Method for manufacturing resin-coated metal foil, method for manufacturing laminated board, method for manufacturing printed wiring board, and method for manufacturing semiconductor package

By applying pressure to resin-coated metal foils using opposing rolls, the warpage issue is addressed, improving productivity and material flexibility in resin-coated metal foil manufacturing.

JP7567541B2Active Publication Date: 2024-10-16RESONAC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021024449
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-18
Publication Date
2024-10-16
Estimated Expiration
2041-02-18

AI Technical Summary

Technical Problem

Existing methods for manufacturing resin-coated metal foils suffer from warpage issues, which reduce productivity and limit material selection flexibility due to the need for temperature-controlled drying ovens.

Method used

Applying pressure to resin-coated metal foils using a pair of opposing rolls, where one roll contacts the metal foil and the other contacts the resin layer, to correct warpage during the manufacturing process.

Benefits of technology

This method effectively reduces warpage in resin-coated metal foils, enhancing productivity and allowing for greater material flexibility while maintaining excellent handling properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567541000003
    Figure 0007567541000003
  • Figure 0007567541000004
    Figure 0007567541000004
  • Figure 0007567541000001
    Figure 0007567541000001
Patent Text Reader

Abstract

To provide a method for manufacturing a metallic foil with a resin which is excellent in productivity and is suppressed in warpage, a method for manufacturing a laminated plate using a metallic foil with a resin manufactured by the method for manufacturing a metallic foil with a resin, a method for manufacturing a printed wiring board and a method for manufacturing a semiconductor package.SOLUTION: There is provided a method for manufacturing a metallic foil with a resin having a metallic foil and a resin layer formed on one surface side of the metallic foil using a thermosetting resin composition, the method includes warpage correction processing of reducing warpage of the metallic foil with the resin, wherein the warpage correction processing is a processing for pressurizing the metallic foil with the resin before the warpage correction processing in which the resin layer is formed on one surface side of the metallic foil by passing the metallic foil with the resin through a gap between a pair of opposite rolls, a roll on the side contacting the metallic foil is a resin roll out of the pair of rolls, and the roll on the side contacting the resin layer is a metallic roll. There are also provided a method for manufacturing a laminated plate, a method for manufacturing a printed wiring board and a method for manufacturing a semiconductor package using a metallic foil with a resin manufactured by the method for manufacturing a metallic foil with a resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present embodiment relates to a method for producing a resin-coated metal foil, a method for producing a laminate, a method for producing a printed wiring board, and a method for producing a semiconductor package. [Background technology]

[0002] 2. Description of the Related Art With the trend toward smaller size and higher performance of electronic devices in recent years, there is a demand for printed wiring boards to have higher wiring density and integration than ever before, as well as thinner substrates. In order to meet these requirements, resin-coated metal foils, which do not use fiber substrates such as glass cloth and have a resin layer formed on a metal foil, are used in the manufacture of printed wiring boards. Since resin-coated metal foils do not contain fiber substrates, they can be made thin, and since they have excellent insulating layer smoothness and fine wiring properties, they are also suitable for high wiring density and high integration. Furthermore, since they do not contain glass cloth, they have excellent dielectric properties and are used in printed wiring boards that require high frequency compatibility.

[0003] The resin-attached metal foil is usually produced by applying a thermosetting resin composition containing a solvent onto a metal foil, and then drying the solvent by heating. At this time, the volume of the thermosetting resin composition shrinks due to the evaporation of the solvent and the B-stage of the thermosetting resin, and the resin-attached metal foil warps toward the resin layer. The occurrence of such warping is a factor that reduces the productivity when manufacturing a printed wiring board using the resin-attached metal foil, so it is desirable to suppress it.

[0004] Patent Document 1 discloses a method for suppressing warping of the ends of resin-coated metal foil, in which a thermosetting resin composition is applied to the surface of the metal foil and then passed through a drying oven to heat and dry it to B stage, characterized in that the heating temperature at a position that is 80% of the total length from the entrance to the exit of the drying oven is 100°C or more higher than the heating temperature near the entrance of the drying oven, and the heating temperature from this position to the exit is 30°C or more lower. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-025624 A Summary of the Invention [Problem to be solved by the invention]

[0006] According to the technology of Patent Document 1, it is said that it is possible to manufacture a resin-coated metal foil with reduced warping at the ends. However, the technology of Patent Document 1 requires a drying furnace capable of multi-stage temperature adjustment, which requires capital investment. In addition, there is a restriction that only materials that are compatible with the drying conditions in the manufacturing method of Patent Document 1 can be used, so there is little freedom in selecting the materials to be used. Therefore, there is a need for a manufacturing method of resin-coated metal foil with reduced warping that is more productive.

