative Examples 1 to 3 is plotted on the vertical axis.

[0058] [Crack occurrence evaluation] For the membrane electrode assemblies of each Example and Comparative Example, the surface of the electrode catalyst layer was observed under a microscope (magnification: 200 times) to confirm the occurrence of cracks, which is one factor in reducing the durability of the membrane electrode assembly. In this evaluation, the occurrence of cracks with a length of 10 μm or more was marked as "X", and the absence of cracks with a length of 10 μm or more was marked as "O". The evaluation results are shown in Table 1.

[0059] [Durability evaluation] The durability was measured by the humidity cycle test described in the above-mentioned "Cell Evaluation and Analysis Protocol", using the same evaluation cell as that used for the measurement of power generation performance. Regarding durability, a battery was rated as "◯" when the power generation performance after the 10,000 cycle test was 70% or more of the power generation performance before the cycle test, and "×" when it was lower than 70%. The evaluation results are shown in Table 1.

[0060] [Table 1]

[0061] As shown in Table 1, the power generation performance was rated as "good" in Examples 1 to 3. That is, in Examples 1 to 3, membrane electrode assemblies capable of forming fuel cells with excellent power generation performance were obtained.

[0062] In Comparative Example 1, the occurrence of cracks is suppressed by adding polymer electrolyte fibers. On the other hand, the power generation performance was rated as "x". This suggests that the large amount of polymer electrolyte fibers added prevents pores from being suitably formed in the electrode catalyst layer. The P / Pt ratio in this case is 3.5, which suggests that high power generation performance can be obtained when the P / Pt ratio is approximately 3.0 or less, as compared with the power generation performance in Example 2, in which the P / Pt ratio is 2.8. In Comparative Example 2, cracks occurred because the electrode catalyst layer did not contain polymer electrolyte fibers (fibrous material). In Comparative Example 3, the occurrence of cracks was suppressed because the electrode catalyst layer contained carbon fibers. On the other hand, the power generation performance was rated as "x". This suggests that sufficient proton conductivity was not obtained compared to Examples 1 and 2 because the electrode catalyst layer did not contain polymer electrolyte fibers.

[0063] As described above, according to the present embodiment, in an electrode catalyst layer for a polymer fuel cell including at least carbon particles supporting a catalyst, a polymer electrolyte, and polymer electrolyte fibers, preferably including carbon fibers, when the amount of P and the amount of Pt obtained by elemental analysis by energy dispersive X-ray analysis (EDX) in the cross-section of the electrode catalyst layer satisfy the following formula (1), both improvement of proton conductivity in the electrode catalyst layer and suitable formation of pores are satisfied, so there is no (extremely few) occurrence of cracks, which is one of the causes of durability degradation of the membrane electrode assembly, and high power generation performance is exhibited. 0 < P / Pt ≦ 3.0 ··· Formula (1)

Industrial Applicability

[0064] The present invention has a remarkable effect on improving the output during power generation of a fuel cell, and thus has high industrial utility value. For example, it is extremely suitable for application to a polymer electrolyte fuel cell.

Explanation of Signs

[0065] 1 Air electrode side electrode catalyst layer 2 Fuel electrode side electrode catalyst layer 3 Polymer electrolyte membrane 4 Gasket 5 Carbon particles 6 Catalyst substance (catalyst particles, catalyst) 7 Aggregate 8 Polymer electrolyte fibers 9 Pore 10 Membrane electrode assembly 11 Catalyst substance-supported carbon body 12 Carbon fiber 20 Single cell (polymer electrolyte fuel cell) 17A Fuel electrode side gas diffusion layer 17C Air electrode side gas diffusion layer 18A Fuel electrode side separator 18C Air electrode side separator 19A Fuel electrode side gas flow path 19C Air electrode side gas flow path

Claims

1. An electrode catalyst layer including at least a catalyst, carbon particles carrying the catalyst, a polymer electrolyte, and a fibrous material, The amount of phosphorus (P) and the amount of platinum (Pt) in the electrode catalyst layer, which are obtained by elemental analysis using energy dispersive X-ray analysis (EDX), satisfy the following formula (1): The electrode catalyst layer is characterized in that the fibrous material is composed of a polymer electrolyte. 0<P / Pt≦3.0...Formula (1)

2. 2. The electrode catalyst layer according to claim 1, wherein the average fiber diameter of the fibrous material is within a range of 100 nm or more and 500 nm or less.

3. 3. The electrode catalyst layer according to claim 1, wherein the average fiber length of the fibrous material is within a range of 1 μm or more and 150 μm or less.

4. The electrode catalyst layer according to claim 1 , further comprising carbon fibers.

5. A polymer electrolyte membrane; a pair of electrode catalyst layers sandwiching the polymer electrolyte membrane; A membrane electrode assembly, wherein at least one of the pair of electrode catalyst layers is the electrode catalyst layer according to claim 1 .

6. A polymer electrolyte fuel cell comprising the membrane electrode assembly according to claim 5 and a pair of separators sandwiching the membrane electrode assembly.

Citation Information

Patent Citations

  • Solid polymer fuel cell

    JP2003115299A

  • Electrode catalyst layer, membrane electrode assembly, and solid polymer-type fuel cell

    WO2019069789A1

  • Membrane-electrode assembly for fuel cells and solid polymer fuel cell

    WO2020075777A1

  • Electrode catalyst layer, membrane electrode assembly, and solid polymer fuel cell

    WO2020138433A1