[0007] In view of the current situation, the present embodiment aims to provide a method for manufacturing a resin-coated metal foil that is highly productive and suppresses warping, as well as a method for manufacturing a laminate using the resin-coated metal foil manufactured by the manufacturing method, a method for manufacturing a printed wiring board, and a method for manufacturing a semiconductor package. [Means for solving the problem]

[0008] As a result of further investigations aimed at solving the above-mentioned problems, the inventors discovered that in a method for manufacturing a resin-coated metal foil, the above-mentioned problems can be solved by subjecting the resin-coated metal foil to a pressurization treatment under specific conditions. That is, the present embodiment relates to the following [1] to

[10] . [1] A method for producing a resin-coated metal foil having a metal foil and a resin layer formed on one side of the metal foil using a thermosetting resin composition, comprising: A warping correction treatment is included to reduce warping of the resin-coated metal foil, The warpage correction treatment is A process for pressing a resin-coated metal foil having a resin layer formed on one side of the metal foil before warping correction by passing the metal foil through a gap between a pair of opposing rolls, The method for producing a resin-coated metal foil, wherein, of the pair of rolls, the roll that comes into contact with the metal foil is a resin roll, and the roll that comes into contact with the resin layer is a metal roll. [2] The method for producing a resin-coated metal foil according to the above [1], wherein the metal foil is a copper foil. [3] The method for producing a resin-coated metal foil according to the above [1] or [2], wherein the metal foil has a thickness of 0.1 to 35 μm. [4] The method for producing a resin-coated metal foil according to any one of the above [1] to [3], wherein the resin layer has a thickness of 5 to 70 μm. [5] The method for producing a resin-coated metal foil according to any one of the above [1] to [4], wherein the roll load in the warping correction treatment is 0.3 to 10 tons. [6] The method for producing a resin-coated metal foil according to any one of the above [1] to [5], wherein the resin roll and the metal roll each have a roll diameter of 100 to 500 mm. [7] The method for producing a resin-coated metal foil according to any one of the above [1] to [6], wherein the feed speed of the pair of rolls is 1.0 to 15.0 m / min. [8] A method for producing a laminate, comprising a step of forming an insulating layer using a resin-coated metal foil obtained by the method for producing a resin-coated metal foil according to any one of the above [1] to [7]. [9] A method for producing a printed wiring board, comprising a step of forming an insulating layer using a resin-coated metal foil obtained by the method for producing a resin-coated metal foil according to any one of the above [1] to [7].

[10] A method for manufacturing a semiconductor package, comprising mounting a semiconductor element on a printed wiring board obtained by the method for manufacturing a printed wiring board according to [9] above. Effect of the Invention

[0009] According to the present embodiment, it is possible to provide a method for manufacturing a resin-coated metal foil that is highly productive and suppresses warping, as well as a method for manufacturing a laminate using the resin-coated metal foil manufactured by the manufacturing method, a method for manufacturing a printed wiring board, and a method for manufacturing a semiconductor package. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic diagram showing one embodiment of a resin-coated metal foil according to the present embodiment. FIG. [Diagram 2] FIG. 2 is a schematic diagram showing another aspect of the resin-coated metal foil of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, the numerical range indicated using "~" indicates a numerical range including the numerical value before "~" as the minimum value and the numerical value after "~" as the maximum value. For example, the expression "X to Y" (X and Y are real numbers) means a range of values ​​that is equal to or greater than X and equal to or less than Y. In this specification, the expression "equal to or greater than X" means X and a value that exceeds X, and this also applies when the values ​​are different. In this specification, the expression "equal to or less than Y" means Y and a value that is less than Y. In the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with values ​​shown in the examples. Unless otherwise specified, each of the components and materials exemplified in this specification may be used alone or in combination of two or more kinds. In this specification, the content of each component in a resin composition means, when a plurality of substances corresponding to each component are present in the resin composition, the total amount of the plurality of substances present in the resin composition, unless otherwise specified. In this specification, the term "resin composition" includes a mixture of the components described below and a semi-cured product of the mixture (so-called B-stage product). Any combination of the descriptions in this specification is also included in this embodiment. The action mechanism described in this specification is merely speculation, and does not limit the mechanism by which the resin composition according to the present embodiment exerts its effects.

[0012] [Method of manufacturing resin-coated metal foil] The method for producing a resin-coated metal foil according to the present embodiment includes the steps of: A method for producing a resin-coated metal foil having a metal foil and a resin layer formed on one surface of the metal foil using a thermosetting resin composition, comprising: A warping correction treatment is included to reduce warping of the resin-coated metal foil, The warpage correction treatment is This is a method for producing a resin-coated metal foil, in which a resin layer is formed on one side of the metal foil before warp correction processing, is pressed by passing it between a gap between a pair of opposing rolls, and of the pair of rolls, the roll that comes into contact with the metal foil is a resin roll, and the roll that comes into contact with the resin layer is a metal roll.

[0013] According to the manufacturing method of the resin-coated metal foil of the present embodiment, it is possible to manufacture a resin-coated metal foil with suppressed warping. Although the reason for this is unclear, it is believed that the warping correction treatment included in the manufacturing method of the present embodiment contributes to reducing the warping of the resin-coated metal foil. In order to correct the warpage of the resin-coated metal foil, it is necessary to apply a shear force to the resin layer near the contact interface with the metal foil to displace the resin layer in the direction of elongation. In addition, the amount of displacement of the resin layer must be relatively larger than the amount of displacement of the metal foil. In the manufacturing method of the resin-coated metal foil of this embodiment, the roll on the side in contact with the metal foil is a resin roll, and the roll on the side in contact with the resin layer is a metal roll. This makes it possible to increase the amount of displacement of the resin layer, particularly near the interface with the metal foil, which is thought to cause plastic deformation of the resin layer and effectively reduce warping.

[0014] Hereinafter, each member constituting the resin-coated metal foil produced by the production method of this embodiment will be described, and then the warpage correction treatment will be described in detail.

[0015] 1 is a schematic diagram of a resin-coated metal foil 10, which is one embodiment of the resin-coated metal foil obtained by the manufacturing method of this embodiment. The resin-coated metal foil 10 has a configuration in which a resin layer 2 is formed on one surface of a metal foil 1. 2 is a schematic diagram of a resin-coated metal foil 20, which is another embodiment of the resin-coated metal foil obtained by the manufacturing method of this embodiment. The resin-coated metal foil 20 has a structure in which a resin layer 2 is formed on one surface of a metal foil 1. Furthermore, on the surface of the metal foil 1 opposite to the resin layer 2, a release layer 3 and a carrier foil 4 are laminated in this order. The resin-coated metal foil obtained by the production method of this embodiment may have the metal foil 1 and the resin layer 2 laminated directly thereon, or may have another layer between the metal foil 1 and the resin layer 2.

[0016] <Metal foil> Examples of the metal foil include copper foil, tin foil, tin-lead alloy foil, nickel foil, etc. Among these, copper foil is preferable. The copper foil preferably has a copper content of 95% by mass or more. From the viewpoint of use in semiconductor packages, the metal foil is preferably one that complies with the JIS standard (electrolytic copper foil for printed wiring boards: JIS C6512, rolled copper foil for printed wiring boards: JIS C6513) or the IPC standard (IPC 4562 standard Grades 1, 2, 3).

[0017] The surface of the metal foil on which the resin layer is to be formed may be subjected to a roughening treatment from the viewpoint of adhesion. The roughening treatment can be carried out by forming roughening particles on the surface of the metal foil. The roughening particles are preferably, for example, electrodeposited particles made of a simple substance selected from copper, nickel, phosphorus, tungsten, arsenic, molybdenum, chromium, cobalt, and zinc, or electrodeposited particles made of an alloy containing at least one of these elements. The roughening particles may be used alone or in combination of two or more kinds.

[0018] In addition to the above-mentioned roughening treatment, the metal foil may have secondary particles, tertiary particles, an anti-rust layer, a heat-resistant layer, or the like formed of, for example, a simple substance selected from nickel, cobalt, copper, and zinc, or an alloy containing any one or more of these. In addition to the above layers, the surface may be subjected to a surface treatment such as a chromate treatment or a silane coupling treatment.

[0019] The thickness of the metal foil is not particularly limited and may be appropriately adjusted depending on the use of the resin-coated metal foil, but is preferably 0.1 to 35 μm, more preferably 0.3 to 15 μm, even more preferably 0.5 to 5 μm, and particularly preferably 1 to 2 μm. When the thickness of the metal foil is equal to or greater than the above lower limit, the resin-coated metal foil obtained by the manufacturing method of the present embodiment tends to be easier to handle. On the other hand, when the thickness of the metal foil is equal to or greater than the above lower limit, the resin-coated metal foil obtained by the manufacturing method of the present embodiment tends to be more suitable for making the substrate thinner.

[0020] <Carrier foil> The carrier foil corresponds to a support provided as necessary to improve the handling property when the metal foil is thin. Therefore, the carrier foil is removed during the manufacturing process of the printed wiring board, etc. In this embodiment, the carrier foil is not included in the metal foil constituting the resin-coated metal foil. Examples of the carrier foil include copper foil, aluminum foil, nickel foil, etc. Among these, copper foil is preferred.

[0021] The thickness of the carrier foil is preferably 5 to 50 μm, more preferably 10 to 35 μm, and further preferably 10 to 25 μm, from the viewpoints of improving the handleability of the resin-coated metal foil and production costs. When the thickness of the carrier foil is equal to or greater than the lower limit, the handleability of the resin-coated metal foil obtained by the manufacturing method of the present embodiment tends to be further improved. On the other hand, when the thickness of the carrier foil is equal to or less than the upper limit, the cost of the resin-coated metal foil obtained by the manufacturing method of the present embodiment tends to be further reduced.

[0022] <Release layer> The release layer is a layer that is provided between the metal foil and the carrier layer as needed to facilitate peeling of the carrier foil from the metal foil. Note that in this embodiment, the release layer is not included in the metal foil that constitutes the resin-coated metal foil. The release layer may be, for example, a layer containing one or more metals selected from chromium, nickel, cobalt, iron, molybdenum, titanium, tungsten, phosphorus, copper, and aluminum. These metals may be alloys, hydrates, oxides, etc. The release layer may be a single layer or multiple layers. The release layer can be formed by, for example, wet plating such as electroplating, electroless plating, and immersion plating; or dry plating such as sputtering, chemical vapor deposition (CVD), and physical vapor deposition (PDV).

[0023] <Resin layer> The resin layer is a layer formed on one side of the metal foil using a thermosetting resin composition, and is generally used as an insulating layer in applications such as printed wiring boards. The thickness of the resin layer may be appropriately adjusted depending on the application of the resin-coated metal foil, and is not particularly limited, but is preferably 5 to 70 μm, more preferably 10 to 50 μm, and further preferably 15 to 30 μm. When the thickness of the resin layer is equal to or greater than the lower limit, the insulating properties of the insulating layer formed from the resin-coated metal foil obtained by the manufacturing method of this embodiment tend to be further improved. On the other hand, when the thickness of the resin layer is equal to or less than the upper limit, the resin-coated metal foil obtained by the manufacturing method of this embodiment tends to be more suitable for making the substrate thinner.

[0024] The composition of the thermosetting resin composition used to form the resin layer may be appropriately determined depending on the application of the resin-coated metal foil, etc. Examples of the thermosetting resin contained in the thermosetting resin composition include epoxy resin, phenol resin, unsaturated imide resin, cyanate resin, isocyanate resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin, silicone resin, triazine resin, melamine resin, etc. Among these, epoxy resin and unsaturated imide resin are preferred, unsaturated imide resin is more preferred, and maleimide resin is even more preferred. The maleimide resin may be a prepolymer obtained by Michael addition of a maleimide compound and a diamine compound. The thermosetting resin may be used alone or in combination of two or more kinds.

[0025] The thermosetting resin composition may contain, in addition to the thermosetting resin, for example, an inorganic filler, a curing agent, a curing accelerator, a thermoplastic resin, an elastomer, a flame retardant, other additives, etc. Each of these may be used alone or in combination of two or more. Examples of inorganic fillers include silica, alumina, talc, mica, aluminum hydroxide, magnesium hydroxide, calcium carbonate, aluminum borate, and borosilicate glass. Examples of the curing agent include phenol compounds, amine compounds, acid anhydrides, etc. It is preferable to appropriately select the curing agent depending on the type of the thermosetting resin. Examples of the curing accelerator include imidazoles and derivatives thereof; organic phosphorus compounds; secondary amines, tertiary amines, and quaternary ammonium salts. Examples of the thermoplastic resin and elastomer include polyphenylene ether and its derivatives, polybutadiene and its derivatives, and styrene-based thermoplastic elastomers. Examples of the flame retardant include phosphorus-based flame retardants, metal hydrates, and halogen-based flame retardants. Other additives include ultraviolet absorbers such as benzotriazoles; antioxidants such as hindered phenol antioxidants and styrenated phenol antioxidants; photopolymerization initiators such as benzophenones, benzil ketals, and thioxanthone; fluorescent brightening agents such as stilbene derivatives, urea compounds, and adhesion improvers such as silane coupling agents.

[0026] The content of the thermosetting resin in the thermosetting resin composition is preferably 30 to 95 parts by mass, more preferably 50 to 90 parts by mass, and even more preferably 70 to 85 parts by mass, per 100 parts by mass of the total of the resin components in the thermosetting resin composition. The content of the thermoplastic resin in the thermosetting resin composition is preferably 1 to 30 parts by mass, more preferably 3 to 20 parts by mass, and even more preferably 5 to 15 parts by mass, per 100 parts by mass of the total of the resin components in the thermosetting resin composition. The content of the elastomer in the thermosetting resin composition is preferably 1 to 30 parts by mass, more preferably 3 to 20 parts by mass, and further preferably 5 to 15 parts by mass, per 100 parts by mass of the total of the resin components in the thermosetting resin composition. The content of the curing accelerator in the thermosetting resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 2 parts by mass, and even more preferably 0.3 to 1 part by mass, per 100 parts by mass of the total of the resin components in the thermosetting resin composition. The content of the inorganic filler in the thermosetting resin composition is preferably 50 to 300 parts by mass, more preferably 100 to 250 parts by mass, and even more preferably 150 to 200 parts by mass, per 100 parts by mass of the total of the resin components in the thermosetting resin composition. The content of the flame retardant in the thermosetting resin composition is preferably 10 to 80 parts by mass, more preferably 20 to 60 parts by mass, and even more preferably 30 to 50 parts by mass, per 100 parts by mass of the total of the resin components in the thermosetting resin composition. In this specification, the term "resin component" refers to a resin and a compound that forms a resin through a curing reaction. For example, thermosetting resins, thermoplastic resins, elastomers, etc. correspond to the resin component. Furthermore, when the thermosetting resin composition contains, as optional components, a resin or a compound that forms a resin through a curing reaction in addition to the above components, these optional components are also included in the resin component. On the other hand, curing accelerators, inorganic fillers and flame retardants are not included in the resin component.

[0027] The thermosetting resin composition may contain an organic solvent to facilitate layer formation. Hereinafter, the thermosetting resin composition containing an organic solvent may be referred to as a "resin varnish." Examples of organic solvents include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; acetate-based solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitol-based solvents such as cellosolve and butyl carbitol; aromatic hydrocarbon-based solvents such as toluene and xylene; and amide-based solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. The organic solvent may be used alone or in combination of two or more. Among these, toluene and methyl isobutyl ketone are preferred from the viewpoint of solubility.

[0028] When the thermosetting resin composition contains an organic solvent, the solid content thereof is not particularly limited, but from the viewpoint of facilitating coatability and control of the thickness of the resin layer, it is preferably 30 to 80 mass%, more preferably 40 to 75 mass%, and even more preferably 45 to 70 mass%. In this embodiment, the solid content refers to a non-volatile resin component, and includes those that are liquid, syrup-like, or waxy at room temperature around 25° C., and does not necessarily mean that they are solid.

[0029] The thermosetting resin composition can be produced by blending each of the above components with an organic solvent as necessary and mixing them using a known stirrer or the like. When mixing, each component may be dissolved or dispersed while being stirred. In addition, the order of mixing the raw materials, mixing temperature, mixing time, and other conditions are not particularly limited and may be set arbitrarily depending on the type of raw materials, etc. Next, the manufacturing method of this embodiment will be described.

[0030] <Preparation of resin-coated metal foil before warping treatment> The warp straightening treatment in the manufacturing method of this embodiment is a treatment in which the resin-coated metal foil before warp straightening treatment, which has the resin layer formed on one side of the metal foil, is pressed by passing it through the gap between a pair of opposing rolls.

[0031] The resin-coated metal foil before warpage correction treatment can be obtained, for example, by applying a resin varnish onto the metal foil and then drying it by heating. It is preferable that the heat drying removes the organic solvent contained in the resin varnish and also converts the thermosetting resin into a B-stage. The heating temperature in the heat drying is preferably 80 to 200°C, more preferably 90 to 170°C, and even more preferably 100 to 150°C, from the viewpoints of productivity and appropriately bringing the thermosetting resin into the B-stage. The heating time in the heat drying is preferably 0.5 to 30 minutes, more preferably 1 to 10 minutes, and even more preferably 2 to 5 minutes, from the viewpoints of productivity and appropriately bringing the thermosetting resin into the B-stage. However, the heating temperature and heating time in the heat drying are conditions that are adjusted depending on the type of material used in the resin layer, the content of the organic solvent, the use of the obtained resin-coated metal foil, etc., and are not limited to the above ranges. The preferred embodiments of the metal foil, the thermosetting resin composition, and the resin layer are as described above.

[0032] <Warping correction treatment> Next, the warp straightening treatment is carried out by passing the resin-coated metal foil prepared above before the warp straightening treatment through a gap between a pair of opposing rolls to apply pressure. Of the pair of rolls, the roll in contact with the metal foil is a resin roll, and the roll in contact with the resin layer is a metal roll.

[0033] The shape of the resin roll and the metal roll is not particularly limited as long as they are rotatable, and examples of such shapes include a cylinder, a cylindrical body, etc. Among these, a cylinder having a perfectly circular cross section is preferred from the viewpoint of the homogeneity of the resulting resin-coated metal foil. Examples of the resin roll include a fluororesin roll, a polyimide resin roll, a polyurethane resin roll, a polyolefin resin roll, etc. Among these, a polyurethane resin roll is preferable. Examples of the metal roll include a stainless steel roll, a chrome molybdenum steel roll, etc. Among these, the stainless steel roll is preferred from the viewpoints of mechanical strength, abrasion resistance, handling properties, etc. The metal roll may be surface-treated from the viewpoint of suppressing scratches and wear on the surface. Examples of the surface treatment method for the metal roll include nickel plating, electroless nickel plating, nickel-boron plating, hard chrome plating, Parker plating, etc. Among these, hard chrome plating is preferable. From the viewpoint of uniformity of the resin-coated metal foil to be obtained, it is preferable that the resin roll and the metal roll both have a smooth surface.

[0034] The roll diameters of the resin roll and the metal roll are not particularly limited, but from the viewpoint of preventing cracks and reducing warping, each is preferably 100 to 500 mm, more preferably 200 to 400 mm, and further preferably 250 to 300 mm.

[0035] The feed speed of the resin-coated metal foil by the resin roll and metal roll is not particularly limited, but from the viewpoints of productivity and warp correction effect, it is preferably 1.0 to 15.0 m / min, more preferably 2.0 to 10.0 m / min, and even more preferably 3.0 to 7.0 m / min.

[0036] The roll load in the warping straightening treatment is not particularly limited, but is preferably 0.3 to 10 tons, more preferably 1 to 8 tons, and further preferably 3 to 7 tons. When the roll load in the warp straightening treatment is equal to or greater than the lower limit, a more excellent warp straightening effect tends to be obtained. On the other hand, when the roll load in the warp straightening treatment is equal to or less than the upper limit, unintended deformation of the resin-coated metal foil due to the load tends to be suppressed.

[0037] The resin roll and the metal roll may have a heat source inside the roll and a mechanism for heating the roll surface. In this case, the resin roll and the metal roll may be heated, but from the viewpoint of suppressing deterioration of the resin-coated metal foil, it is preferable not to heat them. The roll surface temperatures of the resin roll and the metal roll are not particularly limited, but from the viewpoints of productivity and warp correction effect, as well as suppressing deterioration of the resin-coated metal foil, each is preferably 10 to 40°C, more preferably 15 to 35°C, and even more preferably 20 to 30°C.

[0038] The warpage straightening treatment may be a treatment in which the resin-coated metal foil before the warpage straightening treatment is passed through the gap between the pair of opposing rolls only once, or may be a treatment in which the resin-coated metal foil is passed through the gap between the pair of opposing rolls two or more times. When the resin-coated metal foil is passed through the gap between the pair of opposing rolls two or more times, the resin-coated metal foil may be passed through the same rolls or through different rolls.

[0039] [Laminate manufacturing method] The method for producing a laminated board of this embodiment includes a step of forming an insulating layer using the resin-coated metal foil obtained by the method for producing a resin-coated metal foil of this embodiment. The method for producing the laminate of the present embodiment is, for example, a method of laminating the resin-coated metal foil of the present embodiment on a core material such as a prepreg with the resin layer facing the core material side, and then performing heat and pressure molding, whereby the resin layer is cured to form an insulating layer. The heating temperature during hot and pressure molding is preferably 150 to 250°C, more preferably 160 to 220°C, and further preferably 160 to 200°C. The pressure during the hot pressing is preferably 2 to 5 MPa, more preferably 3 to 5 MPa, and even more preferably 3 to 4 MPa. There is no particular limitation on the pressing method, and a multi-stage pressing method may be used. After the hot pressing is completed, the material may be depressurized and cooled. Thereafter, if necessary, the metal foil may be subjected to circuit processing, etching, etc., and further, the steps of laminating another resin-coated metal foil and hot-press molding may be repeated to form a multi-layer structure.

[0040] [Manufacturing method for printed wiring boards] The method for producing a printed wiring board of this embodiment includes a step of forming an insulating layer using the resin-coated metal foil obtained by the method for producing a resin-coated metal foil of this embodiment. The method for producing a printed wiring board of this embodiment is, for example, a method for forming a wiring pattern on a laminate obtained by the above-mentioned method for producing a laminate of this embodiment. Examples of methods for forming a wiring pattern include known methods such as a subtractive method, a full-additive method, a semi-additive method (SAP: Semi Additive Process), and a modified semi-additive method (m-SAP: modified Semi Additive Process).

[0041] [Semiconductor package manufacturing method] The method for manufacturing a semiconductor package according to the present embodiment is a method for manufacturing a semiconductor package in which a semiconductor element is mounted on a printed wiring board obtained by the manufacturing method according to the present embodiment. Specifically, for example, a semiconductor element such as a semiconductor chip or memory is mounted by a known method at a predetermined position on the printed wiring board obtained by the manufacturing method of this embodiment, and the semiconductor element is sealed with a sealing resin or the like. EXAMPLES

[0042] The present embodiment will be specifically described below with reference to examples, although the present embodiment is not limited to the following examples.

[0043] [Crack occurrence] The resin layer of the resin-coated metal foil after warp straightening treatment produced in each example was visually observed, and if any missing resin was confirmed, it was judged as having cracks "present," and if no missing resin was confirmed, it was judged as having cracks "not present."

[0044] [Measurement of warpage] The resin-coated metal foil after warping correction treatment produced in each example was cut into a size of 515 mm x 415 mm, placed on a flat desk, and the height of the warped corners was measured with a ruler. The maximum value of these was evaluated as the amount of warping (mm).

[0045] [Production of Thermosetting Resin Composition] Manufacturing Example 1 The components were mixed in the proportions shown in Table 1, and a thermosetting resin composition with a solid content concentration of 56 mass % was prepared using toluene and methyl isobutyl ketone as organic solvents. The numerical values ​​of the compounding compositions shown in Table 1 are parts by mass of solid content except for the numerical values ​​in parentheses, and are solid content equivalent amounts in the case of solutions (excluding organic solvents) or dispersions. The numerical values ​​in parentheses for the flame retardant indicate the content (unit: mass%) of phosphorus atoms derived from the flame retardant in the solid content of the resin composition excluding the inorganic filler.

[0046] [Table 1]

[0047] [Manufacturing of resin-coated metal foil] Examples 1 to 6, Comparative Examples 1 to 3 The thermosetting resin composition obtained in Production Example 1 was applied onto a roll of copper foil with a carrier foil (manufactured by Mitsui Mining & Smelting Co., Ltd., product name "MT18FL-1.5", width: 540 mm, copper foil thickness: 1.5 μm, carrier foil thickness: 18 μm) and dried by heating at 130° C. for 3 minutes to form a resin layer with a thickness of 20 μm on one side of the copper foil. This copper foil with the resin layer corresponds to the resin-attached metal foil before the warp correction treatment, and was in a warped state toward the resin layer side. The resin-coated metal foils before warping straightening obtained above were pressed through the gap between a pair of rolls shown in Table 2 to obtain resin-coated metal foils A to I after warping straightening. The details of the rolls and pressure conditions shown in Table 2 are as follows. Resin roll: Polyurethane resin roll with a roll diameter of 300 mm Metal roll: Stainless steel roll (hard chrome plated) with a roll diameter of 300 mm Feed speed: 5.0m / min

[0048] Comparative Example 4 A resin-coated metal foil before warping was obtained in the same manner as in Example 1. The resin-coated metal foil before warping was wound around a core material having a diameter of 76.2 mm with the resin layer facing outward, and stored in this state at 25° C. for 5 days to obtain resin-coated metal foil J.

[0049] Comparative Example 5 The resin-coated metal foil before warping correction treatment obtained in the same manner as in Example 1 was cut into a size of 515 mm x 415 mm, 10 sheets were stacked with the resin layer facing up, and vacuum-packed in an aluminum pack. A 30 kg weight with a flat surface larger than the area of ​​the resin-coated metal foil was placed on top of the aluminum pack in which the resin-coated metal foil was packed, in a position where the resin-coated metal foil was contained within the flat surface. The resin-coated metal foil K was stored in this state at 25°C for 5 days.

[0050] Comparative Example 6 The resin-coated metal foil before warping correction treatment obtained in the same manner as in Example 1 was bent 100 to 170° along a stainless steel round bar with a diameter of 7.0 mm. At this time, the resin-coated metal foil was bent in a state where the metal foil was in contact with the round bar. Next, while keeping the resin-coated metal foil bent 100 to 170°, the position of the resin-coated metal foil was slowly slid in the circumferential direction of the round bar fixed so as not to rotate, and the entire surface of the resin-coated metal foil was bent at least once by the round bar. This was the resin-coated metal foil L.

[0051] Comparative Example 7 The resin-coated metal foil before the warp straightening treatment obtained in the same manner as in Example 1 was designated as resin-coated metal foil M.

[0052] The resin-coated metal foils obtained above were evaluated for the presence or absence of cracks and the amount of warping by the above-mentioned methods. The results are shown in Table 2.

[0053] [Table 2]

[0054] As is clear from the results shown in Table 2, the resin-coated metal foils obtained by the manufacturing method of this embodiment, Examples 1 to 6, did not develop cracks and had a reduced amount of warping compared to the resin-coated metal foil of Comparative Example 7, which was not subjected to warping correction treatment. On the other hand, the reduction in the amount of warping was insufficient in the resin-coated metal foils obtained by the methods of Comparative Examples 1 to 5. Moreover, the resin-coated metal foil obtained by the method of Comparative Example 6 had cracks. [Industrial Applicability]

[0055] The manufacturing method of this embodiment is excellent in productivity and can manufacture a resin-coated metal foil with suppressed warping. The resin-coated metal foil obtained by the manufacturing method of this embodiment is easy to handle and is therefore suitable for manufacturing semiconductor packages, and is suitable for semiconductor packages of electronic devices used in computers, information device terminals, etc. that process large amounts of data at high speed. [Explanation of symbols]

[0056] 1 Metal foil 2 Resin layer 3. Peel layer 4 Carrier foil 10, 20 Metal foil with resin

Claims

1. A method for producing a resin-coated metal foil having a metal foil and a resin layer formed on one surface side of the metal foil using a thermosetting resin composition, comprising: A warping correction treatment is included to reduce warping of the resin-coated metal foil, The warpage correction treatment is A process for pressing a resin-coated metal foil having a resin layer formed on one side of the metal foil before warping correction by passing the metal foil through a gap between a pair of opposing rolls, The method for producing a resin-coated metal foil, wherein, of the pair of rolls, the roll that comes into contact with the metal foil is a resin roll, and the roll that comes into contact with the resin layer is a metal roll.

2. The method for producing a resin-coated metal foil according to claim 1 , wherein the metal foil is a copper foil.

3. The method for producing a resin-coated metal foil according to claim 1 or 2, wherein the metal foil has a thickness of 0.1 to 35 μm.

4. The method for producing a resin-coated metal foil according to any one of claims 1 to 3, wherein the resin layer has a thickness of 5 to 70 µm.

5. The method for producing a resin-coated metal foil according to any one of claims 1 to 4, wherein a load applied to the roll in the warping correction treatment is 0.3 to 10 tons.

6. The method for producing a resin-coated metal foil according to any one of claims 1 to 5, wherein the resin roll and the metal roll each have a roll diameter of 100 to 500 mm.

7. The method for producing a resin-coated metal foil according to any one of claims 1 to 6, wherein a feed speed of the pair of rolls is 1.0 to 15.0 m / min.

8. A method for producing a laminate, comprising a step of forming an insulating layer using a resin-coated metal foil obtained by the method for producing a resin-coated metal foil according to any one of claims 1 to 7.

9. A method for producing a printed wiring board, comprising a step of forming an insulating layer using a resin-coated metal foil obtained by the method for producing a resin-coated metal foil according to any one of claims 1 to 7.

10. A method for producing a semiconductor package, comprising mounting a semiconductor element on a printed wiring board obtained by the method for producing a printed wiring board according to claim 9.

Citation Information

Patent Citations

  • Continuous manufacture of one-surface metallic foil lined laminated board

    JP1985189441A

  • Method and device for correcting warpage of one-side metallic-foil lined laminated board for printed circuit substrate

    JP1985260336A

  • Correction of warpage of laminate clad with metallic foil

    JP1990204030A

  • Method for manufacturing metallic foil with resin, and metallic foil with resin